Optical glass and optical element
The optical glass composition with specific SiO 2 , B 2 O 3 , and ZrO 2 /Nb 2 O 5 ratios addresses the challenge of achieving low partial dispersion ratio and high quality, enhancing optical element performance by minimizing chromatic aberration.
Patent Information
- Application Number
- JP2023052148
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing optical glasses with refractive index (n d ) less than 1.64000 and Abbe number (ν d ) 43.00 or less face challenges in achieving a small partial dispersion ratio while maintaining high quality, with B 2 O 3 content leading to volatilization and striae issues.
Optical glass composition with SiO 2 20.00% to 50.00%, B 2 O 3 0% to 25.0%, and a mass ratio of ZrO 2 /Nb 2 O 5 0.200 to 0.900, ensuring refractive index and Abbe number within desired ranges and minimizing partial dispersion ratio.
The solution provides high-quality optical glass with a small partial dispersion ratio, reducing chromatic aberration and improving optical element performance.
Smart Images

Figure 2024140808000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical glass and an optical element. [Background technology]
[0002] Optical glass and optical elements can be used in applications such as combining lenses of different optical regions to improve the optical characteristics of cameras and imaging devices, and incorporating them into optical equipment to realize various optical designs.
[0003] Optical systems contain aberrations, to varying degrees. These aberrations are classified as monochromatic and chromatic aberrations, and chromatic aberration in particular is highly dependent on the material properties of the lenses used in the optical system. Chromatic aberration can be eliminated by combining a high dispersion lens with a low dispersion lens and a lens with a large partial dispersion ratio with a small partial dispersion ratio. However, due to the material properties, it is difficult to obtain optical glass that has both low dispersion and a small partial dispersion ratio.
[0004] In addition, optical glass containing Nb2O5 contains a given amount of SiO2 and B2O3 components to promote the stability of the glass. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2008-297198 A [Patent Document 2] JP 2016-222511 A Summary of the Invention [Problem to be solved by the invention]
[0006] The optical glass disclosed in Patent Document 1 has a refractive index (n d ) is 1.64000 or less, and the Abbe number (ν d There is no disclosure of glasses with a .DELTA.M.sub.O of 43.00 or less.
[0007] The optical glass disclosed in Patent Document 2 has a refractive index (n d ) is 1.64000 or less, and the Abbe number (ν d Although there is disclosure of glasses having a B2O3 content of 43.00 or less, these contain a large amount of the B2O3 component. Glass with a high B2O3 content is more likely to suffer from the generation of striae due to volatilization of the B2O3 component and from deterioration of quality due to volatilization.
[0008] The present invention has been made in consideration of the above problems, and its object is to provide a method for reducing the refractive index (n d ) is 1.64000 or less, and the Abbe number (ν d ) is 43.00 or less, the partial dispersion ratio is small, and high quality optical glass is obtained. [Means for solving the problem]
[0009] The present inventors have conducted extensive testing and research in order to solve the above problems, and as a result have found that by containing the SiO2 component and the B2O3 component and setting the mass ratio ZrO2 / Nb2O5 in the range of 0.200 to 0.900, it is possible to obtain a high-quality optical glass having a small partial dispersion ratio while keeping the refractive index and Abbe number within the desired ranges, and have completed the present invention. Specifically, the present invention provides the following:
[0010] (1) Refractive index (n d ) is less than or equal to 1.64000 Abbe number (ν d ) is less than or equal to 43.00, Oxide based mass% SiO2 content is 20.00-50.00%, B2O3 content is over 0% and 25.0%. Mass ratio ZrO2 / Nb2O5 is 0.200~0.900, Optical glass.
[0011] (2) An optical element made of the optical glass according to (1). Effect of the Invention
[0012] According to the present invention, the refractive index (n d ) is 1.64000 or less, and the Abbe number (ν d ) is 43.00 or less, the partial dispersion ratio is small, and high quality optical glass and optical elements can be provided. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a graph showing the relationship between the partial dispersion ratio (θg,F) and the Abbe number (νd) for glasses of the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the embodiments of the optical glass of the present invention will be described in detail. The present invention is not limited to the following embodiments, and can be practiced with appropriate modifications within the scope of the object of the present invention. Note that, although explanations of duplicated parts may be omitted as appropriate, this does not limit the gist of the invention.
