Gas separation membrane, gas separation device, and method for producing gas separation membrane
A gas separation membrane with a polyethylene oxide structure and specific antioxidants improves durability against oxidizing gases, ensuring effective carbon dioxide and nitrogen separation while supporting sustainable practices.
Patent Information
- Application Number
- JP2023052239
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional gas separation membranes suffer from polymer deterioration due to oxidizing gases, which compromises their durability and performance.
Incorporating a polymer with a polyethylene oxide structure and an antioxidant with an I/O value of 0.4 or less, along with a porous support layer, to enhance the membrane's resistance to oxidizing gases.
The resulting gas separation membrane exhibits excellent durability against polymer deterioration, maintaining high performance in separating carbon dioxide from nitrogen, thereby contributing to efficient gas separation and reuse, aligning with sustainable development goals.
Smart Images

Figure 2024140880000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas separation membrane, a gas separation apparatus, and a method for producing a gas separation membrane. [Background technology]
[0002] It is known that polymer separation membranes are used as gas separation membranes for separating specific gas components from mixed gases. For example, Patent Document 1 discloses a method for producing a polymer gel composite membrane, which is characterized by irradiating a hydrophobic porous membrane surface with radiation while the surface is in contact with a liquid containing a hydrophilic polymer, its oligomer, or its monomer, to form a hydrophilic polymer gel membrane on the porous membrane surface. Patent Document 1 discloses that the polymer gel composite membrane thus obtained can be used as a carbon dioxide separation membrane or the like. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 7-275672 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the above-mentioned conventional techniques have room for improvement in terms of preventing the polymer in the gas separation membrane from being deteriorated by oxidizing gases.
[0005] An object of one aspect of the present invention is to provide a gas separation membrane that is highly resistant to polymer degradation caused by oxidizing gases. [Means for solving the problem]
[0006] In order to solve the above problems, one aspect of the present invention includes the following configuration. [1] A gas separation membrane comprising a separation functional layer containing a polymer having a polyethylene oxide structure and an antioxidant, wherein the polymer having a polyethylene oxide structure contains 57% or more ethyleneoxy units in 100% of main chain constituent units by weight, and the antioxidant has an I / O value of 0.4 or less in an organic conceptual diagram. [2] The gas separation membrane according to [1], wherein the antioxidant has an organic value of 300 to 1500 and an inorganic value of 0 to 300 in an organic conceptual diagram. [3] The gas separation membrane according to [1] or [2], wherein the antioxidant is in a liquid state under conditions of 1 atm and 25°C. [4] The gas separation membrane according to any one of [1] to [3], wherein the separation functional layer contains, as the antioxidant, a primary antioxidant and a secondary antioxidant. [5] The gas separation membrane according to any one of [1] to [4], further comprising a porous support layer, wherein the separation function layer is provided on the porous support layer. [6] The gas separation membrane according to any one of [1] to [5], which is used to selectively allow carbon dioxide to permeate from a mixed gas containing carbon dioxide and nitrogen. [7] A gas separation device comprising the gas separation membrane according to any one of [1] to [6]. [8] A method for producing a gas separation membrane, comprising a step of forming a separation functional layer containing a polymer having a polyethylene oxide structure and an antioxidant on a porous support layer, wherein the polymer having a polyethylene oxide structure contains 57% or more ethyleneoxy units in 100% of main chain constituent units by weight, and the antioxidant has an I / O value of 0.4 or less in an organic conceptual diagram. [9] A gas separation membrane comprising a separation functional layer containing at least one selected from the group consisting of vitamin E and its analogues, and a porous support layer. Effect of the Invention
[0007] According to one aspect of the present invention, a gas separation membrane having excellent durability against polymer degradation due to oxidizing gases can be provided. [Brief description of the drawings]
[0008] [Figure 1] 1 is a cross-sectional view illustrating a gas separation membrane according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a gas separation membrane according to another embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram illustrating a gas separation apparatus used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an example of an embodiment of the present invention will be described in detail, but the present invention is not limited thereto. Unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less."
[0010] [1. Gas separation membrane] A gas separation membrane according to one embodiment of the present invention has a separation functional layer containing a polymer having a polyethylene oxide structure and an antioxidant, wherein the polymer having a polyethylene oxide structure contains 57% or more ethyleneoxy units in 100% of the main chain constituent units by weight, and the antioxidant has an I / O value of 0.4 or less in an organic conceptual diagram.
[0011] As a result of the studies by the present inventors, there was room for improvement in gas separation membranes using polyethylene oxide from the viewpoint of suppressing degradation of the polymer due to oxidizing gases. Furthermore, the present inventors also found that when a gas separation membrane is obtained by a method including a step of irradiating polyethylene oxide with an electron beam or the like, the polyethylene oxide is easily oxidized due to the generation of radicals.
[0012] As a result of investigations, the present inventors have found that a gas separation membrane with excellent durability against polymer degradation due to oxidizing gases can be realized by combining a polymer having a polyethylene oxide structure with an antioxidant having an I / O value of 0.4 or less in the organic conceptual diagram.
[0013] An I / O value of 0.4 or less in the organic conceptual diagram of an antioxidant means that the organic value of the antioxidant is higher than the inorganic value. This indicates that the antioxidant is fat-soluble and has high lipophilicity. As described in Patent Document 1, polyethylene oxide is known as a hydrophilic polymer. Therefore, it was expected that polyethylene oxide would be compatible with water-soluble antioxidants, but the present inventors unexpectedly found that polyethylene oxide is compatible with fat-soluble antioxidants from the viewpoint of improving durability in gas separation membrane applications.
[0014] Facilitated transport membranes and dissolution-diffusion membranes are known as gas separation membranes. Facilitated transport membranes have excellent gas selectivity, but because they contain gas carriers, there is a concern that the gas carriers may leak out of the membrane during use, resulting in a decrease in gas separation ability. Dissolution-diffusion membranes are gas separation membranes that do not use gas carriers. Dissolution-diffusion membranes can selectively allow specific gas components to permeate by utilizing the difference in solubility of gas components contained in a mixed gas in the membrane material and the difference in diffusion coefficient of gas components contained in a mixed gas in the membrane material.
