Production method and production device of particles of compound by crystallization operation
The three-layer liquid tank system using buoyancy and air bubbles efficiently produces high-sphericity compound particles by avoiding solvent evaporation, addressing inefficiencies in conventional crystallization methods and enabling rapid, controlled production of spherical and hollow particles.
Patent Information
- Application Number
- JP2023052208
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional crystallization methods for producing compound particles face inefficiencies due to the need for solvent evaporation or cooling to create a supersaturated state, which can take a long time and are difficult to control, leading to challenges in achieving desired particle size and distribution.
A method involving a three-layer liquid tank system with a poor solvent, separation solvent, and good solvent layers, utilizing buoyancy and air bubbles to transport granules from the separation layer to the poor solvent layer, allowing for supersaturation without cooling or evaporation, enabling efficient production of spherical and hollow particles under normal conditions.
This approach allows for rapid production of high-sphericity compound particles with controlled size and distribution, enhancing efficiency and stability, and enables the production of hollow particles with unique properties for various applications.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to a method and an apparatus for producing particles of a compound by crystallization. [Background technology]
[0002] Conventionally, particles of compounds have been used in various applications, such as resin fillers, light diffusing materials, paints, medical products, and cosmetics. Such particles of compounds may be produced by using a crystallization procedure. According to the crystallization procedure, a compound dissolved in a good solvent is brought into a supersaturated state, so that nucleation and particle growth can proceed. Therefore, the crystallization procedure is suitable for separating and refining compounds and producing particles.
[0003] Various crystallization methods for producing particles of a compound have been disclosed so far. For example, Non-Patent Document 1 below discloses a reprecipitation method in which a solution in which a compound is dissolved in a good solvent is injected into a poor solvent using a microsyringe to obtain particles. In addition, Non-Patent Document 2 discloses a double emulsion solvent distillation method and an emulsion solvent diffusion method in which particles of a compound are obtained by evaporating a good solvent or mixing a poor solvent after forming a W / O / W emulsion. Patent Document 1 discloses an evaporation crystallization method in which a solution in which a poorly water-soluble compound is dissolved or dispersed in a poorly water-soluble organic solvent is supplied to stirred water, and the organic solvent is evaporated at a high temperature below the boiling point of water to obtain particles of the compound. [Prior art documents] [Patent documents]
[0004] [Non-Patent Document 1] Hitoshi Kasai, Koichi Baba, Hachiro Nakanishi, Yosuke Miyashita, J.Jpn.Soc.Colour Mate.,82(9),411-416(2009) [Non-Patent Document 2] Kohei Tahara, Hiromitsu Yamamoto, Hirofumi Takeuchi, Yoshiaki Kawashima, YAKUGAKU ZASSHI, 127(10), 1541-1548(2007) [Patent Document 1] Patent No. 4395897 Summary of the Invention [Problem to be solved by the invention]
[0005] In the crystallization process for producing the above-mentioned compound particles, in many cases, a supersaturated state is produced by evaporation or cooling of a good solvent. However, in such a method, the particles are grown while the compound concentration increases due to evaporation of the solvent and the solubility changes due to cooling, so that it may take a very long time. In addition, it may not be easy to control the conditions such as the concentration and temperature of the solution to obtain desired particles having a suitable size and particle size distribution, or to control the growth of the particles. Thus, there is still room for improvement in the technology for producing compound particles by crystallization process in terms of improving the production efficiency. [Means for solving the problem]
[0006] The inventors of the present invention have succeeded in developing a technology for more efficiently producing compound particles by a novel crystallization procedure that differs from the method of creating a supersaturated state by cooling or evaporating a good solvent through their own research. The present invention can be realized, for example, in the following forms.
[0007] [First embodiment] The first embodiment of the present invention is provided as a method for producing particles of a compound by a crystallization operation. The production method of the first embodiment includes the steps of: preparing a liquid tank having a poor solvent layer made of a poor solvent for the compound, and a separation layer arranged below the poor solvent layer, the separation layer being made of a separation solvent that is denser than the poor solvent, immiscible with the poor solvent, and undergoes phase separation; generating granules of a good solvent solution in the separation layer by dissolving the compound in a good solvent that is immiscible with the separation solvent; and transporting the granules from the separation layer to the poor solvent layer by buoyancy, thereby precipitating the compound in the poor solvent layer. According to this embodiment of the manufacturing method, the good solvent solution in which the compound is dissolved can be made into a granular state close to a sphere, and can be easily transported to the poor solvent layer by utilizing the buoyancy in the separation layer. In addition, in the poor solvent layer, the good solvent solution can be made into a supersaturated state while still in the granular state, so that compound particles with high sphericity can be precipitated. This crystallization operation does not require cooling or evaporation of the good solvent, and can be performed even under conditions of room temperature and normal pressure, and compound particles can be easily obtained in a short time. In addition, by continuously introducing the granular body into the separation layer, compound fine particles can be continuously generated in large quantities in the poor solvent layer at high speed. Therefore, compound particles can be manufactured more efficiently.
[0008] [Second mode] In the manufacturing method of the first mode, the liquid tank further has a good solvent layer composed of the good solvent solution having a higher density than the separation solvent, the good solvent layer, the separation layer and the poor solvent layer are stacked in order from the bottom up in the liquid tank, and the granules are formed by introducing air bubbles into the good solvent layer, and may be transported from the good solvent layer through the separation layer to the poor solvent layer by the buoyancy of the air bubbles. According to the second embodiment of the manufacturing method, the good solvent solution can be easily transported in a granular state to the poor solvent layer by introducing air bubbles into the good solvent layer, making it easier to manufacture compound particles. In addition, the granular body can be continuously transported to the poor solvent layer simply by continuously introducing air bubbles into the good solvent layer, so a large amount of particles can be continuously manufactured. Furthermore, hollow particles are easily formed with the air bubbles as cores, so that hollow particles can be efficiently manufactured without performing a process of removing the cores of the particles.
[0009] [Third Mode] In the manufacturing method of the second mode, the granules may be formed by introducing the air bubbles from the separation layer into the good solvent layer. According to the manufacturing method of the third embodiment, particles with higher sphericity can be easily formed.
