Spark plug

The spark plug's insulator design with controlled porosity and pore distribution addresses thermal shock and dielectric strength issues by limiting alkaline intrusion and stress, enhancing performance in high-temperature environments.

JP2024141053AInactive Publication Date: 2024-10-10NITERRA CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052491
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing spark plugs face issues with reduced thermal shock resistance and dielectric strength due to abnormal grain growth in the insulator, which can be exacerbated by alkaline components in high-temperature environments.

Method used

The spark plug design incorporates an insulator with specific pore distribution and porosity control, ensuring a porosity of 5% or less and an average pore size of 26.3 μm with a maximum of 37 μm and a minimum distance of 36.3 μm between pores, using a ceramic material like alumina and sealing materials with controlled thermal expansion.

Benefits of technology

This design enhances dielectric strength and thermal shock resistance by limiting the intrusion of alkaline components and managing thermal stress, thereby improving the insulator's performance in high-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141053000001_ABST
    Figure 2024141053000001_ABST
Patent Text Reader

Abstract

To provide a spark plug that can ensure dielectric strength and thermal shock resistance.MEANS FOR SOLVING THE PROBLEM: A spark plug includes a sealing material that is arranged around a center electrode inside an insulator. In a cross section including the center line of an axial hole, a rectangle having an axial length of 1920 μm and a radial length of 510 μm is set in the insulator such that the tip of the long side of the rectangle touches the tip of a first hole and the rear end of the long side touches the first hole. When an area obtained by dividing the short side of the rectangle in half and dividing the long side of the rectangle into ten equal parts, and dividing the rectangle into twenty equal parts is set in the insulator, the porosity of the rectangle is 5% or less; the average area of specific pores selected ten by ten in order of size from the largest among the pores appearing in the area is 26.3 μm2 or less; the number of specific pores with an area of 37 μm2 or more is 30 or less; and the number of pores with an area of 51 μm2 or more is 8 or more.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a spark plug having an insulator disposed therein. [Background technology]

[0002] Patent document 1 discloses a prior art technique for suppressing abnormal grain growth in an insulator in order to ensure the dielectric strength of a spark plug in which a center electrode is fixed to an insulator by a sealing material placed around the center electrode. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2022-190529 A Summary of the Invention [Problem to be solved by the invention]

[0004] The prior art may result in reduced thermal shock resistance of the insulator.

[0005] The present invention has been made to solve this problem, and has an object to provide a spark plug which can ensure both dielectric strength and thermal shock resistance. [Means for solving the problem]

[0006] In order to achieve this object, a first aspect of the present invention is a spark plug comprising: an insulator provided with an axial hole in which a first hole and a second hole having a smaller diameter than the first hole are connected in the axial direction via a connection portion; a center electrode extending from the first hole through the second hole toward the tip side; and a sealing material arranged inside the insulator on the rear end side of the center electrode, wherein in any cross section including the center line of the axial hole, when a rectangle having an axial length of 1920 μm and a radial length of 510 μm is set in the insulator such that the tip of one long side of the rectangle contacts the tip of the first hole and the rear end of the long side contacts the first hole, the ratio of the area of ​​the pores appearing in the rectangle to the area of ​​the rectangle is 5% or less. The short side of a rectangle is divided into two equal parts, and the long side of the rectangle is divided into ten equal parts, resulting in 20 equal areas set in the insulator. Among the pores appearing in each area, the 10 largest ones are selected as specific pores. The average area of ​​the specific pores is 26.3μm 2 The area of ​​the specific pore is 37 μm or less. 2 The number of pores is 30 or less, and the area is 51 μm 2 The number of pores is 8 or more.