[0015] [Glass composition] The composition range of each component constituting the optical glass of the present invention is described below. Unless otherwise specified in this specification, the content of each component is expressed as mass% relative to the total substance amount of the glass in terms of oxide. Here, "composition in terms of oxide" refers to a composition in which each component contained in the glass is expressed, assuming that oxides, composite salts, metal fluorides, etc. used as raw materials for the glass components of the present invention are all decomposed and converted to oxides during melting, with the total mass of the generated oxides being 100 mass%.
[0016] The SiO2 component is a component that promotes stable glass formation. In particular, by making the content of the SiO2 component 20.0% or more, devitrification can be reduced and moldability can be improved without significantly increasing the partial dispersion ratio. Therefore, the lower limit of the content of the SiO2 component is preferably 20.0% or more, more preferably 23.00% or more, even more preferably 25.0% or more, even more preferably 27.0% or more, even more preferably 30.0% or more, even more preferably 32.0% or more, and even more preferably 35.0% or more. On the other hand, by making the content of SiO2 component 50.0% or less, the increase in the partial dispersion ratio can be suppressed. This also makes it possible to suppress the decrease in the melting property of the glass raw material. Therefore, the content of SiO2 component is preferably 50.0% or less, more preferably 48.0% or less, even more preferably 47.0% or less, even more preferably 46.0% or less, and even more preferably 45.0% or less as the upper limit.
[0017] The B2O3 component is a component that can promote stable glass formation, reduce devitrification, and improve the melting property of glass raw materials. Therefore, the content of the B2O3 component is preferably more than 0%, more preferably 1.0% or more, even more preferably 3.0% or more, even more preferably 5.0% or more, even more preferably 8.0% or more, and even more preferably 10.0% or more as the lower limit. On the other hand, by keeping the content of the B2O3 component at 25.0% or less, deterioration of glass quality can be suppressed and an increase in the partial dispersion ratio can be suppressed. The B2O3 component is a component that easily volatilizes, and suppressing volatilization can suppress the occurrence of striae and deterioration of glass quality. The content of the B2O3 component is preferably 25.0% or less, more preferably 23.0% or less, even more preferably 20.0% or less, even more preferably 18.0% or less, and even more preferably 15.0%. The upper limit is more preferably 13.0% or less, and even more preferably 11.0% or less.
[0018] The Nb2O5 component is a component that can reduce the Abbe number and partial dispersion ratio. Therefore, the content of the Nb2O5 component is preferably 5.0% or more, more preferably 8.0% or more, even more preferably 10.0% or more, even more preferably 12.0% or more, and even more preferably 15.0% or more as the lower limit. On the other hand, the refractive index can be reduced by setting the content of the Nb2O5 component to 40.0% or less. Therefore, the upper limit of the content of the Nb2O5 component is preferably 40.0% or less, more preferably 35.0% or less, even more preferably 30.0% or less, even more preferably 28.0% or less, and even more preferably 25.0% or less.
[0019] By setting the content of the Li2O component to 10.0% or less, it is possible to suppress an increase in the refractive index, and to reduce deterioration of reheat pressability and devitrification due to excessive content. Therefore, the upper limit of the content of the Li2O component is preferably 10.0% or less, more preferably 7.0% or less, even more preferably 5.0% or less, even more preferably 4.0% or less, even more preferably 3.0% or less, even more preferably 2.0% or less, and even more preferably 1.0% or less.
[0020] By setting the content of the K2O component to 10.0% or less, deterioration of reheat pressability and devitrification due to excessive content can be reduced. Therefore, the upper limit of the content of the K2O component is preferably set to 10.0% or less, more preferably 7.0% or less, even more preferably 5.0% or less, and even more preferably 3.0% or less.
