Thermosetting resin composition and cured product
By incorporating a hindered phenolic antioxidant into a thermosetting resin composition with epoxidized lignin, the heat resistance and thermal decomposition temperature of cured products are enhanced, addressing the lower resistance issues of epoxidized lignin-based resins.
Patent Information
- Application Number
- JP2023051897
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The thermal decomposition temperature of cured resins using epoxidized lignin is lower than those using lignin as a curing agent, primarily due to the loss of antioxidant ability from epoxidized lignin, leading to reduced heat resistance.
A thermosetting resin composition is developed by blending epoxidized lignin with a specific antioxidant, such as a hindered phenolic antioxidant having a 3,5-di-tert-butyl-4-hydroxyphenyl group, to enhance heat resistance.
The composition achieves a cured product with improved heat resistance and thermal decomposition temperature, suitable for applications in electrical and electronic materials and fiber-reinforced plastics.
Smart Images

Figure 2024140645000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition containing an epoxy resin made from lignin as a raw material, and a cured product thereof. [Background technology]
[0002] Lignin, obtained by separating cellulose, hemicellulose, etc. from wood, is carbon-neutral and is a plant-derived substance that exists in large quantities, so various technical studies are being conducted to utilize it as a resin raw material to replace petroleum. The structure of lignin varies widely depending on the tree species, habitat, and even its extraction method, but it is generally characterized by being rich in phenolic skeletons. Taking advantage of this characteristic, it is being considered for use as a base and hardener for phenolic resins and epoxy resins as thermosetting resins.
[0003] For example, Patent Document 1 describes a phenolic resin obtained by reacting lignin with a phenol and an aldehyde, a method for producing the same, and a cured product of the phenolic resin. Furthermore, Patent Document 2 describes an epoxy resin obtained by epoxidation through a reaction between a hydroxyl group of lignin and an epihalohydrin, a method for producing the same, and a cured product of the epoxy resin.
[0004] When lignin is used in an epoxy resin cured product, lignin can be blended together with the main agent as a polyphenol-based curing agent, or, as described in Patent Document 2, lignin itself can be epoxidized and the obtained epoxidized lignin can be blended with a curing agent normally used for epoxy resins. A wide variety of curing agents, such as polyamine-based, imidazole-based, acid anhydride-based, and polyphenol-based, are commercially available as curing agents normally used for epoxy resins. By using epoxidized lignin, the blending options are broader than when lignin is used as a polyphenol-based curing agent, making it possible to provide a thermosetting resin composition that can meet a wider variety of characteristics.
[0005] On the other hand, as described in Non-Patent Document 1, the thermal decomposition temperature of the cured resin obtained from epoxidized lignin tends to be lower than that of the cured resin obtained from lignin using lignin as a curing agent as described in Patent Document 1. According to Non-Patent Document 1, this is due to the decomposition of the lignin skeleton in the cured resin. The reason why the thermal decomposition temperature of the cured resin obtained from epoxidized lignin is lowered is thought to be because the phenolic groups derived from lignin function as an antioxidant (radical trapping ability) in the cured resin obtained from epoxidized lignin, while the phenolic groups derived from lignin are epoxidized in the cured resin obtained from epoxidized lignin, and therefore the antioxidant ability is lost. Since the cured resin using lignin is expected to have high heat resistance (glass transition temperature, etc.) derived from the molecular skeleton containing a large amount of phenolic groups of lignin, a method for improving its thermal decomposition resistance is required in order to fully demonstrate its performance. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-199561 A [Patent Document 2] JP 2018-178023 A [Non-patent literature]
[0007] [Non-Patent Document 1] DKShen et al. / Bioresource Technology 101(2010)6136-6146 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention has been made in consideration of the above-mentioned problems of the conventional art. That is, an object of the present invention is to improve the heat resistance of a cured product of a thermosetting resin composition containing an epoxidized lignin as an epoxy resin. [Means for solving the problem]
[0009] As a result of intensive research into solving the above problems, the present inventors have found that a thermosetting resin composition comprising an epoxidized lignin and a curing agent and a specific antioxidant can solve the above problems, and have completed the invention. That is, the gist of the present invention is as follows.