[0007] In the second embodiment, the area of ​​the specific pore is 37 μm in the first embodiment. 2 The distance between the pores is 36.3 μm or more. Effect of the Invention

[0008] The porosity of a rectangular area with an axial length of 1920 μm and a radial length of 510 μm set on the cross section of the insulator adjacent to the sealing material is 5% or less, and the average area of ​​the specific pores selected from the 10 largest pores in each of the 20 equal parts of the rectangle is 26.3 μm. 2 The area of ​​the specific pore is 37 μm or less. 2 Since the number of pores is 30 or less, the dielectric strength can be ensured. Furthermore, the area of ​​the specific pores is 51 μm 2 Since the number of pores is eight or more, the thermal shock resistance of the insulator can be ensured. [Brief description of the drawings]

[0009] [Figure 1] 1 is a half-sectional view of a spark plug according to an embodiment; [Diagram 2] 2 is an enlarged cross-sectional view of the spark plug shown in FIG. 1. [Diagram 3] FIG. 2 is a schematic diagram showing an enlarged binary image of a cross section of an insulator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Preferred embodiments of the present invention will now be described with reference to the accompanying drawings. Fig. 1 is a half-sectional view combining an outline view and a full cross-sectional view taken along the center line X of an axial hole 12 of a spark plug 10 in one embodiment. The lower side of Fig. 1 is the leading end side of the spark plug 10, and the upper side is the trailing end side of the spark plug 10 (the same applies to Fig. 2). The spark plug 10 includes an insulator 11 and a center electrode 16.

[0011] The insulator 11 is a cylindrical member having an axial hole 12 extending along the axis O, and is made of ceramic such as alumina, which has excellent insulating properties and mechanical properties at high temperatures. In this embodiment, the insulator 11 is an alumina-based sintered body. The axial hole 12 is connected to the first hole 13, the connection part 14, and the second hole 15 in this order from the rear end to the front end of the insulator 11. In this embodiment, the first hole 13 and the second hole 15 are cylindrical surfaces with the same diameter over their entire length, and the connection part 14 is a conical surface whose diameter decreases toward the front end. The connection part 14 may be an annular plane perpendicular to the center line X of the first hole 13 or the second hole 15. The diameter of the second hole 15 is smaller than the diameter of the first hole 13.

[0012] A rod-shaped metal center electrode 16 is disposed in the axial hole 12 of the insulator 11. The center electrode 16 has a core material with excellent thermal conductivity embedded in a base material. The base material is formed of an alloy mainly made of Ni or a metal material made of Ni. The core material is formed of copper or an alloy mainly made of copper. The core material can be omitted. The center electrode 16 has a head 17 disposed in the first hole 13 and in contact with the connection part 14, and a leg part 18 extending from the head 17 toward the tip side and disposed in the second hole 15. The head 17 and the leg part 18 are integrally formed.

[0013] The terminal fitting 19 is a rod-shaped member to which an ignition device (not shown) is connected, and is made of a conductive metal material (such as low carbon steel). The tip side of the terminal fitting 19 is disposed in the first hole 13 of the insulator 11, and the rear end side of the terminal fitting 19 protrudes from the insulator 11. In the first hole 13 of the insulator 11, a seal material 20, a resistor 21, and a seal material 22 are disposed between the center electrode 16 and the terminal fitting 19 in this order from the tip side.

[0014] The seal material 20 has a function of fixing the head 17 of the center electrode 16 to the insulator 11 and closing the first hole 13, and is disposed around the head 17. The seal material 22 has a function of fixing the terminal fitting 19 to the insulator 11. The seal materials 20 and 22 are conductive and contain, for example, glass particles and metal particles (Cu, Fe, etc.) in a ratio of about 1:1. As the glass particles, for example, B2O3-SiO2-based, BaO-B2O3-based, SiO2-B2O3-CaO-BaO-based materials can be used. The thermal expansion coefficient of the seal materials 20 and 22 is between that of the ceramic insulator 11 and that of the metal center electrode 16.

[0015] The resistor 21 is a member for suppressing radio noise generated at the time of sparking. The resistor 21 is a mixture containing glass particles as a main component, ceramic particles other than glass, and a conductive material. As the material of the glass particles, for example, B2O3-SiO2, BaO-B2O3, SiO2-B2O3-CaO-BaO, etc. can be used. As the material of the ceramic particles, for example, TiO2, ZrO2, etc. can be used. As the conductive material, for example, non-metallic conductive materials such as carbon particles (carbon black, etc.), TiC particles, TiN particles, etc., and metals such as Al, Mg, Ti, Zr, and Zn can be used. Since the seal materials 20 and 22 are in contact with the resistor 21, the center electrode 16 and the terminal metal fitting 19 are electrically connected via the seal materials 20 and 22 and the resistor 21.

