Method for producing film laminate
The method improves adhesion and reduces transmission loss by surface treating fluororesin films with rare earth elements or Mg/Al and forming a metal copper layer, with optional intermediate layers, suitable for high-frequency signal transmission.
Patent Information
- Application Number
- JP2023052708
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for laminating a metal copper layer on a fluororesin film face challenges such as poor adhesion and increased transmission loss due to the chemical stability of fluororesin surfaces, which affects the bonding with other materials.
A method involving surface treatment of the fluororesin film with rare earth elements or Mg and Al, followed by forming a metal copper layer, optionally with an intermediate layer of Ta alloy or amorphous oxide, to enhance adhesion and reduce transmission loss.
The method achieves strong and stable adhesion between the fluororesin film and metal copper layer, ensuring low transmission loss and heat resistance for high-frequency signal transmission applications.
Smart Images

Figure 2024141196000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film. [Background technology]
[0002] Generally, a film laminate in which a metallic copper layer is laminated as a conductive layer or a heat transfer layer on the surface of an insulating resin layer is used as a wiring substrate for use in electronic and electric devices. Here, wiring boards for high-frequency signal transmission devices such as antennas and radars in the GHz band or above are required to have low transmission loss when used in the high-frequency range. In view of this, for example, film laminates using fluororesin films have been provided as shown in Patent Documents 1 and 2. Fluororesins have a low dielectric constant and low dielectric loss, and are therefore particularly suitable as resin films constituting wiring boards for high-frequency signal transmission.
[0003] Incidentally, since the surface of a fluororesin film is very chemically stable, the adhesive strength with other materials tends to be low. Therefore, in Patent Document 1, protrusions are formed on the surface of the fluororesin, the metal foil is roughened, and the conditions for pressure lamination are optimized to improve the adhesion between the copper film and the fluororesin through the anchor effect. In addition, in Patent Document 2, a thin metal film (nickel film or titanium film) is formed on the surface of the fluororesin by physical vapor deposition, and then a copper film is formed by copper plating on this thin metal film, thereby improving the adhesion between the copper film and the fluororesin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-019932 A [Patent Document 2] International Publication No. 2018 / 179904 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in Patent Document 1, the interface between the fluororesin and the metal foil becomes rough, which causes an increase in transmission loss. In addition, in Patent Document 2, a thin metal film (nickel film or titanium film) is formed, but the fluororesin and the thin metal film cannot be firmly bonded together, and the adhesion between the fluororesin and the copper film cannot be sufficiently improved.
[0006] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a method for producing a film laminate that is particularly excellent in adhesion between a fluororesin film and a metallic copper layer, which has low transmission loss in the high frequency range, and can be stably used for wiring boards for high frequency signal transmission, etc. [Means for solving the problem]
[0007] In order to solve the above problems, the manufacturing method of a film laminate according to aspect 1 of the present invention is a manufacturing method of a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, and is characterized by comprising: a fluororesin film surface treatment step of forming a film of one or more rare earth elements having a thickness in the range of 0.5 nm to 2.0 nm by a PVD method on the surface of the fluororesin film, or forming a film of at least one or two of Mg and Al having a thickness in the range of 0.5 nm to 10.0 nm, and a metallic copper layer formation step of forming the metallic copper layer on the surface of the fluororesin film after the fluororesin film surface treatment step. The target film thickness is the expected film thickness (not the actually measured film thickness) that is obtained when a material with a certain film formation rate (measured by a step gauge after film formation for a certain time on a dummy substrate and dividing the film thickness by the film formation time) is formed for a certain time. For example, if a material with a film formation rate of 1 nm / sec is used to form a film with a target film thickness of 1 nm, the film formation time is set to 1 second.
[0008] According to the method for producing a film laminate of the first aspect of the present invention, the surface of the fluororesin film is provided with a fluororesin film surface treatment step of forming a film of one or more rare earth elements with a thickness of 0.5 nm to 2.0 nm or forming a film of at least one or two of Mg and Al with a thickness of 0.5 nm to 10.0 nm by a PVD method on the surface of the fluororesin film, so that the rare earth elements or Mg and Ge cut the C-F bonds on the outermost surface of the fluororesin and capture the liberated F to become fluorides, forming dangling bonds on the surface of the fluororesin film. The dangling bonds are modified with oxygen, and functional groups containing oxygen are formed on the surface, improving adhesion to other materials. In order to expose the functional groups, the film thickness is set as described above so that the rare earth elements or at least one or two of Mg and Al formed in the film grow by aggregation without forming a continuous film. This makes it possible to greatly improve the adhesion between the fluororesin film and the metallic copper layer.
