R-t-b base sintered magnet, method for producing the same and composition design method
By optimizing the composition and manufacturing method of R-T-B sintered magnets with controlled grain boundary thickness using boron, carbon, oxygen, and nitrogen, the magnets achieve enhanced coercive force and magnetic flux density, addressing the limitations of heavy rare earth element dependency.
Patent Information
- Application Number
- JP2023052596
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
R-T-B sintered magnets face challenges in maintaining high coercive force (HcJ) at high temperatures due to irreversible thermal demagnetization, and the use of heavy rare earth elements like Dy and Tb, which are scarce and volatile in supply, leading to price fluctuations.
The composition and manufacturing method of R-T-B sintered magnets are optimized by controlling the thickness of the two-grain grain boundary through precise regulation of boron concentration and additional elements like carbon, oxygen, and nitrogen, ensuring a balanced distribution of elements to enhance coercive force without relying heavily on heavy rare earths.
This approach results in R-T-B sintered magnets with improved coercive force and residual magnetic flux density, while reducing the reliance on scarce and expensive heavy rare earth elements, thus stabilizing supply and cost.
Smart Images

Figure 2024141121000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an RTB based sintered magnet, a manufacturing method thereof, and a composition design method. [Background technology]
[0002] RTB sintered magnets (R is at least one rare earth element. T is at least one transition metal element, always including Fe. B is boron) are known as the most high-performance magnets among permanent magnets, and are used in a variety of motors, including electric vehicle motors (EV, HV, PHV, etc.), industrial equipment motors, and home appliances. RTB sintered magnets are mainly R2T 14 It is composed of a main phase made of B compounds and a grain boundary phase (hereinafter sometimes simply referred to as "grain boundary") located at the grain boundary portion of this main phase. 14 The B compound is a ferromagnetic phase with high magnetization.
[0003] RTB sintered magnets have a coercive force H cJ (Hereinafter, simply "coercive force" or "H cJ This causes a problem of irreversible thermal demagnetization, as the magnetization temperature drops and the magnetization rate drops. For this reason, RTB sintered magnets, which are used in electric vehicle motors in particular, have a high H cJ It is required that the applicant have:
[0004] In RTB sintered magnets, R2T 14 When a part of the light rare earth elements (mainly Nd and / or Pr) contained in R in the B compound is replaced with heavy rare earth elements (mainly Dy and / or Tb), H cJ It is known that the H cJ will improve.
[0005] However, R2T 14 When the light rare earth elements in the B compound are replaced with heavy rare earth elements, the H of the RTB sintered magnet cJ While the residual magnetic flux density B r (Hereinafter, simply "Br In addition, heavy rare earth elements, especially Dy, are scarce and have limited production areas, so their supply is unstable and their prices fluctuate greatly. For this reason, in recent years, users have been promoting the use of H as little as possible without using heavy rare earth elements. cJ There is a need to improve this.
[0006] Patent Document 1 discloses an RTB rare earth sintered magnet with increased coercivity while reducing the Dy content. The composition of this sintered magnet is limited to a specific range in which the amount of B is relatively small compared to commonly used RTB alloys, and contains one or more metal elements M selected from Al, Ga, and Cu. As a result, R2T is formed at the grain boundaries. 17 Phase is generated and this R2T 17 Transition metal-rich phase (R6T 13 As the volume ratio of H cJ will improve. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2013 / 008756 Summary of the Invention [Problem to be solved by the invention]
[0008] High B while reducing the content of heavy rare earth elements r and high H cJIn order to realize an RTB based sintered magnet having this property, technology has been investigated for controlling the thickness of the two-particle grain boundary by relatively reducing the amount of B (boron concentration). However, it has been found that the conditions for thickening the two-particle grain boundary do not depend only on the amount of B, but also on other conditions (e.g., the amount of C, O, and N), and that the boundary conditions for the amount of B (conditions that determine the preferred range of the amount of B) vary depending on these other conditions. The manufacturing method and composition design method for an RTB based sintered magnet disclosed herein specify the ranges of the amounts of C, O, N, and B required to improve the two-particle grain boundary, making it possible to realize an excellent RTB based sintered magnet. [Means for solving the problem]
[0009] In a non-limiting exemplary embodiment, the RTB based sintered magnet of the present disclosure is R2T 14 An RTB sintered magnet comprising a main phase of a B compound and a grain boundary phase located at grain boundaries of the main phase (R is a rare earth element, which necessarily contains at least one of Nd and Pr, and T is a group of elements consisting of Fe, Co, Ni, Al, Mn, Cr and V, which necessarily contains Fe), The content (mol%) of element or element group X is represented by [X], [R eff ]=[R]-0.789[N]-1.58[O], [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb], [C eff ]=[C]+0.123[N]-0.754[O], The element contents of the RTB based sintered magnet are as follows: [C]≧0.754[O]-0.123[N], 14.13≦[T] / ([B eff ]+[C eff ])≦15.50, 5.1≦[T] / [R eff ]≦6.7, 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0 ≦ [Nb] ≦ 0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7, Satisfy.
[0010] In a non-limiting exemplary embodiment, the method for producing an RTB based sintered magnet according to the present disclosure includes the following steps: A step of preparing a sintered body material; Providing a diffusion source; diffusing the elements contained in the diffusion source from the surface of the sintered body to the inside; Including, The content (mol%) of element or element group X is represented by [X], [R eff ]=[R]-0.789[N]-1.58[O], [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb], [C eff ]=[C]+0.123[N]-0.754[O], The element content of the sintered body material is: [C]≧0.754[O]-0.123[N], 14.13≦[T] / ([B eff ]+[C eff ])≦15.50, 5.1≦[T] / [R eff ]≦6.7, 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0 ≦ [Nb] ≦ 0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7, Satisfy.