[0021] The Na2O component is a component that can reduce the partial dispersion ratio of the glass and improve the melting property of the glass raw material. Therefore, the content of the Na2O component is preferably 3.0% or more, more preferably 4.0% or more, even more preferably 5.0% or more, even more preferably 7.0% or more, even more preferably 10.0% or more, even more preferably 11.0% or more, and even more preferably 12.0% or more as the lower limit. On the other hand, by setting the content of the Na2O component to 25.0% or less, devitrification due to excessive content can be reduced. Therefore, the upper limit of the content of the Na2O component is preferably 25.0% or less, more preferably 23.0% or less, even more preferably 20.0% or less, and even more preferably 18.0% or less.
[0022] By setting the content of the MgO component to 10.0% or less, it is possible to suppress an increase in the refractive index while reducing devitrification. Therefore, the upper limit of the content of the MgO component is preferably set to 10.0% or less, more preferably set to 5.0% or less, even more preferably set to 3.0% or less, and even more preferably set to 1.0% or less.
[0023] By setting the CaO content at 10.0% or less, it is possible to suppress an increase in the refractive index while reducing devitrification. Therefore, the upper limit of the CaO content is preferably 10.0% or less, more preferably 5.0% or less, even more preferably 3.0% or less, and even more preferably 1.0% or less.
[0024] By setting the content of the BaO component to 10.0% or less, it is possible to reduce devitrification while suppressing an increase in the refractive index and an increase in the Abbe number. Therefore, the upper limit of the content of the BaO component is preferably 10.0% or less, more preferably 5.0% or less, even more preferably 3.0% or less, and even more preferably 1.0% or less.
[0025] By setting the content of the SrO component to 10.0% or less, it is possible to reduce devitrification while suppressing a decrease in the refractive index and an increase in the Abbe number. Therefore, the upper limit of the content of the SrO component is preferably set to 10.0% or less, more preferably 5.0% or less, even more preferably 3.0% or less, and even more preferably 1.0% or less.
[0026] The ZrO2 component is a component that can increase the refractive index of the glass, reduce the Abbe number, lower the partial dispersion ratio, and reduce devitrification. This also reduces devitrification and coloring during reheating. Therefore, the lower limit of the content of the ZrO2 component is preferably more than 0%, more preferably 1.0% or more, even more preferably 2.0% or more, even more preferably 3.0% or more, and even more preferably 4.0% or more. On the other hand, by keeping the content of the ZrO2 component at 25.0% or less, it is possible to reduce devitrification due to excessive content and to easily obtain a more homogeneous glass. Therefore, the upper limit of the content of the ZrO2 component is preferably 25.0% or less, more preferably less than 20.0%, even more preferably less than 15.0%, and even more preferably less than 13.0%.
[0027] By keeping the content of the TiO2 component at 10.0% or less, it is possible to suppress increases in the refractive index and dispersion due to excessive content. Therefore, the upper limit of the content of the TiO2 component is preferably 10.0% or less, more preferably 8.0% or less, even more preferably 7.0% or less, even more preferably 5.0% or less, even more preferably 3.0% or less, even more preferably 2.0% or less, and even more preferably 1.0% or less.
[0028] The WO3 and Bi2O3 components are components that increase the refractive index of glass, but if they are contained in large amounts, they cause the glass to become colored and its specific gravity to increase. The preferred ranges of the WO3 and Bi2O3 components are as follows:
[0029] The upper limit of the content of the WO3 component is preferably 10.0% or less, more preferably 5.0% or less, even more preferably 3.0% or less, and even more preferably 1.0% or less, but may be 0%.
[0030] The upper limit of the content of the Bi2O3 component is preferably 10.0% or less, more preferably 5.0% or less, further preferably 3.0% or less, and even more preferably 1.0% or less, but may be 0%.
[0031] If the content of the La2O3 component, the Y2O3 component, the Gd2O3 component, and the Yb2O3 component is high, the refractive index increases, the stability is lost, and the specific gravity increases. The preferred ranges of the La2O3 component, the Y2O3 component, the Gd2O3 component, and the Yb2O3 component are as follows:
[0032] The upper limit of the content of the La2O3 component is preferably 12.0% or less, more preferably less than 10.0%, even more preferably 8.0% or less, even more preferably 5.0% or less, even more preferably 3.0% or less, and even more preferably 1.0% or less, but may be 0%.
