Culture vessel for adhesive cells and culture method for adhesive cells using the same

A culture container with a polymer surface containing alicyclic structures and controlled oxygen and π-π transitions enhances cell cluster formation by promoting adherent cell adhesion, addressing the limitations of conventional methods.

JP2024140707APending Publication Date: 2024-10-10ZEON CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023052006
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional methods for culturing adherent cells to form cell clusters have limitations in increasing the proportion of cells that form cell clusters, also known as the cell cluster formation rate.

Method used

A culture container with a culture surface made of a polymer composition containing an alicyclic structure-containing polymer, where the amount of surface oxygen and π-π transitions is less than 1 atomic%, enhancing the cell cluster formation rate.

Benefits of technology

The culture container and method significantly improve the cell cluster formation rate by ensuring adequate adhesion of adherent cells to form clusters without excessive scaffold protein adsorption, leading to higher cell mass formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140707000001
    Figure 2024140707000001
  • Figure 2024140707000002
    Figure 2024140707000002
  • Figure 2024140707000003
    Figure 2024140707000003
Patent Text Reader

Abstract

To provide a culture vessel for adhesive cells with a high rate of cell cluster formation, and a culture method for adhesive cells using the culture vessel.SOLUTION: A culture vessel for adhesive cells has a culture face composed of a polymer composition that comprises an alicyclic structure-containing polymer. As measured by X-ray photoelectron spectroscopy, the total of the surface oxygen levels (atom%) and π-π* transition levels (atom%) on the cultured face is less than 1 atom%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a culture vessel for adherent cells and a method for culturing adherent cells using the same. [Background technology]

[0002] In recent years, cell clusters consisting of multiple adherent cells have been attracting attention in the field of regenerative medicine. Such cell clusters can be used for applications such as organ regeneration, organoid culture, and drug screening.

[0003] Therefore, in recent years, attempts have been made to improve the culture method of adhesive cells capable of forming cell clusters. Specifically, Patent Document 1 discloses a method for culturing adherent cells, including a step of culturing the adherent cells in a state adhered to the bottom surface of a culture vessel or suspended in a liquid medium by contacting the adherent cells with an alicyclic structure-containing polymer body, a step of forming cell masses of the adherent cells cultured in the suspended state and culturing them in the suspended state, and a step of culturing the cell masses cultured in the suspended state in a state adhered to the bottom surface of a culture vessel. According to Patent Document 1, by using this culture method, cell death is not promoted even when cell masses are formed, and protein production ability is improved. In addition, Patent Document 2 states that the albumin adsorption amount on the cell culture surface is 830 ng / cm 2 According to Patent Document 2, by using the adhesive cell culture substrate, spheroids can be formed in an attached state on the substrate surface without the need for nanoimprinting of a concave-convex structure, even after gamma ray sterilization. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-79658 A [Patent Document 2] JP 2017-77240 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the above-mentioned conventional techniques have room for improvement in terms of further increasing the ratio of adherent cells that form cell clusters (ie, cell cluster formation rate).

[0006] Therefore, an object of the present invention is to provide a culture vessel for adherent cells that has an excellent cell aggregate formation rate, and a method for culturing adherent cells using the culture vessel. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems. The present inventors have developed a method for detecting the amount of surface oxygen and the amount of π-π on a culture surface comprising a culture surface comprising a polymer composition containing an alicyclic structure-containing polymer. * The inventors have found that an adhesive cell culture vessel having a total transition amount of less than 1 atomic % has an excellent cell aggregate formation rate, and have completed the present invention.

[0008] That is, the present invention aims to advantageously solve the above-mentioned problems, and provides the following (1) culture vessel for adherent cells and the following (2) to (4) methods for culturing adherent cells.

[0009] (1) A culture vessel for adherent cells having a culture surface formed using a polymer composition containing an alicyclic structure-containing polymer, wherein the surface oxygen amount (atomic %) and π-π * A culture vessel for adherent cells, in which the total transition amount (atomic %) is less than 1 atomic %. A culture surface is provided using a polymer composition containing an alicyclic structure-containing polymer, and the surface oxygen amount and π-π * An adherent cell culture vessel (hereinafter sometimes simply abbreviated as "culture vessel") in which the total transition amount is less than 1 atomic % is excellent in cell aggregate formation rate. In the present invention, the term "culture surface" refers to the surface of a culture vessel to which adherent cells can adhere during culture. In the present invention, the "surface oxygen amount" and "π-π * The "transition amount" can be measured using the method described in the Examples of this specification.

[0010] (2) A method for culturing adherent cells using the culture vessel for adherent cells described in (1) above. The method for culturing adherent cells using the above-mentioned culture vessel (hereinafter sometimes simply abbreviated as "culturing method") is excellent in the rate of cell aggregate formation.

[0011] (3) A method for culturing adherent cells described in (2) above, comprising a cell cluster formation step in which adherent cells form cell clusters on the culture surface, and a culture step in which the cell clusters are cultured in a state adhered to the culture surface. By using the culture method including the above-mentioned cell cluster formation step and culture step, the cell cluster formation rate can be further increased. In the present invention, the term "cell mass" refers to a cell mass other than a single cell, and refers to a state in which two or more cells are bound together.

[0012] (4) The method for culturing adherent cells according to (3) above, further comprising an adhesion step of adhering the adherent cells to the culture surface prior to the cell cluster formation step. If a culture method further including the adhesion step described above is used prior to the cell cluster formation step, the cell cluster formation rate can be further increased. Effect of the Invention

[0013] According to the present invention, it is possible to provide a culture vessel for adherent cells which has an excellent cell aggregate formation rate, and a method for culturing adherent cells using the culture vessel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail. Here, the culture vessel of the present invention is not particularly limited as long as it is intended to culture adherent cells therein. Specific examples of the culture vessel of the present invention include dishes, plates, microchannel chips, bags, tubes, scaffolds, cups, jar fermenters, etc. The culture method of the present invention is characterized by using the culture vessel of the present invention.