[0015] 1 and 2 are cross-sectional views that diagrammatically show a gas separation membrane according to one embodiment of the present invention. The gas separation membrane 10 has a separation functional layer 15. The gas separation membrane 10 may be a solution-diffusion membrane. The gas separation membrane 10 contains a polymer having a polyethylene oxide structure, and therefore has a high solubility in carbon dioxide (CO 2 ) has a high affinity for CO 2 and nitrogen (N 2 ) from a mixed gas (raw material gas) containing CO 2 The gas separation membrane 10 can be suitably used for gas separation performed under temperature conditions of 20° C. or higher and 60° C. or lower, and can be used, for example, for gas separation of combustion exhaust gas generated in an incinerator.
[0016] According to the above-mentioned configuration, carbon dioxide can be efficiently separated and appropriately reused, etc. Such an effect contributes to the achievement of, for example, Goal 13 of the Sustainable Development Goals (SDGs) advocated by the United Nations, "Take urgent action to combat climate change."
[0017] 1 and 2, the gas separation membrane 10 may further include a porous support layer 11, and the separation functional layer 15 may be provided on the porous support layer 11. The porous support layer 11 and the separation functional layer 15 may be in direct contact with each other, or a gutter layer may be provided between the porous support layer 11 and the separation functional layer 15. When the gas separation membrane 10 includes a gutter layer, it is preferable that the porous support layer 11 and the separation functional layer 15 are in direct contact with the gutter layer.
[0018] As shown in Fig. 2, the gas separation membrane 10 may have a protective layer 12 on the side of the separation functional layer 15 opposite the porous support layer 11 side. As shown in Fig. 2, the gas separation membrane 10 may further have a reinforcing layer 13 on the side of the porous support layer 11 opposite the separation functional layer 15 side. The reinforcing layer 13 may be provided in direct contact with the porous support layer 11, or, for example, the reinforcing layer 13 and the porous support layer 11 may be heat-sealed. Alternatively, the reinforcing layer 13 and the porous support layer 11 may be attached to each other with a pressure-sensitive adhesive or adhesive.
[0019] <1-1. Separation functional layer> The separation functional layer 15 contains a polymer having a polyethylene oxide structure and an antioxidant. The thickness of the separation functional layer 15 is preferably 0.01 μm to 100 μm, more preferably 0.05 μm to 50 μm, and may be 0.1 μm to 20 μm, 0.1 μm to 10 μm, or 0.2 μm to 2 μm.
[0020] (Polymer having a polyethylene oxide structure) Hereinafter, the polymer having a polyethylene oxide structure is also referred to as polymer (p). Polymer (p) contains 57% or more ethyleneoxy units, preferably 60% or more ethyleneoxy units, more preferably 70% or more ethyleneoxy units, and even more preferably 80% or more ethyleneoxy units, based on 100% of the main chain constituent units by weight. For this reason, polymer (p) is a polymer having a polyethylene oxide structure, and is preferably a polymer having a polyethylene oxide structure. 2 The polymer (p) has a high affinity with the polymer. The structural units of the main chain of the polymer (p) may all be ethyleneoxy units. The content of ethyleneoxy units in the structural units of the main chain of the polymer (p) may be 100% or less.
[0021] In the present specification, an ethyleneoxy unit is a -(C 2 H 4 The polyethylene oxide structure refers to a structural unit represented by -(C 2 H 4 O) n The polymer (p) is a repeating structure of ethyleneoxy units represented by -(C 2 H 4 O) n It can also be said that the polymer (p) contains a repeating structure of ethyleneoxy units represented by the formula: - in the main chain. Here, n represents an integer of 2 or more. n is usually 100 or more and 1,000,000 or less, and may be 400 or more and 200,000 or less, or may be 10,000 or more and 100,000 or less. Examples of the polymer (p) include polyethylene oxide (PEO), crosslinked polyethylene oxide (crosslinked PEO) which is a crosslinked product of polyethylene oxide, and copolymers having ethyleneoxy units and structural units other than ethyleneoxy units.
[0022] It can be said that PEO is a homopolymer of ethylene oxide. The crosslinked PEO may be a polymer having a structure in which PEO is crosslinked within a molecule, or may be a polymer having a structure in which PEO is crosslinked between molecules. The crosslinked PEO may be a chemical crosslinked body having a structure crosslinked by a covalent bond, or may be a physical crosslinked body having a structure crosslinked by a coordinate bond and / or a hydrogen bond. These crosslinked PEOs can be formed by irradiating PEO with an electron beam, which will be described later, or by performing a crosslinking treatment with a crosslinking agent. The crosslinked structure of the crosslinked PEO may be a structure in which PEO is crosslinked within a molecule or between molecules by a crosslinking agent, but it is preferable that the carbon atoms constituting the PEO are bonded within a molecule or between molecules by a single bond. The crosslinked PEO has many amorphous parts, and is less likely to be CO2-depleted than the highly crystalline PEO. 2 It is believed to have better permeability.
[0023] Examples of the copolymer include polyether block amide copolymer, ethylene oxide-propylene oxide copolymer, polyether ester block copolymer, polyether amine, and polyether modified silicone.
[0024] The content of the polymer (p) relative to the total amount of the separation functional layer 15 is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and may be 95% by mass or more. The content of the polymer (p) relative to the total amount of the separation functional layer 15 may be less than 100% by mass.
[0025] The weight average molecular weight of the polymer (p) is preferably 10×10 3 More preferably, it is 18×10 3 More than 10000 x 10 3 More preferably, it is 20×10 or less. 3 Over 8000 x 10 3 is less than or equal to 100 x 10 3 Over 5000 x 10 3 It may be less than 300 x 10 3 Over 4500 x 10 3It may be the following.
[0026] The separation functional layer 15 may contain a polymer other than the polymer (p). Examples of such a polymer include polyacrylic acid, polypropylene oxide, polyvinyl alcohol, polyethyleneimine, polyvinylamine, polyallylamine, and polyvinylpyrrolidone.