[0010] [1] A thermosetting resin composition comprising (A) an epoxidized lignin obtained by introducing an epoxy group into a hydroxyl group of lignin, (B) a curing agent, and (C) an antioxidant.
[0011] [2] The thermosetting resin composition according to [1], wherein the antioxidant (C) is a hindered phenol-based antioxidant having a 3,5-di-tert-butyl-4-hydroxyphenyl group.
[0012] [3] The thermosetting resin composition according to [1] or [2], characterized in that the content of the antioxidant (C) is 0.2 to 10 parts by mass per 100 parts by mass of the epoxidized lignin (A) obtained by introducing epoxy groups into hydroxyl groups of lignin.
[0013] [4] The thermosetting resin composition according to [3], characterized in that the content of the antioxidant (C) is 0.2 to 1.2 parts by mass per 100 parts by mass of the epoxidized lignin (A) obtained by introducing epoxy groups into hydroxyl groups of lignin.
[0014] [5] The thermosetting resin composition according to any one of [2] to [4], wherein the antioxidant (C) is pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].
[0015] [6] The thermosetting resin composition according to any one of [1] to [5], wherein the (B) curing agent is a polyfunctional amine having two or more amine groups in one molecule.
[0016] [7] A cured product comprising the thermosetting resin composition according to any one of [1] to [6].
[0017] [8] The cured product according to [7], characterized in that the glass transition temperature measured using a thermomechanical analyzer (TMA) is 100°C or higher. Effect of the Invention
[0018] According to the present invention, there are provided a thermosetting resin composition containing an epoxy resin obtained from epoxidized lignin and a curing agent, the resulting cured product having high heat resistance and an improved thermal decomposition temperature, and a cured product thereof. Because of these characteristics, the thermosetting resin composition of the present invention and its cured product can be used in a wide range of fields, such as electrical and electronic materials and FRP (fiber reinforced plastics), and can be put to practical use as an alternative resin raw material to petroleum. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The following describes in detail the embodiments of the present invention; however, the present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention. In this specification, when "~" is used with a numerical value or a physical property value enclosed therein, the values before and after the "~" are included in the expression.
[0020] [Thermosetting resin composition] The thermosetting resin composition of the present invention is characterized by comprising (A) epoxidized lignin obtained by introducing epoxy groups into hydroxyl groups of lignin (hereinafter, may be simply referred to as "(A) epoxidized lignin"), (B) a curing agent, and (C) an antioxidant.
[0021] [(A) Epoxidized lignin] The epoxidized lignin (A) used in the present invention is obtained by reacting lignin obtained by separating cellulose, hemicellulose, etc. from wood with epihalohydrin using its hydroxyl group as a reaction point. The raw wood species, structure, and production method of the lignin used as the raw material of the epoxidized lignin are not particularly limited, but since epoxidation is performed by reaction with epihalohydrin, it usually has solubility in epihalohydrin. Among them, from the viewpoint of productivity, those having a solubility in epihalohydrin of 100 g / L or more are preferred, and those having a solubility in epichlorohydrin of 100 g / L or more are particularly preferred.
[0022] The lower limit of the epoxy equivalent of the epoxidized lignin (A) used in the present invention is not particularly limited, but is usually 200 g / mol or more, preferably 250 g / mol or more, and more preferably 300 g / mol or more. If the epoxy equivalent is equal to or more than the above lower limit, it is possible to increase the proportion of biomass-derived substances in the thermosetting resin composition. The upper limit of the epoxy equivalent of the epoxidized lignin (A) used in the present invention is not particularly limited, but from the viewpoints of compatibility with other materials and the crosslink density of the resulting cured product, it is usually 200,000 g / mol, preferably 100,000 g / mol, and more preferably 50,000 g / mol. The epoxy equivalent of (A) epoxidized lignin is a value measured by the method described in the Examples section below.