[0015] The adhesive cells contained in the culture vessel of the present invention are not particularly limited and can be selected arbitrarily according to the purpose.Specific examples include fat cells, liver cells, kidney cells, pancreatic cells, mammary gland cells, endothelial cells, epithelial cells, smooth muscle cells, myoblasts, cardiac muscle cells, nerve cells, glial cells, Schwann cells, dendritic cells, chondrocytes, osteoblasts, osteoclasts, osteocytes, fibroblasts, various blood system cells, retinal cells, cornea-derived cells, gonad-derived cells, various fibrocytes, other mesenchymal precursor cells, various cancer cells (e.g., lung cancer cells, breast cancer cells, pancreatic cancer cells, etc.), etc.Among these, kidney cells, cardiac muscle cells, Schwann cells, and cancer cells are preferred. The adhesive cells may be used alone or in combination of two or more types in any ratio.

[0016] (Adhesive cell culture container) At least the culture surface of the culture vessel of the present invention is formed using a polymer composition containing an alicyclic structure-containing polymer. For example, when the culture vessel of the present invention is a multi-well plate, the bottom surface of the inside of the well may be formed using the polymer composition. When the culture vessel of the present invention is a bag having a laminated structure consisting of multiple films, the innermost film (the inner surface of the bag) may be formed using the polymer composition. Alternatively, the entire culture vessel may be formed using the polymer composition. Here, the culture vessel of the present invention has a surface oxygen amount on the culture surface and a π-π * The total amount of transitions is less than 1 atomic %.

[0017] The culture vessel of the present invention has a surface oxygen amount on the culture surface and a π-π *Since the total transition amount is less than 1 atomic %, the use of the culture vessel can improve the cell aggregate formation rate. Although the reason why the above-mentioned effect is obtained by using the culture vessel of the present invention is not clear, it is presumed to be as follows.

[0018] First, the culture vessel of the present invention has a culture surface made of a polymer composition containing an alicyclic structure-containing polymer, and the surface oxygen amount and π-π * The total transition amount is less than 1 atomic %. It is known that adhesive cells usually adhere to the culture surface via scaffold proteins adsorbed on the culture surface. The surface oxygen amount and π-π * The present inventors have newly clarified that the higher the total transition amount, the higher the amount of scaffold protein adsorbed onto the culture surface. * When the total transition amount is high, the scaffold protein is present on the culture surface in sufficient amounts, so that the adherent cells can adhere well to the culture surface without forming cell aggregates. On the other hand, the surface oxygen amount and π-π * When the total transition amount is low, there is not enough scaffold protein on the culture surface, so the adherent cells cannot adhere to the culture surface as it is, and they try to adhere to the culture surface by forming cell clusters. * Since the total transition amount is less than 1 atomic %, there is insufficient scaffold protein on the culture surface, and the adherent cells adhere to the culture surface by forming cell clusters. Therefore, it is considered that culturing adherent cells using the culture vessel of the present invention improves the ratio of the number of cell clusters to the total number of cells in the culture vessel (i.e., cell cluster formation rate). Therefore, by using the culture vessel of the present invention, the cell aggregate formation rate can be improved.

[0019] <Polymer Composition> The polymer composition used to form the culture surface of the culture vessel of the present invention contains an alicyclic structure-containing polymer, and optionally further contains components other than the alicyclic structure-containing polymer (other components).

[0020] <<Polymer containing alicyclic structure>> The alicyclic structure-containing polymer is a resin having an alicyclic structure in the main chain and / or side chain, and from the viewpoint of further increasing the cell mass formation rate, it is preferable that the main chain contains an alicyclic structure, and it is more preferable that the main chain does not have a polar group. Here, the polar group refers to a polar atomic group. Examples of the polar group include an amino group, a carboxyl group, a hydroxyl group, and an acid anhydride group. The alicyclic structure-containing polymers may be used alone or in combination of two or more.

[0021] Examples of the alicyclic structure include a saturated cyclic hydrocarbon (cycloalkane) structure and an unsaturated cyclic hydrocarbon (cycloalkene) structure. From the viewpoints of mechanical strength, heat resistance, and the like, a cycloalkane structure or a cycloalkene structure is preferred, and among these, those having a cycloalkane structure are most preferred.

[0022] The number of carbon atoms constituting the alicyclic structure is not particularly limited, but is usually 4 to 30, preferably 5 to 20, and more preferably 5 to 15. When the number of carbon atoms constituting the alicyclic structure is within this range, the mechanical strength, heat resistance, and moldability are highly balanced, which is preferable.

[0023] The proportion of repeating units having an alicyclic structure in the alicyclic structure-containing polymer may be appropriately selected according to the intended use, but is usually 30% by weight or more, preferably 50% by weight or more, more preferably 70% by weight or more. If the proportion of repeating units having an alicyclic structure in the alicyclic structure-containing polymer is too small, the heat resistance is poor, which is not preferable. The remainder other than the repeating units having an alicyclic structure in the alicyclic structure-containing polymer is not particularly limited and may be appropriately selected according to the intended use.

[0024] Specific examples of the alicyclic structure-containing polymer include (1) norbornene-based polymers, (2) monocyclic olefin-based polymers, (3) cyclic conjugated diene-based polymers, (4) vinyl alicyclic hydrocarbon-based polymers, and hydrogenated products of (1) to (4), etc. Among these, norbornene-based polymers and hydrogenated products thereof are preferred from the viewpoint of further increasing the cell mass formation rate.

[0025] [Norbornene polymer] Norbornene polymers are obtained by polymerizing norbornene monomers, which are monomers having a norbornene skeleton, and are roughly classified into those obtained by ring-opening polymerization and those obtained by addition polymerization.

[0026] Examples of the products obtained by ring-opening polymerization include ring-opening polymers of norbornene-based monomers, ring-opening polymers of norbornene-based monomers and other monomers that can be copolymerized with norbornene-based monomers, and hydrogenated products thereof. Examples of the products obtained by addition polymerization include addition polymers of norbornene-based monomers and addition polymers of norbornene-based monomers and other monomers that can be copolymerized with norbornene-based monomers. Among these, hydrogenated ring-opening polymers of norbornene-based monomers are preferred from the viewpoint of further increasing the cell mass formation rate.