[0009] The method for producing a film laminate of Aspect 2 of the present invention is characterized in that, in the method for producing a film laminate of Aspect 1, it further comprises, after the fluororesin film surface treatment step, an intermediate layer formation step of forming an intermediate layer on a surface of the fluororesin film, and in the metallic copper layer formation step, the metallic copper layer is formed on the intermediate layer. The method for producing a film laminate according to aspect 2 of the present invention includes an intermediate layer formation step of forming an intermediate layer on the surface of the fluororesin film, and this intermediate layer can further improve the adhesion between the fluororesin film and the metallic copper layer.
[0010] The method for producing a film laminate according to the third aspect of the present invention is characterized in that in the method for producing a film laminate according to the first or second aspect, the intermediate layer has a thickness within the range of 10 nm or more and 100 nm or less. According to the method for producing a film laminate of the third aspect of the present invention, the thickness of the intermediate layer is set to 10 nm or more, so that it is possible to reliably improve the adhesion between the fluororesin film and the metallic copper layer, while the thickness of the intermediate layer is set to 100 nm or less, so that it is possible to suppress warping of the film due to membrane stress.
[0011] The method for producing a film laminate of aspect 4 of the present invention is characterized in that, in the method for producing a film laminate of aspect 2 or aspect 3, the intermediate layer is a Ta alloy layer made of a Ta alloy having a composition containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % to 50.0 atomic % with the remainder being Ta and unavoidable impurities. According to the method for producing a film laminate of the fourth aspect of the present invention, a Ta alloy layer is formed as an intermediate layer, which is made of a Ta alloy containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % to 50.0 atomic % and the remainder being Ta and unavoidable impurities, so that Mg and Ge can extract F from the C-F bonds on the outermost surface of the fluororesin to form dangling bonds, which makes the surface active and can realize a strong bond with the Ta alloy of the parent phase. In addition, Ta is chemically stable, and the reaction with free F (fluorine) and adsorbed O (oxygen) present on the surface of the fluororesin is suppressed, and the decrease in adhesion can be suppressed even when used in a high-temperature environment.
[0012] A fifth aspect of the present invention relates to a method for producing a film laminate, and is characterized in that, in the second or third aspect of the present invention, the intermediate layer is an amorphous oxide layer. According to the method for producing a film laminate of the fifth aspect of the present invention, an amorphous oxide layer is formed as an intermediate layer, so that a chemical bond is formed via O (oxygen) on the outermost surface of the fluororesin, and a strong bond can be realized. In addition, since the amorphous oxide layer is chemically stable, the reaction between the amorphous oxide layer and the free F (fluorine) or the adsorbed O (oxygen) present on the surface of the fluororesin is suppressed, and the decrease in adhesion can be suppressed even when used in a high-temperature environment. Furthermore, since it is an amorphous oxide layer, there is no grain boundary, so it has excellent barrier properties, and even when used in a high-temperature environment, it is possible to suppress interdiffusion between the fluororesin and the metallic copper layer, and to suppress the decrease in adhesion due to fluorination and oxidation of copper.
[0013] The method for producing a film laminate of the sixth aspect of the present invention is characterized in that, in the method for producing a film laminate of the fifth aspect, the oxide constituting the amorphous oxide layer contains one or more selected from Ge, Si, Al, Ti, Ta, Zr, and Cr. According to the method for producing a film laminate of the sixth aspect of the present invention, the oxide constituting the amorphous oxide layer contains one or more selected from Ge, Si, Al, Ti, Ta, Zr, and Cr, so that the amorphous oxide layer is more chemically stable and it is possible to suppress the reaction between the amorphous oxide layer and the free F (fluorine) or the adsorbed O (oxygen) present on the surface of the fluororesin. In addition, it is possible to sufficiently secure the barrier property, suppress the interdiffusion between the fluororesin and the metallic copper layer, and appropriately suppress the decrease in adhesion due to the fluorination and oxidation of copper.