[0023] [(B) Hardener] The curing agent (B) used in the present invention is a substance that contributes to the crosslinking reaction and / or chain extension reaction between epoxy groups of an epoxy compound. In the present invention, even substances that are usually called "curing accelerators" are considered to be curing agents as long as they contribute to the crosslinking reaction and / or chain extension reaction between epoxy groups of an epoxy compound.
[0024] As the (B) curing agent, it is preferable to use at least one selected from the group consisting of polyfunctional phenols, polyisocyanate compounds, amine compounds, acid anhydride compounds, imidazole compounds, amide compounds, cationic polymerization initiators, and organic phosphines. As the (B) curing agent, phosphonium salts and tetraphenylboronic acid can also be used.
[0025] Examples of polyfunctional phenols include bisphenols such as bisphenol A, bisphenol F, bisphenol S, bisphenol B, bisphenol AD, bisphenol Z, and tetrabromobisphenol A; biphenols such as 4,4'-biphenol and 3,3',5,5'-tetramethyl-4,4'-biphenol; catechol, resorcin, hydroquinone, and dihydroxynaphthalenes; and compounds in which the hydrogen atoms bonded to the aromatic rings of these compounds are substituted with non-interfering substituents such as halogen groups, alkyl groups, aryl groups, ether groups, ester groups, and organic substituents containing hetero elements such as sulfur, phosphorus, and silicon. Further examples include novolaks and resols which are polycondensates of these phenols, or monofunctional phenols such as phenol, cresol, and alkylphenols with aldehydes.
[0026] Examples of polyisocyanate compounds include polyisocyanate compounds such as tolylene diisocyanate, methylcyclohexane diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, dimer acid diisocyanate, trimethylhexamethylene diisocyanate, lysine triisocyanate, etc. Furthermore, polyisocyanate compounds obtained by reacting these polyisocyanate compounds with compounds having at least two active hydrogen atoms such as amino groups, hydroxyl groups, carboxyl groups, water, etc., or trimers to pentamers of the above polyisocyanate compounds, etc., can be mentioned.
[0027] Examples of the amine compounds include aliphatic primary, secondary, and tertiary amines, aromatic primary, secondary, and tertiary amines, cyclic amines, guanidines, and urea derivatives. Specific examples include triethylenetetramine, diaminodiphenylmethane, diaminodiphenyl ether, m-xylylenediamine, dicyandiamide, 1,8-diazabicyclo(5,4,0)-7-undecene, 1,5-diazabicyclo(4,3,0)-5-nonene, dimethylurea, and guanylurea.
[0028] Examples of the acid anhydride compound include phthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, and condensates of maleic anhydride and unsaturated compounds.
[0029] Examples of the imidazole-based compound include 1-isobutyl-2-methylimidazole, 2-methylimidazole, 1-benzyl-2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, benzimidazole, etc. Although the imidazole-based compound also functions as a curing accelerator, which will be described later, in the present invention it is classified as a curing agent.
[0030] Examples of the amide-based compounds include dicyandiamide and its derivatives, polyamide resins, and the like.
[0031] The cationic polymerization initiator generates cations by heat or irradiation with active energy rays, and examples of the initiator include aromatic onium salts. - , BF4 - , AsF6 - , PF6 - , CF3SO3 2- , B(C6F5)4 - and an aromatic cation component containing an atom of iodine, sulfur, nitrogen, phosphorus, etc. Diaryliodonium salts and triarylsulfonium salts are particularly preferred.
[0032] Examples of the organic phosphines include tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine.
[0033] Examples of the phosphonium salt include tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium ethyltriphenylborate, and tetrabutylphosphonium tetrabutylborate. Examples of tetraphenylboron salts include 2-ethyl-4-methylimidazole·tetraphenylborate, and N-methylmorpholine·tetraphenylborate.
[0034] In addition to the above-mentioned curing agents, for example, mercaptan compounds, organic acid dihydrazides, boron halide amine complexes, etc. can also be used as curing agents in the thermosetting resin composition of the present invention.
[0035] These curing agents may be used alone or in combination of two or more.
[0036] Of these curing agents, the curing agent (B) used in the present invention is preferably an amine compound, particularly a polyfunctional amine having two or more amine groups in one molecule, from the viewpoint of compatibility and reactivity with epoxidized lignin, and in particular a polyfunctional amine having an aromatic ring, such as m-xylylenediamine.