[0010] [Fourth feature] In the manufacturing method according to the second or third feature, the bubbles may be composed of an inert gas. According to the fourth embodiment of the manufacturing method, the bubbles are prevented from shrinking or disappearing due to reaction with other substances or ions present in the liquid tank, which makes it possible to more efficiently transport the good solvent solution by the bubbles, and thus makes it possible to more efficiently manufacture compound particles.
[0011] [Fifth aspect] In the manufacturing method according to any one of the second, third and fourth aspects, the bubbles may have a diameter of less than 200 μm. According to the fifth embodiment of the manufacturing method, by using bubbles equivalent to Fine Bubbles (registered trademark), it is possible to easily manufacture finer particles. In addition, since fine bubbles are prevented from disappearing during the crystallization operation, hollow particles can be obtained more efficiently.
[0012] [Sixth aspect] In the production method according to any one of the first, second, third, fourth and fifth aspects, the compound may be composed of a poorly water-soluble compound, and the good solvent and the poor solvent may be composed of a water-insoluble solvent, respectively. According to the sixth embodiment of the production method, it is possible to promote aggregation of the poorly water-soluble compound dissolved in a good solvent on the bubble surfaces, and it is possible to further increase the efficiency of particle production.
[0013] [Seventh embodiment] In the manufacturing method described in the sixth embodiment, the compound may be composed of a polymer such as polystyrene, polybutylene succinate, polylactic acid, etc., the good solvent and the poor solvent may be composed of an organic solvent such as hexane, toluene, octane, isooctane, decane, chloroform, etc., respectively, and the separation solvent may be composed of a water-soluble solvent such as water. According to the seventh embodiment of the production method, since the separation of the separation solvent can be improved by using a suitable good solvent and poor solvent, the crystallization operation can be performed more easily and stably. Therefore, the compound particles can be produced more efficiently.
[0014] [Eighth embodiment] The eighth embodiment of the present invention is provided as a manufacturing apparatus for manufacturing particles of a compound by a crystallization operation. The manufacturing apparatus of the eighth embodiment includes a liquid tank having a poor solvent layer made of a poor solvent for the compound, and a separation layer made of a separation solvent that is denser than the poor solvent, immiscible with the poor solvent, and undergoes phase separation and is disposed below the poor solvent layer, and a granule generating unit that generates in the separation layer granules that are made of a good solvent solution in which the compound is dissolved in a good solvent immiscible with the separation solvent, are transported to the poor solvent layer by the buoyancy in the separation layer, and are granulated by precipitation of the compound in the poor solvent layer. According to the eighth embodiment of the manufacturing apparatus, the good solvent solution in which the compound is dissolved can be made into granular form close to a sphere, and can be easily transported to the poor solvent layer by utilizing the buoyancy in the separation layer. In addition, since the good solvent solution can be made into a supersaturated state in the granular form in the poor solvent layer, the compound can be precipitated in a particulate state. Therefore, compound particles with high sphericity can be efficiently manufactured.
[0015] [9th form] In the manufacturing apparatus of the 8th form, the liquid vat further has a good solvent layer composed of the good solvent solution having a higher density than the separation solvent, the good solvent layer, the separation layer and the poor solvent layer being stacked in order from the bottom up in the liquid vat, and the granule generation section may include an air bubble introduction section which generates the granules by introducing air bubbles into the good solvent layer. According to the ninth embodiment of the manufacturing apparatus, the good solvent solution can be easily transported in a granular state to the poor solvent layer by introducing bubbles into the good solvent layer using the bubble introduction unit, which makes it easier to manufacture compound particles. In addition, the granular body can be continuously transported to the poor solvent layer simply by continuously introducing bubbles into the good solvent layer using the bubble introduction unit, so a large amount of particles can be continuously manufactured. Furthermore, hollow particles are easily formed with the bubbles as their cores, which makes it possible to efficiently manufacture hollow particles without performing a process of removing the cores of the particles.
[0016] The present invention can be realized in various forms other than the method and apparatus for producing particles of a compound by a crystallization procedure. For example, the present invention can be realized in the form of particles produced by the method or apparatus, or products using the particles. The present invention can also be realized in the form of a method for performing the crystallization procedure, a method for separating and purifying a compound by the crystallization procedure, a machine, tool, or device for performing the crystallization procedure, a control device or control program for controlling an apparatus for producing particles of a compound, etc. [Brief description of the drawings]
[0017] [Figure 1] 1A to 1C are schematic views for explaining a manufacturing method according to a first embodiment. [Diagram 2] FIG. 6 is a schematic diagram for explaining a manufacturing method according to a second embodiment. [Diagram 3] FIG. 11 is a schematic diagram for explaining a manufacturing method according to a third embodiment. [Figure 4] FIG. 2 is an explanatory diagram showing a photographic image of the state of a liquid tank after a crystallization operation obtained in an example. [Diagram 5] FIG. 11 is a first explanatory diagram showing a table summarizing the photographed images obtained in the examples. [Figure 6] FIG. 2 is a second explanatory diagram showing a table summarizing the photographed images obtained in the examples. [Figure 7] FIG. 2 is an explanatory diagram showing a graph created based on the measurement results of hollow particles obtained in the examples. [Figure 8] FIG. 1 is a first explanatory diagram showing the relationship between the concentration of a good solvent solution and the dimensions of hollow particles. [Figure 9] FIG. 2 is a second explanatory diagram showing the relationship between the concentration of a good solvent solution and the dimensions of hollow particles. [Figure 10] FIG. 13 is an explanatory diagram showing a table summarizing photographed images obtained in a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the method for producing particles of a compound by a crystallization procedure according to the present invention will be described with reference to the drawings.
[0019] 1. First embodiment: FIG. 1 is a schematic diagram showing the configuration of a particle production apparatus 10 according to a first embodiment and the particle production process in the production apparatus 10. As shown in FIG.