[0014] A seventh aspect of the present invention relates to a method for producing a film laminate according to the fifth aspect, and is characterized in that the oxide constituting the amorphous oxide layer contains In and Zn. According to the method for producing a film laminate of the seventh aspect of the present invention, the amorphous oxide layer is more chemically stable, and it is possible to suppress the reaction between the amorphous oxide layer and the free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin. In addition, it is possible to sufficiently ensure the barrier properties, suppress the interdiffusion between the fluororesin and the metallic copper layer, and appropriately suppress the decrease in adhesion due to the fluorination and oxidation of copper.
[0015] The film laminate manufacturing method of aspect 8 of the present invention is characterized in that, in the film laminate manufacturing method of any one of aspects 1 to 7, the metal copper layer formation process includes a seed layer formation process of forming a copper seed layer by a PVD method, and a copper plating layer formation process of forming copper plating on the seed layer. According to the method for producing a film laminate of aspect 8 of the present invention, the metallic copper layer formation step includes a seed layer formation step of forming a copper seed layer by a PVD method, and a copper plating layer formation step of forming copper plating on the seed layer, so that the adhesion to the fluororesin film is particularly excellent, and a metallic copper layer of a predetermined thickness can be stably formed. Effect of the Invention
[0016] According to the present invention, it is possible to provide a method for producing a film laminate that is particularly excellent in adhesion between a fluororesin film having low transmission loss in the high frequency range and a metallic copper layer, and that can be stably used for wiring boards for high frequency signal transmission, etc. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic explanatory diagram of a film laminate produced by a film laminate production method according to a first embodiment of the present invention. FIG. [Diagram 2] FIG. 2 is a flow diagram of a method for producing a film laminate according to the first embodiment of the present invention. [Diagram 3] FIG. 4 is a schematic explanatory diagram of a film laminate produced by a film laminate production method according to a second embodiment of the present invention. [Figure 4] FIG. 4 is a flow diagram of a method for producing a film laminate according to a second embodiment of the present invention. [Diagram 5] FIG. 11 is a schematic explanatory diagram of a film laminate produced by a film laminate production method according to a third embodiment of the present invention. [Figure 6] FIG. 4 is a flow diagram of a method for producing a film laminate according to a third embodiment of the present invention. [Figure 7] FIG. 2 is a schematic diagram of a peel test in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] A method for producing a film laminate according to an embodiment of the present invention will be described below. The method for producing a film laminate according to an embodiment of the present invention is for producing a film laminate to be used as a wiring board for transmitting high-frequency signals.
[0019] First embodiment First, a first embodiment of the present invention will be described. A film laminate 10 manufactured by the film laminate manufacturing method of the first embodiment of the present invention includes a fluororesin film 11 and a metallic copper layer 12 laminated on this fluororesin film 11, as shown in FIG.
[0020] The fluororesin film 11 is made of a fluororesin such as PFA (perfluoroalkoxyalkane), PTFE (polytetrafluoroethylene), ETFE (ethylene-tetrafluoroethylene copolymer), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PCTFE (polychlorotrifluoroethylene), etc. Fluororesin has a low dielectric constant and low dielectric loss, and is therefore particularly suitable as a resin film constituting a wiring board for transmitting high-frequency signals. Here, there is no particular limitation on the thickness of the fluororesin film 11, but it is preferable that the thickness is within the range of 5 μm or more and 200 μm or less.
[0021] The metallic copper layer 12 is made of copper or a copper alloy having excellent electrical and thermal conductivity, and functions as an electrically conductive layer or a heat transfer layer. Here, the electrical conductivity of the metallic copper layer 12 is preferably 80% IACS or more, and more preferably 85% IACS or more.