[0033] The upper limit of the Y2O3 content is preferably 10.0% or less, more preferably 8.0% or less, even more preferably 5.0% or less, still more preferably 3.0% or less, and most preferably 1.0% or less, but may be 0%.
[0034] The content of the Gd2O3 component is preferably less than 8.0%, more preferably 5.0% or less, even more preferably 3.0% or less, even more preferably 2.0% or less, even more preferably 1.0% or less, and most preferably 0.5% or less as the upper limit, but may be 0%.
[0035] The upper limit of the Yb2O3 component content is preferably 8.0% or less, more preferably 5.0% or less, even more preferably 2.0% or less, still more preferably 1.0% or less, and most preferably 0.5% or less, but may be 0%.
[0036] The Al2O3 component can reduce the refractive index and dispersion. Therefore, the content of the Al2O3 component may be preferably more than 0%, more preferably 0.5% or more, even more preferably 1.0% or more, and even more preferably 1.5%. In particular, by making the content of the Al2O3 component 10.0% or less, the meltability of the glass can be improved while the tendency of the glass to devitrify can be weakened. Therefore, the content of the Al2O3 component is preferably set to an upper limit of 10.0% or less, more preferably 8.0% or less, and even more preferably 6.0% or less.
[0037] The ZnO component is a component that enhances the devitrification resistance of the glass. In particular, by making the content of the ZnO component 5.0% or less, it is possible to easily obtain a glass with a low refractive index by reducing the specific gravity. Therefore, the upper limit of the content of the ZnO component is preferably 5.0% or less, more preferably 3.0% or less, and most preferably 1.0% or less, but it may be 0%.
[0038] The Ta2O5 component is a component that enhances the devitrification resistance of glass. On the other hand, by making the content of the Ta2O5 component 5.0% or less, the amount of the Ta2O5 component, which is a rare mineral resource, used is reduced, and the glass is more easily melted at a lower temperature, so that the production cost of the glass can be reduced. This also makes it possible to reduce the devitrification and specific gravity of the glass caused by the excessive content of the Ta2O5 component. Therefore, the upper limit of the content of the Ta2O5 component is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably 1.0% or less, but it may be 0%.
[0039] The upper limit of the content of the P2O5 component is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less, but may be 0%.
[0040] The upper limit of the F content is preferably 5.0% or less, more preferably 3.0% or less, more preferably 1.0% or less, further preferably 0.5% or less, and further preferably 0.3% or less, but may be 0%.
[0041] The upper limit of the content of the TeO2 component is preferably 3.0% or less, more preferably 2.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less, but may be 0%.
[0042] The upper limit of the GeO2 component content is preferably 3.0% or less, more preferably 2.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less, but may be 0%.
[0043] The upper limit of the CeO2 content is preferably 3.0% or less, more preferably 2.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less, but may be 0%.
[0044] The content of Er2O3 component and Pr2O3 component is preferably 1.0% or less, more preferably 0.5% or less, more preferably 0.1% or less, and most preferably substantially none is contained.
[0045] The upper limit of the content of the SnO2 component is preferably 2.0% or less, more preferably 1.0% or less, and further preferably 0.5% or less, but may be 0%.
[0046] The Sb2O3 component is an optional component that promotes clarification and defoaming when melting glass. By making the content of the Sb2O3 component 0.20% or less, it is possible to suppress coloring, particularly in high refractive index glass. Furthermore, by making the content 0.20% or less, excessive foaming during glass melting is unlikely to occur, making it difficult for the Sb2O3 component to be alloyed with the melting equipment (particularly precious metals such as Pt). Therefore, the upper limit of the content of the Sb2O3 component is preferably 0.20% or less, more preferably 0.10% or less, and even more preferably 0.08% or less, but it may be 0%.
[0047] The component for clarifying and defoaming the glass is not limited to the above Sb2O3 component, and any fining agent, defoaming agent or combination thereof known in the field of glass manufacturing can be used.