[0027] Norbornene monomers that can be used to synthesize norbornene polymers include bicyclo[2.2.1]hept-2-ene (commonly known as norbornene), 5-methyl-bicyclo[2.2.1]hept-2-ene, 5,5-dimethyl-bicyclo[2.2.1]hept-2-ene, 5-ethyl-bicyclo[2.2.1]hept-2-ene, and 5-ethylidene-bicyclo[2.2.1]hept-2-ene. Bicyclic monomers such as hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene, 5-propenylbicyclo[2.2.1]hept-2-ene, 5-methoxycarbonyl-bicyclo[2.2.1]hept-2-ene, 5-cyanobicyclo[2.2.1]hept-2-ene, 5-methyl-5-methoxycarbonyl-bicyclo[2.2.1]hept-2-ene; Tricyclic monomers such as tricyclo[4.3.01,6.12,5]deca-3,7-diene (commonly known as dicyclopentadiene), 2-methyldicyclopentadiene, 2,3-dimethyldicyclopentadiene, and 2,3-dihydroxydicyclopentadiene; Tetracyclo[4.4.0.12,5.17,10]-3-dodecene (tetracyclododecene), tetracyclo[4.4.0.12,5.17,10]-3-dodecene, 8-methyltetracyclo[4.4.0.12,5.17,10]-3-dodecene, 8-ethyltetracyclo[4.4.0.12,5.17,10]-3-dodecene, 8-ethylidenetetracyclo[4.4.0.12,5.17,10]-3-dodecene, 8,9-dimethyltetracyclo[4.4.0.12,5.17,10]-3-dodecene, 8-ethyl-9-methyltetracyclo[4.4.0.12,5.17,10]-3-dodecene, 8-ethylidene-9-methyltetracyclo[4.4.0.12,5.17,10]-3-dodecene, tetracyclic monomers such as tetracyclo[4.4.0.12,5.17,10]-3-dodecene, 8-methyl-8-carboxymethyltetracyclo[4.4.0.12,5.17,10]-3-dodecene, 7,8-benzotricyclo[4.3.0.12,5]dec-3-ene (commonly known as methanotetrahydrofluorene: 1,4-methano-1,4,4a,9a-tetrahydrofluorene), 1,4-methano-8-methyl-1,4,4a,9a-tetrahydrofluorene, 1,4-methano-8-chloro-1,4,4a,9a-tetrahydrofluorene, and 1,4-methano-8-bromo-1,4,4a,9a-tetrahydrofluorene; and the like.

[0028] Other monomers capable of ring-opening copolymerization with norbornene monomers include monocyclic cycloolefin monomers such as cyclohexene, cycloheptene, cyclooctene, 1,4-cyclohexadiene, 1,5-cyclooctadiene, 1,5-cyclodecadiene, 1,5,9-cyclododecatriene, and 1,5,9,13-cyclohexadecatetraene. These monomers may have one or more kinds of substituents, such as an alkyl group, an alkylene group, an aryl group, a silyl group, an alkoxycarbonyl group, and an alkylidene group.

[0029] Other monomers capable of addition copolymerization with norbornene monomers include α-olefin monomers having 2 to 20 carbon atoms, such as ethylene, propylene, 1-butene, 1-pentene, and 1-hexene; cycloolefin monomers, such as cyclobutene, cyclopentene, cyclohexene, cyclooctene, and tetracyclo[9.2.1.02,10.03,8]tetradeca-3,5,7,12-tetraene (also called 3a,5,6,7a-tetrahydro-4,7-methano-1H-indene); and non-conjugated diene monomers, such as 1,4-hexadiene, 4-methyl-1,4-hexadiene, 5-methyl-1,4-hexadiene, and 1,7-octadiene.

[0030] Among these, as the other monomer capable of addition copolymerization with the norbornene monomer, an α-olefin monomer is preferable, and ethylene is more preferable. These monomers may have one or more kinds of substituents, such as an alkyl group, an alkylene group, an aryl group, a silyl group, an alkoxycarbonyl group, and an alkylidene group.

[0031] The ring-opening polymer of a norbornene monomer, or the ring-opening polymer of a norbornene monomer and another monomer capable of ring-opening copolymerization therewith, can be obtained by polymerizing the monomer components in the presence of a known ring-opening polymerization catalyst. As the ring-opening polymerization catalyst, for example, a catalyst consisting of a metal halide such as ruthenium or osmium, a nitrate or an acetylacetone compound, and a reducing agent, or a catalyst consisting of a metal halide or an acetylacetone compound such as titanium, zirconium, tungsten, or molybdenum, and an organoaluminum compound can be used. The hydrogenated ring-opening polymer of a norbornene monomer can usually be obtained by adding a known hydrogenation catalyst containing a transition metal such as nickel or palladium to a polymerization solution of the ring-opening polymer and hydrogenating the carbon-carbon unsaturated bonds.

[0032] The addition polymer of a norbornene-based monomer or the addition polymer of a norbornene-based monomer and another monomer copolymerizable therewith can be obtained by polymerizing the monomer components in the presence of a known addition polymerization catalyst, such as a catalyst made of a titanium, zirconium or vanadium compound and an organoaluminum compound.

[0033] [Monocyclic olefin polymer] As the monocyclic olefin polymer, for example, an addition polymer of a monocyclic olefin monomer such as cyclohexene, cycloheptene, or cyclooctene can be used.

[0034] [Cyclic conjugated diene polymer] As the cyclic conjugated diene polymer, for example, a polymer obtained by 1,2- or 1,4-addition polymerization of a cyclic conjugated diene monomer such as cyclopentadiene or cyclohexadiene, or a hydrogenated product thereof can be used.

[0035] [Vinyl alicyclic hydrocarbon polymer] Examples of vinyl alicyclic hydrocarbon polymers include polymers of vinyl alicyclic hydrocarbon monomers such as vinylcyclohexene and vinylcyclohexane, and hydrogenated products thereof; hydrogenated aromatic ring moieties of polymers of vinyl aromatic monomers such as styrene and α-methylstyrene; etc. The vinyl alicyclic hydrocarbon polymer may be a copolymer of these monomers with other copolymerizable monomers.