[0011] In a non-limiting exemplary embodiment, the composition design method for an RTB based sintered magnet according to the present disclosure includes the following steps: A composition design method for an RTB sintered magnet having a C+N+O content of 40 to 60 atomic % and including a rare earth oxide phase containing all of C, N, and O at grain boundaries, comprising: The amount of effective C that is not distributed in the rare earth oxide phase is calculated from the contents of C, N and O, and the composition is designed assuming that the amount of effective C is equivalent to B. Effect of the Invention
[0012] According to the embodiments of the present disclosure, the ranges of the C, O, N and B amounts required for improving the two-particle grain boundary are specified, making it possible to realize an excellent RTB based sintered magnet. [Brief description of the drawings]
[0013] [Figure 1A] FIG. 2 is a schematic diagram showing the main phase and grain boundary phase of an RTB based sintered magnet. [Figure 1B] FIG. 1B is a further enlarged schematic diagram of the dashed rectangular area in FIG. 1A. [Diagram 2] 1 is an example of a micrograph showing a cross section of the microstructural structure of an RTB based sintered magnet. [Diagram 3] 1 is a graph showing the atomic ratios (at. %) of nitrogen (N), oxygen (O), carbon (C), rare earth elements (R), etc. in the R oxide phase obtained for samples S1 to S6. [Figure 4] 1 is a graph showing [O]-[N] with white circles and [O]-[C] with black circles for samples S1 to S6. [Diagram 5] 1 is a graph showing the relationship between the coercive force after diffusion and [T] / [Beff] for several samples of RTB based sintered magnets. [Figure 6] 1 is a graph showing the relationship between coercivity after diffusion and [T] / ([Beff]+[Ceff]) for the same sample described above. [Figure 7] Photographs showing BSE (backscattered electron) images of the cross sections of samples No. 2, No. 7, and No. 12 in Table 3. [Figure 8] Photographs showing BSE (backscattered electron) images of the cross sections of samples No. 17 and No. 28 in Table 3. [Figure 9] 1 is a graph showing the distribution of Pr concentration from the surface of the cross section of sample No. 28. [Figure 10] 1 is a graph showing the distribution of Tb concentration from the surface of the cross section of sample No. 28. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present inventors have constructed a physical model in which the amount of C (carbon concentration), the amount of O (oxygen concentration), and the amount of N (nitrogen concentration) affect the range of the amount of B required to improve the two-particle grain boundary, and have found guidelines for composition design to achieve excellent RTB-based sintered magnets. Before describing embodiments and examples of the manufacturing method and composition design method for an RTB-based sintered magnet of the present disclosure, the findings of the present inventors will be described.
[0015] Conventionally, in RTB sintered magnets, for example, when (1) the content of R (at least one of rare earth elements, which necessarily contains at least one of Nd and Pr) is 27 mass% or more and 35 mass% or less of the entire RTB sintered body, (2) T is at least one selected from the group consisting of Fe, Co, Al, Mn, and Si, T necessarily contains Fe, and the content of Fe in the entire T is 80 mass% or more, and (3) the molar ratio of T to B ([T] / [B]) is more than 14.0 and 15.0 or less, an element such as Ga is added to thicken the two-particle grain boundary and increase the H cJ It is known that it is possible to improve
[0016] The molar ratio of T to B ([T] / [B]) is the ratio (a / b) of the number of moles (a) obtained by dividing the analytical value (mass%) of the concentration of each element (Fe and at least one of Co, Al, Mn, and Si) constituting T by the atomic weight of each element, to the number of moles (b) obtained by dividing the analytical value (mass%) of the concentration of B by the atomic weight of B.
[0017] When the molar ratio of T to B ([T] / [B]) exceeds 14.0, the B content is R2T 14 This means that the ratio of the main phase (R2T 14The amount of B is reduced relative to the amount of T used to form the compound (B).
[0018] Next, the basic structure of an RTB based sintered magnet will be described.
[0019] RTB sintered magnets have a structure in which powder particles of raw alloys are bonded together by sintering, and are mainly 14 It is composed of a main phase made of B compounds and a grain boundary phase located at the grain boundaries of this main phase.
[0020] FIG. 1A is a schematic diagram showing the main phase and grain boundary phase of an RTB based sintered magnet, and FIG. 1B is a schematic diagram further enlarging the dashed rectangular area in FIG. 1A. In FIG. 1A, an arrow of 5 μm in length is shown as an example for reference, showing the reference length of the size. As shown in FIG. 1A and FIG. 1B, an RTB based sintered magnet is mainly composed of R2T 14 The grain boundary phase 14 is composed of a main phase 12 made of a B compound and a grain boundary phase 14 located at the grain boundary portion of the main phase 12. As shown in FIG. 1B, the grain boundary phase 14 is composed of two R2T 14 B compound grains are adjacent to each other in the two-particle grain boundary phase 14a, and there are three or more R2T 14 The B compound grains include adjacent grain boundary triple junctions 14b.
[0021] R2T, which is main phase 12 14 The B compound is a ferromagnetic phase with high saturation magnetization and anisotropic magnetic field. Therefore, in RTB sintered magnets, the R2T 14 By increasing the proportion of B compounds, r It can improve R2T 14 In order to increase the ratio of B compounds, the amounts of R, T, and B in the raw alloy should be adjusted to R2T 14 The best way is to get the stoichiometric ratio of B compound (R amount:T amount:B amount = 2:14:1). 14 When the amount of B or R for forming the B compound is less than the stoichiometric ratio, the grain boundary phase 14 generally contains an Fe phase or an R2T phase. 17 Soft magnetic phases such as H cJ However, the amount of B is reduced by R2T14 When the amount of B compound is less than the stoichiometric ratio and one or more metal elements M selected from Al, Ga, and Cu are contained, R2T 17 The grain boundaries become thicker due to the formation of transition metal-rich phases (e.g., RT-Ga phases) at the grain boundaries from the phase, resulting in high H cJ can be obtained.
[0022] According to the study by the present inventors, in order to thicken the two-particle grain boundary in RTB sintered magnets, it was found that not only the amount of B but also the amount of carbon (C), which acts similarly to boron (B), is important. However, it was found that not only the simple sum of the amounts of B and C, but also the amounts of oxygen (O) and nitrogen (N) are important conditions for thickening the two-particle grain boundary. This is thought to be because a part of the total carbon (C) contained in the RTB sintered magnet is contained in the rare earth oxide phase of the grain boundary together with oxygen (O) and nitrogen (N), and the remaining carbon (C) acts as surplus carbon and, together with boron (B), affects the conditions for thickening the two-particle grain boundary. Here, carbon (C) that is not distributed in a stable phase such as the rare earth oxide phase is called "effective carbon" or "effective C," and its amount is called the "effective C amount."
[0023] As described above, if the mechanism by which the total amount of carbon (C) contained in an RTB sintered magnet is distributed between the effective amount of C and the remaining amount of C is understood better, it will be possible to calculate the effective amount of C from the total amount of carbon (C).
[0024] The present inventors have come up with the idea of using the molar ratio of T to (B+effective C) ([T] / [B+effective C]), which is a corrected molar ratio of T to B, as an index, rather than the molar ratio of T to B ([T] / [B]), and have found a method for appropriately calculating the amount of effective C. The method for appropriately calculating the amount of effective C will be described below.
[0025] First, Figure 2 is a photomicrograph showing a cross section of the microstructure of an RTB sintered magnet. The photo in Figure 2 shows relatively large particulate rare earth oxide phases located at the grain boundaries between particulate main phases. Analysis has revealed that this rare earth oxide (R oxide) phase contains carbon (C), oxygen (O), and nitrogen (N). The main phase is R2T 14 It is composed of B compounds, but R2T 14 Some of the boron (B) in B compounds is replaced by carbon (C).