[0048] The C component is a component that can maintain a reducing atmosphere in the platinum crucible, suppress the incorporation of platinum into the glass due to oxidation, and improve the transmittance, but if the content is high, the cationic components in the glass are reduced, causing coloring of the glass. Therefore, the content of the C component is preferably 10.0% or less, more preferably 8.0% or less, more preferably 6.0% or less, and most preferably 5.0% or less as the upper limit. On the other hand, the content of the C component is preferably more than 0%, more preferably 0.5% or more, even more preferably 1.0% or more, and most preferably 2.0% or more as the lower limit, but may be 0%.
[0049] The S component is a component that can maintain a reducing atmosphere in the platinum crucible, suppress the incorporation of platinum into the glass due to oxidation, and improve the transmittance, but if the content is high, the cationic components in the glass are reduced, causing coloring of the glass. Therefore, the upper limit of the S component content is preferably 10.0% or less, more preferably 8.0% or less, more preferably 6.0% or less, and most preferably 5.0% or less. On the other hand, the lower limit of the S component content is preferably more than 0%, more preferably 0.5% or more, even more preferably 1.0% or more, and most preferably 2.0% or more, but it may be 0%.
[0050] Organic components such as sucrose are components that can maintain a reducing atmosphere in the platinum crucible, suppress the incorporation of platinum into the glass due to oxidation, and improve the transmittance, but if the content is high, the cationic components in the glass are reduced, causing coloring of the glass. Therefore, the content of organic components such as sucrose is preferably 10.0% or less, more preferably 8.0% or less, more preferably 6.0% or less, and most preferably 5.0% or less as the upper limit. On the other hand, the content of organic components such as sucrose is preferably more than 0%, more preferably 0.5% or more, even more preferably 1.0% or more, and most preferably 2.0% or more as the lower limit, but may be 0%.
[0051] By setting the sum of the contents (sum of mass) of the Ln2O3 component (wherein Ln is one or more selected from the group consisting of La, Y, Gd, and Yb) to 12.0% or less, devitrification due to excessive content can be suppressed and the refractive index can be maintained. Therefore, the upper limit is preferably 12.0% or less, more preferably 10.0% or less, even more preferably 8.0% or less, even more preferably 6.0% or less, even more preferably 4.0% or less, and even more preferably 2.0% or less, but it may be 0%.
[0052] By setting the sum of the contents of Rn2O components (wherein Rn is one or more selected from the group consisting of Li, Na, and K) to 5.0% or more, the melting property of the glass raw material can be improved, and the partial dispersion ratio can be reduced while maintaining a low transition point. Therefore, the sum of the contents of Rn2O components is preferably set to 5.0% or more, more preferably 8.0% or more, even more preferably 10.0% or more, even more preferably 12.0% or more, and even more preferably 13.0% or more as the lower limit. On the other hand, by setting the sum of the contents of Rn2O components to 25.0% or less, the increase in the Abbe number can be suppressed. The sum of the contents of Rn2O components is preferably set to 25.0% or less, more preferably 23.0% or less, even more preferably 20.0% or less, and even more preferably 18.0% or less as the upper limit.
[0053] By setting the sum of the contents of RO components (wherein R is one or more selected from the group consisting of Mg, Ca, Sr, and Ba) to 10.0% or less, it is possible to suppress an increase in the Abbe number and reduce devitrification of the glass due to the excessive content of these components. Therefore, the upper limit of the mass sum of the RO components is preferably 25.0% or less, more preferably less than 15.0%, even more preferably less than 10.0%, even more preferably less than 5.0%, and even more preferably less than 2.0%.
[0054] The mass ratio ZrO2 / Nb2O5, which is the ratio of ZrO2 to the Nb2O5 component, can be set to 0.900 or less to improve devitrification resistance. The mass ratio ZrO2 / Nb2O5 is preferably set to 0.900 or less, more preferably 0.870 or less, even more preferably 0.850 or less, even more preferably 0.830 or less, even more preferably 0.800 or less, even more preferably 0.780 or less, and even more preferably 0.750 or less as the upper limit. On the other hand, the mass ratio ZrO2 / Nb2O5 can be set to 0.200 or more to lower the partial dispersion ratio and reduce the Abbe number. Therefore, the mass ratio Nb2O5 / ZrO2 is preferably set to 0.200 or more, more preferably 0.230 or more, and even more preferably 0.250 or more as the lower limit.