[0027] (Antioxidants) The separation functional layer 15 contains an antioxidant with an I / O value of 0.4 or less in the organic conceptual diagram. The organic conceptual diagram divides the properties of organic compounds into organicity (covalent bonding) based mainly on the number of carbon atoms and inorganicity (ionic bonding) based on the properties and tendency of the substituents, and positions the organic compounds on an orthogonal coordinate system named the organic axis and inorganic axis to allow the reader to understand the general nature of the compounds (Fujita Atsushi, "Organic Analysis", Kaniya Shoten, 1930). The carbon and substituents of an organic compound are given organic and inorganic values, and the sum of the organic values calculated from the structure of the organic compound is called the organic value, and the sum of the inorganic values is called the inorganic value. The value obtained by dividing the inorganic value by the organic value is called the I / O value. The organic value and inorganic value in this specification refer to values calculated based on "New Edition Organic Conceptual Diagram: Basics and Applications" (Koda Yoshio et al., Sankyo Publishing, 2008).
[0028] The I / O value of the antioxidant is preferably 0.35 or less, more preferably 0.3 or less. The I / O value of the antioxidant is preferably 0.1 or more, more preferably 0.2 or more. The I / O value in the above range is preferable from the viewpoint of the balance between inorganicity and organicity.
[0029] The antioxidant preferably has an organic value of 300 to 1500 and an inorganic value of 0 to 300 in an organic conceptual diagram. The antioxidant more preferably has an organic value of 400 to 1200, and even more preferably has an inorganic value of 500 to 900. The antioxidant more preferably has an inorganic value of 50 to 250, and even more preferably has an inorganic value of 100 to 200.
[0030] The antioxidant is preferably liquid under conditions of 1 atm and 25° C. Such an antioxidant has excellent compatibility with a polymer having a polyethylene oxide structure. In addition, such an antioxidant is easily mixed when preparing a coating liquid.
[0031] The antioxidant may be a primary antioxidant (radical scavenger), a secondary antioxidant (peroxide decomposer), or a combination thereof. That is, the separation functional layer 15 may contain a primary antioxidant and a secondary antioxidant as the antioxidant.
[0032] Specific antioxidants include vitamin E (tocopherol, organic value: 550, inorganic value: 145, I / O value: 0.26), Irganox 1520 (BASF Japan, organic value: 580, inorganic value: 155, I / O value: 0.27), 2,6-di-t-butyl-4-s-butylphenol (organic value: 320, inorganic value: 115, I / O value: 0.36), Irganox 1076 (manufactured by BASF Japan, organic value: 660, inorganic value: 175, I / O value: 0.27), 4,6-bis(octylthiomethyl)-o-cresol (organic value: 580, inorganic value: 140, I / O value: 0.24), tris(2,4-di-t-butylphenyl)phosphite (organic value: 740, inorganic value: 175, I / O value: 0.24), Adeka STAB HP-10 (manufactured by ADEKA, organic value: 680, inorganic value: 160, I / O value: 0.24), Irgafos 38 (BASF Japan, organic value: 580, inorganic value: 160, I / O value: 0.28), triisodecyl phosphite (organic value: 620, inorganic value: 130, I / O value: 0.21), tris(2-ethylhexyl) phosphite (organic value: 500, inorganic value: 130, I / O value: 0.26), tri-o-tolyl phosphite (organic value: 500, inorganic value: 130, I / O value: 0.26), organic value: 440, inorganic value: 175, I / O value: 0.40), tris(2,4-di-tert-butylphenyl)phosphite (organic value: 740, inorganic value: 175, I / O value: 0.24), 2-methyl-4,6-bis[(n-octylthio)methyl]phenol (organic value: 580, inorganic value: 155, I / O value: 0.27), stearyl Examples of the antioxidant include 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (organic value: 660, inorganic value: 175, I / O value: 0.27), hexadecyl 3,5-di-tert-butyl-4-hydroxybenzoate (organic value: 620, inorganic value: 175, I / O value: 0.28), and 2,4-bis[(dodecylthio)methyl]-6-methylphenol (organic value: 700, inorganic value: 155, I / O value: 0.22). One type of antioxidant may be used alone, or two or more types may be used in combination.
[0033] The content of the antioxidant in the separation functional layer 15 is preferably 100 ppm by weight or more, and more preferably 1000 ppm by weight or more. From the viewpoint of membrane performance, the upper limit of the content of the antioxidant in the separation functional layer 15 is preferably 30% by weight or less, more preferably 10% by weight or less, and may be 5% by weight or less.
[0034] An embodiment of the present invention also includes a gas separation membrane comprising a separation functional layer containing at least one selected from the group consisting of vitamin E and its analogs, and a porous support layer. In this specification, a vitamin E analog means a compound having a structure similar to that of vitamin E and having a substituent or the like within a range that does not impair the effect of one embodiment of the present invention. Examples of vitamin E analogs include DL-α-tocopherol acetate, D-α-tocopherol succinate, (±)-α-tocopherol nicotinate, DL-α-tocopherol methoxypolyethylene glycol succinate, etc.
[0035] (Other Ingredients) In addition to the polymer (p) and the antioxidant, the separation functional layer 15 may contain a surfactant, a filler, a crosslinking agent, a liquid medium, and the like (described later) contained in the composition for forming the separation functional layer 15. When the gas separation membrane of this embodiment is used as a dissolution-diffusion membrane, it is preferable that the separation functional layer 15 does not contain a gas carrier. Examples of the gas carrier include substances that react reversibly with carbon dioxide, and specific examples of the gas carrier include alkali metal carbonates, alkali metal bicarbonates, alkanolamines, and alkali metal hydroxides. "Doing not contain a gas carrier" means that the content of the gas carrier is less than 0.1% by mass with respect to the total mass of the separation functional layer 15.