[0020] In the manufacturing method of the first embodiment, particles of a compound are manufactured by a crystallization operation in which a compound dissolved in a good solvent is made supersaturated using a poor solvent and precipitated. The compound targeted by this manufacturing method may be any compound that has a solvent in which it can be dissolved. In this embodiment, the compound is a poorly water-soluble compound, for example, a polyester resin such as polystyrene (PS), polybutylene succinate (PBS), or polylactic acid (PLA).
[0021] The compound is not limited to the above-mentioned polymer, and may be another polymer. The compound is not limited to the polymer. In another embodiment, the compound may be another organic compound or an inorganic compound. The compound may not be a poorly water-soluble compound, and may be a water-soluble compound.
[0022] In the following, first, the configuration of the production apparatus 10 for carrying out the crystallization operation will be described, and then the method for producing particles of a compound by the crystallization operation in the production apparatus 10 will be described.
[0023] 1-1. Manufacturing equipment configuration: The production apparatus 10 includes a liquid tank 11, an air bubble introducing section 20, and a stirrer 25. The liquid tank 11 contains a liquid that is separated into a poor solvent layer 12, a separating layer 13, and a good solvent layer 14.
[0024] The poor solvent layer 12 is composed of a poor solvent for the compound. The type of poor solvent can be appropriately selected according to the type of compound. As the poor solvent, for example, hydrocarbons such as hexane, benzene, toluene octane, 2,2,4-trimethylpentane (isooctane), and decane, halogenated hydrocarbons such as chloroform, dichloromethane, and dichlorobenzene, ketones such as cyclohexanone and methyl isobutyl ketone, and ethers such as diisopropyl ether can be adopted. In order to improve the separation property with respect to a separation solvent described later that is composed of a water-soluble solvent, it is preferable that the poor solvent is composed of a water-insoluble solvent. In addition, when the separation solvent is composed of water, the above-mentioned type of poor solvent is preferable because it has a lower specific gravity than water.
[0025] When the compound is a polymer such as PS, PBS, or PLA, the poor solvent may be, for example, hexane. Alternatively, an organic solvent such as octane, isooctane, decane, or diisopropyl ether may be used as the poor solvent. The poor solvent may be an organic solvent other than those mentioned above. In another embodiment, the poor solvent may be a water-soluble solvent.
[0026] The separation layer 13 is composed of a separation solvent that is a solvent that has a higher density than the poor solvent, is immiscible with the poor solvent, and undergoes phase separation. Thus, the separation layer 13 is disposed under the poor solvent layer 12 in the liquid tank 11 in a separated state.
[0027] In this embodiment, the separation solvent is composed of a water-soluble solvent. When the separation solvent is composed of a water-soluble solvent, if the poor solvent is composed of a water-insoluble solvent, the separation property between the poor solvent and the separation solvent can be improved, and therefore, the poor solvent in the poor solvent layer 12 and the separation solvent in the separation layer 13 can be further prevented from being mixed during the crystallization operation.
[0028] As the separation solvent for the water-soluble solvent, for example, water, glycerin, ethylene glycol, etc. can be adopted. In addition, in another embodiment, the separation solvent may be composed of a water-insoluble solvent that is immiscible with the poor solvent and the good solvent.
[0029] Good solvent layer 14 is composed of a good solvent solution in which a compound is dissolved in a good solvent that has a higher density than the separation solvent and is immiscible with the separation solvent. As a result, good solvent layer 14 is disposed in a separated state below separation layer 13 in liquid tank 11. The concentration of the compound in the good solvent solution can be, for example, about 0.1 to 1.0 wt %. However, the concentration of the compound in the good solvent solution is not limited to this numerical range.
[0030] The type of the good solvent may be appropriately selected depending on the type of compound. Although it depends on the type of compound, the good solvent may be, for example, an organic solvent such as a hydrocarbon such as hexane, benzene, toluene, octane, isooctane, or decane, a halogenated hydrocarbon such as chloroform, dichloromethane, or dichlorobenzene, a ketone such as cyclohexanone or methyl isobutyl ketone, or an ether such as diisopropyl ether.
[0031] When the compound is a polymer such as PS, PBS, or PLA, the good solvent is preferably, for example, chloroform, but is not limited to chloroform and may be other organic solvents or inorganic solvents.
[0032] As described above, in this embodiment, since the separation solvent is composed of a water-soluble solvent, it is preferable that the good solvent is composed of a water-insoluble solvent, similar to the poor solvent. This can enhance the separability between the good solvent solution and the separation solvent, and can prevent the good solvent solution in the good solvent layer 14 and the separation solvent in the separation layer 13 from being mixed during the crystallization operation. The good solvent is not limited to a water-insoluble solvent, and may be composed of a water-soluble solvent.
[0033] The air bubble introducing section 20 is configured to be able to introduce air bubbles into the good solvent layer 14. The air bubble introducing section 20 constitutes a granular material generating section that generates granular materials 16 (described later) in the separation layer 13 by introducing air bubbles 14 into the good solvent layer 14. The air bubble introducing section 20 can be configured, for example, by a sparger, which is a fine bubble generator using a micropore system. The air bubble introducing section 20 has a cylindrical main body, with a front end side disposed within the liquid tank 11 and a rear end side disposed outside the liquid tank 11.
[0034] A gas for generating bubbles is supplied from a gas supply unit (not shown) through an opening at the rear end into the inside of the main body of the air bubble introduction part 20. In this embodiment, for example, an inert gas such as nitrogen is supplied. A large number of fine pores are densely formed on the tip side of the air bubble introduction part 20, and bubbles are generated by gas flowing out of the fine pores into the liquid.
[0035] According to the air bubble introducing section 20 having the above-mentioned configuration, air bubbles can be easily generated while suppressing turbulence in the layers 12, 13, 14 in the liquid tank 11. Therefore, mixing of the layers 12, 13, 14 due to the introduction of air bubbles can be suppressed.
[0036] The air bubble introduction part 20 preferably has micropores with a diameter of less than 200 μm. This allows the air bubble introduction part 20 to generate air bubbles with a diameter of less than 200 μm. The air bubble introduction part 20 may have micropores with a diameter of less than 100 μm. With such an air bubble introduction part 20, it is possible to generate fine air bubbles equivalent to fine bubbles with a diameter of 100 μm or less.