[0016] The metallic shell 23 is a substantially cylindrical member made of a conductive metal material (such as low carbon steel). The metallic shell 23 is disposed on the outer periphery of the insulator 11. The ground electrode 24 is a rod-shaped metallic member (such as a nickel-based alloy) connected to the metallic shell 23. A spark gap is formed between the ground electrode 24 and the leg 18 of the center electrode 16. A plurality of ground electrodes 24 may be connected to the metallic shell 23.

[0017] The spark plug 10 is manufactured, for example, by the following method. First, the center electrode 16 is inserted from the first hole 13 of the insulator 11. The head 17 of the center electrode 16 is disposed in the first hole 13 in contact with the connection portion 14 of the insulator 11, and the leg portion 18 is disposed in the second hole 15.

[0018] Next, raw material powder for sealing material 20 is poured through first hole 13 to fill the area around head 17 and the area of ​​first hole 13 rearward of head 17, and then the raw material powder is pre-compressed using a compression rod (not shown). Next, raw material powder for resistor 21 is filled on top of the raw material powder for sealing material 20, and then the raw material powder is pre-compressed using a compression rod. Finally, raw material powder for sealing material 22 is filled on top of the raw material powder for resistor 21, and then the raw material powder is pre-compressed using a compression rod.

[0019] The terminal fitting 19 is inserted from the rear end side of the first hole 13 so that the tip end of the terminal fitting 19 comes into contact with the raw material powder of the sealing material 22, and then the terminal fitting 19 is pressed into the raw material powder while heating the raw material powder to a temperature higher than the softening point of the glass component contained in each raw material powder, for example, so that the terminal fitting 19 applies an axial load to the raw material powder. Each raw material powder is compressed and sintered, and the sealing materials 20, 22 and resistor 21 are produced in the first hole 13. Next, the metallic shell 23 to which the ground electrode 24 is connected is assembled on the outer periphery of the insulator 11, and then the ground electrode 24 is bent to set a spark gap between the ground electrode 24 and the center electrode 16, thereby obtaining the spark plug 10.

[0020] 2 is an enlarged cross-sectional view of a portion indicated by II in FIG. 1, the cross-sectional view including the center line X of the axial hole 12 of the spark plug 10, and illustrates the vicinity of the head 17 of the center electrode 16. A sealant 20 is disposed around the head 17 disposed in the first hole 13 of the insulator 11. In the spark plug 10 mounted on an engine (not shown), heat in the combustion chamber is transferred from the leg 18 of the center electrode 16 (see FIG. 1) to the head 17, and then from the head 17 to the sealant 20. Since the thermal conductivity of the sealant 20 is lower than that of the center electrode 16, the thermal conductivity of the sealant 20 becomes the rate-limiting factor for heat transfer, and the sealant 20 is heated.

[0021] Because the head 17 is thicker than the leg portions 18, the distance between the head 17 and the metal shell 23 (see FIG. 1) is shorter than the distance between the leg portions 18 and the metal shell 23. Therefore, the electric field between the head 17 and the metal shell 23 is stronger than the electric field between the leg portions 18 and the metal shell 23.

[0022] The sealant 20 contains an alkaline component derived from glass particles, which is the main component of the material. The insulator 11 made of an alumina-based sintered body has excellent resistance to alkaline corrosion, but in a high-temperature, high-voltage environment in which the spark plug 10 is installed in an engine, alkaline components may penetrate through the pores of the insulator 11, which may cause a decrease in dielectric strength. In order to ensure the dielectric strength, attention is focused on the pores in the portion of the insulator 11 adjacent to the sealant 20.

[0023] A rectangle 25 is set in a portion of the insulator 11 adjacent to the sealing material 20, and the rectangle 25 has long sides 26, 29 each having a length of 1920 μm, and short sides 30, 31 each having a length of 510 μm. The rectangle 25 has short sides 30, 31 set along the radial direction of the insulator 11, and the long sides 26, 29 set along the axial direction of the insulator 11 so that a leading end 27 of the long side 26 contacts the leading end of the first hole 13 and a trailing end 28 of the long side 26 contacts the first hole 13. Since the corner of the insulator 11 where the first hole 13 and the connection portion 14 intersect is rounded, the leading end of the first hole 13 is set as the leading end of the straight part of the first hole 13 (the intersection of the rounded part (curve) and the straight line).