[0036] <2-2. Porous support layer> The porous support layer 11 can support the separation functional layer 15. The porous support layer 11 can selectively transmit the mixed gas supplied to the separation functional layer 15 and the gas (e.g., CO 2It is preferable that the porous support layer 11 has a high gas permeability so as not to become a diffusion resistance of the porous support layer 11. The porous support layer 11 can be formed of a resin material or an inorganic material. The porous support layer 11 may have a single layer structure or a multilayer structure.
[0037] Examples of the resin material constituting the porous support layer 11 include polyolefin resins such as polyethylene (PE) and polypropylene (PP); fluorine-containing resins such as polytetrafluoroethylene (PTFE), polyvinyl fluoride (PVF), and polyvinylidene fluoride (PVDF); polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate; polystyrene (PS), polyethersulfone (PES), polyphenylene sulfide (PPS), polysulfone (PSF), polyacrylonitrile (PAN), polyphenylene oxide (PPO), polyamide (PA), polyimide (PI), polyetherimide (PEI), polyetheretherketone (PEEK), high molecular weight polyester, heat-resistant polyamide, aramid, polycarbonate, and mixtures of two or more of these resin materials. Among these, it is preferable to include a polyolefin resin, and it is more preferable to include one or more of polyethylene and polypropylene. Examples of the inorganic material constituting the porous support layer 11 include metal, glass, ceramics, and the like.
[0038] The porous support layer 11 is not particularly limited as long as it is a porous body. The porous support layer 11 may be a sheet-like porous body such as a porous resin film, nonwoven fabric, woven fabric, foam, mesh, net, etc. The porous support layer 11 is preferably a porous resin film.
[0039] <2-3. Gutter layer> The gas separation membrane 10 can have a gutter layer between the porous support layer 11 and the separation functional layer 15. The gutter layer can suppress excessive penetration of the composition into the porous support layer 11 when the composition for forming the separation functional layer 15 is applied onto the porous support layer 11, thereby enabling the separation functional layer 15 to be successfully formed on the porous support layer 11. The gutter layer can also suppress leakage of the mixed gas (raw material gas) from defects occurring in the separation functional layer 15.
[0040] The gas permeation rate of the gutter layer is preferably higher than that of the separation functional layer 15. The material for forming the gutter layer is not particularly limited. The gutter layer can be formed using a resin having gas permeability, and examples of the resin include silicone resin and amorphous fluororesin. The gutter layer may have a single layer structure or a multilayer structure.
[0041] <2-4.Protective layer> In order to protect the separation functional layer 15, the gas separation membrane 10 can have a protective layer 12 on the side of the separation functional layer 15 opposite the porous support layer 11 side. The protective layer 12 can be formed of a resin material or an inorganic material, and can be formed of, for example, the materials described as the materials that can be used for the porous support layer 11. The protective layer 12 may have a single-layer structure or a multi-layer structure.
[0042] <2-5. Reinforcement layer> The gas separation membrane 10 may have a reinforcing layer 13 on the side of the porous support layer 11 opposite to the separation functional layer 15 side. The reinforcing layer 13 may be provided to improve the handleability of the gas separation membrane 10 during production and to impart appropriate strength to the gas separation membrane 10. The reinforcing layer 13 may have a thickness greater than that of the porous support layer 11. The reinforcing layer 13 is configured to selectively transmit the mixed gas supplied to the separation functional layer 15 and a gas (e.g., CO 2The reinforcing layer 13 may have a high gas permeability so as not to become a diffusion resistance of the porous support layer 11. The reinforcing layer 13 may be formed of a resin material or an inorganic material, and may be a nonwoven fabric, a woven fabric, or a net. The reinforcing layer 13 may be formed of, for example, the material described as the material usable for the porous support layer 11.
[0043] 2. Method for producing gas separation membrane A method for producing a gas separation membrane 10 according to one embodiment of the present invention includes a step of forming a separation functional layer 15 containing a polymer having a polyethylene oxide structure and an antioxidant on a porous support layer 11, the polymer having the polyethylene oxide structure containing 57% or more ethyleneoxy units in 100% of main chain constituent units by weight, and the antioxidant having an I / O value of 0.4 or less in an organic conceptual diagram. The matters already explained in [1. Gas separation membrane] above will not be explained below.
[0044] The step of forming the separation functional layer 15 on the porous support layer 11 may include a step of applying a composition containing a polymer (p), an antioxidant, and a liquid medium for dissolving or dispersing them onto the porous support layer 11. The manufacturing method may also include a step of filtering the composition before the step of applying the composition onto the porous support layer 11. By filtering the composition, air bubbles and insoluble matter contained in the composition can be removed when the composition is applied onto the porous support layer 11, and defects can be suppressed in the layer of the composition applied onto the porous support layer 11 and the separation functional layer formed from the layer.
[0045] The liquid medium is not particularly limited as long as it is a liquid medium capable of dissolving or dispersing the polymer (p) and the antioxidant. Examples of the liquid medium include protic polar solvents such as water, alcohols such as methanol, ethanol, 1-propanol, and 2-propanol; non-polar solvents such as toluene, xylene, and hexane; ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, and aprotic polar solvents such as N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, and acetonitrile. The liquid medium may be used alone or in combination with two or more types within the range of compatibility. Among these, a liquid medium containing at least one selected from the group consisting of water, methanol, ethanol, 1-propanol, and 2-propanol is preferred, and a liquid medium containing water is more preferred.
[0046] The composition may contain a surfactant, a filler, a crosslinking agent, etc., in addition to the polymer (p), the antioxidant, and the liquid medium. The surfactant is not particularly limited, and may be an anionic surfactant, a cationic surfactant, an amphoteric surfactant, or a nonionic surfactant. Examples of the surfactant include known surfactants such as fluorine-based surfactants and silicone-based surfactants. One type of surfactant may be used alone, or two or more types may be used in combination. By containing a surfactant in the composition, when the composition is applied onto a porous support layer, the wettability between the application surface of the composition and the composition can be improved, and the occurrence of unevenness in the film thickness of the separation functional layer 15 can be suppressed.