[0055] When the total mass of the SiO2 component and the B2O3 component, SiO2+B2O3, is 27.0% or more, the devitrification resistance and chemical durability of the glass can be improved. The total mass of the SiO2+B2O3 is preferably 27.0% or more, more preferably 30.0% or more, even more preferably 33.0% or more, and even more preferably 35.0% or more as the lower limit. On the other hand, when the total mass of the SiO2+B2O3 is 50.0% or less, the deterioration of stability due to excessive content can be suppressed. Therefore, the total mass of the SiO2+B2O3 is preferably 50.0% or less, more preferably 53.0% or less, even more preferably 50.0% or less, and even more preferably 48.0% or less as the upper limit.
[0056] When the mass sum Nb2O5+ZrO2, which is the total amount of the Nb2O5 component and the ZrO2 component, is 20.0% or more, the partial dispersion ratio can be lowered, the dispersion can be increased, and the chemical durability can be improved. The mass sum Nb2O5+ZrO2 is preferably 20.0% or more, more preferably 23.0% or more, even more preferably 25.0% or more, and even more preferably 27.0% or more as the lower limit. On the other hand, when the mass sum Nb2O5+ZrO2 is 40.0% or less, the deterioration of stability due to excessive content can be suppressed. Therefore, the mass sum Nb2O5+ZrO2 is preferably 40.0% or less, more preferably 38.0% or less, even more preferably 35.0% or less, and even more preferably 33.0% or less as the upper limit.
[0057] The mass ratio (SiO2+B2O3) / Rn2O, which is the sum of the total amount of the SiO2 component and the B2O3 component relative to the sum of the contents of the Rn2O component, is set in the range of more than 0 and not more than 10.0, thereby improving the devitrification resistance and chemical durability of the glass, improving the reheat press moldability, and suppressing a decrease in the refractive index. The mass ratio (SiO2+B2O3) / Rn2O is preferably more than 0, more preferably 1.00 or more, even more preferably 2.00 or more, and even more preferably 3.00 or more as the lower limit. On the other hand, the mass ratio (SiO2+B2O3) / Rn2O is preferably 10.0 or less, more preferably 8.00 or less, even more preferably 7.00 or less, and even more preferably 6.00 or less as the upper limit.
[0058] <Ingredients that should not be included> Next, components that should not be contained in the optical glass of the present invention and components that are undesirable to be contained therein will be described. The ingredients will be explained.
[0059] Other components may be added as necessary to the extent that they do not impair the properties of the glass of the present invention. However, transition metal components such as Nd, V, Cr, Mn, Fe, Co, Ni, Cu, Ag, and Mo, excluding Ti, Zr, Nb, W, La, Gd, Y, Yb, and Lu, have the property of coloring the glass and absorbing specific wavelengths in the visible range even when contained alone or in combination in small amounts, so that it is preferable that they are substantially free of such components, particularly in optical glasses that use wavelengths in the visible range.
[0060] Furthermore, since lead compounds such as PbO and arsenic compounds such as As2O3 are components that have a high environmental impact, it is desirable that they are not contained substantially, that is, that they are not contained at all except for unavoidable contamination.
[0061] Furthermore, in recent years, there has been a trend to refrain from using the components Th, Cd, Tl, Os, Be, and Se as harmful chemical substances, and environmental measures are required not only in the glass manufacturing process but also in the processing process and disposal after commercialization. Therefore, when environmental impact is important, it is preferable that these components are not substantially contained.
[0062] [Physical Properties] The refractive index (n d ) is preferably 1.64000 or less, more preferably 1.63500 or less, and even more preferably 1.63000 or less. On the other hand, this refractive index (n d ) may have a lower limit of preferably 1.58000 or more, more preferably 1.59000 or more, and even more preferably 1.60000 or more. On the other hand, the Abbe number (ν d )This Abbe number (ν d The upper limit of the Abbe number (ν d ) may have a lower limit of preferably 35.00 or more, more preferably 36.00 or more, and even more preferably 38.00 or more.