[0036] [Weight average molecular weight] There is no particular restriction on the molecular weight of the alicyclic structure-containing polymer, but the weight average molecular weight, calculated as polyisoprene, measured by gel permeation chromatography of a cyclohexane solution (a toluene solution if the polymer is not soluble) is usually 5,000 or more, preferably 5,000 to 500,000, more preferably 8,000 to 200,000, and particularly preferably 10,000 to 100,000. When the weight average molecular weight is within this range, the mechanical strength and moldability are well balanced, which is preferable.

[0037] [Glass transition temperature] The glass transition temperature of the alicyclic structure-containing polymer may be appropriately selected depending on the intended use, but is preferably 50° C. or higher, more preferably 70° C. or higher, and even more preferably 90° C. or higher, and is preferably 200° C. or lower, more preferably 180° C. or lower, even more preferably 160° C. or lower, even more preferably 150° C. or lower, and particularly preferably 140° C. or lower. When the glass transition temperature of the alicyclic structure-containing polymer is within this range, it is preferable because it has a high balance between heat resistance and molding processability. The glass transition temperature of the alicyclic structure-containing polymer in the present invention is measured based on JIS K 7121.

[0038] <<Other ingredients>> The polymer composition used to form the culture surface of the cell culture vessel of the present invention may further contain components other than the above-mentioned alicyclic structure-containing polymer (other components). The other components include compounding agents commonly used in thermoplastic resin materials, such as polymers other than the alicyclic structure-containing polymer (hereinafter simply referred to as "other polymers"), antioxidants, ultraviolet absorbers, light stabilizers, near-infrared absorbers, release agents, colorants such as dyes and pigments, plasticizers, antistatic agents, and fluorescent whitening agents. The other components may be used alone or in any combination of two or more kinds in any ratio.

[0039] Here, from the viewpoint of further increasing the cell mass formation rate, the content of the other polymer in the polymer composition is preferably 50 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 1 part by mass or less, even more preferably 0.1 part by mass or less, and particularly preferably 0 part by mass (i.e., the polymer composition does not contain other polymers) per 100 parts by mass of the alicyclic structure-containing polymer.

[0040] <<Method for preparing polymer composition>> The mixing method for obtaining a polymer composition containing the above-mentioned alicyclic structure-containing polymer and optionally other components is not particularly limited, and can be performed using, for example, a known melt kneader such as a single screw extruder, a twin screw extruder, a Banbury mixer, a kneader, a feeder ruder, etc. After mixing, the mixture can be extruded into a rod shape according to a conventional method, and cut to an appropriate length with a strand cutter to form pellets.

[0041] [Surface oxygen content] In addition, the culture vessel of the present invention needs to have a surface oxygen content of less than 1 atomic % on the culture surface. If the surface oxygen content of the culture surface is 1 atomic % or more, the cell aggregate formation rate decreases. The surface oxygen content of the culture surface is preferably 0.1 atomic % or more, more preferably 0.2 atomic % or more, preferably 0.9 atomic % or less, more preferably 0.8 atomic % or less, even more preferably 0.7 atomic % or less, even more preferably 0.6 atomic % or less, and particularly preferably 0.5 atomic % or less. If the surface oxygen content of the culture surface is 0.1 atomic % or more, the ease of manufacture of the culture vessel can be well ensured. On the other hand, if the surface oxygen content of the culture surface is 0.9 atomic % or less, the cell aggregate formation rate can be further increased. The surface oxygen amount on the culture surface can be adjusted, for example, by changing the molding conditions when forming the culture surface from the polymer composition, whether or not the culture surface is subjected to a surface treatment, and, when the culture surface is formed by injection molding, the temperature of the cylinder of the injection molding machine (hereinafter, sometimes simply abbreviated as "cylinder temperature"). Specifically, the surface oxygen amount can be reduced by lowering the cylinder temperature, and the surface oxygen amount can be increased by increasing the cylinder temperature. In addition, the surface oxygen amount can be reduced by not performing a surface treatment on the culture surface.

[0042] [π-π * Transition amount] In addition, the culture vessel of the present invention has a π-π * The transition amount must be less than 1 atomic %. *If the transition amount is 1 atomic % or more, the cell aggregate formation rate decreases. * The transition amount is preferably 0.8 atomic % or less, more preferably 0.4 atomic % or less, even more preferably 0.2 atomic % or less, even more preferably 0.1 atomic % or less, and particularly preferably 0 atomic %. * If the transition amount is 0.8 atomic % or less, the cell aggregate formation rate can be further increased. * The lower limit of the transition amount is not particularly limited, and can be, for example, 0.1 atomic % or more, or 0.2 atomic % or more. In addition, the π-π * The transition amount can be adjusted, for example, by changing the type of polymer (alicyclic structure-containing polymer and other polymer) in the polymer composition used to form the culture surface. Specifically, by using a polymer that does not have an aromatic ring, the π-π * The amount of transition can be reduced.

[0043] [Surface oxygen content and π-π * Total transition amount] The culture vessel of the present invention has a surface oxygen amount on the culture surface and a π-π * The total amount of transition must be less than 1 atomic %. * If the total transition amount is 1 atom % or more, the cell aggregate formation rate decreases. * The total transition amount is preferably 0.1 atomic % or more, more preferably 0.2 atomic % or more, preferably 0.9 atomic % or less, more preferably 0.8 atomic % or less, even more preferably 0.7 atomic % or less, even more preferably 0.6 atomic % or less, and particularly preferably 0.5 atomic % or less. * If the total transition amount is 0.1 atomic % or more, the ease of manufacturing the culture vessel can be ensured. *If the total transition amount is 0.9 atom % or less, the cell aggregate formation rate can be further increased.

[0044] <Manufacturing method of culture vessel> The method for producing the culture vessel of the present invention is not particularly limited, but the culture vessel of the present invention can be produced, for example, through a step (molding step) of forming a polymer composition containing the above-mentioned alicyclic structure-containing polymer and optionally other components to obtain a culture surface. Note that the culture vessel of the present invention may be produced, optionally, through a step (other step) other than the above-mentioned molding step.

[0045] <<Forming process>> Here, the method of forming the polymer composition to obtain the culture surface is not particularly limited, and can be appropriately selected from known forming methods according to the desired shape of the culture surface. Examples of such known forming methods include extrusion molding, injection molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, press molding, vacuum molding, powder slush molding, calendar molding, foam molding, thermoforming, etc. Among these, it is preferable to use injection molding as the forming method.