[0047] The filler may be an inorganic filler such as zeolite, silica, or carbon, an organic filler such as resin particles, or an organic-inorganic filler such as a metal-organic framework (MOF), or two or more of these.
[0048] Examples of the crosslinking agent include acrylic esters. The composition may not contain a crosslinking agent for crosslinking PEO. Not containing a crosslinking agent means that the content of the crosslinking agent is less than 0.1% by mass relative to the total mass of PEO in the composition. When the composition contains a crosslinking agent, the content of the crosslinking agent may be 0.1% by mass or more and 50% by mass or less, 1% by mass or more and 20% by mass or less, or 1% by mass or more and 10% by mass or less, relative to the total mass of PEO in the composition.
[0049] The content of the polymer (p) in the composition may be from 0.1% by mass to 70% by mass, from 1.0% by mass to 60% by mass, or from 1.5% by mass to 55% by mass.
[0050] When the gas separation membrane 10 has a gutter layer, the manufacturing method may include a step of forming the gutter layer on the porous support layer 11. The gutter layer can be formed by, for example, applying a material for forming a gutter layer to the porous support layer 11. When the gutter layer is formed on the porous support layer 11, the composition is applied to the side of the porous support layer 11 on which the gutter layer is formed.
[0051] There is no particular limitation on the method for applying the composition onto the porous support layer 11. Examples of the application method include spin coating, bar coating, die coating, blade coating, air knife coating, gravure coating, roll coating, spray coating, dip coating, comma roll coating, kiss coating, screen printing, inkjet printing, etc. The application amount of the composition is such that the basis weight (solid content per unit area) is 1 g / m 2 More than 1000g / m 2 The range is preferably 5 g / m 2 More than 750g / m 2 More preferably, the range is 10 g / m 2 More than 500g / m 2It is more preferable that the coating weight is in the following range: The coating weight can be adjusted by controlling the coating film formation speed (for example, the conveying speed of the porous support layer), the concentration of the composition, the discharge amount of the composition, and the like.
[0052] When gas separation membrane 10 has reinforcing layer 13, it is preferable to prepare a laminated support of reinforcing layer 13 and porous support layer 11, and apply the composition to the porous support layer 11 side of this laminated support.
[0053] The manufacturing method may include a step of removing the liquid medium from the composition. For example, the liquid medium can be removed by air drying, forced air drying, heat drying, etc. When the gas separation membrane 10 has a protective layer 12, the protective layer 12 may be laminated before the step of removing the liquid medium from the composition, or the protective layer 12 may be laminated after the step of removing the liquid medium from the composition.
[0054] Alternatively, the step of forming the separation functional layer 15 on the porous support layer 11 may include a step of applying a first composition containing a polymer (p) and a liquid medium for dissolving or dispersing the polymer (p) onto the porous support layer 11, and a step of applying a second composition containing an antioxidant and a liquid medium for dissolving or dispersing the antioxidant onto the layer of the first composition. In addition, between the step of applying the first composition onto the porous support layer 11 and the step of applying the second composition onto the layer of the first composition, a step of irradiating the first composition with an electron beam may be provided. This allows the polymer (p) to be crosslinked with the electron beam. For example, when the first composition contains PEO, crosslinked PEO is obtained by electron beam crosslinking. By irradiating with an electron beam before applying the second composition, the effect of the electron beam on the antioxidant can be prevented.
[0055] The irradiation dose of the electron beam is preferably 10 kGy or more, more preferably 15 kGy or more and 400 kGy or less, even more preferably 20 kGy or more and 400 kGy or less, and may be 30 kGy or more and 350 kGy or less, or 40 kGy or more and 300 kGy or less.
[0056] The first composition applied on the porous support layer 11 may be irradiated with an electron beam from the porous support layer 11 side, from the first composition side, or both. The electron beam may be irradiated in an air atmosphere, or in an atmosphere of an inert gas such as nitrogen gas, argon gas, or helium gas.
[0057] [3. Gas separation device] The gas separation device can include the above-mentioned gas separation membrane 10. Since the gas separation device includes the gas separation membrane 10, it is advantageous for long-term operation. For example, the gas separation device of the present embodiment can be suitably used to separate combustion exhaust gas generated in an incinerator.
[0058] The gas separation membrane 10 can be incorporated into a gas separation apparatus as a gas separation membrane element of a known form such as a spiral type, flat membrane type, pleated type, plate-and-frame type, etc. The gas separation membrane element may have a laminate in which a feed-side gas flow path member through which a raw material gas (mixed gas) and a non-permeable gas flow, and a permeable-side gas flow path member through which a permeable gas flows are laminated on the gas separation membrane 10. The gas separation membrane element may have a sealing portion for preventing mixing of the raw material gas and the non-permeable gas with the permeable gas.
[0059] In addition to the gas separation membrane 10 (a gas separation membrane element having the gas separation membrane 10), the gas separation device can have a supply section for supplying a mixed gas to the gas separation membrane 10, a permeable gas discharge section for discharging the permeable gas that has permeated through the gas separation membrane 10, and a non-permeable gas discharge section for discharging the non-permeable gas that has not permeated through the gas separation membrane 10.
[0060] The operating temperature of the gas separation unit may be from 20°C to 60°C, preferably from 30°C to 55°C, and more preferably from 35°C to 50°C.
[0061] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope shown in the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
Example
[0062] Hereinafter, the present invention will be described more specifically by showing examples and comparative examples, but the present invention is not limited by these examples.
[0063] [Measurement of Oxidation Induction Time (OIT)] The oxidation induction time used in the examples and comparative examples was measured under the following conditions using a differential scanning calorimeter (DSC).
[0064] As the measuring device, DSC7020 manufactured by Hitachi High-Tech Corporation was used. 5 mg of the sample was weighed into an aluminum pan for DSC measurement, placed in the furnace, and the inner lid was closed. Then, while flowing nitrogen gas into the furnace at 25 mL / min, the temperature was raised to 160°C at a rate of 20°C / min. After that, it was left standing for 5 minutes in the same state (i.e., while flowing nitrogen gas and maintaining at 160°C). After standing, the nitrogen gas was switched to oxygen gas, and the measurement was started. The sampling interval during the measurement was set to 0.5 seconds. The oxidation induction time was measured by calculating the time from the moment the nitrogen gas was switched to oxygen gas until the rise of the exothermic peak due to oxidation.