[0024] Furthermore, the short sides 30, 31 of the rectangle 25 are each divided into two equal parts, and the long sides 26, 29 are each divided into ten equal parts, thereby setting 20 ranges 32 by dividing the rectangle 25 into 20 equal parts. The length of the short side of the range 32 extending in the axial direction is 192 μm, and the length of the long side extending in the radial direction is 255 μm. The size of the range 32 is equal to the size of one field of view observed using an SEM.

[0025] In order to obtain an SEM image of the cross section of the insulator 11 and calculate the area of ​​the pores, the cross section of the insulator 11 is polished to a degree of precision that allows the shape of the pores appearing in the cross section to be identified. The surface roughness (Ra) of the insulator 11 after polishing is, for example, about 0.001 μm. In this embodiment, the acceleration voltage of the SEM is set to 20 kV, and the magnification of the SEM is set to 500 times.

[0026] After acquiring an SEM image for each of the 20 ranges 32, image analysis is performed using known image analysis software (for example, WinROOF (registered trademark), manufactured by Mitani Shoji Co., Ltd.). In the image analysis, the size of each SEM image is calibrated based on the scale bar attached to the SEM image, and then the SEM image is binarized. In the binarization process, the brightness (lightness) of each pixel of the SEM image is binarized using a predetermined threshold (for example, a threshold of 118). In other words, pixels whose brightness is below the threshold are set to a brightness of zero, and pixels whose brightness is above the threshold are set to a brightness of "255". A binarized image is obtained by binarizing the pixels and eliminating intermediate gradations.

[0027] FIG. 3 is a schematic diagram showing an enlarged binary image of the cross section of insulator 11. In FIG. 3, pores are shown in black, and other parts (ceramic particles and grain boundaries) are shown in white. Using the binary image of range 32, all pores (voids) contained in range 32 are extracted by a known image analysis method, and the area of ​​the extracted pores is calculated for each pore. The total area of ​​all pores contained in 20 ranges 32 divided by the area of ​​rectangle 25 is the porosity of insulator 11 (%). The porosity of insulator 11 is 5% or less. This is to ensure the mechanical strength of insulator 11.

[0028] Next, from all the pores contained in the ranges 32, the 10 pores with the largest area are selected. The 10 pores selected for each range 32 in order of area are referred to as specific pores. There are 200 specific pores in the rectangle 25. The total area of ​​the specific pores is calculated for each range 32, and the average of the 20 ranges 32 is calculated. The total area of ​​the specific pores calculated for each range 32 is then averaged over the 20 ranges 32, and the average is then divided by 200, and the sum of the areas of the 200 specific pores is rounded off to one decimal place to obtain a value of 26.3 μm 2 The reason is as follows. This is to limit the size of large pores (specific pores) into which alkaline components may penetrate and which may lead to a decrease in dielectric strength, thereby reducing the penetration of alkaline components.

[0029] In addition, the distribution of the specific pores is obtained by a known image analysis method. 2 The number of pores having an area of ​​51 μm or less is 30 or less. This is to limit the number of large pores into which alkaline components may infiltrate and lead to a decrease in dielectric strength, thereby reducing the infiltration of alkaline components. Furthermore, the insulator 11 has a specific pore with an area of ​​51 μm or less. 2 The number of pores is 8 or more. This is to ensure a particularly large number of pores and to ensure the thermal shock resistance of the insulator 11.

[0030] Furthermore, as shown in FIG. 3, a known image analysis method was used to determine that the area of ​​a specific pore was 37 μm 2 Calculate the distance L between the pores 33 and 34. The area is 37 μm2 When determining the distance L between the pores 33 and 34, it is necessary to determine not only the distance L between the pores present in each range 32, but also the distance L between the pores present in each different range 32 across adjacent ranges 32. The distance L of the insulator 11 is 36.3 μm or more. This is because the intrusion of alkaline components is further reduced by having large pores spaced apart from each other, into which alkaline components may intrude and lead to a decrease in dielectric strength.

[0031] An example of a method for manufacturing the insulator 11 will be described. The insulator 11 is manufactured through the steps of slurry preparation, degassing, granulation, molding, grinding, and firing. Each step will be described below in order.