[0063] The optical glass of the present invention has a low partial dispersion ratio (θg,F). More specifically, the upper limit of the partial dispersion ratio (θg,F) of the optical glass of the present invention is preferably 0.586 or less, more preferably 0.585 or less, and further preferably 0.584 or less. This makes it possible to obtain an optical glass having a low partial dispersion ratio (θg,F), and therefore an optical element formed from this optical glass can be used to reduce chromatic aberration in an optical system.
[0064] On the other hand, in the optical glass of the present invention, the partial dispersion ratio (θg,F) and the Abbe number (ν d ) but θg,F≦(-0.00187×ν d It is preferable that the relationship θg,F≦(−0.00187×ν +0.651) is satisfied. d It is more preferable that the relationship θg,F≦(−0.00187×ν +0.650) is satisfied. d It is more preferable that the relationship θg,F≦(−0.00187×ν d It is even more preferable that the relationship be satisfied.
[0065] Furthermore, since the optical glass of the present invention has small anomalous dispersion (Δθg,F), it is easy to obtain a lens that can correct chromatic aberration with high accuracy. The upper limit of the anomalous dispersion (Δθg,F) is preferably −0.0020 or less, more preferably −0.0030 or less, even more preferably −0.0040 or less, and still more preferably −0.0050 or less.
[0066] Generally, chromatic aberration is corrected by combining a low-dispersion convex lens with a high-dispersion concave lens, but this combination can only correct aberrations in the red and green regions, and aberrations in the blue region remain. This aberration in the blue region that cannot be completely removed is called the secondary spectrum. To correct the secondary spectrum, it is necessary to carry out optical design that takes into account the trends of the g-line (435.835 nm) in the blue region. At this time, the partial dispersion ratio (θg,F) is used as an index of optical characteristics that are focused on in optical design. In an optical system that combines the above-mentioned low-dispersion lens and high-dispersion lens, the secondary spectrum is well corrected by using an optical material with a large partial dispersion ratio (θg,F) for the lens on the low-dispersion side and an optical material with a small partial dispersion ratio (θg,F) for the lens on the high-dispersion side.
[0067] The partial dispersion ratio (θg,F) is expressed by the following formula (1). θg,F=(ng-nF) / (nF-nC) (1)
[0068] Optical glass has a partial dispersion ratio (θg,F) that indicates partial dispersion in the short wavelength range and an Abbe number (ν d ) is approximately linearly related to the Abbe number (ν d ) on the horizontal axis, it is represented by a straight line connecting two points on which the partial dispersion ratio and Abbe number of NSL7 and PBM2 are plotted, and is called the normal line. The normal glass that is the standard for the normal line varies depending on the optical glass manufacturer, but each company defines it with roughly the same slope and intercept. (NSL7 and PBM2 are optical glasses manufactured by Ohara Inc., and the Abbe number (ν d ) is 36.3, the partial dispersion ratio (θg,F) is 0.5828, and the Abbe number of NSL7 (ν d ) is 60.5, and the partial dispersion ratio (θg,F) is 0.5436.
[0069] [Manufacturing method] The optical glass of the present invention is produced, for example, as follows. That is, the above-mentioned raw materials are mixed uniformly so that each component falls within a predetermined content range, the mixture produced is put into a platinum crucible, and melted in an electric furnace at a temperature range of 1100 to 1400°C for 1.5 to 5 hours depending on the degree of difficulty of melting the glass raw materials, stirred and homogenized, then cooled to an appropriate temperature, cast into a mold, and slowly cooled to produce the glass. Melting may be performed using a quartz crucible and then using a platinum crucible.
[0070] [Glass molding] The glass of the present invention can be melt-molded by a known method. However, the means for shaping the glass melt is not limited.