[0022] The thickness of the metallic copper layer 12 is preferably within the range of 2 μm to 20 μm. If the thickness of the metallic copper layer 12 is 2 μm or more, the effect of radiation loss can be ignored without being equivalent to the skin effect. On the other hand, if the thickness t2 of the metallic copper layer 12 is 20 μm or less, when a circuit pattern is formed on the metallic copper layer 12 by etching, the etching can be performed efficiently and accurately. The lower limit of the thickness of the metallic copper layer 12 is more preferably 5 μm or more, and even more preferably 10 μm or more, and the upper limit of the thickness of the metallic copper layer 12 is more preferably 18 μm or less, and even more preferably 15 μm or less.
[0023] Next, a method for producing the film laminate 10 according to this embodiment will be described with reference to the flow chart of FIG.
[0024] (Fluororesin film surface treatment process S01) First, on the surface of the fluororesin film 11, a film containing one or more rare earth elements (Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu) is formed to a thickness of 0.5 nm or more and 2.0 nm or less, or a film containing at least one or two of Mg and Al is formed to a thickness of 0.5 nm or more and 10.0 nm or less. The method for depositing at least one or two of rare earth elements, Mg, and Al is a PVD method (physical vapor deposition method) such as sputtering, ion plating, or molecular beam epitaxy. From the viewpoints of mass productivity and particle energy, sputtering is most preferable.
[0025] By forming a film of at least one or two of rare earth elements or Mg and Al on the surface of the fluororesin film 11 by a PVD method, the C-F bonds on the outermost surface of the fluororesin film 11 are broken and the liberated F is captured to become a fluoride, thereby forming dangling bonds on the surface of the fluororesin film 11. These dangling bonds are oxygen-modified by adsorbed oxygen or the like present on the surface of the fluororesin film 11, and functional groups containing oxygen are formed on the surface of the fluororesin film 11. This improves the adhesion between the fluororesin film 11 and other materials (metallic copper layer 12).
[0026] Here, in order to expose the oxygen-containing functional groups formed on the surface of the fluororesin film 11, the thickness of the film to be formed is set so that the rare earth elements or at least one or two of Mg and Al grow in a coagulated manner without forming a continuous film. Specifically, when forming a film containing one or more rare earth elements (Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu), the target film thickness is in the range of 0.5 nm or more and 2.0 nm or less. When forming a film containing at least one or both of Mg and Al, the target film thickness is set within the range of 0.5 nm to 10.0 nm.
[0027] When forming a film of a rare earth element, the target thickness is preferably 0.6 nm or more, more preferably 0.8 nm or more, whereas when forming a film of a rare earth element, the target thickness is preferably 1.8 nm or less, more preferably 1.5 nm or less. When depositing at least one or both of Mg and Al, the target thickness is preferably 1.0 nm or more, more preferably 1.5 nm or more, whereas when depositing at least one or both of Mg and Al, the target thickness is preferably 8.0 nm or less, more preferably 7.0 nm or less.
[0028] When a rare earth element or at least one or two of Mg and Al are deposited to the above-mentioned target thickness, a continuous film that covers the entire surface of the fluororesin film 11 is not formed, but aggregates are formed and distributed in islands. Therefore, the oxygen-containing functional groups formed on the surface of the fluororesin film 11 are exposed. Since a continuous film is not formed, it is difficult to confirm the actual film thickness.
[0029] (Metallic copper layer formation process S02) Next, a metallic copper layer 12 is formed on the fluororesin film 11 on which at least one or two of a rare earth element, Mg, and Al are formed. In this embodiment, the metallic copper layer forming step S02 includes a seed layer forming step S21 and a copper plating layer forming step S22.
[0030] In the seed layer formation step S21, a seed layer made of copper is formed by a PVD method such as sputtering. The thickness of the seed layer is preferably within a range of 10 nm to 1000 nm. It is preferable that the seed layer is formed continuously after forming a film of at least one or two of the above rare earth elements, Mg, and Al, without exposing the film to the atmosphere.
[0031] In the copper plating step S22, a copper plating layer having a predetermined thickness is formed on the formed seed layer by electrolytic plating. The seed layer and the copper plating layer then form the metallic copper layer 12.
[0032] The film laminate 10 of this embodiment is manufactured by the above-mentioned steps. When forming the metallic copper layers 12 on both sides of the fluororesin film 11, the fluororesin film surface treatment step S01 and the seed layer formation step S21 are performed on one side of the fluororesin film 11, and then the fluororesin film surface treatment step S01 and the seed layer formation step S21 are performed on the opposite side, and then the copper plating layer formation step S22 is performed.