[0037] The air bubble introducing part 20 is disposed so as to introduce air bubbles into the layer below the poor solvent layer 12. In this embodiment, the tip of the air bubble introducing part 20 is disposed so as to be located in the good solvent layer 14. This allows the air bubble introducing part 20 to generate air bubbles directly in the good solvent layer 14. The air bubble introducing part 20 may be configured so as to generate air bubbles in the separation layer 13 as well as in the good solvent layer 14.
[0038] Stirrer 25 is, for example, a magnetic stirrer. Stirrer 25 is disposed at the bottom of liquid tank 11. In this embodiment, stirrer 25 is disposed in good solvent layer 14 and stirs the good solvent solution in good solvent layer 14. By stirring with stirrer 25, it is possible to adjust the particle size and dispersibility of the bubbles introduced into good solvent layer 14. In other embodiments, stirrer 25 may be omitted.
[0039] 1-2. Manufacturing method of compound particles: The manufacturing process of compound particles in the manufacturing apparatus 10 will be described with reference to Fig. 1. For convenience, Fig. 1 shows a schematic diagram of a trajectory of one air bubble 15 and a granular material 16 moving due to buoyancy, but in reality, a large number of air bubbles 15 and granular material 16 are continuously formed in the good solvent layer 14 and transported to the separation layer 13 and the poor solvent layer 12.
[0040] In the first step, a liquid tank 11 is prepared in a state in which the above-mentioned good solvent layer 14, separation layer 13, and poor solvent layer 12 are laminated in this order from the bottom. In the liquid tank 11, the air bubble introduction section 20 and the stirrer 25 are disposed at the above-mentioned positions. The concentration of the good solvent solution constituting the good solvent layer 14 is preferably adjusted in advance according to the target dimensions of the particles to be produced, such as the particle size and shell thickness of the particles. As will be described in the examples below, the relationship between the concentration of the good solvent solution and the dimensions of the particles to be produced can be obtained in advance by experiments, etc.
[0041] In the second step, the air bubble introducing part 20 introduces the air bubbles 15 into the good solvent layer 14. In this embodiment, the air bubble introducing part 20 introduces the air bubbles 15 having a diameter of less than 200 μm. The particle size of the air bubbles 15 can be adjusted by the flow rate of the gas supplied to the air bubble introducing part 20 or by stirring with the stirrer 25. The dispersibility of the air bubbles 15 may also be adjusted by stirring with the stirrer 25.
[0042] The air bubbles 15 introduced into the good solvent layer 14 move to the separation layer 13 by buoyancy. At this time, the good solvent solution adsorbed to the air bubbles 15 is introduced into the separation layer 13 together with the air bubbles 15 by the buoyancy of the air bubbles 15, and granular bodies 16, which will be described below, are generated. In this specification, the term "granular bodies" is used as a broad concept to represent an object having a granular external shape. Therefore, when simply calling it a "granular body," its components and size are not particularly limited, and there is no distinction between gas, liquid, and solid, and there is no distinction between hollow and solid. The good solvent solution adsorbed to the air bubbles 15 and transported to the separation layer 13 forms a thin film of the good solvent solution that covers the entire air bubbles 15 due to the effects of the viscosity and surface tension of the good solvent solution, and forms hollow granular bodies 16 with the air bubbles 15 as the core. Alternatively, although not shown, the good solvent solution transported to separation layer 13 while adsorbed to air bubbles 15 may form droplet-like granules 16 adsorbed to a portion of air bubbles 15. The hollow or solid granules 16 of the good solvent solution introduced into separation layer 13 are transported to poor solvent layer 12 by the buoyancy of air bubbles 15.
[0043] The granules 16 are transported to the poor solvent layer 12 in a state close to a sphere, i.e., in a state of high sphericity. When the granules 16 are introduced into the poor solvent layer 12, a state of supersaturation of the compound occurs in the granules 16 due to contact between the good solvent solution and the poor solvent, and the compound precipitates. In the hollow granules 16, aggregation of the precipitated compound progresses along the gas-liquid interface, and hollow particles are formed with the air bubbles 15 as nuclei. As the precipitation and aggregation of the compound progresses, it may become impossible to maintain the state of covering the entire air bubbles 15, but even in this case, solid particles with high sphericity are formed. Also, even in the solid granules 16, the compound precipitates and aggregates inside, maintaining the high sphericity and forming solid particles.
[0044] As described above, according to the manufacturing method of the first embodiment, the granules 16 of the good solvent solution can be easily generated in the separation layer 13 by introducing the bubbles 15 into the good solvent layer 12 by the bubble introducing unit 20. In addition, the granules 16 can be easily transported from the separation layer 13 to the poor solvent layer 12 in a state of high sphericity by utilizing buoyancy. In addition, in the poor solvent layer 12, the compound can be precipitated due to the supersaturated state caused by contact between the good solvent solution and the poor solvent, and the granules 16 can be granulated in a state in which the decrease in sphericity is suppressed. Therefore, particles of the compound with high sphericity can be easily manufactured. According to the crystallization operation of this manufacturing method, the compound can be precipitated in the liquid tank 11 without cooling or evaporating the good solvent, so that it can be performed under conditions of room temperature and normal pressure, and the compound particles can be obtained in a short time.
[0045] According to the manufacturing method of the first embodiment, a large amount of bubbles 15 can be continuously generated in the good solvent layer 14 by the bubble introduction section 20, and a large amount of granules 16 can be continuously transported to the separation layer 13 and the poor solvent layer 12. Therefore, fine particles of the compound can be continuously generated in the poor solvent layer in a short time, and the compound particles can be more efficiently manufactured. In addition, the particle size and particle size distribution of the manufactured particles can be easily controlled by adjusting the particle size and particle size distribution of the introduced bubbles 15.
[0046] In the manufacturing method of the first embodiment, as described above, a poorly water-soluble compound is adopted as the compound, and the poor solvent and the good solvent are composed of the organic solvent specifically exemplified in the above embodiment. This promotes the aggregation of the poorly water-soluble compound dissolved in the good solvent on the bubble surface. Therefore, the production efficiency of the particles can be further improved. In addition, in the manufacturing method of the first embodiment, the separation solvent is composed of a water-soluble solvent such as water that is immiscible with the good solvent and the poor solvent. This enhances the separability of the poor solvent layer 12 and the good solvent layer 14 with respect to the separation layer 13, so that the crystallization operation can be performed more easily and stably.