[0026] The present inventors conducted concentration analysis of the R oxide phase, as exemplified in FIG. 2, on many samples of RTB sintered magnets having various compositions, and obtained many findings, which are described below.
[0027] First, refer to FIG. 3. FIG. 3 is a graph showing the atomic ratios (at.%) of nitrogen (N), oxygen (O), carbon (C), and rare earth elements (R) in the R oxide phase obtained for six representative samples S1 to S6. The "rare earth elements (R), etc." are mainly composed of rare earth elements, but may contain trace amounts of elements such as iron (Fe). Here, the atomic ratios of nitrogen (N), oxygen (O), and carbon (C) are [N], [O], and [C], respectively. Samples S1 to S6 are examples of RTB-based sintered magnets with relatively little [O]. In such samples, the R oxide phase is composed of a NaCl-type R oxide phase. However, when the oxygen (O) in the RTB-based sintered magnet increases, the R2O3 phase may also be generated as the R oxide phase.
[0028] As can be seen from FIG. 3, the total atomic ratio of nitrogen (N), oxygen (O), and carbon (C) contained in the R-oxide phase, i.e., [N]+[O]+[C], is about 50 at.% in all samples. FIG. 4 is a graph showing [O]-[N] with white circles and [O]-[C] with black circles for each of the above samples. As can be seen from FIG. 4, [O]-[C] is about 7 at.% in all samples. The reason why a 1:1 balance is established between [N]+[O]+[C] and [R, etc.], and also between [O] and [C], is presumably due to the fact that in the R-oxide phase, the valence of the R ion is about +3, the valence of the O ion is -2, the valence of the N ion is -3, and the valence of the C ion is -4. To maintain electrical neutrality, the atomic ratio [R] of the rare earth element R in the R oxide phase, which has a charge of +3, must be balanced with the total atomic ratio of oxygen (O), nitrogen (N), and carbon (C), which have an average charge of -3. In addition, the atomic ratio of O ions with a charge of -2 and C ions with a charge of -4 is approximately equal, which means that the average charge of the O ions, N ions, and C ions is close to -3, and charge compensation is achieved with the charge of the R ions, which is +3.
[0029] Based on the above experimental facts and theoretical considerations, and also on measurement data obtained from a large number of samples, the inventors have constructed the following physical model. Hereinafter, the atomic ratio (mol%) of element X in a magnet is represented as [X]. (1) [R]: The sum of the atomic ratio (mol%) of rare earth elements (excluding Sc) (2) [T]=[Fe]+[Co]+[Al]+[Mn]+[Ni]+[Cr]+[V] (3) All N is distributed in the NaCl-type R-oxide phase. (4) O is distributed to the NaCl-type R-oxide phase as much as possible, and the excess is distributed to the R2O3 phase. (5) C is distributed as much as possible to the NaCl-type R-oxide phase, and the excess is replaced by C eff (Valid C). (6) The composition (atomic ratio) of the NaCl-type R oxide phase is [R]:[T]:([C]+[N]+[O])=45:5:50 (7) In the composition (atomic ratio) of the NaCl-type R oxide phase, [O]-[C]=7at.%
[0030] Based on this physical model, we calculate the distribution of elements. First, the atomic ratio (mol%) of element X distributed in the NaCl-type R oxide phase and the R2O3 phase is defined as [X NaCl ], [X R2O3 ], the following equation can be established from the physical models (3) and (4). [N NaCl ]=[N] (8) [O NaCl ]+[O R2O3 ]=[O] (9)
[0031] Next, the amount of C distributed in the NaCl-type R-oxide phase ([C NaCl From the physical models (6) and (7), the following equation can be established: ([C NaCl ]+[N NaCl ]+[O NaCl ]):([O NaCl ]-[C NaCl ])=50:7 (10)
[0032] Equation (10) is expressed as [C NaCl ], we obtain the following equation:
number
[0033] Here, we distinguish between cases where the R2O3 phase is generated and cases where it is not. In cases where the R2O3 phase is not generated, such as when the [O] is sufficiently low in low-acid materials, the formula (9) becomes [O NaCl ]=[O] (12) Therefore, [C NaCl ] can be written as the following formula: [C NaCl ]=0.754[O]-0.123[N] (13)
[0034] Conversely, when the oxygen-introducing material has a large amount of [O], and the R2O3 phase is formed, it can be considered that the entire amount of C is distributed to the NaCl-type R oxide phase. In this case, [C NaCl ] can be written as the following formula: [C NaCl ]=[C] (14)
[0035] Therefore, the case where the R2O3 phase is generated can be determined by the magnitude relationship between formula (13) and formula (14). When [C] ≧ 0.754[O]-0.123[N], the R2O3 phase is not generated and [C NaCl ] can be written as (13). Conversely, when [C]<0.754[O]-0.123[N], the R2O3 phase is formed and [C NaCl ] can be written as Equation (14). In the composition region where the R2O3 phase is formed, in addition to the R distributed to the NaCl-type R oxide phase, R distributed to the R2O3 phase is also required. Therefore, in the composition region where the R2O3 phase is formed, the R required for the formation of the two-particle grain boundary is insufficient, and H cJ In this embodiment, the composition of the RTB sintered magnet is designed in a composition range in which the R2O3 phase does not form. Hereinafter, it is assumed that the relationship [C] ≥ 0.754[O]-0.123[N] holds. From equation (13) and model (5), the effective C amount ([C eff ]) can be expressed by the following formula: [C eff ]=[C]-[C NaCl ]=[C]-0.754[O]+0.123[N] (15)
[0036] Next, calculate the distribution for other elements. First, [O NaCl Regarding [, we are considering the case where the R2O3 phase does not form, so it can be written as the following equation. [O NaCl ]=[O] (16)
[0037] [R NaCl] can be expressed by the following equation using the physical model (6), equations (8), (13), and (16).
number
[0038] The amount of effective R that is not distributed in the oxide phase ([R eff ]) can be calculated from equation (17) as follows: [R eff ]=[R]-[R NaCl ]=[R]-0.789[N]-1.58[O] (18)
[0039] As described above, by considering the physical models (1) to (7), we were able to derive an equation that allows the distribution of each element to be calculated from the overall composition alone.
[0040] In addition, [B eff ] is expressed by the following formula, taking into account the formation of borides: [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb] (19)
[0041] Figure 5 shows the relationship between the coercivity after diffusion and [T] / [B eff ]. FIG. 5 shows the relationship between [T] / [B eff A dashed line is shown indicating the position where [T] / ([B eff ]+[C eff 6 is a graph showing the relationship between [T] / ([B eff ]+[C eff ])=14.0. As is clear from FIG. 6, the dashed line indicates the position where [T] / ([B eff ]+[C eff ]) is used as an index, and whether or not this index exceeds the value of "14.0" is effective as a condition for determining whether the coercivity is high or low, in other words, whether or not a "thick two-grain grain boundary" is realized.