[0065] [Quantification of Antioxidant] The content of the antioxidant in the film was determined by measuring the solution obtained by immersing the film in acetonitrile overnight under the following measurement conditions using liquid chromatography (LC).
[0066] <LC Measurement Conditions> Device: LC-40A (manufactured by Shimadzu Corporation) Column: L-Column3 (manufactured by the National Institute of Advanced Industrial Science and Technology) Mobile Phase A: H 2 O, B: Acetonitrile (Water used was Milli-Q water, and acetonitrile was HPLC grade.) Gradient: B40%(15)-10-B100%(25) postrun15min Flow rate: 1mL / min Measurement time: 40 minutes Column oven: 40℃ Detection: UV detector (detection wavelength: 254 nm) Injection volume: 20μL.
[0067] [Evaluation of gas permeability] (Evaluation Test 1) The separation performance of the gas separation membranes obtained in each Example and Comparative Example was evaluated using a gas separation apparatus 100 equipped with a gas separation membrane cell 61 shown in Fig. 3. Specifically, the produced gas separation membrane was cut to an appropriate size to form a flat membrane shape, and the obtained gas separation membrane 10 was fixed between the feed side chamber 62 and the permeation side chamber 63 of a stainless steel gas separation membrane cell 61. The temperature of the gas separation membrane cell was kept at 40°C. A raw material gas (CO 2 : 8.4% by volume, N 2 : 90.9% by volume, H 2 O: 1.7% by volume was supplied to the supply side chamber 62 of the gas separation membrane cell 61 at a flow rate of 31.7 NL / h. 2 and N 2 The flow rate of water was controlled by a mass flow controller (MFC). Water was fed by a constant-volume liquid pump 81, heated and evaporated to produce H 2 The pressure in the feed side chamber 62 was adjusted to 120 kPaA (absolute pressure) by a back pressure regulator 65 provided downstream of a cooling trap 64 in the discharge path for the non-permeate gas. A back pressure regulator 69 and a pressure reducing pump 71 were provided between a cooling trap 66 downstream of the permeate side chamber 63 and a gas chromatograph 67, and these were used to adjust the pressure in the permeate side chamber 63 to 10 kPaA.
[0068] After the gas separation apparatus 100 starts operating, when the apparatus reaches a steady state, the permeated gas is analyzed by a gas chromatograph 67 to determine N 2 Permeance [mol / (m 2The permeate gas to be analyzed here is the permeate gas discharged from the permeation side chamber 63 after the water vapor contained therein has been removed by the cooling trap 66.
[0069] The durability of the film is N 2 It was evaluated as the time it took for the permeance to increase by 50% from the initial value.
[0070] Example 1 (Preparation of Coating Solution (A0)) 4.0 g of polyethylene oxide (Meisei Chemical Industry Co., Ltd., Alkox E-160), 196.0 g of water, and 1.1 g of a 10 wt % aqueous solution of a surfactant (AGC Seimi Chemical Co., Ltd., Surflon S-242) were mixed and stirred, and then filtered through a filter with a pore size of 2 μm to obtain a coating solution (A0).
[0071] (Preparation of Coating Solution (A1)) 0.1 g of an ethanol solution containing 0.1 wt % DL-α-tocopherol (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5.0 g of the coating liquid (A0) were mixed and stirred to obtain a coating liquid (A1).
[0072] (Preparation and Evaluation of Samples for OIT Testing) 1.0 g of the coating solution (A1) was applied to a glass plate and dried in a vacuum oven for 12 hours to obtain a sample. The sample was peeled off from the glass plate and evaluated in the OIT test.
[0073] (Preparation of gas separation membrane) A polypropylene (PP) porous film (Polypore Corporation, Celgard (registered trademark) 2500) was prepared as the first porous layer. Using a corona surface modification evaluation device (Kasuga Electric Co., Ltd., TEC-4AX, treatment electrode width: 21 cm), corona treatment was performed on one side of the first porous layer under conditions of discharge output of 75 W and treatment speed of 1 m / min.
[0074] The coating solution (A0) was applied to the corona-treated surface of the first porous layer using a tabletop applicator set to a coating thickness of 100 μm to form a coating film.
[0075] The coating film was subjected to electron beam irradiation treatment using an electron beam irradiation device (EC250, manufactured by Iwasaki Electric Co., Ltd.) under the conditions of an irradiation dose of 50 kGy, a current of 5.6 mA, a voltage of 225 kV, a speed of 8 m / min, and a number of times of irradiation of 1. Thereafter, the coating film was dried at 25° C. for 12 hours.
[0076] (Application of antioxidant) 5 mL of an ethanol solution containing 0.025 wt% DL-α-tocopherol (Tokyo Chemical Industry Co., Ltd.) was applied to the dried coating film (78 cm 2 ) was sprayed using an airbrush, and then dried at 25°C for 12 hours to obtain a gas separation membrane.
[0077] (Evaluation of permeability) The gas permeability of the gas separation membrane obtained above was evaluated.
[0078] Example 2 (Preparation of Coating Solution (A2)) 0.1 g of an ethanol solution containing 0.1 wt % DL-α-tocopherol (manufactured by Tokyo Chemical Industry Co., Ltd.) and 0.1 wt % Irganox 1520 (manufactured by BASF Japan) and 5.0 g of the coating liquid (A0) were mixed and stirred to obtain a coating liquid (A2).
[0079] (Preparation and Evaluation of Samples for OIT Testing) Sample preparation and OIT test evaluation were performed in the same manner as in Example 1, except that coating liquid (A2) was used instead of coating liquid (A1).
[0080] (Preparation of gas separation membrane) In the same manner as in Example 1, a coating film was formed on the corona-treated surface of the first porous layer, and then the coating film was subjected to electron beam irradiation treatment, and then the coating film was dried.