[0047] In the manufacturing method of the first embodiment, hollow compound particles can be easily obtained by generating hollow granular bodies 16 with bubbles 15 as nuclei during the crystallization operation. Such hollow particles are expected to be used in various applications. For example, hollow particles can reduce the weight of particles. In addition, hollow particles can easily form thin films with high thermal insulation and low dielectric constant. Furthermore, hollow particles can easily produce paints that easily reflect light, and can also produce sound-absorbing members with high sound-absorbing properties. In addition, hollow particles can utilize the physical properties of the gas contained therein, and can also express new functions by filling the inside with other substances.
[0048] As described above, in the manufacturing method of the first embodiment, bubbles are generated by an inert gas. Bubbles generated by an inert gas are prevented from shrinking or disappearing due to reactions with other substances, ions, etc., before being transported to the poor solvent layer 12. Therefore, it is possible to more efficiently manufacture desired particles and to increase the production rate of hollow particles.
[0049] In the manufacturing method of the first embodiment, as described above, air bubbles having a diameter of less than 200 μm are introduced by the air bubble introduction unit 20. This makes the core air bubbles finer, so that finer particles can be obtained. In addition, if the air bubbles introduced by the air bubble introduction unit 20 are fine air bubbles equivalent to fine bubbles having a diameter of 100 μm or less, the disappearance during transportation to the poor solvent layer 12 or during the crystallization operation is suppressed, so that the generation rate of hollow particles can be further increased. In addition, the variation in particle size distribution of the formed particles can be further suppressed.
[0050] Incidentally, various techniques using bubbles such as fine bubbles have been proposed for the production of compound particles. However, most of these techniques are based on polymerization at the gas-liquid interface of bubbles, and produce particles of a specific polymer. In contrast, the production method of the above embodiment uses a crystallization operation, so the compound is not limited to a specific polymer to which polymerization has been applied, and it is possible to produce particles of more various types of compounds. For example, it is possible to easily produce not only polymers from which fine particles can be obtained by emulsion polymerization such as PS, but also fine particles of polyester resins such as PBS and PLA, which are generally not easy to produce particles by polymerization. In addition, the conventional particle production techniques using bubbles such as fine bubbles are batch-type or precipitate compounds by evaporation of a solvent, so the production efficiency of particles cannot be said to be high. In contrast, according to the production method of the present embodiment, as described above, it is possible to efficiently and quickly produce compound particles.
[0051] 2. Second embodiment: 2 is a schematic diagram showing the configuration of a particle production apparatus 10A according to the second embodiment and the particle production process in the production apparatus 10A. The configuration of the production apparatus 10A according to the second embodiment is almost the same as the configuration of the production apparatus 10 according to the first embodiment, except that the tip of the air bubble introduction part 20 is located in the separation layer 13.
[0052] The particle manufacturing method of the second embodiment is almost the same as the particle manufacturing method described in the first embodiment, except that the air bubbles 15 are introduced into the separation layer 13 above the poor solvent layer 14 by the air bubble introducing part 20. In the second embodiment, at least a part of the air bubbles 15 introduced into the separation layer 13 by the air bubble introducing part 20 moves from the separation layer 13 to the good solvent layer 14 due to the pressure of the gas when it is ejected from the air bubble introducing part 20 and the flow of the liquid in the liquid tank 11.
[0053] As described in the first embodiment, the air bubbles 15 that have moved to the good solvent layer 14 form granules 16 of the good solvent solution, which are transported by buoyancy to the separation layer 13 and further from the separation layer 13 to the poor solvent layer 12. In the poor solvent layer 12, the compound precipitates and aggregates to form particles of the compound, as described in the first embodiment.
[0054] According to the manufacturing method of the second embodiment, it is possible to obtain compound particles having higher sphericity and higher strength, as shown in the experimental examples described later. In addition, according to the manufacturing apparatus 10A and the manufacturing method of the second embodiment, it is possible to achieve various effects similar to those described in the first embodiment.
[0055] 3. Third embodiment: 3 is a schematic diagram showing the configuration of a particle production apparatus 10B according to a third embodiment and the particle production process in the production apparatus 10B. The configuration of the production apparatus 10B according to the third embodiment is substantially the same as the configuration of the production apparatus 10 according to the first embodiment, except for the points described below.
[0056] In the manufacturing apparatus 10B of the third embodiment, the liquid tank 11 does not have a good solvent layer 14, and the separation layer 13 is disposed below the poor solvent layer 12. A stirrer 25 is disposed in the separation layer 13. Furthermore, in the manufacturing apparatus 10B, a good solvent solution introduction section 28 is provided instead of the air bubble introduction section 20. In the manufacturing apparatus 10B of the third embodiment, the good solvent solution introduction section 28 constitutes a granule generation section that generates granules 16 in the separation layer 13. The good solvent solution introduction section 28 introduces droplets 18 of a good solvent solution in which a compound is dissolved in a good solvent, into the separation layer 13.
[0057] The good solvent solution introducing part 28 is configured by, for example, a microsyringe. The good solvent solution introducing part 28 has a cylindrical main body, with a rear end portion disposed outside the liquid tank 11 and a front end portion disposed in the separation layer 13. The good solvent solution is introduced into the cylinder from the rear end portion of the good solvent solution introducing part 28. A minute opening is provided at the front end of the good solvent solution introducing part 28, and droplets 18 of the good solvent solution are discharged from the front end opening due to the pressure inside the cylinder.