[0046] When injection molding is used as the molding method, the cylinder temperature is preferably 250° C. or higher, more preferably 260° C. or higher, and is preferably 320° C. or lower, more preferably 310° C. or lower. If the cylinder temperature is within the above-mentioned range, the surface oxygen amount on the culture surface and π-π * It becomes easy to keep the total transition amount below 1 atomic %, and the cell aggregate formation rate can be further increased.

[0047] Furthermore, when injection molding is used as the molding method, the temperature of the mold used in injection molding (hereinafter sometimes simply abbreviated as "mold temperature") is preferably (Tg-50)°C or higher, more preferably (Tg-40)°C or higher, preferably (Tg-20)°C or lower, and more preferably (Tg-25)°C or lower, where Tg (°C) is the glass transition temperature of the alicyclic structure-containing polymer in the polymer composition. If the mold temperature is within the above-mentioned range, the surface oxygen amount on the culture surface and π-π * It becomes easy to keep the total transition amount below 1 atomic %, and the cell aggregate formation rate can be further increased.

[0048] <<Other processes>> Other steps include, for example, a step of pre-drying the polymer composition prior to the molding step (pre-drying step), a step of combining the culture surface with other components to assemble the culture vessel (assembly step), a step of sterilizing the culture vessel (sterilization step), and a step of surface-treating the culture surface (surface treatment step).

[0049] The culture vessel of the present invention is preferably manufactured through a sterilization process in addition to the above-mentioned molding process. The sterilization method in the sterilization process is not particularly limited, and can be appropriately selected from methods generally adopted in the medical field, such as heating methods such as high-pressure steam method and dry heat method; radiation methods using radiation such as gamma rays and electron beams, and irradiation methods using high-frequency waves; gas methods using gas such as ethylene oxide gas (EOG) in contact; and filtration methods using sterilization filters. Among them, the gas method is preferred because it is easy to maintain the surface free energy of the culture surface within a specific range.

[0050] In the surface treatment step, the culture surface is subjected to surface treatment such as plasma treatment, corona discharge treatment, ozone treatment, ultraviolet irradiation treatment, etc. However, it is preferable not to perform the surface treatment step because the costs incurred by performing these surface treatments can be reduced, there is a risk of the cleanliness being impaired due to partial decomposition of the culture surface accompanying the surface treatment, and there is a risk of the surface oxygen amount increasing due to the surface treatment, resulting in a decrease in the cell mass formation rate. In addition, when the surface treatment step is performed, it is preferable to perform the surface treatment step by comparing the surface oxygen amount and π-π * It is preferable to carry out only a weak surface treatment that can keep the total amount of transitions below 1 atomic %.

[0051] (Method for culturing adherent cells) The culture method of the present invention is characterized by using the above-mentioned culture vessel of the present invention. And, since the culture method of the present invention uses the culture vessel of the present invention, it is excellent in the cell aggregate formation rate.

[0052] Here, the culture method of the present invention is not particularly limited as long as the culture vessel of the present invention is used. For example, the above-mentioned culture vessel of the present invention can accommodate adherent cells and a liquid medium, and the adherent cells can be cultured in the liquid medium.

[0053] The liquid medium used here is generally one that has a pH buffering effect, has an osmotic pressure suitable for cells, contains nutrients for cells, and is non-toxic to cells. Examples of components that exhibit a pH buffering effect include tris hydrochloride, various phosphates, and various carbonates. The osmotic pressure of a liquid medium is usually adjusted using an aqueous solution in which the concentrations of potassium ions, sodium ions, calcium ions, glucose, etc. are adjusted so that the osmotic pressure is approximately the same as that of the cells. Specific examples of such aqueous solutions include physiological saline such as phosphate buffered saline, Tris buffered saline, and HEPES buffered saline; Ringer's solutions such as lactate Ringer's solution, acetate Ringer's solution, and bicarbonate Ringer's solution; and the like. Nutrients for cells include amino acids, nucleic acids, vitamins, minerals, and the like. As liquid media, various commercially available products such as RPMI-1640, HAM, α-MEM, Dulbecco's modified Eagle's medium (DMEM), Eagle's minimum essential medium (EMEM), HAM's F-12K (Kaighn's) medium, F-12, F-10, and M-199 can be used.

[0054] The liquid medium may also contain additives such as serum (e.g. fetal bovine serum (FBS)), antibiotics (e.g. penicillin, streptomycin), differentiation-inducing factors, various growth factors, hormones, minerals, metals, vitamins, etc. These medium additives can be used alone or in combination of two or more.

[0055] The culture conditions are not particularly limited and can be appropriately determined depending on the type of adherent cells used and the purpose of the culture. For example, cells can be cultured in a humidified incubator with a carbon dioxide concentration of about 5% and a temperature maintained constant within the range of 20°C to 37°C.

[0056] From the viewpoint of maintaining the health of the cells in a good condition, it is preferable to passage the adhesive cells appropriately according to the culture density, etc. Passage of the adhesive cells can be carried out, for example, by detaching the adhesive cells from the culture surface by trypsin treatment, diluting the detached adhesive cells with a new liquid medium, and reseeding the cells.

[0057] <Suitable culture method> Here, from the viewpoint of further increasing the cell cluster formation rate, the culture method of the present invention preferably includes a step in which adhesive cells form cell clusters on the culture surface (cell cluster formation step), and a step in which the formed cell clusters are cultured in a state adhered to the culture surface (culture step).

[0058] <Cell cluster formation step> In the cell aggregate formation step, at least a part of the adhesive cells form cell aggregates on the culture surface of the culture vessel of the present invention. Usually, the adhesive cells immediately after seeding exist in a state of being suspended alone in the liquid medium. As the culture time passes, at least a part of the adhesive cells existing in a state of being suspended in the liquid medium start to form cell aggregates on the culture surface. The time from seeding to the formation of cell aggregates on the culture surface depends on the type of cells, the seeding amount, etc., and is not particularly limited, but is usually 3 to 7 days. Note that the adhesive cells that do not form cell aggregates on the culture surface in the cell aggregate formation step usually exist in a state of being alone adhered to the culture surface without forming cell aggregates, or exist in a state of being suspended in the liquid medium.