[0032] The slurry preparation process is a process of preparing a slurry by mixing a raw material powder, a binder, and a solvent. The raw material powder mainly contains a powder of a compound that is converted to alumina by firing (hereinafter referred to as "Al compound powder"). As the Al compound powder, for example, alumina powder is used.

[0033] In the slurry preparation process, a pulverization process is carried out for the purpose of mixing and pulverizing the raw material powder. The pulverization process is carried out using a wet pulverizer using a ball mill or the like. The diameter of the balls used in the wet pulverizer is not particularly limited as long as it does not impair the object of the present invention, but is preferably 2 mm to 20 mm, more preferably 2 mm to 10 mm, and even more preferably 2 mm to 6 mm. Two or more types of balls having different diameters may be combined. By such a pulverization process, the raw material powder has a small variation in particle size (particle size) and a sharp particle size distribution. By using such a raw material powder, the distribution and number of pores can be controlled in the alumina-based sintered body obtained after sintering, and the sintering density can be increased.

[0034] The particle size (particle size after pulverization) of the Al compound powder (alumina powder, etc.) is not particularly limited as long as it does not impair the object of the present invention, but is preferably 1.5 μm or more, more preferably 1.7 μm or more, more preferably 2.5 μm or less, and more preferably 2.0 μm or less. When the particle size of the Al compound powder is in this range, the number of defects in the insulator is suppressed and an appropriate sintering density is obtained. The particle size is the volume-based median diameter (D50) measured by a laser diffraction method (Microtrack particle size distribution measuring device, product name "MT-3000", manufactured by Nikkiso Co., Ltd.).

[0035] The Al compound powder is preferably prepared so that it is 90% by mass or more in terms of oxide when the mass (oxide equivalent) of the alumina-based sintered body after firing is taken as 100% by mass. More preferably, it is 90% by mass or more and 98% by mass or less, and even more preferably, it is 90% by mass or more and 97% by mass or less. As long as it does not impair the object of the present invention, the raw material powder may contain powder other than the Al compound powder.

[0036] The binder is added to the slurry for the purpose of improving the moldability of the raw material powder. Examples of such binders include hydrophilic binders such as polyvinyl alcohol, aqueous acrylic resin, gum arabic, and dextrin. These may be used alone or in combination of two or more. The amount of the binder is not particularly limited as long as it does not impair the object of the present invention, but for example, it is mixed in a ratio of 1 to 10 parts by mass, preferably 3 to 7 parts by mass, per 100 parts by mass of the raw material powder.

[0037] The solvent is used for the purpose of dispersing the raw material powder, etc. Examples of the solvent include water, alcohol, etc. These may be used alone or in combination of two or more. The amount of the solvent is not particularly limited as long as it does not impair the object of the present invention, but for example, it is mixed in a ratio of 23-40 parts by mass, preferably 25-35 parts by mass, per 100 parts by mass of the raw material powder. The slurry may contain other components other than the raw material powder, binder, and solvent as necessary. A known stirring / mixing device or the like can be used to mix the slurry.

[0038] The prepared slurry may be degassed as necessary. In the degassing step, for example, a container containing the mixed (kneaded) slurry is placed in a vacuum degassing device, and the pressure is reduced to place it in a low-pressure environment, thereby removing the bubbles contained in the slurry. The amount of bubbles in the slurry can be determined by comparing the density of the slurry before and after degassing.

[0039] The granulation process is a process of producing spherical granulated powder from a slurry containing raw material powders and the like. The method of producing granulated powder from a slurry is not particularly limited as long as it does not impair the object of the present invention, and for example, a spray drying method can be mentioned. In the spray drying method, a granulated powder having a predetermined particle size is obtained by spray drying the slurry using a predetermined spray dryer device. The particle size of the granulated powder is not particularly limited as long as it does not impair the object of the present invention, and for example, 212 μm pass ≧ 95% or less is preferable, and 180 μm pass ≧ 95% or less is more preferable.

[0040] The molding process is a process in which the granulated powder is molded into a predetermined shape using a mold to obtain a molded body. The molding process is performed by rubber press molding, die press molding, or the like. In the case of this embodiment, the pressure (press pressure rise rate) applied to the mold (e.g., the inner rubber mold and the outer rubber mold of a rubber press molding machine) from the outer periphery is adjusted so as to increase in stages. In addition, it is preferable to adjust the pressure range to a higher pressure range than before (e.g., 100 MPa or more). The upper limit of the pressure is not particularly limited as long as it does not impair the object of the present invention, but may be adjusted to, for example, 200 MPa or less.