[0058] The good solvent in the third embodiment has immiscibility with the separation solvent as in the first embodiment, but has a lower density than the separation solvent, unlike the first embodiment. When the droplets 18 of the good solvent solution are introduced into the separation layer 13 by the good solvent solution introduction section 28, the droplets 18 become solid spherical granules 16 of the good solvent solution, and are transported to the poor solvent layer 12 by buoyancy caused by the density difference between the separation solvent and the good solvent. Upon contact with the poor solvent in the poor solvent layer 12, the compound precipitates and aggregates in the granules 16, forming particles of the compound. In another embodiment, a good solvent solution that has been foamed by stirring in advance may be introduced into the good solvent solution introduction section 28, and the droplets 18 of the good solvent solution containing bubbles may be introduced into the separation layer 13 by the good solvent solution introduction section 28. With this configuration, even if the good solvent solution has a higher density than the separation solvent, the granules 16 of the good solvent solution can be transported to the poor solvent layer 12 by the buoyancy of the bubbles.
[0059] According to the manufacturing method of the third embodiment, compound particles can be manufactured by a crystallization operation using a poor solvent and a good solvent, even if the good solvent layer 14 described in the first and second embodiments is not provided in the liquid tank 11. Also, as in the first and second embodiments, granules 16 of the good solvent solution are formed in the separation layer 13 and are transported to the poor solvent layer 12 by buoyancy, so that compound particles with high sphericity can be easily manufactured. In addition, according to the manufacturing apparatus 10B and manufacturing method of the third embodiment, various effects similar to those described in the first and second embodiments can be achieved. EXAMPLES
[0060] 4. Experimental examples by the inventors: Hereinafter, experimental examples by the present inventors will be described as examples of the present invention and comparative examples with reference to Table 1 and Figures 4 to 9 in order. Table 1 summarizes the types of compounds, good solvents, and poor solvents in Examples 1 to 9 and Comparative Examples 1 to 4, as well as the positions in the liquid tank where bubbles were introduced by the bubble introduction part.
[0061] [Table 1]
[0062] (1) Examples 1 to 3: In Examples 1, 2, and 3, particles were manufactured using the same configuration as that described in the first embodiment. In Examples 1, 2, and 3, PS, PBS, and PLA were used as compounds, and chloroform was used as a good solvent, to prepare and use a good solvent solution with a concentration of 0.3 wt%. In addition, pure water was used as a separation solvent, and hexane was used as a poor solvent. A 500 ml eggplant flask was used as a liquid tank, and a magnetic stirrer was placed at the bottom.
[0063] First, 5 g of the good solvent solution was placed in a recovery flask to form a good solvent layer. After that, 400 g of pure water was poured onto the good solvent layer and allowed to stand for a while. Since chloroform, a good solvent, is immiscible with pure water and has a high density, the good solvent solution precipitated without mixing with the pure water, which is the separation solvent. As a result, a good solvent layer was formed under the separation layer made of pure water.
[0064] Next, 50 g of hexane, a poor solvent, was gently poured into the recovery flask onto the separation layer to form a poor solvent layer on the separation layer. In Example 1, at this stage, a thin film of PS precipitated was formed between the poor solvent layer of hexane and the separation layer of pure water. This thin film is considered to have been formed by mixing a small amount of good solvent solution with the pure water, but since it did not have a significant effect on the experimental results, a detailed explanation will be omitted here.
[0065] Next, a sparger, which is an air bubble introduction part, was placed in the recovery flask in which the poor solvent layer, separation layer, and good solvent layer were formed, so that its tip was located in the good solvent layer. An inert gas was supplied to the sparger to generate fine bubbles with a diameter of less than 200 μm in the good solvent layer. At this time, the size of the fine bubbles was adjusted by adjusting the flow of the liquid caused by stirring with a magnetic stirrer and the flow rate of the inert gas. Within about a few minutes after the introduction of air bubbles by the sparger was started, most of the good solvent solution was transported as granules through the separation layer to the poor solvent layer, and the reaction was completed.
[0066] Fig. 4 is a photographed image of the liquid tank 11 after the reaction in Example 1. As shown in the photographed image in Fig. 4, the poor solvent layer 12 on the separation layer 13 was clouded due to particles of the compound PS.
[0067] The table in Fig. 5 shows SEM images E1a, E1b, E2a, E2b, E3a, and E3b, which are images taken by a scanning electron microscope (SEM) of particles of the compound recovered from the poor solvent layer in Examples 1, 2, and 3. The table in Fig. 5 also shows TEM images E1c and E2c, which are images taken by a transmission electron microscope (TEM) of particles of the compound obtained in Examples 1 and 2.
[0068] As shown in SEM images E1a, E2a, and E3a, a large amount of fine particles with high sphericity were generated in each of Examples 1, 2, and 3. SEM images E1b, E2b, and E3b were taken at a higher magnification than SEM images E1a, E2a, and E3a. In SEM images E1b, E2b, and E3b, the particles are shown in a crushed state due to the influence of the electron beam irradiated for imaging, but from the way they are crushed, it was confirmed that there is a cavity inside the particle.
[0069] In the TEM image E2c of Example 2, the cavity inside the particle is shown as a whitish image in the center of the particle. The production rate of hollow particles was high in Example 2. On the other hand, in Example 1, the production rate of hollow particles was lower than that in Example 2, so the image of the cavity inside the particle could not be confirmed in the TEM image E1c.
[0070] As described above, in Examples 1, 2, and 3, we succeeded in mass-producing fine particles with high sphericity in a short period of time of about several minutes. We were also able to obtain hollow particles.
[0071] (2) Example 4: In Example 4, particles were produced by introducing air bubbles into the separation layer using a configuration similar to that described in the second embodiment. Example 4 was carried out under almost the same conditions as Example 1, except that 10 g of good solvent solution was used and the tip of the sparger was positioned in the separation layer to generate fine bubbles in the separation layer. In Example 4, most of the fine bubbles generated in the separation layer rose from the separation layer to the poor solvent layer and disappeared, but some reached the good solvent layer. The fine bubbles that reached the good solvent layer adsorbed the good solvent solution and were transported to the poor solvent layer through the separation layer by buoyancy as granular bodies of the good solvent solution. Two hours after the start of the introduction of fine bubbles, PS particles were collected from the poor solvent layer.