[0042] From the above, the available C amount [C eff ], the range of so-called low B required to thicken the two-grain boundary is 14.0≦[T] / ([B eff ]+[C eff ]) can be corrected as follows.
[0043] The present disclosure provides a composition design method for an RTB sintered magnet in which the C+N+O content is 40-60 atomic % and the grain boundaries contain a rare earth oxide phase that contains all of C, N and O, and the composition is designed by calculating the amount of effective C that is not distributed to the rare earth oxide phase from the C, N and O contents, and assuming that C in the effective C amount is equivalent to B. In this composition design method, 14.13≦[T] / ([B eff ]+[C eff ])≦15.50 (20) The composition can be determined so that R6T is satisfied at the grain boundary. 13 Ga is formed, making it possible to control the thickness of the two-particle grain boundary. The above calculations were performed based on models (1) to (7), but in some cases the coefficients in the formulas may deviate from these models and change slightly. For example, in model (7), the composition (atomic ratio) of the NaCl-type R oxide phase was set to [O]-[C]=7 at.%, but the value of [O]-[C] may change because the valence of stable ions differs depending on the rare earth species. In that case, the distribution of each element can be calculated in the same manner as above by resetting the value of [O]-[C] to match the valence of the rare earth species ions.
[0044] <Embodiment> Hereinafter, embodiments of the RTB based sintered magnet and the manufacturing method thereof according to the present disclosure will be described.
[0045] The RTB based sintered magnet in this embodiment is 14The magnet is an RTB sintered magnet including a main phase of a B compound and a grain boundary phase located at the grain boundaries of the main phase (R is a rare earth element and always includes at least one of Nd and Pr, and T is a group of elements consisting of Fe, Co, Ni, Al, Mn, Cr and V and always includes Fe).
[0046] As described above, the content (mol %) of an element or group of elements X is represented by [X]. In this embodiment, the amount defined by the right side of each of the following equations is equal to the symbol on the left side. [R eff ]=[R]-0.789[N]-1.58[O], [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb], [C eff ]=[C]+0.123[N]-0.754[O]
[0047] The element contents of the RTB sintered magnet in this embodiment satisfy the following relationships. [C]≧0.754[O]-0.123[N], 14.13≦[T] / ([B eff ]+[C eff ])≦15.50, 5.1≦[T] / [R eff ]≦6.7, 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0 ≦ [Nb] ≦ 0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7.
[0048] In one embodiment, the rare earth oxide phase contained in the grain boundary phase has a C+N+O content of 40 to 60 atomic %, and contains all of O, C and N. In a cross section of the RTB sintered magnet, the ratio of the cross-sectional area of the rare earth oxide phase to the cross-sectional area of the grain boundary phase is, for example, 20% or more and 80% or less.
[0049] In this embodiment, it is preferable to diffuse at least one of Nd and Pr from the magnet surface toward the magnet interior. As a result of such diffusion, the RTB based sintered magnet includes a portion where at least one of the Nd concentration and the Pr concentration gradually decreases from the magnet surface toward the magnet interior. Similarly, it is preferable to diffuse at least one of the Tb concentration and the Dy concentration from the magnet surface toward the magnet interior. As a result of such diffusion, the RTB based sintered magnet includes a portion where at least one of the Tb concentration and the Dy concentration gradually decreases from the magnet surface toward the magnet interior.
[0050] In the RTB sintered magnet of this embodiment, the grain boundaries are 13 Ga is formed and the grain boundary becomes thicker, resulting in a high H exceeding 1950kA / m cJ will be realized.
[0051] Next, an embodiment of a method for producing an RTB based sintered magnet according to the present disclosure will be described.
[0052] The method for producing an RTB based sintered magnet of this embodiment includes the steps of preparing a sintered body material, preparing a diffusion source, and diffusing elements contained in the diffusion source from the surface of the sintered body to the inside.
[0053] And the element content of the sintered body material is: [C]≧0.754[O]-0.123[N], 14.13≦[T] / ([B eff ]+[C eff ])≦15.50, 5.1≦[T] / [R eff ]≦6.7, 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0 ≦ [Nb] ≦ 0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7, Satisfy.
[0054] In addition to the above elements, the sintered body material may contain unavoidable impurity elements such as Cu, Ag, Zn, In, Sn, Ni, Hf, Ta, W, Ge, Mo, V, Y, La, Ce, Sm, Ca, Mg, Cr, H, F, P, S, and Cl.
[0055] [T] and [R eff ] ratio [T] / [R eff ] is between 5.1 and 6.7. eff If the value is less than 5.1, sintering may be difficult. cJ The decrease in [T] / [R eff If the ratio exceeds 6.7, the main phase ratio decreases and B r is significantly reduced.
[0056] The range of [B] is 5.0≦[B]≦6.5. If [B] is less than 5.0, the amount of C, etc. can be adjusted to 14.13≦[T] / ([B eff ]+[C eff It is possible to keep the value within the range of 14.13 ≦ [T] / ([B]) ≦ 15.50, but the magnetic properties of the main phase decrease as the amount of C substituted in the main phase increases. Also, if [B] exceeds 6.5, the addition of Zr, Ti, Nb, etc., which contribute to the formation of borides, will result in a decrease in the value of 14.13 ≦ [T] / ([B eff ]+[C eff ])≦15.50, but since these elements are also present in the main phase, the magnetic properties of the main phase decrease.
[0057] The range of [Ga] is 0.1≦[Ga]≦1.5. If [Ga] is less than 0.1, sufficient R6T 13 Ga phase is not formed and H cJ In addition, when [Ga] exceeds 1.5, the ratio of the main phase decreases and B r is significantly reduced.
[0058] Co is a rare metal, and since it is only produced in a limited number of countries, it is preferable to avoid using it whenever possible. In this embodiment, the range of [Co] is 0≦[Co]≦2. In this embodiment, sufficient magnetic properties can be obtained even when [Co]=0.
[0059] The range of [Nb] is 0≦[Nb]≦0.35. Nb has the role of reducing the effective amount of B by forming a compound with Fe and B, but it is also important for the main phase and R6T 13 Since even Fe necessary for forming the Ga phase is consumed, if [Nb] exceeds 0.35, the magnetic properties are degraded.
[0060] The range of [Zr], [Ti], and [Nb] that contribute to boride formation is 0≦[Zr]+[Ti]+[Nb]≦0.7. If the sum of the contents of these elements exceeds 0.7, the magnetic properties decrease significantly due to main phase substitution.