[0033] According to the method for producing a film laminate of the present embodiment configured as described above, the fluororesin film surface treatment step S01 is provided, in which a film is formed on the surface of the fluororesin film 11 by a PVD method, targeting one or more rare earth elements with a thickness of 0.5 nm to 2.0 nm, or targeting at least one or two of Mg and Al with a thickness of 0.5 nm to 10.0 nm, so that the rare earth elements or at least one or two of Mg and Al break the C-F bonds on the outermost surface of the fluororesin and capture the liberated F to become fluorides, forming dangling bonds on the surface of the fluororesin film. The dangling bonds are modified with oxygen, and functional groups containing oxygen are formed on the surface, improving adhesion to other materials. This makes it possible to significantly improve the adhesion between the fluororesin film 11 and the metallic copper layer 12.
[0034] In the manufacturing method of the film laminate of this embodiment, the metal copper layer forming step S02 includes a seed layer forming step S21 of forming a copper seed layer by a PVD method, and a copper plating layer forming step S22 of forming copper plating on the seed layer, so that the adhesion to the fluororesin film 11 is particularly excellent, and a metal copper layer 12 of a predetermined thickness can be stably formed.
[0035] Second Embodiment Next, a second embodiment of the present invention will be described. Note that the same members as those in the first embodiment are given the same reference numerals and detailed descriptions thereof will be omitted.
[0036] 3, a film laminate 110 manufactured by the film laminate manufacturing method according to the second embodiment of the present invention includes a fluororesin film 11 and a metal copper layer 12 laminated on the fluororesin film 11. An intermediate layer 13 is formed between the fluororesin film 11 and the metal copper layer 12. In the film laminate 110 shown in FIG. 3, an intermediate layer 13 is formed between the fluororesin film 11 and the metallic copper layer 12 to further improve the adhesion between the fluororesin film and the metallic copper layer.
[0037] In this embodiment, the thickness of the intermediate layer 13 is preferably within the range of 10 nm to 100 nm. When the thickness of the intermediate layer 13 is 10 nm or more, it is possible to sufficiently improve the adhesion between the fluororesin film 11 and the metal copper layer 12. On the other hand, when the thickness of the intermediate layer 13 is 100 nm or less, it is possible to suppress the occurrence of warping of the film due to membrane stress. The lower limit of the thickness of the intermediate layer 13 is more preferably 15 nm or more, and even more preferably 20 nm or more. The upper limit of the thickness of the intermediate layer 13 is more preferably 80 nm or less, and even more preferably 50 nm or less.
[0038] Here, in this embodiment, the intermediate layer 13 is a Ta alloy layer made of a Ta alloy having a composition containing at least one or two of Mg and Ge in a total amount ranging from 0.5 atomic % to 50.0 atomic % with the remainder being Ta and unavoidable impurities. The Mg and Ge contained in this intermediate layer 13 (Ta alloy layer) extract F from the C-F bonds on the outermost surface of the fluororesin film 11 to form dangling bonds, activating the surface and achieving a strong bond with the Ta parent phase, significantly improving the adhesion between the fluororesin film 11 and the intermediate layer 13 (Ta alloy layer). In addition, the intermediate layer 13 and the metallic copper layer 12 are bonded to each other by metal to metal, resulting in a strong bond. Therefore, the fluororesin film 11 and the metallic copper layer 12 are strongly bonded via the intermediate layer 13, and the adhesion between the fluororesin film 11 and the metallic copper layer 12 can be further improved. Furthermore, since Ta is chemically stable, even when the film is used in a high-temperature environment, the reaction between the free F (fluorine) and adsorbed O (oxygen) present on the surface of the fluororesin film 11 and the intermediate layer 13 (Ta alloy layer) is suppressed, thereby improving the heat resistance.