[0059] <Culture step> In the culture step, at least a part of the cell aggregates formed on the culture surface in the cell aggregate formation step are cultured in a state of adhering to the culture surface without floating in the liquid medium. It is preferable to replace the liquid medium as needed from the viewpoint of preventing deterioration of the health of the cells due to a decrease in the liquid medium due to evaporation, depletion of nutrients in the liquid medium, etc. Note that a part of the cell aggregates may be separated from the culture surface and float in the liquid medium.

[0060] <Adhesion step> Here, from the viewpoint of further increasing the cell aggregate formation rate, the culture method of the present invention preferably further includes a step (adhesion step) in which the adhesive cells adhere to the culture surface prior to the above-mentioned cell aggregate formation step. Usually, the adhesive cells immediately after seeding exist in the liquid medium in a state of being suspended alone. In the adhesion step, at least a part of the adhesive cells existing in a state of being suspended in the liquid medium adheres to the culture surface of the above-mentioned culture vessel of the present invention. The manner in which the adhesive cells adhere to the culture surface is not particularly limited. For example, a scaffold protein derived from serum or the like contained as a medium additive in the liquid medium is adsorbed to the culture surface, and a cell adhesion protein existing on the cell membrane of the adhesive cells is bound to the scaffold protein, so that the adhesive cells can adhere to the culture surface. Note that the adhesive cells that do not adhere to the culture surface in the adhesion step usually exist in a state of being suspended in the liquid medium.

[0061] The culture method of the present invention may include steps (other steps) other than the above-mentioned adhesion step, cell cluster formation step, and culture step. Examples of the other steps include a step of subculturing the adherent cells before they reach a confluent state. EXAMPLES

[0062] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" expressing amounts are based on mass unless otherwise specified. In the examples and comparative examples, the surface oxygen amount and π-π * The transition amount and the cell aggregate formation rate were evaluated by the following methods.

[0063] <Surface oxygen content> The bottom surface (culture surface) of the 96-well plate prepared in the examples and comparative examples was cut out and used as a test piece. Then, the wide spectrum (measurement range: 0 eV to 1100 eV) and narrow spectrum (measurement range: 520 eV to 545 eV) of this test piece were measured using X-ray photoelectron spectroscopy (XPS). The bond energy correction was performed based on the hydrocarbon-derived C1s spectrum peak position of 284.8 eV. Then, the sum of the areas of all peaks detected in the wide spectrum was set as S0, and the area of ​​the O1s peak (peak present in the range of 530 to 535 eV) in the narrow spectrum was set as S1, and the surface oxygen amount (atomic %) was calculated by the following formula. Surface oxygen content (atomic%) = (S1 / S0) x 100 The measurement conditions for the XPS spectrum are as follows. [XPS spectrum measurement conditions] Equipment: GCIB-XPS analysis equipment (ULVAC-PHI, product name "PHI5000 Versa Probe II") Excitation X-ray: Monochromatic AlKα radiation (50W, 15kV) Analysis area: 200μm x 200μm Electron / Ion Neutralization Gun: ON [Details of wide spectrum measurement conditions] Pass Energy: 187.85eV Step: 0.8 eV Number of times: 3 [Details of narrow spectrum measurement conditions] Pass Energy: 23.5eV Step: 0.1 eV Number of times: 5 <π-π * Transition amount> The bottom surface (culture surface) of the 96-well plate prepared in the examples and comparative examples was cut out and used as a test piece. Then, the wide spectrum (measurement range: 0 eV to 1100 eV) and narrow spectrum (measurement range: 275 eV to 300 eV) of this test piece were measured using X-ray photoelectron spectroscopy (XPS). Binding energy correction was performed based on the hydrocarbon-derived C1s spectrum peak position of 284.8 eV. The C1s peak (peak present in the range of 285 to 294 eV) in the obtained narrow spectrum was waveform separated using curve fitting by the nonlinear least squares method. For the curve fitting by the nonlinear least squares method, analysis software MULTIPACK (manufactured by ULVAC-PHI, Inc.) was used. The area of ​​the C1s peak was defined as S2, and the π-π obtained by waveform separation of the C1s peak was calculated. * The area of ​​the peak due to the transition (peak in the range of 290 to 294 eV) is S3, and the π-π * The amount of transition (atomic %) was calculated. Pi-pi * Transition amount (atomic %)=(S3 / S2)×100 The measurement conditions for the XPS spectrum were the same as those described above in the section "Surface oxygen content," except that the number of narrow spectrum integrations was changed from 5 to 3. <Cell cluster formation rate> The dormant (thawed) adherent cells were subcultured twice. Thereafter, the adherent cells were seeded in a 96-well plate under the following conditions and cultured at 37°C. On the third day of culture, phase contrast images of the cells were taken (4x objective) using an all-in-one fluorescent microscope (Keyence Corporation, model number "BZ-X710"), and the total number of cells and the number of cell clusters in the well were counted. Then, the cell cluster formation rate (%) was calculated as the ratio of the number of cell clusters to the total number of cells in the well, and evaluated according to the following criteria. The higher the cell cluster formation rate, the better the cell cluster formation ability. A: Cell cluster formation rate is 90% or more B: Cell cluster formation rate is 50% or more but less than 90% C: Cell cluster formation rate is less than 50% [A549 (human lung cancer cells)] Source: European Collection of Authenticated Cell Cultures (ECACC), strain number "86012804" Liquid medium: Ham's F-12K (Kaighn's) medium (Thermo Fisher Scientific, product number "#21127022") Medium additives: 10% fetal bovine serum (Thermo Fisher Scientific, product number "#172012-500mL"; hereinafter abbreviated as "FBS") + 1% penicillin-streptomycin (Nacalai Tesque, product number "26253-84"; hereinafter abbreviated as "P / S") Seeding conditions: 10,000 cells / well [MCF7 (human breast cancer cells)] Source: ECACC, stock number "86012803" Liquid medium: MEM medium (Nacalai Tesque, product number "#21443-15") Media additives: 10% FBS + 1% P / S Seeding conditions: 10,000 cells / well [PANC-1 (human pancreatic cancer cells)] Source: ECACC, stock number "87092802" Liquid medium: DMEM medium (Nacalai Tesque, product number "#08458-45") Media additives: 10% FBS + 1% P / S Seeding conditions: 10,000 cells / well [HEK293 cells (human embryonic kidney cells)] Source: ECACC, stock number "85120602" Liquid medium: DMEM medium (Nacalai Tesque, product number "#08458-45") Media additives: 10% FBS + 1% P / S Seeding conditions: 10,000 cells / well [Mouse Schwann cells (IMS32)] Source: Cosmo Bio Co., Ltd., product number "SWN-IMS32C" Culture medium: Mouse Schwann cell (IMS32) medium (Cosmo Bio, product number "SWNMM") Seeding conditions: 10,000 cells / well [iCell(R) Cardiomytocytes] Source: Fujifilm Wako Pure Chemical Industries, product number "C1016" Liquid medium (for thawing): iCell Cardiomyocyte Plating Medium (manufactured by Fujifilm Wako Pure Chemical Industries, product number "#M1001") Liquid medium (for maintenance): iCell Cardiomyocyte Maintenance Medium (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., "#M1003") Seeding conditions: 1.56×10 5 cells / cm 2 (Cell seeding was performed according to the iCell Cardiomytocytes2 User's Guide.)