[0081] (Application of antioxidant) 5 mL of an ethanol solution containing 0.025 wt% DL-α-tocopherol (Tokyo Chemical Industry Co., Ltd.) and 0.025 wt% Irganox 1520 (BASF Japan Ltd.) was applied to the dried coating film (78 cm 2 ) was sprayed using an airbrush, and then dried at 25°C for 12 hours to obtain a gas separation membrane.
[0082] (Antioxidant content) The gas separation membrane was subjected to LC measurement. From the LC measurement, the amount of the antioxidant in the separation functional layer was found to be 261 ppm by weight for DL-α-tocopherol and 100 ppm by weight or less, which is the lower limit of quantification, for Irganox 1520.
[0083] (Evaluation of permeability) The gas separation membrane obtained above was used to evaluate the permeation performance.
[0084] Example 2' (Preparation of gas separation membrane) In the same manner as in Example 1, a coating film was formed on the corona-treated surface of the first porous layer, and then the coating film was subjected to electron beam irradiation treatment, and then the coating film was dried.
[0085] (Application of antioxidant) 5 mL of an ethanol solution containing 2.5 wt% DL-α-tocopherol (Tokyo Chemical Industry Co., Ltd.) and 2.5 wt% Irganox 1520 (BASF Japan) was applied to the dried coating film (78 cm 2 ) was sprayed using an airbrush, and then dried at 25°C for 12 hours to obtain a gas separation membrane.
[0086] (Antioxidant content) The gas separation membrane was subjected to LC measurement. From the LC measurement, the amount of the antioxidant in the separation functional layer was found to be 8658 ppm by weight for DL-α-tocopherol and 37173 ppm by weight for Irganox 1520.
[0087] (Evaluation of permeability) The gas separation membrane obtained above was used to evaluate the permeation performance.
[0088] Example 3 (Preparation of Coating Solution (A3')) 4.0g of polyether block amide (Arkema, Pebax MH1657), 137.2g of ethanol, 58.8g of water, and 1.1g of 10% by weight surfactant (AGC Seimi Chemical, Surflon S-242) ethanol solution were mixed and stirred, and then filtered through a filter with a pore size of 2 μm to obtain coating solution (A3'). The content of ethyleneoxy units in the polyether block amide was 60% by weight.
[0089] (Preparation of Coating Solution (A3)) 0.1 g of an ethanol solution containing 0.1 wt % DL-α-tocopherol (Tokyo Chemical Industry Co., Ltd.) and 0.1 wt % Irganox 1520 (BASF Japan) was mixed with 5.0 g of coating liquid (A3') and stirred to obtain coating liquid (A3).
[0090] (Preparation of samples for OIT test) Sample preparation and OIT test evaluation were performed in the same manner as in Example 1, except that coating solution (A3) was used instead of coating solution (A1).
[0091] (Preparation of gas separation membrane) A polypropylene (PP) porous film (Polypore Corporation, Celgard (registered trademark) 2500) was prepared as the first porous layer. Using a corona surface modification evaluation device (Kasuga Electric Co., Ltd., TEC-4AX, treatment electrode width: 21 cm), corona treatment was performed on one side of the first porous layer under conditions of discharge output of 75 W and treatment speed of 1 m / min.
[0092] The coating solution (A3) was applied to the corona-treated surface of the first porous layer using a tabletop applicator set to a coating thickness of 100 μm to form a coating film, which was then dried at 25° C. for 12 hours to obtain a gas separation membrane.
[0093] (Evaluation of permeability) The gas separation membrane obtained above was used to evaluate the permeation performance.
[0094] Example 4 (Preparation of Coating Solution (A4')) 8.0g of ethylene oxide-propylene oxide copolymer (Meisei Chemical Industry Co., Ltd., Alkox EP1550H), 192g of water, and 1.1g of 10% by weight surfactant (AGC Seimi Chemical Co., Ltd., Surflon S-242) aqueous solution were mixed and stirred, and then filtered through a filter with a pore size of 2μm to obtain coating solution (A4'). The content of ethyleneoxy units in the ethylene oxide-propylene oxide copolymer was 90% by weight.
[0095] (Preparation of Coating Solution (A4)) 0.2 g of an ethanol solution containing 0.1 wt % DL-α-tocopherol (Tokyo Chemical Industry Co., Ltd.) and 0.1 wt % Irganox 1520 (BASF Japan) was mixed with 5.0 g of coating liquid (A4') and stirred to obtain coating liquid (A4).
[0096] (Preparation of samples for OIT test) Sample preparation and OIT test evaluation were performed in the same manner as in Example 1, except that coating solution (A4) was used instead of coating solution (A1).
[0097] (Preparation of gas separation membrane) A gas separation membrane was obtained in the same manner as in Example 3, except that the coating liquid (A4) was used instead of the coating liquid (A3).
[0098] (Evaluation of permeability) The gas separation membrane obtained above was used to evaluate the permeation performance.
[0099] Comparative Example 1 (Preparation of Coating Solution (A0)) In the same manner as in Example 1, a coating liquid (A0) was obtained.
[0100] (Preparation of samples for OIT testing) Sample preparation and OIT test evaluation were performed in the same manner as in Example 1, except that the coating liquid (A0) was used instead of the coating liquid (A1).
[0101] (Preparation of gas separation membrane) A polypropylene (PP) porous film (Polypore Corporation, Celgard (registered trademark) 2500) was prepared as the first porous layer. Using a corona surface modification evaluation device (Kasuga Electric Co., Ltd., TEC-4AX, treatment electrode width: 21 cm), corona treatment was performed on one side of the first porous layer under conditions of discharge output of 75 W and treatment speed of 1 m / min.
[0102] The coating solution (A0) was applied to the corona-treated surface of the first porous layer using a tabletop applicator set to a coating thickness of 100 μm to form a coating film.