[0061] Hereinafter, examples of the above-mentioned "step of preparing a sintered body material", "step of preparing a diffusion source", and "step of diffusing elements contained in the diffusion source from the surface of the sintered body to the inside" will be described.
[0062] -Preparing the sintered material The sintered body material can be prepared by a general manufacturing method such as that for RTB sintered magnets. 50 (Volume center value obtained by measurement using airflow dispersion laser diffraction method = D 50 It is preferable to crush the raw alloy into particles having a particle size D of 2.5 μm to 10 μm, and then orient the particles in a magnetic field and sinter them. For example, a raw alloy produced by a strip casting method or the like is crushed into particles having a particle size D of 2.5 μm to 10 μm, and then sintered. 50 The raw alloy can be prepared by crushing the raw alloy into a powder having a particle size of 2.5 μm to 10 μm, molding the powder in a magnetic field, and sintering the powder at a temperature of 900°C to 1100°C. 50 If the particle size is less than 2.5 μm, it is very difficult to prepare the pulverized powder, and the production efficiency is significantly reduced, which is not preferable. 50 If the grain size exceeds 10 μm, the final sintered material will have too large a grain size, resulting in a high H cJ It is not preferable because it becomes difficult to obtain the particle size D. 50 is preferably 2.5 μm or more and 5 μm or less.
[0063] As long as the above-mentioned conditions are satisfied, the sintered body material may be produced from one type of raw material alloy (single raw material alloy) or may be produced by using two or more types of raw material alloys and mixing them (blending method). Furthermore, the obtained sintered body material may be subjected to a known mechanical processing such as cutting or machining as necessary, and then to the first heat treatment and the second heat treatment described below.
[0064] -Preparing the diffusion source First, the composition of the diffusion source in the step of preparing the diffusion source will be described.
[0065] The diffusion source may be composed of heavy rare earth elements such as Dy, Tb, Gd, and Ho. Preferably, the rare earth elements include at least one of Nd and Pr. It is preferable that 50 mass% or more of the rare earth elements is Pr. It is possible to obtain a higher H while suppressing the content of valuable heavy rare earth elements. cJ According to the present disclosure, it is possible to obtain a sufficiently high H cJ Therefore, the content of the heavy rare earth element is preferably 10 mass% or less of the entire diffusion source, more preferably 5 mass% or less, and further preferably none (substantially 0 mass%). Even when the diffusion source contains a heavy rare earth element, it is preferable that 50% or more of the rare earth element is Pr, and it is more preferable that the rare earth element excluding the heavy rare earth element is only Pr (including unavoidable impurities).
[0066] When at least one of Nd and Pr is necessarily contained as a rare earth element, the content is preferably, for example, 35 mass% or more and less than 85 mass% of the entire diffusion source. If the content of the rare earth element is less than 35 mass%, the diffusion may not proceed sufficiently in the first heat treatment described later. On the other hand, if the content of the rare earth element is 85 mass% or more, the alloy powder becomes very active during the manufacturing process of the diffusion source. As a result, the alloy powder may be significantly oxidized or ignited.
[0067] The content of Ga in the diffusion source is preferably 2.5 mass% or more and 30 mass% or less. If the content of Ga is less than 2.5 mass%, it is difficult to introduce Ga into the sintered body material. On the other hand, if the content of Ga exceeds 30 mass%, B r The Ga content in the diffusion source is more preferably 4 mass% or more and 20 mass% or less, and even more preferably 4 mass% or more and 10 mass% or less. r and high H cJ Because you can get it.
[0068] In addition to the above elements, the diffusion source may contain Fe, Cu, Co, Al, Ag, Zn, Si, In, Sn, Zr, Nb, Ti, Ni, Hf, Ta, W, Ge, Mo, V, Y, La, Ce, Sm, Ca, Mg, Mn, Cr, H, F, P, S, Cl, O, N, C, etc.
[0069] The contents of Al are preferably 1.0 mass% or less, Ag, Zn, Si, In, Sn, Zr, Nb, and Ti are each 0.5 mass% or less, Ni, Hf, Ta, W, Ge, Mo, V, Y, La, Ce, Sm, Ca, Mg, Mn, Si, and Cr are each 0.2 mass% or less, H, F, P, S, and Cl are each 500 ppm or less, O is 6000 ppm or less, N is 1000 ppm or less, and C is 1500 ppm or less.
[0070] The diffusion source can be prepared by a method for producing a raw material alloy that is employed in a general manufacturing method typified by Nd-Fe-B sintered magnets, such as a die casting method, a strip casting method, a single roll super-quenching method (melt spinning method), or an atomizing method. The diffusion source may also be an alloy obtained by the above method, which has been pulverized by a known pulverizing means such as a pin mill. In order to improve the pulverizability of the alloy obtained by the above method, the alloy may be subjected to a heat treatment at 700°C or less in a hydrogen atmosphere to incorporate hydrogen, and then pulverized.
[0071] A process in which elements contained in the diffusion source are diffused from the surface of the sintered body to the inside. By performing heat treatment at a temperature of 700°C or higher and 1100°C or lower in a vacuum or inert gas atmosphere, the elements contained in the diffusion source are diffused from the surface of the sintered body to the inside. In the present disclosure, this heat treatment is referred to as the first heat treatment. If the heat treatment temperature for diffusion is less than 700°C, the diffusion is insufficient and a high H cJ On the other hand, if the temperature exceeds 1100℃, abnormal grain growth of the main phase occurs and H cJ The heat treatment temperature for diffusion is preferably 800°C or higher and 1000°C or lower. cJ This is because it is possible to obtain the above. The heat treatment time is set to an appropriate value depending on the composition and dimensions of the sintered body material and the diffusion source, the heat treatment temperature, etc., but is preferably 5 minutes to 30 hours, more preferably 10 minutes to 25 hours, and even more preferably 30 minutes to 20 hours. It is also preferable to prepare the diffusion source in an amount of 1 mass% to 30 mass% of the weight of the sintered body material. If the diffusion source is less than 1 mass% of the weight of the sintered body material, H cJ On the other hand, if it exceeds 30 mass%, B r may decrease.
[0072] The heat treatment for diffusion can be performed using a known heat treatment method. For example, the surface of the sintered body material can be covered with a powder layer of the diffusion source, and the first heat treatment can be performed. For example, the diffusion source can be coated on the surface of the sintered body material by a sputtering method, and then the first heat treatment can be performed. For example, a slurry in which the diffusion source is dispersed in a dispersion medium can be applied to the surface of the sintered body material, and the dispersion medium can be evaporated to bring the diffusion source into contact with the sintered body material. Examples of the dispersion medium include alcohol (ethanol, etc.), NMP (N-methylpyrrolidone), aldehydes, and ketones. In addition, the sintered body material that has been subjected to the first heat treatment can be subjected to known mechanical processing such as cutting or machining.