[0072] The table in Fig. 5 shows SEM images E4a and E4b of PS particles recovered from the poor solvent layer in Example 4. In Example 4, particles with higher sphericity were obtained than in any of Examples 1, 2, and 3. In Example 4, the particles were not crushed even in the high-magnification SEM image E4b, and it is believed that high-strength particles were formed.
[0073] As described above, in Example 4, as described in the second embodiment, air bubbles were generated in the separation layer and introduced into the good solvent layer. As a result, particles with higher sphericity than those in Examples 1, 2, and 3 were obtained.
[0074] (3) Example 5: In Example 5, particles were produced by introducing droplets of a good solvent solution into a separation layer without providing a good solvent layer and without using air bubbles, using a configuration similar to that described in the third embodiment. In Example 5, similar to the above Examples 1 to 4, a separation layer and a poor solvent layer were formed in a recovery flask, which was a liquid tank, using 400 g of pure water as a separation solvent and 50 g of hexane as a poor solvent.
[0075] In Example 5, PS as a compound was dissolved in toluene, which is a good solvent with a lower density than pure water, to prepare a good solvent solution with a concentration of 0.3 wt%, which was then injected into the separation layer using a syringe. As a result, the granular material composed of droplets of the good solvent solution was transported to the poor solvent layer by buoyancy due to the density difference between the separation solvent and the good solvent, forming PS particles.
[0076] The table in Fig. 5 shows an SEM image E5a of the fine particles collected in Example 5. As shown in SEM image E5a, a large amount of particles with high sphericity were obtained in Example 5 as in Examples 1 to 4. Note that, in SEM image E5a, particles with open holes can be visually recognized, and the open holes are considered to be derived from small amounts of air bubbles contained in the good solvent solution.
[0077] (4) Examples 6 to 9: In Examples 6, 7, 8, and 9, PBS was used as the compound, and chloroform was used as the good solvent to prepare a good solvent solution. In Examples 6, 7, 8, and 9, octane, decane, 2,2,4-trimethylpentane, and diisopropyl ether were used as the poor solvent, respectively. Other conditions in Examples 6, 7, 8, and 9 were almost the same as those in Examples 1 to 3.
[0078] The table in FIG. 6 shows TEM images E6, E7, E8, and E9 of particles recovered in Examples 6, 7, 8, and 9. From TEM images E6, E7, E8, and E9, it was confirmed that particles with high sphericity were formed in all of Examples 6, 7, 8, and 9. It was also confirmed that hollow particles were formed in Examples 6, 7, and 8. In particular, many hollow particles were confirmed in Examples 7 and 8.
[0079] (5) Verification results of hollow particles in Examples 2, 6, 7, and 8: Figure 7 shows a bar graph of the measurement results of the dimensions of the hollow particles obtained in Examples 2, 6, 7, and 8. The graph in Figure 7 was created using average values measured in TEM images of the outer diameter, inner diameter, and shell thickness of the hollow particles obtained in Examples 2, 6, 7, and 8. The hollow particles obtained in Examples 2, 6, 7, and 8 had outer diameters of about 700 to 800 nm, inner diameters of about 250 to 350 nm, and shell thicknesses of 150 to 250 nm.
[0080] In addition, under the same conditions as in Examples 2, 6, 7, and 8, when the flow rate of the inert gas supplied to the sparger was changed to 10 mL / min and 100 mL / min, no change was observed in the shape of the hollow particles, but the production rate of hollow particles was higher at 100 mL / min.
[0081] (6) Effect of concentration of good solvent solution (Examples 10 and 11): Figures 8 and 9 show graphs of Examples 10 and 11, respectively, showing the change in the outer diameter, inner diameter, and shell thickness of hollow particles when the concentration of a compound dissolved in a good solvent solution is changed. In each of the graphs of Figures 8 and 9, the horizontal axis shows the concentration of the compound in the good solvent solution, and the vertical axis shows the dimensions of the obtained hollow particles. In Examples 10 and 11, the outer diameter and inner diameter were measured as the dimensions of the hollow particles, and the shell thickness was calculated from the difference between the measured values. The graphs of Figures 8 and 9 were created based on the average values of the measured values.
[0082] In Examples 10 and 11, hollow particles were produced by carrying out a crystallization operation under the same conditions as in Examples 2 and 8, except that the concentration of the compound in the good solvent solution was changed. As shown in the graphs of Figures 8 and 9, in both Examples 10 and 11, the higher the concentration of the compound in the good solvent solution, the thicker the shell of the hollow particles became. Thus, it was found that the concentration of the compound in the good solvent solution affects the dimensions of the obtained hollow particles.
[0083] (7) Comparative Example 1: 10 shows an image C1 of the liquid SC recovered from the poor solvent layer in Comparative Example 1. For comparison, the image C1 also shows the liquid SE recovered from the poor solvent layer after the crystallization procedure in Example 1.
[0084] In Comparative Example 1, a good solvent layer, a separation layer, and a poor solvent layer were prepared in a recovery flask as a liquid tank under the same conditions as in Example 1, and the liquid was stirred for 4 hours by a magnetic stirrer without introducing fine bubbles. The liquid SC in the photographed image C1 is after the stirring.
[0085] The liquid SC recovered in Comparative Example 1 was almost transparent compared to the liquid SE obtained in Example 1. This indicates that in Comparative Example 1, the separation state between the good solvent layer and the poor solvent layer was maintained by the separation solvent, and PS did not precipitate. This result shows that using the buoyancy of air bubbles is effective for transporting the good solvent solution from the good solvent layer formed below the separation layer to the poor solvent layer.
[0086] (8) Comparative Example 2: The table in FIG. 10 shows an SEM image C2 of particles of the compound recovered in Comparative Example 2.
[0087] In Comparative Example 2, 5 g of a good solvent solution with a concentration of 0.3 wt% in chloroform as a good solvent and 400 g of pure water as a separation solvent were used to form a good solvent layer and a separation layer without providing a poor solvent layer in a liquid tank. Fine bubbles were generated in this liquid for 1 hour, and then the particles generated in the liquid were collected, washed, and observed by SEM.