[0103] Using an electron beam irradiation device (Iwasaki Electric Co., Ltd., EC250), the coated membrane was subjected to electron beam irradiation treatment under the conditions of an irradiation dose of 50 kGy, a current of 5.6 mA, a voltage of 225 kV, a speed of 8 m / min, and a number of times of 1. Thereafter, the membrane was dried at 25°C for 12 hours to obtain a gas separation membrane.
[0104] (Evaluation of permeability) The gas separation membrane obtained above was used to evaluate the permeation performance.
[0105] Comparative Example 2 (Preparation of Coating Solution (B2)) 0.1 g of an ethanol solution containing 0.1 wt % of 2,6-di-tert-butyl-p-cresol (Tokyo Chemical Industry Co., Ltd.) and 5.0 g of the coating liquid (A0) were mixed and stirred to obtain a coating liquid (B2).
[0106] (Preparation of samples for OIT test) Sample preparation and OIT test evaluation were performed in the same manner as in Example 1, except that coating solution (B2) was used instead of coating solution (A1).
[0107] Comparative Example 3 (Preparation of Coating Solution (B3)) 0.1 g of an ethanol solution containing 0.1 wt % D-sorbitol (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5.0 g of the coating liquid (A0) were mixed and stirred to obtain a coating liquid (B3).
[0108] (Preparation of samples for OIT testing) Sample preparation and OIT test evaluation were performed in the same manner as in Example 1, except that coating solution (B3) was used instead of coating solution (A1).
[0109] Comparative Example 4 (Preparation of Coating Solution (B4)) 0.1 g of an ethanol solution containing 0.1 wt % N,N-diethylhydroxylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5.0 g of the coating liquid (A0) were mixed and stirred to obtain a coating liquid (B4).
[0110] (Preparation of samples for OIT testing) Sample preparation and OIT test evaluation were performed in the same manner as in Example 1, except that coating solution (B4) was used instead of coating solution (A1).
[0111] Comparative Example 5 (Preparation of Coating Solution (B5)) 0.1 g of an ethanol solution containing 0.1% by weight of L-ascorbic acid (Tokyo Chemical Industry Co., Ltd.) and 5.0 g of the coating liquid (A0) were mixed and stirred to obtain a coating liquid (B5).
[0112] (Preparation of samples for OIT testing) Sample preparation and OIT test evaluation were performed in the same manner as in Example 1, except that coating solution (B5) was used instead of coating solution (A1).
[0113] [Evaluation results] The evaluation results of the examples and comparative examples are shown in Table 1.
[0114] [Table 1]
[0115] The inorganic value, organic value, and I / O value of each antioxidant are shown in Table 2. These values were calculated based on "New Edition Organic Concept Diagram: Basics and Applications" (Yoshio Koda et al., Sankyo Publishing, 2008).
[0116] [Table 2]
[0117] As shown in Tables 1 and 2, Examples 1 to 4, which used antioxidants with an I / O value of 0.4 or less, showed superior results in the OIT test compared to Comparative Examples 1 to 5, which used antioxidants with an I / O value of more than 0.4. Furthermore, Examples 1 to 4 also showed superior results in the gas permeation test compared to Comparative Example 1. Thus, it was found that a gas separation membrane with excellent durability against degradation of the polymer by oxidizing gas can be provided by combining a polymer having a polyethylene oxide structure with an antioxidant with an I / O value of 0.4 or less. Since Comparative Examples 2 to 5 showed the same results as Comparative Example 1 in the OIT test, it is presumed that they will also show the same results as Comparative Example 1 in the gas permeation test. [Industrial Applicability]
[0118] One aspect of the present invention can be used in a gas separation membrane that separates a specific gas component from a mixed gas. [Explanation of symbols]
[0119] 10 Gas separation membrane 11 Porous support layer 12 Protective layer 13 Reinforcement layer 15 Separation functional layer 61 Gas separation membrane cell 62 Supply Side Room 63 Transmitting side chamber 64 Cooling trap 65 Back pressure regulator 66 Cooling Trap 67 Gas Chromatograph 81 Fixed-volume liquid delivery pump 69 Back pressure regulator 71 Pressure reducing pump 100 Gas separation device
Claims
1. A separating functional layer is provided, the separating functional layer including a polymer having a polyethylene oxide structure and an antioxidant, The polymer having a polyethylene oxide structure contains, in terms of weight ratio, 57% or more of ethyleneoxy units relative to 100% of main chain constituent units, The gas separation membrane, wherein the antioxidant has an I / O value in an organic conceptual diagram of 0.4 or less.
2. 2. The gas separation membrane according to claim 1, wherein the antioxidant has an organic value of 300 to 1500 and an inorganic value of 0 to 300 in an organic conceptual diagram.
3. The gas separation membrane according to claim 1 , wherein the antioxidant is in a liquid state under conditions of 1 atm and 25° C.
4. The gas separation membrane according to claim 1 , wherein the separation functional layer contains, as the antioxidant, a primary antioxidant and a secondary antioxidant.
5. Further comprising a porous support layer; The gas separation membrane according to claim 1 , wherein the separation functional layer is provided on the porous support layer.
6. 2. The gas separation membrane according to claim 1, which is used to selectively permeate carbon dioxide from a mixed gas containing carbon dioxide and nitrogen.
7. A gas separation device comprising the gas separation membrane according to any one of claims 1 to 6.
8. The method includes forming a separation functional layer containing a polymer having a polyethylene oxide structure and an antioxidant on a porous support layer, The polymer having a polyethylene oxide structure contains, in terms of weight ratio, 57% or more of ethyleneoxy units relative to 100% of main chain constituent units, The method for producing a gas separation membrane, wherein the antioxidant has an I / O value in an organic conceptual diagram of 0.4 or less.
9. A gas separation membrane comprising a separation functional layer containing at least one member selected from the group consisting of vitamin E and its analogues, and a porous support layer.
Citation Information
Patent Citations
Polymeric separation membrane
JP2003205224A
Membrane for selective gas separation
JP2004508187A
Gas separation membrane
JP2005074317A
Gas separation membrane
JP2005305371A
Porous membrane for water treatment and method for manufacturing same
JP2021505358A