[0073] The sintered body material that has been subjected to the heat treatment for diffusion may be subjected to a heat treatment at a temperature of 450° C. or more and 600° C. or less in a vacuum or in an inert gas atmosphere. In the present disclosure, this heat treatment is referred to as a second heat treatment. By performing the second heat treatment, a high Br and high H cJ By setting the temperature of the second heat treatment to 450°C or higher and 600°C or lower, R6T 13 The formation of the Ga phase progresses. The second heat treatment temperature is preferably 480°C or higher and 560°C or lower. cJ The heat treatment time is set to an appropriate value depending on the composition and dimensions of the sintered body material, the heat treatment temperature, etc., and is preferably from 5 minutes to 20 hours, more preferably from 10 minutes to 15 hours, and even more preferably from 30 minutes to 10 hours.
[0074] The above-mentioned considerations and physical model of the present invention provide a composition design method for an RTB sintered magnet that contains a rare earth oxide phase containing O, C, and N at the grain boundaries. Here, the C+N+O content is 40-60 atomic %. According to the composition design method for an RTB sintered magnet, the amount of effective C that is not distributed to the rare earth oxide phase is calculated from the C, O, and N contents, and the composition is designed assuming that C in the effective amount of C is equivalent to B. Specifically, the composition can be designed as follows.
[0075] The content of available C that is not distributed in the rare earth oxide phase is [C eff ]=[C]-0.754[O]+0.123[N], The content of available R that is not distributed in the rare earth oxide phase is [R eff ]=[R]-0.789[N]-1.58[O], The content of available B that is not distributed in the boride phase is [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb], Let us assume that.
[0076] And the overall composition is: [C] ≥ 0.754[O]-0.123[N], and 14.13≦[T] / ([B eff ]+[C eff ])≦15.50 In a preferred embodiment, the ratio is determined so as to satisfy 5.1≦[T] / [R eff The composition is determined so as to satisfy the condition: ]≦6.7.
[0077] In a preferred embodiment, the composition is determined so as to satisfy the following formula: 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0 ≦ [Nb] ≦ 0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7.
[0078] It is preferable that [R]≦14.0 is satisfied, and it is more preferable that 5.1≦[B]≦5.6 is satisfied.
[0079] It is preferable that the oxygen concentration is less than 3000 ppm, the nitrogen concentration is less than 1000 ppm, and the carbon concentration is less than 2000 ppm. Therefore, it is preferable to satisfy at least one of 0≦[O]≦1.2, 0≦[N]≦0.4, and 0≦[C]≦1.0.
[0080] The Ga concentration is preferably 0.1 to 0.7 mass %. EXAMPLES
[0081] The present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited thereto.
[0082] A flake-shaped alloy for RTB sintered magnet was produced by strip casting so as to have the composition of the RTB sintered magnet shown in Samples No. 1 to 29 in Table 1 (excluding O, C, and N). The obtained flake-shaped alloy was hydrogen embrittled in a pressurized hydrogen atmosphere, and then heated to 550°C in a vacuum and cooled for dehydrogenation to obtain a coarsely pulverized powder. The coarsely pulverized powder was heated to 450°C in Ar and then cooled. By changing the cooling gas at this time to N2, a coarsely pulverized powder with a large amount of N was produced, and by changing the cooling gas to Ar, a coarsely pulverized powder with a small amount of N was produced. The heat-treated coarsely pulverized powder was mixed with an organic grinding aid and put into an airflow pulverizer (jet mill device) to obtain a finely pulverized powder. In this example, Ar gas was used as the inert gas, and the O amount of the finely pulverized powder was adjusted by adjusting the dew point.
[0083] A lubricant was added to the finely pulverized powder, and the powder was immersed in mineral oil to prepare a slurry. The obtained slurry was molded in a magnetic field (wet molding) to obtain a green body. The molding device used was a so-called perpendicular magnetic field molding device (horizontal magnetic field molding device), in which the magnetic field application direction and the pressure direction are perpendicular to each other.
[0084] The obtained green bodies were sintered in a vacuum at 1020 to 1050°C (a temperature at which densification by sintering is sufficient) for about 5 hours to obtain sintered bodies. The density of each sintered body was 7.5 g / cm. 3 The sintered body was heat-treated in a vacuum at 800°C for 2 hours, and then processed into a cube with a side length of 7.2 mm. The processed cube sample was then heat-treated at 500°C for 2 hours, after which the six faces of the cube sample were ground to be processed into a cube with a side length of 7 mm. r and H cJ The amounts of iron, arsenic, and manganese were measured. In addition, a portion of the sintered body that was not used in the magnetic force measurement was pulverized in a mortar and the content of each element was analyzed. The contents of Fe, Nd, Pr, B, Co, Al, Cu, Ga, Zr, Ce, Mg, Mn, Si, and Ni were analyzed by ICP (inductively coupled plasma) optical emission spectroscopy, the amount of oxygen was analyzed by gas fusion-infrared absorption method, the amount of nitrogen was analyzed by gas fusion-thermal conduction method, and the amount of carbon was analyzed by combustion-infrared absorption method. The results of the component analysis (mass%) are shown in Table 1.
[0085] [Table 1]
[0086] The atomic percentage of each element was calculated from the analysis results in Table 1. r and H cJ is shown in Table 2.
[0087] [T] / ([B eff ]+[C eff ]) is 14.13 or more and 15.50 or less, H cJ In addition, [T] / ([B eff ]+[C eff ]) is 14.35 or more and 15.00 or less, H cJ reached a higher level of over 1500kA / m.
[0088] [Table 2]
[0089] (Diffusion and structure observation of some samples) For some samples, the samples after sintering were used as sintered bodies, and diffusion sources were attached to the surfaces of the samples and subjected to diffusion heat treatment to produce diffusion magnets. First, the samples after sintering were processed into cubes with sides of 7.2 mm to produce sintered bodies. On the other hand, diffusion source powder was produced by disk atomization to have a composition of 10Pr-80Tb-7.4Ga-2.6Cu (mass%).
[0090] Next, an adhesive was applied to the entire surface of the cube of the sintered body material, and the diffusion source powder was attached on top of the adhesive. The weight of the diffusion source powder attached was about 2.7% of the weight of the sintered body material.
[0091] Next, the diffusion source-attached sample was subjected to diffusion heat treatment by holding it in a vacuum at 900°C for 10 hours, then cooling it to room temperature, and then holding it in a vacuum at 500°C for 1 hour, then cooling it to room temperature. After the diffusion heat treatment, the six faces of the sample were ground to make it into a cube with a side length of 6.9 mm, and the BH tracer was used to measure the B r and H cJ Table 3 shows the B r and H cJ [T] / ([B eff ]+[C eff In sample No. 28, where the value of H is 14.13 or more, cJ was at a high level exceeding 1950kA / m.