[0037] The content of the (B) curing agent in the thermosetting resin composition of the present invention is preferably 0.1 to 1000 parts by mass, more preferably 100 parts by mass or less, even more preferably 80 parts by mass or less, and particularly preferably 60 parts by mass or less, relative to 100 parts by mass of the total epoxy compound components as solid contents in the thermosetting resin composition of the present invention.
[0038] In the present invention, the term "solid content" means components excluding the solvent, and includes not only solid epoxy compounds but also semi-solid and viscous liquid substances. Furthermore, the term "total epoxy compound components" refers to (A) epoxidized lignin when the thermosetting resin composition of the present invention contains only epoxidized lignin (A) as an epoxy compound, and refers to the sum of (A) epoxidized lignin and epoxy compounds other than (A) epoxidized lignin when the thermosetting resin composition of the present invention contains epoxy compounds other than epoxidized lignin (A) described below.
[0039] More preferred amounts of the curing agent are as described below depending on the type of the curing agent.
[0040] When a polyfunctional phenol, an amine compound, or an acid anhydride compound is used as a curing agent, it is preferable to use it so that the equivalent ratio of the functional groups in the curing agent (the hydroxyl groups of the polyfunctional phenol, the amino groups of the amine compound, or the acid anhydride groups of the acid anhydride compound) to the total epoxy groups in the thermosetting resin composition is in the range of 0.8 to 1.5. When a polyisocyanate compound is used as the (B) curing agent, the number of isocyanate groups in the polyisocyanate compound relative to the number of hydroxyl groups in the thermosetting resin composition is preferably used in an equivalent ratio within the range of 1:0.01 to 1:1.5. When an imidazole-based compound is used as the (B) curing agent, it is preferably used in the range of 0.5 to 10 parts by mass per 100 parts by mass of the total epoxy compound components as solid contents in the thermosetting resin composition. When an amide compound is used as the (B) curing agent, it is preferably used in an amount of 0.1 to 20 mass % based on the total amount of all epoxy compound components and amide compound as solid contents in the thermosetting resin composition. When a cationic polymerization initiator is used as the (B) curing agent, it is preferably used in the range of 0.01 to 15 parts by mass per 100 parts by mass of the total epoxy compound components as solid contents in the thermosetting resin composition. When an organic phosphine is used as the (B) curing agent, it is preferably used in an amount of 0.1 to 20 mass % based on the total amount of all epoxy compound components and the organic phosphines as solid contents in the thermosetting resin composition.
[0041] [(C) Antioxidants] The (C) antioxidant is not particularly limited, but preferred examples include hindered phenol-based antioxidants, and in particular, hindered phenol-based antioxidants having a 3,5-di-tert-butyl-4-hydroxyphenyl group. A hindered phenol-based antioxidant, in particular a hindered phenol-based antioxidant having a 3,5-di-tert-butyl-4-hydroxyphenyl group, can be uniformly mixed well with the thermosetting resin composition of the present invention, and can effectively improve the heat resistance of a cured product made of the thermosetting resin composition of the present invention.
[0042] Specific examples of hindered phenol-based antioxidants include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesityle) 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl -4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, and the like.
[0043] Among them, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Commercially available products of such phenolic antioxidants include "Irganox (registered trademark) 1010", "Irganox (registered trademark) 1076", and "Irganox (registered trademark) 1135" manufactured by BASF, and "Adeka STAB (registered trademark) AO-50" and "Adeka STAB (registered trademark) AO-60" manufactured by ADEKA.
[0044] These (B) curing agents may be used alone or in any combination of two or more in any ratio.