[0039] If the total content of at least one or two of Mg and Ge in the intermediate layer 13 (Ta alloy layer) is less than 0.5 atomic %, the surface of the fluororesin film may not be sufficiently activated. On the other hand, if the total content of at least one or two of Mg and Ge in the intermediate layer 13 (Ta alloy layer) exceeds 50.0 atomic %, the Ta content may be insufficient, and the heat resistance may not be sufficiently improved. The lower limit of the total content of at least one or two of Mg and Ge in the intermediate layer 13 (Ta alloy layer) is preferably 1.0 atomic % or more, and more preferably 2.0 atomic % or more. On the other hand, the upper limit of the total content of at least one or two of Mg and Ge in the intermediate layer 13 (Ta alloy layer) is preferably 40.0 atomic % or less, and more preferably 20.0 atomic % or less.
[0040] Next, a method for producing the film laminate 110 according to this embodiment will be described with reference to the flow diagram of FIG.
[0041] (Fluororesin film surface treatment process S101) In this fluororesin film surface treatment step S101, similar to the fluororesin film surface treatment step S01 of the first embodiment, a film containing one or more rare earth elements (Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu) is formed on the surface of the fluororesin film 11 to a thickness of 0.5 nm or more and 2.0 nm or less, or a film containing at least one or two of Mg and Al is formed to a thickness of 0.5 nm or more and 10.0 nm or less.
[0042] (Intermediate layer formation step S102) Next, the intermediate layer 13 is formed on the fluororesin film 11 on which at least one or two of a rare earth element, Mg, and Al are deposited. In this embodiment, a Ta alloy layer is deposited as the intermediate layer 13 to a predetermined thickness. Here, in the intermediate layer formation step S102, the film is formed using a sputtering target composed of a Ta alloy containing at least one or two of Mg and Ge in a total amount ranging from 0.5 atomic % to 50.0 atomic % with the remainder being Ta and unavoidable impurities.
[0043] (Metallic copper layer formation step S103) Next, a metallic copper layer 12 is formed on the fluororesin film 11 on which the intermediate layer 13 has been formed. In this embodiment, the metallic copper layer forming step S103 includes a seed layer forming step S131 and a copper plating layer forming step S132, similar to the first embodiment. The seed layer and the copper plating layer then form the metallic copper layer 12.
[0044] The film laminate 110 of this embodiment is manufactured by the above-mentioned steps. When forming the metallic copper layers 12 on both sides of the fluororesin film 11, the fluororesin film surface treatment step S101, the intermediate layer formation step S102, and the seed layer formation step S131 may be performed on one side of the fluororesin film 11, and then the fluororesin film surface treatment step S101, the intermediate layer formation step S102, and the seed layer formation step S131 may be performed on the opposite side, followed by the copper plating layer formation step S132.
[0045] According to the manufacturing method of the film laminate of this embodiment configured as described above, the method includes a fluororesin film surface treatment step S101 in which one or more rare earth elements are deposited on the surface of the fluororesin film 11 by a PVD method to a thickness of 0.5 nm to 2.0 nm, or a film of at least one of Mg and Al is deposited on the surface of the fluororesin film 11 to a thickness of 0.5 nm to 10.0 nm, and an intermediate layer formation step S102 in which an intermediate layer 13 is formed on the surface of the fluororesin film 11. This activates the surface of the fluororesin film 11, making it possible to firmly bond the fluororesin film 11 and the intermediate layer 13, and the adhesion between the fluororesin film 11 and the metal copper layer 12 can be significantly improved via this intermediate layer 13.
[0046] Furthermore, in this embodiment, when the thickness of the intermediate layer 13 is within the range of 10 nm or more and 100 nm or less, it is possible to reliably improve the adhesion between the fluororesin film 11 and the metallic copper layer 12, and also to suppress warping of the film due to membrane stress.
[0047] In this embodiment, when the intermediate layer 13 is a Ta alloy layer made of a Ta alloy containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % to 50.0 atomic % with the remainder being Ta and unavoidable impurities, the Mg and Ge contained in the Ta alloy layer can extract F from the C-F bonds on the outermost surface of the fluororesin to form dangling bonds, which makes the surface active and can achieve strong bonding with the Ta alloy of the parent phase. Ta is also chemically stable, and the reaction with free F (fluorine) and adsorbed O (oxygen) present on the surface of the fluororesin is suppressed, so that the decrease in adhesion can be suppressed even when used in a high-temperature environment. Therefore, a film laminate 110 having excellent adhesion and heat resistance can be manufactured.