[0064] (Production Example 1) <Preparation of culture vessel (96-well plate)> A 96-well plate having 96 cylindrical wells (bottom area of ​​each well: 0.32 cm) was injection molded using a ring-opening polymer hydrogenated product of a norbornene monomer as an alicyclic structure-containing polymer (manufactured by Zeon Corporation, product name "ZEONOR (registered trademark) 1060R", glass transition temperature (Tg): 100°C, hereinafter referred to as "COP1"). 2The injection molding conditions were as follows: Injection molding machine: FANUC, product name "ROBOSHOTα100B" Cylinder temperature: 270℃ Mold temperature: 70℃ Injection pressure: 170MPa The resulting 96-well plate was then sterilized with ethylene oxide gas. The surface oxygen amount and π-π * The amount of transition was measured, and the results are shown in Table 1.

[0065] (Production Example 2) A 96-well plate (hereinafter referred to as "P2") was prepared in the same manner as in Production Example 1, except that a ring-opening polymer hydride of a norbornene monomer (manufactured by Zeon Corporation, product name "ZEONEX (registered trademark) F52R", Tg: 155°C, hereinafter referred to as "COP2") was used instead of COP1 as the alicyclic structure-containing polymer, and the cylinder temperature was changed from 270°C to 300°C and the mold temperature was changed from 70°C to 125°C. Then, measurements were performed in the same manner as in Production Example 1. The results are shown in Table 1.

[0066] (Production Example 3) A 96-well plate (hereinafter referred to as "P3") was prepared in the same manner as in Production Example 1, except that a ring-opening polymer hydride of a norbornene monomer (manufactured by Zeon Corporation, product name "ZEONEX 690R", Tg: 136°C, hereinafter referred to as "COP3") was used instead of COP1 as the alicyclic structure-containing polymer, and the cylinder temperature was changed from 270°C to 300°C and the mold temperature was changed from 70°C to 106°C. Then, measurements were performed in the same manner as in Production Example 1. The results are shown in Table 1.

[0067] (Production Example 4) A 96-well plate (hereinafter referred to as "P4") was prepared in the same manner as in Production Example 1, except that an addition copolymer of norbornene and ethylene (manufactured by Polyplastics Co., Ltd., product name "TOPAS (registered trademark) 6013-M07", Tg: 142°C, hereinafter referred to as "COC1") was used instead of COP1 as the alicyclic structure-containing polymer, and the cylinder temperature was changed from 270°C to 300°C, and the mold temperature was changed from 70°C to 112°C. Then, measurements were performed in the same manner as in Production Example 1. The results are shown in Table 1.

[0068] (Production Example 5) A 96-well plate (hereinafter referred to as "P5") was prepared in the same manner as in Production Example 1, except that a ring-opening polymer hydride of a norbornene monomer (manufactured by Zeon Corporation, product name "ZEONEX 790R", Tg: 163°C, hereinafter referred to as "COP4") was used instead of COP1 as the alicyclic structure-containing polymer, and the cylinder temperature was changed from 270°C to 320°C and the mold temperature was changed from 70°C to 125°C. Then, measurements were performed in the same manner as in Production Example 1. The results are shown in Table 1.

[0069] (Production Example 6) A 96-well plate (hereinafter referred to as "P6") was prepared in the same manner as in Production Example 1, except that COP4 was used instead of COP1 as the alicyclic structure-containing polymer, the cylinder temperature was changed from 270°C to 330°C, and the mold temperature was changed from 70°C to 125°C. Then, measurements were performed in the same manner as in Production Example 1. The results are shown in Table 2.

[0070] (Production Example 7) A 96-well plate (hereinafter referred to as "P7") was prepared in the same manner as in Production Example 1, except that COP4 was used instead of COP1 as the alicyclic structure-containing polymer, the cylinder temperature was changed from 270°C to 335°C, and the mold temperature was changed from 70°C to 125°C. Then, measurements were performed in the same manner as in Production Example 1. The results are shown in Table 2.

[0071] (Production Example 8) A 96-well plate (hereinafter referred to as "P8") was prepared in the same manner as in Production Example 1, except that COP4 was used instead of COP1 as the alicyclic structure-containing polymer, the cylinder temperature was changed from 270°C to 340°C, and the mold temperature was changed from 70°C to 125°C. Then, measurements were performed in the same manner as in Production Example 1. The results are shown in Table 2.

[0072] (Production Example 9) A 96-well plate (hereinafter referred to as "P9") was prepared in the same manner as in Production Example 1, except that COC1 was used instead of COP1 as the alicyclic structure-containing polymer, the cylinder temperature was changed from 270°C to 330°C, and the mold temperature was changed from 70°C to 112°C. Then, measurements were performed in the same manner as in Production Example 1. The results are shown in Table 2.