[0045] The content of the (C) antioxidant in the thermosetting resin composition of the present invention is not particularly limited, but is preferably 0.2 to 10 parts by mass, particularly 0.25 parts by mass, and particularly 0.2 to 1.2 parts by mass, relative to 100 parts by mass of the (A) epoxidized lignin. If the content of the (C) antioxidant is equal to or greater than the above lower limit, the effect of improving heat resistance due to the inclusion of the (C) antioxidant can be sufficiently obtained. On the other hand, if the content of the (C) antioxidant is equal to or less than the above upper limit, the deterioration of the physical properties of the resulting cured product due to the inhibition of the curing reaction caused by the (C) antioxidant itself reacting with the epoxy group can be suppressed.
[0046] [Other epoxy compounds] The thermosetting resin composition of the present invention may contain an epoxy compound other than the above-mentioned (A) epoxidized lignin (sometimes referred to as "other epoxy compounds" in this specification). Examples of other epoxy compounds include glycidyl ether type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, biphenyl type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, tetrabromobisphenol A type epoxy resins, and other polyfunctional phenol type epoxy resins, epoxy resins obtained by hydrogenating the aromatic rings of the above aromatic epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, linear aliphatic epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. The above-listed other epoxy compounds may be used alone or in combination of two or more.
[0047] When the thermosetting resin composition of the present invention contains (A) epoxidized lignin and other epoxy compounds, the ratio of the other epoxy compounds in the total epoxy compound components as solids in the thermosetting resin composition is preferably 1% by mass or more, more preferably 5% by mass or more, and on the other hand, preferably 50% by mass or less, more preferably 30% by mass or less. By the ratio of the other epoxy compounds being equal to or more than the above lower limit, the effect of improving the physical properties by blending the other epoxy compounds can be sufficiently obtained. On the other hand, by the ratio of the other epoxy compounds being equal to or less than the above upper limit, the effect of effectively utilizing resin raw materials instead of petroleum by using (A) epoxidized lignin can be obtained, and the effect of improving heat resistance by blending the above-mentioned (C) antioxidant can be significantly obtained.
[0048] [solvent] The thermosetting resin composition of the present invention may be diluted by blending a solvent in order to appropriately adjust the viscosity of the thermosetting resin composition when handling it during the formation of a coating film, etc. In the thermosetting resin composition of the present invention, the solvent is used to ensure the handleability and workability in molding the thermosetting resin composition, and there is no particular restriction on the amount of the solvent used. The solvent that the thermosetting resin composition of the present invention may contain is not particularly limited, but is usually an organic solvent.
[0049] Examples of the organic solvent include aromatic solvents, ketone solvents, amide solvents, glycol ether solvents, halogen solvents, etc. Specific examples of aromatic solvents include benzene, toluene, xylene, etc. Specific examples of ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, 2-heptanone, 4-heptanone, 2-octanone, cyclopentanone, cyclohexanone, acetylacetone, etc. Specific examples of amide solvents include formamide, N-methylformamide, N,N-dimethylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, 2-pyrrolidone, N-methylpyrrolidone, etc. Specific examples of glycol ether solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol dimethyl ether, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol dimethyl ether, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether, propylene glycol mono-n-butyl ether, propylene glycol monomethyl ether acetate, etc. Specific examples of halogen-based solvents include chloroform, dichloromethane, 1,1,2,2-tetrachloroethane, etc. The above-mentioned solvents may be used alone or in combination of two or more.
[0050] [Other ingredients] The thermosetting resin composition of the present invention may contain other components in addition to the components listed above. Examples of other components include curing accelerators (excluding those corresponding to the above-mentioned curing agents), coupling agents, flame retardants, light stabilizers, plasticizers, reactive diluents, pigments, inorganic fillers, organic fillers, etc. The other components listed above may be used in appropriate combinations depending on the desired physical properties of the thermosetting resin composition.
[0051] [Cured product] A cured product can be obtained by curing the thermosetting resin composition of the present invention. The term "curing" as used herein means intentionally curing an epoxy compound by heat and / or light or the like, and the degree of curing may be controlled depending on the desired physical properties and applications.
[0052] The method of curing the thermosetting resin composition of the present invention to obtain a cured product varies depending on the components and amounts of the components in the thermosetting resin composition and the form of the components, but typically includes heating conditions of 5 seconds to 180 minutes at 50 to 200° C. This heating is preferably performed in two stages, namely, primary heating at 50 to 160° C. for 5 seconds to 120 minutes and secondary heating at 90 to 200° C., which is 40 to 120° C. higher than the primary heating temperature, for 1 minute to 180 minutes, in order to reduce poor curing.