[0092] [Table 3]
[0093] The samples in Table 3 after the diffusion heat treatment were cut and processed, and as a pretreatment for SEM (scanning electron microscope) observation, they were embedded in resin, the cross section of the sample was polished, and further finishing treatment was performed by ion milling. The samples were then observed with FE-SEM (field emission scanning electron microscope) and local composition analysis was performed with EDX / WDX (energy dispersive X-ray analysis / wavelength dispersive X-ray analysis) (Fe and Nd were EDX, Pr, Zr, C, N, and O were WDX). The observation and analysis area was a region 500 μm deep from the interface between the diffusion source and the sintered body material. BSE (backscattered electron) images of the cross section are shown in Figures 11 and 12.
[0094] [T] / ([B eff ]+[C eff In specimens No. 2, 7, 12, and 17, where the value of β is less than 14.13, the width of the two-grain grain boundary phase is thin, and R6Fe 13 The Ga phase was hardly observed. In contrast, [T] / ([B eff ]+[C eff In the sample No. 28, where the value of R6T is 14.13 or more, a thick two-grain grain boundary phase is formed, and the R6T 13 The Ga phase was observed.
[0095] In addition, rare earth oxide phases containing O, N, and C were observed in all samples. The content of O+N+C was 40-60 atomic % of the rare earth oxide phase. Hereinafter, such rare earth oxide phases are referred to as "R-(O,N,C) phases". Table 4 shows the point analysis results of the R-(O,N,C) phase and the cross-sectional area ratio of the R-(O,N,C) phase to the cross-sectional area of the grain boundary phase. The point analysis results are the average of the results of three analysis points. The cross-sectional area ratio of the R-(O,N,C) phase and the grain boundary phase was calculated by assigning phases to each brightness range of the BSE image using image analysis software and counting the number of pixels. The BSE image of an area of 180 μm in length and 240 μm in width was analyzed, and the average value of two fields of view was recorded. The composition of O, N, and C in the R-(O,N,C) phase differs greatly depending on the O and N amounts of the material, but in common, O+N+C was about 50 atomic %. In addition, while ON differed greatly depending on the sample, OC was commonly about 7 atomic percent. The cross-sectional area ratio of the R-(O,N,C) phase to the grain boundary phase increased or decreased depending on the O and N contents of the material, but was between 10% and 70% in all cases.
[0096] [Table 4]
[0097] A line analysis of Pr and Tb by WDX was performed on the cross section of sample No. 28 to investigate the concentration gradient from the sample surface. Figure 13 shows the WDX intensity at the depth of each sample surface for Pr, and Figure 14 shows that for Tb. The beam diameter was set to φ10μm×100μm, and data was acquired at 5μm intervals, after which a moving average process was performed at 5 points for smoothing. A negative concentration gradient was observed for both Pr and Tb, particularly at the sample surface (near a depth of 0mm), a characteristic unique to diffusing materials.
[0098] As described above, the present disclosure includes the RTB based sintered magnets and their manufacturing methods and composition design methods described in the following items.
[0099] [Item 1] R2T 14An RTB sintered magnet comprising a main phase of a B compound and a grain boundary phase located at grain boundaries of the main phase (R is a rare earth element, which necessarily contains at least one of Nd and Pr, and T is a group of elements consisting of Fe, Co, Ni, Al, Mn, Cr and V, which necessarily contains Fe), The content (mol%) of element or element group X is represented by [X], [R eff ]=[R]-0.789[N]-1.58[O], [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb], [C eff ]=+0.123[N]-0.754[O] When The element contents of the RTB based sintered magnet are as follows: [C]≧0.754[O]-0.123[N], 14.13≦[T] / ([B eff ]+[C eff ])≦15.50, 5.1≦[T] / [R eff ]≦6.7, 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0 ≦ [Nb] ≦ 0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7, RTB sintered magnets that satisfy the above requirements. [Item 2] 2. The RTB sintered magnet according to item 1, wherein the grain boundary phase contains a rare earth oxide phase, the rare earth oxide phase has a C+N+O content of 40 to 60 atomic %, and contains all of O, C and N. [Item 3] 2. The RTB based sintered magnet according to item 1, wherein in a cross section of the RTB based sintered magnet, the ratio of a cross-sectional area of the rare earth oxide phase to a cross-sectional area of the grain boundary phase is 20% or more and 80% or less. [Item 4] 4. An RTB based sintered magnet according to any one of items 1 to 3, comprising a portion in which at least one of the Nd concentration and the Pr concentration gradually decreases from the magnet surface toward the magnet interior. [Item 5] 5. An RTB based sintered magnet according to any one of items 1 to 4, comprising a portion in which at least one of the Tb concentration and the Dy concentration gradually decreases from the magnet surface toward the magnet interior. [Item 6] 6. An RTB based sintered magnet according to any one of items 1 to 5, which satisfies [R]≦14.0. [Item 7] 7. An RTB based sintered magnet according to any one of items 1 to 6, which satisfies 5.1≦[B]≦5.6. [Item 8] 8. An RTB based sintered magnet according to any one of items 1 to 7, which satisfies 0≦[O]≦1.2. [Item 9] 9. An RTB based sintered magnet according to any one of items 1 to 8, which satisfies 0≦[N]≦0.4. [Item 10] 10. An RTB based sintered magnet according to any one of items 1 to 9, which satisfies 0≦[C]≦1.0. [Item 11] 11. An RTB based sintered magnet according to any one of items 1 to 10, which satisfies 0.1≦[Ga]≦0.7. [Item 12] 14.35≦[T] / ([B eff ]+[C eff ])≦15.00 12. An RTB based sintered magnet according to any one of items 1 to 11, which satisfies the above. [Item 13] A method for producing an RTB based sintered magnet, comprising the steps of: A step of preparing a sintered body material; Providing a diffusion source; diffusing the elements contained in the diffusion source from the surface of the sintered body to the inside; Including, The content (mol%) of element or element group X is represented by [X], [Reff ]=[R]-0.789[N]-1.58[O], [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb], [C eff ]=[C]+0.123[N]-0.754[O], The element content of the sintered body material is: [C]≧0.754[O]-0.123[N], 14.13≦[T] / ([B eff ]+[C eff ])≦15.50, 5.1≦[T] / [R eff ]≦6.7, 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0 ≦ [Nb] ≦ 0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7, A method for producing RTB sintered magnets that satisfies the above requirements. [Item 14] A composition design method for an RTB sintered magnet having a C+N+O content of 40 to 60 atomic % and including a rare earth oxide phase containing all of