[0073] (Production Example 10) A commercially available polystyrene 96-well microplate (Greiner, product number "665185", hereinafter referred to as "P10") was used. Measurements were carried out in the same manner as in Production Example 1. The results are shown in Table 2.

[0074] (Examples 1 to 6) P1 was used as the culture vessel, and A549 (Example 1), MCF7 (Example 2), PANC-1 (Example 3), HEK293 cells (Example 4), mouse Schwann cells (Example 5), and cardiomyocytes (Example 6) were used as the adherent cells. The cell aggregate formation rate was then evaluated. The results are shown in Table 3.

[0075] (Examples 7 to 12) P2 was used as the culture vessel, and A549 (Example 7), MCF7 (Example 8), PANC-1 (Example 9), HEK293 cells (Example 10), mouse Schwann cells (Example 11), and cardiomyocytes (Example 12) were used as the adherent cells. Evaluation was performed in the same manner as in Example 1. The results are shown in Table 3.

[0076] (Examples 13 to 18) P3 was used as the culture vessel, and A549 (Example 13), MCF7 (Example 14), PANC-1 (Example 15), HEK293 cells (Example 16), mouse Schwann cells (Example 17), and cardiomyocytes (Example 18) were used as the adherent cells. Evaluation was performed in the same manner as in Example 1. The results are shown in Table 3.

[0077] (Examples 19 to 24) P4 was used as the culture vessel, and A549 (Example 19), MCF7 (Example 20), PANC-1 (Example 21), HEK293 cells (Example 22), mouse Schwann cells (Example 23), and cardiomyocytes (Example 24) were used as the adherent cells. Evaluation was performed in the same manner as in Example 1. The results are shown in Table 3.

[0078] (Examples 25 to 30) P5 was used as the culture vessel, and A549 (Example 25), MCF7 (Example 26), PANC-1 (Example 27), HEK293 cells (Example 28), mouse Schwann cells (Example 29), and cardiomyocytes (Example 30) were used as the adherent cells. Evaluation was performed in the same manner as in Example 1. The results are shown in Table 4.

[0079] (Comparative Examples 1 to 6) P6 was used as the culture vessel, and A549 (Comparative Example 1), MCF7 (Comparative Example 2), PANC-1 (Comparative Example 3), HEK293 cells (Comparative Example 4), mouse Schwann cells (Comparative Example 5), and cardiomyocytes (Comparative Example 6) were used as the adherent cells. Evaluation was performed in the same manner as in Example 1. The results are shown in Table 4.

[0080] (Comparative Examples 7 to 12) P7 was used as the culture vessel, and A549 (Comparative Example 7), MCF7 (Comparative Example 8), PANC-1 (Comparative Example 9), HEK293 cells (Comparative Example 10), mouse Schwann cells (Comparative Example 11), and cardiomyocytes (Comparative Example 12) were used as the adherent cells. Evaluation was performed in the same manner as in Example 1. The results are shown in Table 4.

[0081] (Comparative Examples 13 to 18) P8 was used as the culture vessel, and A549 (Comparative Example 13), MCF7 (Comparative Example 14), PANC-1 (Comparative Example 15), HEK293 cells (Comparative Example 16), mouse Schwann cells (Comparative Example 17), and cardiomyocytes (Comparative Example 18) were used as the adherent cells. Evaluation was performed in the same manner as in Example 1. The results are shown in Table 5.

[0082] (Comparative Examples 19 to 24) P9 was used as the culture vessel, and A549 (Comparative Example 19), MCF7 (Comparative Example 20), PANC-1 (Comparative Example 21), HEK293 cells (Comparative Example 22), mouse Schwann cells (Comparative Example 23), and cardiomyocytes (Comparative Example 24) were used as the adherent cells. Evaluation was performed in the same manner as in Example 1. The results are shown in Table 5.

[0083] (Comparative Examples 25 to 30) P10 was used as the culture vessel, and A549 (Comparative Example 25), MCF7 (Comparative Example 26), PANC-1 (Comparative Example 27), HEK293 cells (Comparative Example 28), mouse Schwann cells (Comparative Example 29), and cardiomyocytes (Comparative Example 30) were used as the adherent cells. Evaluation was performed in the same manner as in Example 1. The results are shown in Table 5.

[0084] In addition, in Tables 1 to 5 shown below, "Schwann" refers to mouse Schwann cells; "Tg" refers to the glass transition temperature.

[0085] [Table 1]

[0086] [Table 2]

[0087] [Table 3]

[0088] [Table 4]

[0089] [Table 5]

[0090] From Tables 1 to 5, a culture surface made of a polymer composition containing an alicyclic structure-containing polymer and a surface oxygen amount and a π-π * It is apparent that in Examples 1 to 30, in which a culture vessel in which the total transition amount was less than 1 atomic % was used, the cell aggregate formation rate was sufficiently high. On the other hand, the surface oxygen content and π-π * It is apparent that in Comparative Examples 1 to 30, in which the culture vessels having a total transition amount of 1 atom % or more were used, the cell aggregate formation rate was decreased. [Industrial Applicability]

[0091] According to the present invention, it is possible to provide a culture vessel for adherent cells which has an excellent cell aggregate formation rate, and a method for culturing adherent cells using the culture vessel.

Claims

1. A culture vessel for adhesive cells having a culture surface made of a polymer composition containing an alicyclic structure-containing polymer, The surface oxygen amount (atomic %) on the culture surface measured by X-ray photoelectron spectroscopy and π-π * A culture vessel for adherent cells, in which the total transition amount (atomic %) is less than 1 atomic %.

2. A method for culturing adherent cells, using the culture vessel for adherent cells according to claim 1 .

3. A cell cluster forming step in which adhesive cells form cell clusters on the culture surface; a culturing step in which the cell clusters are cultured in a state of being attached to the culture surface; The method for culturing adherent cells according to claim 2 , comprising:

4. The method for culturing adherent cells according to claim 3 , further comprising, prior to the cell cluster formation step, an adhesion step in which the adherent cells adhere to the culture surface.

Citation Information

Patent Citations

  • Adhesive cell culturing substrate, and cell culture vessel and cell culture method using the same

    JP2017077240A

  • Culture method of adhesive cells and production method of proteins

    JP2017079658A