[0053] When producing a cured product as a semi-cured product, the curing reaction of the thermosetting resin composition may be allowed to proceed to an extent that the shape can be maintained by heating, etc. When the thermosetting resin composition contains a solvent, most of the solvent is removed by techniques such as heating, decompression, and air drying, but 5% by mass or less of the solvent may remain in the semi-cured product.
[0054] [Application] The thermosetting resin composition of the present invention is capable of effectively utilizing resin raw materials that can replace petroleum and gives cured products with excellent heat resistance, and therefore can be suitably used in a wide range of fields, such as coating materials, electric and electronic materials, adhesives, and fiber reinforced plastics (FRP). EXAMPLES
[0055] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples. Note that the values of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values of the examples.
[0056] [Measurement and evaluation method] The measurement and evaluation methods in the following Production Examples, Examples and Comparative Examples are as follows.
[0057] <Epoxy equivalent of epoxidized lignin> The epoxy equivalent of the epoxidized lignin produced in the production examples was measured using an internal standard substance. 1 The epoxidized lignin and 1,1,2,2-tetrachloroethane (TCE) as an internal standard were dissolved in deuterated chloroform. 1 H-NMR (Bruker Ascend MMR 400) measurements were performed. The epoxy equivalent of the epoxidized lignin was calculated from the signal intensity of each structural unit and the following formula (1). Note that 167.85 in formula (1) is the molecular weight of TCE. Epoxy equivalent (g / mol) = (A / B) × (D / C) × 167.85 (1) A: Weight of epoxidized lignin (mg) B: 1 Integral value of epoxy group proton signals (2.6-3.0 ppm) on H-NMR spectrum C: Weight of TCE (mg) D: 1 Integral value of TCE proton signals (5.9-6.0 ppm) on H-NMR spectrum
[0058] <5% mass loss temperature (Td5)> Approximately 5 mg of a measurement sample was cut out from each of the cured products (samples) obtained in the Examples and Comparative Examples, and measurements were carried out under the following conditions. The temperature at which the mass decreased by 5% from the start of the temperature rise was determined as the 5% mass loss temperature (Td5). Equipment: Rigaku Corporation Differential thermal and thermogravimetric simultaneous measurement equipment "TG-DTA8812" Sample weighing pan: Aluminum Measurement atmosphere gas: Nitrogen (flow rate 300 mL / min) Measurement temperature: 35℃~550℃ Heating rate: 10℃ / min
[0059] <Glass transition temperature (Tg)> Using the cured products (samples) obtained in the examples and comparative examples, TMA measurements were performed under the following conditions. The extrapolated onset temperature of the TMA curve (the point where the linear extrapolation of the region before and after the slope of the TMA curve changes with the glass transition intersects) was determined as the glass transition temperature (Tg). If no change in slope of the TMA curve was observed within the measurement temperature range, the Tg was determined to be higher than 150°C. Equipment: Thermomechanical analyzer "TMA7100" manufactured by Hitachi High-Tech Science Co., Ltd. Probe material: Quartz Measurement mode: Compression mode Load: 100 mN / m 2 Measurement temperature: 30℃~180℃ Heating rate: 10℃ / min
[0060] [raw materials] The raw materials used in the following Production Examples, Examples and Comparative Examples are as follows.
[0061] <Lignin 1> SIP lignin SIP-R559-PEG200 is a lignin produced under the Strategic Innovation Creation Program (next-generation agriculture, forestry and fisheries creative technology) "Development of high value-added materials from wood lignin, etc." (SIP lignin).
[0062] <Lignin 2> Bloom Lignin Oligomer Modified Lignin is a lignin manufactured by Bloom.
[0063] <Hardening agent> MXDA: m-Xylylenediamine (Tokyo Chemical Industry Co., Ltd.) 2E4MZ: 2-ethyl-4-methylimidazole (Tokyo Chemical Industry Co., Ltd.)