[0088] The particles of Comparative Example 2 are considered to have been formed by the aggregation of PS precipitated by the evaporation of chloroform, a good solvent, during the generation of fine bubbles. As shown in SEM image C2, the particles were amorphous and far from spherical. From this result, it can be seen that in order to obtain particles with high sphericity, it is effective to precipitate a compound by transporting granular bodies of a good solvent solution to a poor solvent layer.
[0089] (9) Comparative Example 3: The table in FIG. 10 shows an SEM image C3 of particles of the compound recovered in Comparative Example 3.
[0090] In Comparative Example 3, a poor solvent addition method was performed as the crystallization operation. A fine bubble generator was immersed in 200 g of a good solvent solution with a concentration of 0.3 wt%, in which PS as a compound was dissolved in chloroform as a good solvent, and 400 g of hexane as a poor solvent was dropped little by little into the good solvent solution while generating fine bubbles. The PS particles precipitated with the drop of the poor solvent were collected, washed, and observed by SEM. As shown in SEM image C3, spherical particles were formed, but the particle size distribution had a significant difference between large and small diameters. From this result, it can be seen that in order to obtain particles with high sphericity and small particle size variation, it is effective to precipitate the compound by transporting the granular body of the good solvent solution to the poor solvent layer through a separation layer.
[0091] (10) Comparative Example 4: The table in FIG. 10 shows an SEM image C4 of the particles of the compound recovered in Comparative Example 4. In Comparative Example 4, PS was precipitated by dropping a good solvent solution in which PS as a compound was dissolved in toluene as a good solvent into 50 g of hexane as a poor solvent. As shown in SEM image C4, in Comparative Example 4, the precipitate of PS could not be obtained as particles. Comparing Comparative Example 4 with the above-mentioned Example 5, it can be seen that the configuration in which the granular body of the solvent solution is transported to the poor solvent layer through the separation layer is effective in obtaining particles of a compound with high sphericity.
[0092] (11) Summary: As described above, from the results of Examples 1 to 9 and Comparative Examples 1 to 4, it was found that the manufacturing methods of the first, second, and third embodiments described above make it possible to easily and efficiently obtain compound particles having high sphericity.
[0093] 5. Other embodiments: The present invention is not limited to the configurations of the above-mentioned embodiments and examples, and can be realized, for example, in the following forms. In the following, any configuration described as another embodiment is positioned as an example form for implementing the present invention, similar to the above-mentioned embodiments and examples.
[0094] 5-1. Other embodiment 1: In each of the above-described embodiments, the good solvent and the poor solvent may be water-soluble, and the separation layer may be water-insoluble. Even in such a configuration, the separation property of the poor solvent and the good solvent in the separation layer can be improved.
[0095] 5-2. Other embodiment 2: In each of the above embodiments, the air bubble introduction unit 20 does not have to be constituted by a sparger, and may be constituted by other air bubble generating devices. In addition, the air bubble introduction unit 20 may introduce air bubbles having a diameter of 200 μm or more when producing compound particles. In each of the above embodiments, the air bubbles 15 do not have to be generated by an inert gas, and may be generated by, for example, air. [Explanation of symbols]
[0096] 10, 10A, 10B... manufacturing apparatus, 11... liquid tank, 12... poor solvent layer, 13... separation layer, 14... good solvent layer, 15... air bubbles, 16... granular material, 18... liquid droplets, 20... air bubble introduction section, 25... stirrer, 28... good solvent solution introduction section
Claims
1. A method for producing particles of a compound by crystallization, comprising the steps of: preparing a liquid tank having a poor solvent layer formed of a poor solvent for the compound, and a separation layer disposed below the poor solvent layer, the separation layer being formed of a separation solvent that is denser than the poor solvent, immiscible with the poor solvent, and undergoes phase separation; a step of dissolving the compound in a good solvent that is immiscible with the separation solvent to produce granules of a good solvent solution in the separation layer, and transporting the granules from the separation layer to the poor solvent layer by buoyancy, thereby precipitating the compound in the poor solvent layer; A manufacturing method comprising:
2. The method according to claim 1, the liquid tank further has a good solvent layer formed of the good solvent solution having a density higher than that of the separation solvent, the good solvent layer, the separation layer, and the poor solvent layer are laminated in this order from the bottom in the liquid tank, The granular material is formed by introducing air bubbles into the good solvent layer, and is transported by the buoyancy of the air bubbles from the good solvent layer through the separation layer to the poor solvent layer.
3. The method according to claim 2, The granules are formed by introducing the air bubbles from the separation layer into the good solvent layer.
4. The method according to claim 2, The method of manufacturing, wherein the bubbles are composed of an inert gas.
5. The method according to claim 2, The method of manufacturing, wherein the bubbles are less than 200 μm in diameter.
6. The method according to any one of claims 1 to 5, The compound is a poorly water-soluble compound, and the good solvent and the poor solvent are each a water-insoluble solvent.
7. The method according to claim 6, further comprising the steps of: The compound is composed of a polymer such as polystyrene, polybutylene succinate, or polylactic acid, The good solvent and the poor solvent are each composed of an organic solvent such as hexane, toluene, octane, isooctane, decane, or chloroform, The method according to claim 1, wherein the separation solvent is composed of a water-soluble solvent such as water.
8. A manufacturing apparatus for producing particles of a compound by a crystallization operation, comprising: a liquid tank having a poor solvent layer formed of a poor solvent for the compound, and a separation layer disposed below the poor solvent layer, the separation layer being formed of a separation solvent that is denser than the poor solvent, immiscible with the poor solvent, and undergoes phase separation; a granule generating unit configured to generate, in the separation layer, granules that are constituted by a good solvent solution in which the compound is dissolved in a good solvent that is immiscible with the separation solvent, the good solvent solution being transported to the poor solvent layer by buoyancy in the separation layer, and the compound is granulated in the poor solvent layer; A manufacturing apparatus comprising:
9. The manufacturing apparatus according to claim 8, the liquid tank further has a good solvent layer formed of the good solvent solution having a density higher than that of the separation solvent, the good solvent layer, the separation layer, and the poor solvent layer are laminated in this order from the bottom in the liquid tank, The granular material generating unit includes an air bubble introducing unit that generates the granular material by introducing air bubbles into the good solvent layer.