[0041] The grinding process is a process for removing the machining allowance of the molded body obtained after the molding process and polishing the surface of the molded body. In the grinding process, the machining allowance is removed and the surface of the molded body is polished by grinding with a resinoid grinding wheel or the like. By such a grinding process, the shape of the molded body is adjusted.

[0042] The firing step is a step of firing the molded body, the shape of which has been adjusted by the grinding step, to obtain an insulator. In the firing step, for example, firing is performed in an air atmosphere at 1450°C to 1650°C for 1 to 8 hours. After firing, the molded body is cooled to obtain the insulator 11 made of an alumina-based sintered body. EXAMPLES

[0043] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.

[0044] (Making an insulator) Four insulators each having the same basic configuration as the insulator 11 of the spark plug 10 exemplified in the embodiment were produced in the same manner as the embodiment, for samples No. 1 to 17. The radial thickness of the insulator 11 at the tip of the first hole 13 was 3 mm. The insulator of sample No. 1 was prepared by mixing 50% by mass of 2 mm diameter pebbles and 50% by mass of 6 mm diameter pebbles when grinding the raw material powder with a wet grinder in the slurry preparation process. The insulators of samples No. 2 to 8 were produced in the same manner as sample No. 1, except that the ratio of the pebbles used when grinding the raw material powder in the slurry preparation process was appropriately changed.

[0045] For the insulator sample No. 9, 8 mm diameter pebbles and 12 mm diameter pebbles were mixed in a ratio of 50% by mass and 50% by mass, respectively, when the raw powder was crushed in a wet grinder in the slurry preparation process. The insulators of samples No. 10-15 and 17 were prepared in the same manner as sample No. 9, except that the ratio of the pebbles used when crushing the raw powder in the slurry preparation process was appropriately changed. The insulator sample No. 16 was prepared in the same manner as sample No. 1, except that the amount of silica in the raw powder was increased and the pressure in the molding process was made higher than the pressure in the molding process of the insulator sample No. 1.

[0046] (Voltage Test) Using two of each of the four insulators of Sample No. 1-17, two samples of the spark plug 10 described in the embodiment were produced. For one sample, the ground electrode 24 was removed so as not to cause discharge between the center electrode 16 and the ground electrode 24 in accordance with the withstand voltage test specified in JIS B8031:2006, and then the metal shell 23 was tightened to a specified torque in a pressure chamber. Carbon dioxide gas was supplied to the pressure chamber to a pressure of about 5 MPa, and then the voltage applied between the terminal metal 19 and the metal shell 23 of the sample was increased from 0 V at a rate of 0.1 kV / sec to check the dielectric breakdown voltage when the insulator 11 was penetrated. The dielectric breakdown voltage was in the range of 40 kV to 42 kV.

[0047] For the other sample, the ground electrode 24 was removed to prevent discharge between the center electrode 16 and the ground electrode 24, and the tip of the insulator 11 was covered with a heat-resistant insulating tube. The sample was then placed in a heating furnace maintained at approximately 200°C, and a voltage of 35 kV was applied between the terminal fitting 19 and the metal shell 23 for 100 hours. This is because the sample was placed in an environment where the insulator 11 would be easily corroded by the alkaline components contained in the sealant 20 arranged around the head 17 of the center electrode 16. The presence or absence of alkaline corrosion can be determined by measuring the presence or absence of alkali metals such as Na and alkaline earth metals in the insulator 11 using an electron probe microarray (EPMA).

[0048] After the sample was removed from the heating furnace, the metal shell 23 was tightened in the pressure chamber with a specified torque in accordance with the withstand voltage test specified in JIS B8031:2006. After supplying carbon dioxide gas to the pressure chamber to a pressure of about 5 MPa, the voltage applied between the terminal metal 19 and the metal shell 23 of the sample was increased from 0 V at a rate of 0.1 kV / sec, and the dielectric breakdown voltage when the dielectric breakdown voltage penetrated the insulator 11 was measured. Samples with a dielectric breakdown voltage of 38 kV or more after alkali erosion were judged as A, samples with a dielectric breakdown voltage of 36 kV or more and less than 38 kV were judged as B, samples with a dielectric breakdown voltage of 33 kV or more and less than 36 kV were judged as C, and samples with a dielectric breakdown voltage of less than 33 kV were judged as D. The results are shown in the dielectric strength column of Table 1.