[0071] [Optical elements] A glass molded body can be produced from the produced optical glass by, for example, polishing means or mold press molding means such as reheat press molding or precision press molding. That is, a glass molded body can be produced by subjecting the optical glass to mechanical processing such as grinding and polishing. The means for producing the glass molded body are not limited to these means.
[0072] Thus, the optical glass of the present invention is useful for various optical elements and optical designs. Among them, it is particularly preferable to manufacture optical elements such as lenses and prisms. This not only reduces the weight of the optical elements, but also realizes high-definition and high-precision imaging and projection characteristics when used in optical instruments such as cameras and projectors. EXAMPLES
[0073] The compositions of the examples and comparative examples of the glass of the present invention and the refractive index (n d ), Abbe number (ν d ), partial dispersion ratio (θg,F), and anomalous dispersion (Δθg,F) are shown in Tables 1 to 4. The glass of the comparative example is the glass of Example 1 of JP-A 2008-297198.
[0074] The glasses of the examples of the present invention were all produced by selecting high-purity raw materials for each component that are used in ordinary optical glass, such as the corresponding oxides, hydroxides, carbonates, nitrates, sulfates, fluorides, and metaphosphate compounds, weighing them out to give the composition ratios of each example shown in the table, mixing them uniformly, and then placing them in a platinum crucible and melting them in an electric furnace at a temperature range of 1100 to 1400°C for 1.5 to 5 hours depending on the melting difficulty of the glass raw materials.Then, after stirring and homogenizing the mixture, the mixture was poured into a mold or the like and allowed to cool slowly.
[0075] The refractive index (n d ), Abbe number (ν d ), partial dispersion ratio (θg,F), and anomalous dispersion (Δθg,F) were measured according to the V-block method specified in JIS B 7071-2:2018. Here, the refractive index (n d ) is shown as a measurement value for the d line (587.56 nm) of a helium lamp. d ) is the refractive index for the d line of the helium lamp (n d ) and the refractive index (n F ), and the refractive index for the C line (656.27 nm) (n C ) value, the Abbe number (ν d )=[(n d -1) / (n F -n C The refractive indexes (n d ), Abbe number (ν d ) was determined by measuring the glass obtained by cooling at a rate of -25°C / hr. And the resulting Abbe number (ν d ) and the partial dispersion ratio (θg,F), the relation (θg,F=-a×ν d +b) We found the intercept b when the slope a is 0.00187. Furthermore, the normal line (a straight line connecting two points on which the partial dispersion ratio and Abbe number of NSL7 and PBM2 are plotted) is the Abbe number (ν d) is 36.3, the partial dispersion ratio (θg,F) is 0.5828, and the Abbe number of NSL7 (ν d ) is 60.5, and the partial dispersion ratio (θg,F) is 0.5436. The anomalous dispersion (Δθg,F) was calculated from the difference between the partial dispersion ratio (θg,F) value shown above and the measured partial dispersion ratio (θg,F) value.
[0076] [Table 1]
[0077] [Table 2]
[0078] [Table 3]
[0079] [Table 4]
[0080] As shown in the table, the glasses of the examples of the present invention all have a refractive index (n d ) is 1.64000 or less, and the Abbe number (ν d ) was less than or equal to 43.00, which was within the desired range.
[0081] The optical glass of the embodiment has an Abbe number (ν d ) is within a desired range, and the partial dispersion ratio (θ g,F) is an optical glass with a small
[0082] Although the present invention has been described in detail for purposes of illustration, it will be understood that the present embodiments are for illustrative purposes only and that numerous modifications may be made by those skilled in the art without departing from the spirit and scope of the invention.
Claims
1. Refractive index (n d ) is less than or equal to 1.64000 Abbe number (ν d ) is 43.00 or less, Oxide based mass% SiO 2 Ingredients: 20.00-50.00%, B 2 O 3 Ingredients are over 0% 25.0% Mass ratio ZrO 2 / Nb 2 O 5 is 0.200 to 0.900, Optical glass.
2. An optical element comprising the optical glass according to claim 1.
Citation Information
Patent Citations
Optical glass of dense barium flint position
JP2008297198A
Optical glass, optical element prepared with optical glass, and optical device
JP2016222511A