[0064] <Reference Example Epoxy Compound> Bisphenol A type epoxy resin "jER828" (Mitsubishi Chemical Corporation)
[0065] <Antioxidants> Hindered phenol antioxidant "Irganox (registered trademark) 1010" (manufactured by BASF) (Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate])
[0066] [Production Example 1: Synthesis of epoxidized lignin 1] In a 200 mL test tube containing a stirrer tip, 3 g of SIP lignin SIP-R559-PEG200, 30 mL of epichlorohydrin, 15 mL of isopropanol, 4.11 mL of a 10% by weight aqueous solution of tetramethylammonium chloride, and 4.73 mL of pure water were charged, and an adapter was connected. The mixture was stirred while being heated to 40°C to dissolve uniformly, and stirred at 40°C for 1 hour. Then, 2.62 mL of a 10% by weight aqueous solution of sodium hydroxide was dropped, the mixture was heated to 65°C, and heated and stirred for 6 hours. Then, the mixture was washed three times with 100 mL of water to remove inorganic salts. The obtained oil layer was evaporated, and then vacuum dried at 110°C for 2 hours to obtain a brown powder. The epoxy equivalent of the obtained sample: epoxidized lignin 1 is 1 The molecular weight was determined to be 888 g / mol by H-NMR measurement.
[0067] [Production Example 2: Synthesis of epoxidized lignin 2] In a 200 mL test tube containing a stirrer tip, Bloom's lignin oligomer modified lignin: 3 g, epichlorohydrin: 30 mL, isopropanol: 15 mL, 10 mass% aqueous solution of tetramethylammonium chloride: 4.11 mL, and pure water: 4.73 mL were charged, an adapter was connected, and the mixture was stirred while heating to 40 ° C. to dissolve uniformly, and stirred at 40 ° C. for 1 hour. Then, 2.62 mL of a 10 mass% aqueous solution of sodium hydroxide was dropped, the temperature was raised to 65 ° C., and heating and stirring were continued for 6 hours. Then, the mixture was washed with 100 mL of water three times to remove inorganic salts. The obtained oil layer was evaporated, and then vacuum dried at 110 ° C. for 2 hours to obtain a viscous dark brown substance. The epoxy equivalent of the obtained sample: epoxidized lignin 2 is 1 The molecular weight was determined to be 435 g / mol by H-NMR measurement.
[0068] [Example 1] Epoxidized lignin 1:100 parts by mass, MXDA:11.36 parts by mass, Irganox 1010:0.36 parts by mass were dissolved in chloroform:600 parts by mass to prepare a homogeneous solution of chloroform. This was applied to a silicone-coated PET film, and the chloroform was dried to obtain a brown cast film. This cast film was heated and cured at 70°C for 1 hour, then cut with a cutter knife, and five sheets were stacked, and then heated and cured at 150°C for 1 hour to obtain a brown cured product with a thickness of 0.944 mm.
[0069] [Example 2] A thermosetting resin composition and a cured product were obtained in the same manner as in Example 1 using 100 parts by mass of epoxidized lignin 1, 7.6 parts by mass of MXDA, and 0.98 parts by mass of Irganox 1010. The exact amounts of each component and the thickness of the resulting cured product are shown in Table 1.
[0070] [Example 3] A thermosetting resin composition and a cured product were obtained in the same manner as in Example 1 using 100 parts by mass of epoxidized lignin 2, 23.4 parts by mass of MXDA, and 1.20 parts by mass of Irganox 1010. The exact amounts of each component and the thickness of the resulting cured product are shown in Table 1.
[0071] [Example 4] A thermosetting resin composition and a cured product were obtained in the same manner as in Example 1 using 100 parts by mass of epoxidized lignin 1, 10 parts by mass of 2E4MZ, and 0.44 parts by mass of Irganox 1010. The exact amounts of each component and the thickness of the resulting cured product are shown in Table 1.