[0049] (Cross-section observation of insulator) Each of the four insulators 11 of Sample No. 1-17 was cut at a position including the center line X of the axial hole 12. The cut surface of the insulator 11 was polished to a mirror finish, and the structure of the polished surface was observed with an SEM (JEM-IT300LA, manufactured by JEOL Ltd.). Ten rectangular areas 32 (long side length 255 μm, short side length 195 μm) whose short sides contact the first hole 13 of the insulator 11 were set, and ten areas 32 adjacent to the outside of the ten areas 32 in the radial direction were set. After acquiring 20 SEM images corresponding to the 20 areas 32, processing was performed using image processing software WinROOF2013 (WinROOF is a registered trademark), and the ratio (porosity) of the total area of ​​pores appearing in the entire 20 areas 32 (rectangle 25) to the area of ​​the rectangle 25 was calculated. The porosity of the insulator 11 of sample No. 1-17 was 5% or less.

[0050] Using image analysis, the 10 largest pores were selected from all pores contained in the range 32, the total area of ​​the 10 selected pores (specific pores) was calculated for each range 32, and the average (rounded to the nearest tenth) of the 20 ranges 32 was calculated. The results are shown in the "Area of ​​specific pores" column in Table 1.

[0051] Image analysis revealed that the area of ​​a specific pore was 37 μm 2 The number and area of ​​pores above 51μm 2 The number of pores was calculated for each of the above. The number of pores was calculated by adding up the numbers in each of the 20 ranges. The results are shown in Table 1, "37 μm 2 "Porosity of 51μm or more" 2 The above pores are noted in the "Porosity" column.

[0052] Image analysis revealed that the area of ​​a specific pore appearing in the rectangle 25 is 37 μm 2 Select two of the above pores and divide them into two groups with an area of ​​37 μm 2 The distance between pores, L, was calculated for all combinations of two pores. The shortest distance among all distances, L, is shown in the "Distance between pores" column of Table 1.

[0053] (Thermal shock test) The insulators 11 of Samples No. 1-17 were each stored in a thermostatic chamber maintained at a predetermined temperature for 30 minutes, and then immediately immersed in water at 20°C for rapid cooling. The orientation of the insulators 11 when immersed in water was such that the center line X of the axial hole 12 of the insulators 11 was parallel to the water surface. The presence or absence of cracks in the insulators 11 taken out of the water was visually confirmed by applying a penetrant inspection liquid. The temperature of the thermostatic chamber in which the insulators 11 were stored was increased in 10°C increments from 150°C until a crack was found in the insulators 11, and the temperature difference (critical temperature difference) between the temperature of the thermostatic chamber and the water temperature (20°C) when a crack was found in the insulators 11 was examined. Samples with a critical temperature difference of 210°C or more were judged to be A, and samples with a critical temperature difference of less than 210°C were judged to be D. The results are shown in the column of thermal shock properties in Table 1.

[0054] [Table 1]

[0055] As shown in Table 1, the average area of ​​specific pores is 26.3 μm 2 and the area is 37 μm 2 Samples No. 1-8 and No. 16, which had 30 or fewer pores, were rated A or B for dielectric strength. On the other hand, the average area of ​​specific pores was 26.3 μm 2 Samples No. 11-15 and 17, which had a dielectric strength rating of D, were also given a rating of D. The average area of ​​specific pores was 26.3 μm 2 Even if the area is less than 37 μm 2 Samples 9 and 10, which had more than 30 pores, were rated C for dielectric strength. The average area of ​​the specific pores in insulator 11 was 26.3 μm 2 The dielectric strength rating of A or B is a necessary condition for the area of ​​37μm2 or less. 2 It was found that a number of pores of 30 or less is a sufficient condition for obtaining an A or B rating for dielectric strength.