C, N, and O at grain boundaries, comprising: A composition design method for an RTB sintered magnet, comprising: calculating the amount of available C that is not distributed in the rare earth oxide phase from the contents of C, O, and N; and designing the composition assuming that the amount of available C is equivalent to B. [Item 15] The content (mol%) of element or element group X is represented by [X], The content of C distributed in the rare earth oxide phase is defined as [C NaCl ], the content of the available C that is not distributed in the rare earth oxide phase is [C eff ], [R eff ]=[R]-0.789[N]-1.58[O], [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb], [C eff]=[C]+0.123[N]-0.754[O] When [C] ≥ 0.754[O]-0.123[N] and 14.13 ≤ [T] / ([B eff ]+[C eff Item 15. The method for designing a composition of an RTB based sintered magnet according to item 14, wherein the composition is determined so as to satisfy the formula: [Item 16] 5.1≦[T] / [R eff ]≦6.7 17. The method for designing a composition of an RTB based sintered magnet according to item 15 or 16, wherein the composition is determined so as to satisfy the following: [Item 17] 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0 ≦ [Nb] ≦ 0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7, Item 17. The method for designing a composition of an RTB based sintered magnet according to item 16, wherein the composition is determined so as to satisfy the following: [Industrial Applicability]
[0100] The RTB based sintered magnet and its manufacturing method and composition design method disclosed herein can be widely used in the field of manufacturing RTB based sintered magnets that contain rare resource elements in the raw material alloy. [Explanation of symbols]
[0101] 1 Sintered material 2. Source of spread 3 Processing vessel 12 Main phase 14 Grain boundary phase 14a Two-grain grain boundary phase 14b Grain boundary triple point
Claims
1. R 2 T 14 An R-T-B based sintered magnet (R is a rare earth element, which necessarily contains at least one of Nd and Pr, and T is a group of elements consisting of Fe, Co, Ni, Al, Mn, Cr and V, which necessarily contains Fe) including a main phase of a B compound and a grain boundary phase located at grain boundaries of the main phase, The content (mol %) of an element or group of elements X is represented by [X], [R eff ]=[R]-0.789[N]-1.58[O]、 [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb]、 [C eff ]=[C]+0.123[N]-0.754[O] When The element contents of the R-T-B based sintered magnet are as follows: [C]≧0.754[O]-0.123[N], 14.13≦[T] / ([B eff ]+[C eff ])≦15.50、 5.1≦[T] / [R eff ]≦6.7、 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0≦[Nb]≦0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7, An RTB based sintered magnet that satisfies the above requirements.
2. 2. The R-T-B system sintered magnet according to claim 1, wherein the grain boundary phase contains a rare earth oxide phase, the rare earth oxide phase has a C+N+O content of 40 to 60 atomic %, and contains all of O, C, and N.
3. 2. The R-T-B based sintered magnet according to claim 1, wherein in a cross section of the R-T-B based sintered magnet, the ratio of a cross-sectional area of the rare earth oxide phase to a cross-sectional area of the grain boundary phase is 20% or more and 80% or less.
4. 2. The R-T-B based sintered magnet according to claim 1, which includes a portion in which at least one of the Nd concentration and the Pr concentration gradually decreases from the surface of the magnet toward the interior of the magnet.
5. 5. The R-T-B based sintered magnet according to claim 4, which includes a portion in which at least one of the Tb concentration and the Dy concentration gradually decreases from the magnet surface toward the magnet interior.
6. 6. The RTB based sintered magnet according to claim 1, wherein [R]≦14.0 is satisfied.
7. 6. The RTB based sintered magnet according to claim 1, which satisfies 5.1≦[B]≦5.
6.
8. 6. The RTB based sintered magnet according to claim 1, which satisfies 0≦[O]≦1.
2.
9. 6. The RTB based sintered magnet according to claim 1, which satisfies 0≦[N]≦0.
4.
10. 6. The RTB based sintered magnet according to claim 1, which satisfies 0≦[C]≦1.
0.
11. 6. The RTB based sintered magnet according to claim 1, which satisfies 0.1≦[Ga]≦0.
7.
12. 14.35≦[T] / ([B eff ]+[C eff ])≦15.00 6. The RTB based sintered magnet according to claim 1, which satisfies the above.
13. A method for producing an R-T-B based sintered magnet, comprising the steps of: A step of preparing a sintered body material; Providing a diffusion source; diffusing the elements contained in the diffusion source from the surface of the sintered body to the inside; Including, The content (mol %) of an element or group of elements X is represented by [X], [R eff ]=[R]-0.789[N]-1.58[O]、 [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb]、 [C eff ]=[C]+0.123[N]-0.754[O], The element content of the sintered body material is: [C]≧0.754[O]-0.123[N], 14.13≦[T] / ([B eff ]+[C eff ])≦15.50、 5.1≦[T] / [R eff ]≦6.7、 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0≦[Nb]≦0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7, The present invention relates to a method for producing an RTB based sintered magnet that satisfies the above requirements.
14. A composition design method for an R-T-B based sintered magnet having a C+N+O content of 40 to 60 atomic % and including a rare earth oxide phase containing all of O, C, and N at grain boundaries, comprising: A composition design method for an R-T-B based sintered magnet, comprising: calculating an effective amount of C that is not distributed in the rare earth oxide phase from the contents of C, O, and N; and designing a composition on the assumption that C in the effective amount of C is equivalent to B.
15. The content (mol %) of an element or group of elements X is represented by [X], [R eff ]=[R]-0.789[N]-1.58[O]、 [B eff ]=[B]-0.8[Zr]-0.8[Ti]-0.4[Nb]、 [C eff ]=[C]+0.123[N]-0.754[O] When [C] ≧ 0.754[O] − 0.123[N] and 14.13 ≦ [T] / ([B eff ]+[C eff 15. The composition design method for an RTB based sintered magnet according to claim 14, wherein the composition is determined so as to satisfy the formula:
16. 5.1≦[T] / [R eff ]≦6.7、 17. The method for designing a composition of an RTB based sintered magnet according to claim 15, wherein the composition is determined so as to satisfy the following:
17. 5.0≦[B]≦6.5, 0.1≦[Ga]≦1.5, 0≦[Co]≦2, 0≦[Nb]≦0.35, and 0≦[Zr]+[Ti]+[Nb]≦0.7, The composition design method for an R-T-B based sintered magnet according to claim 16, wherein the composition is determined so as to satisfy the following:
Citation Information
Patent Citations
Alloy for r-t-b-based rare earth sintered magnet, process for producing alloy for r-t-b-based rare earth sintered magnet, alloy material for r-t-b-based rare earth sintered magnet, r-t-b-based rare earth sintered magnet, process for producing r-t-b-based rare earth sintered magnet, and motor
WO2013008756A1