[0072] [Example 5] A thermosetting resin composition and a cured product were obtained in the same manner as in Example 1 using 100 parts by mass of epoxidized lignin 1, 20 parts by mass of 2E4MZ, and 0.22 parts by mass of Irganox 1010. The exact amounts of each component and the thickness of the resulting cured product are shown in Table 1.
[0073] [Comparative Examples 1 to 5] Thermosetting resin compositions and cured products were obtained in accordance with Examples 1 to 5, respectively, except that Irganox 1010 was not added in Examples 1 to 5. The exact amounts of each component and the thickness of the resulting cured product are shown in Table 1.
[0074] [Reference example 1] A thermosetting resin composition and a cured product were obtained in the same manner as in Example 1 using 100 parts by mass of jER828, 34 parts by mass of MXDA, and 0.20 parts by mass of Irganox 1010. The exact amounts of each component and the thickness of the resulting cured product are shown in Table 1.
[0075] [Reference example 2] A thermosetting resin composition and a cured product were obtained in the same manner as in Reference Example 1, except that Irganox 1010 was not added. The exact amounts of each component and the thickness of the resulting cured product are shown in Table 1.
[0076] [Heat resistance evaluation] For the cured products obtained in Examples 1 to 5, Comparative Examples 1 to 5, and Reference Examples 1 and 2, the 5% mass loss temperature (Td5) and glass transition temperature (Tg) were measured as described above. The results are shown in Table 1.
[0077] [Table 1]
[0078] [Evaluation Results] A comparison of Reference Examples 1 and 2 reveals that when jER828, a petroleum-derived epoxy resin, is used, the 5% mass loss temperature (Td5) decreases when 0.2 parts by mass of Irganox 1010 is added. The reason for this result is presumed to be as follows. Hindered phenol compounds such as Irganox 1010 are themselves reactive with epoxy groups, and some of them react with the epoxy groups, inhibiting the original curing reaction. This causes unreacted curing agent to remain in the cured product, which volatilizes when heated, lowering the 5% mass loss temperature (Td5).
[0079] On the other hand, the results of each of the Examples and Comparative Examples showed that in the cured material using epoxidized lignin, the 5% mass loss temperature (Td5) increased with the addition of Irganox 1010. The reason for this is unclear, but it is thought that when epoxidized lignin is used, the inhibition of the hardening reaction as shown in the Reference Example is less likely to occur. These results show that by blending an antioxidant (C) with a thermosetting resin composition containing an epoxidized lignin (A) and a curing agent (B), it is possible to obtain an effect specific to the epoxidized lignin (A), namely, improvement in heat resistance, specifically, improvement in the thermal decomposition temperature.
Claims
1. A thermosetting resin composition comprising (A) an epoxidized lignin obtained by introducing an epoxy group into a hydroxyl group of lignin, (B) a curing agent, and (C) an antioxidant.
2. 2. The thermosetting resin composition according to claim 1, wherein the antioxidant (C) is a hindered phenol-based antioxidant having a 3,5-di-tert-butyl-4-hydroxyphenyl group.
3. The thermosetting resin composition according to claim 1, characterized in that the content of the antioxidant (C) is 0.2 to 10 parts by mass per 100 parts by mass of the epoxidized lignin (A) obtained by introducing an epoxy group into a hydroxyl group of lignin.
4. The thermosetting resin composition according to claim 3, characterized in that the content of the antioxidant (C) is 0.2 to 1.2 parts by mass per 100 parts by mass of the epoxidized lignin (A) obtained by introducing an epoxy group into a hydroxyl group of lignin.
5. 3. The thermosetting resin composition according to claim 2, wherein the antioxidant (C) is pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].
6. 2. The thermosetting resin composition according to claim 1, wherein the curing agent (B) is a polyfunctional amine having two or more amine groups in one molecule.
7. A cured product comprising the thermosetting resin composition according to any one of claims 1 to 6.
8. The cured product according to claim 7, characterized in that the glass transition temperature measured using a thermomechanical analyzer (TMA) is 100°C or higher.
Citation Information
Patent Citations
Friction material
JP2013199561A
Method for producing lignin-derived epoxy resin, lignin-derived epoxy resin, epoxy resin composition and cured product thereof
JP2018178023A