[0056] Area is 51μm 2 Samples No. 1-12, 14, 15, and 17, which had 8 or more pores, were rated as A for thermal shock resistance. 2Samples No. 13 and No. 16, which had seven or fewer pores, were rated D for thermal shock resistance. 2 It has been found that the critical temperature difference of the insulator 11 can be increased, that is, the resistance to quenching is improved, when the number of pores is eight or more. It is believed that the pores relieve the tensile stress generated in the insulator 11 by quenching.

[0057] Since sample No. 1-8 was judged as A or B for dielectric strength and A for thermal shock resistance, in order to ensure the dielectric strength and thermal shock resistance of the spark plug 10 used in a high-temperature environment, the porosity of the insulator 11 is set to 5% or less, and the average area of ​​the specific pores is set to 26.3 μm 2 Below, the area is 37μm 2 The number of pores is 30 or less and the area is 51 μm 2 It was found that it is effective to have eight or more pores.

[0058] Sample No. 1-7 was judged to have an A for both dielectric strength and thermal shock resistance, so the porosity of the insulator 11 was 5% or less, and the average area of ​​the specific pores was 26.3 μm 2 Below, the area is 37μm 2 30 or less pores, area 51μm 2 More than 8 pores and an area of ​​37μm 2 It was found that setting the distance between pores to 36.3 μm or more was particularly effective in ensuring dielectric strength and thermal shock resistance.

[0059] Although the present invention has been described above based on the embodiment, the present invention is not limited to the above embodiment, and it can be easily assumed that various improvements and modifications are possible without departing from the spirit of the present invention. For example, the shape and size of the head 17 of the center electrode 16 are merely examples and can be appropriately set.

[0060] In the embodiment, the spark plug 10 in which the resistor 21 is disposed inside the insulator 11 has been described, but the present invention is not necessarily limited to this. It is of course possible to apply the configuration of the embodiment to a spark plug that does not incorporate the resistor 21. This is because, as long as the head 17 of the center electrode 16 is fixed by the seal material 20, the same effects as those of the above embodiment can be achieved.

[0061] In the embodiment, the spark plug 10 in which the ground electrode 24 is exposed in the combustion chamber when the spark plug 10 is attached to an engine (not shown) has been described, but the present invention is not necessarily limited to this. It is of course possible to apply the configuration of the embodiment to a spark plug in which the ground electrode 24 is covered with a cap having a through hole (a spark plug in which a sub-chamber is provided in the combustion chamber).

[0062] In the embodiment, the spark plug 10 in which spark discharge occurs between the center electrode 16 and the ground electrode 24 has been described, but the present invention is not necessarily limited to this. It is of course possible to apply the configuration of the embodiment to a spark plug that utilizes non-equilibrium plasma generated around the leg portion 18 of the center electrode 16. [Explanation of symbols]

[0063] 10 Spark plug 11 Insulators 12 Shaft hole 13 Hole 1 14 Connection 15 2nd hole 16 Center electrode 20 Sealing material 25 rectangle 26 Long Side 27 End of long side 28 Rear end of long side 30,31 Short side 32 Range X center line

Claims

1. an insulator having an axial hole that connects a first hole and a second hole having a diameter smaller than that of the first hole via a connection part; a center electrode extending from the first hole through the second hole toward a tip side; a sealant disposed inside the insulator on a rear end side of the center electrode, In any cross section including the center line of the shaft hole, When a rectangle having a length of 1920 μm in the axial direction and a length of 510 μm in the radial direction is set in the insulator such that a tip end of one long side of the rectangle is in contact with a tip end of the first hole and a rear end of the long side is in contact with the first hole, A spark plug, wherein a ratio of an area of ​​the pores appearing in the rectangle to an area of ​​the rectangle is 5% or less, a short side of the rectangle is divided into two equal parts and a long side of the rectangle is divided into ten equal parts, and the resulting range is set in the insulator; Among the pores appearing in each of the above ranges, ten pores are selected in order of area from the largest to the smallest and are regarded as specific pores. The average area of ​​the specific pores is 26.3 μm 2 is as follows: The area of ​​the specific pore is 37 μm 2 The number of pores is 30 or less, and the area is 51 μm 2 A spark plug having eight or more pores.

2. The area of ​​the specific pore is 37 μm 2 2. The spark plug according to claim 1, wherein the distance between the pores is 36.3 [mu]m or more.

Citation Information

Patent Citations

  • Spark plug

    JP2022190529A