[0048] Third embodiment Next, a third embodiment of the present invention will be described. Note that the same members as those in the first and second embodiments are denoted by the same reference numerals, and detailed description thereof will be omitted.
[0049] 5, a film laminate 210 manufactured by the film laminate manufacturing method according to the third embodiment of the present invention includes a fluororesin film 11 and a metal copper layer 12 laminated on the fluororesin film 11. An intermediate layer 23 is formed between the fluororesin film 11 and the metal copper layer 12. In the film laminate 210 shown in FIG. 5, an intermediate layer 23 is formed between the fluororesin film 11 and the metallic copper layer 12 to further improve the adhesion between the fluororesin film and the metallic copper layer.
[0050] In this embodiment, the intermediate layer 23 is an amorphous oxide layer made of an amorphous oxide. This intermediate layer 23 (amorphous oxide layer) firmly bonds the fluororesin film 11 and the intermediate layer 23 (amorphous oxide layer) through a chemical bond COM (M is a metal contained in the amorphous oxide layer) mediated by O (oxygen). In addition, the intermediate layer 23 (amorphous oxide layer) is chemically stable, and reaction between the intermediate layer 23 (amorphous oxide layer) and free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin film 11 is suppressed. Furthermore, since the intermediate layer 23 (amorphous oxide layer) has no grain boundaries and has excellent barrier properties, it can suppress interdiffusion between the fluororesin film 11 and the metallic copper layer 12, and can suppress a decrease in adhesion due to fluorination and oxidation of copper.
[0051] Here, the oxide constituting the amorphous oxide layer preferably contains one or more elements selected from the group consisting of Ge, Si, Al, Ti, Ta, Zr and Cr. When the oxides of these metals are formed into a film by sputtering or the like, an amorphous oxide film is formed, making it possible to ensure sufficient barrier properties.
[0052] Alternatively, the oxide constituting the amorphous oxide layer preferably contains In and Zn. When the oxides of these metals are formed into a film by sputtering or the like, an amorphous oxide film is formed, making it possible to ensure sufficient barrier properties.
[0053] Moreover, the thickness of the intermediate layer 23 (amorphous oxide layer) is preferably within the range of 10 nm to 100 nm. If the thickness of the intermediate layer 23 (amorphous oxide layer) is 10 nm or more, the barrier properties can be sufficiently ensured. On the other hand, if the thickness of the intermediate layer 23 (amorphous oxide layer) is 100 nm or less, the warping of the film due to the membrane stress can be suppressed. The lower limit of the thickness of the intermediate layer 23 (amorphous oxide layer) is more preferably 15 nm or more, and even more preferably 20 nm or more. The upper limit of the thickness of the intermediate layer 23 (amorphous oxide layer) is more preferably 80 nm or less, and even more preferably 50 nm or less.
[0054] Next, a method for producing the film laminate 210 according to this embodiment will be described with reference to the flow diagram of FIG.
[0055] (Fluororesin film surface treatment process S201) In this fluororesin film surface treatment step S201, similar to the fluororesin film surface treatment step S01 of the first embodiment, a film containing one or more rare earth elements (Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu) is formed on the surface of the fluororesin film 11 to a thickness of 0.5 nm or more and 2.0 nm or less, or a film containing at least one or two of Mg and Al is formed to a thickness of 0.5 nm or more and 10.0 nm or less.
[0056] (Intermediate layer formation step S202) Next, the intermediate layer 13 is formed on the fluororesin film 11 on which at least one or two of a rare earth element, Mg, and Al are deposited. In this embodiment, an amorphous oxide layer is deposited to a predetermined thickness as the intermediate layer 13. Here, in the intermediate layer forming step S202, the intermediate layer 23 (amorphous oxide layer) is formed to a predetermined thickness by sputtering. As the sputtering target, an oxide target of a predetermined composition may be used, or a metal target may be used to introduce oxygen for film formation.
[0057] (Metallic copper layer formation step S203) Next, a metallic copper layer 12 is formed on the fluororesin film 11 on which the intermediate layer 23 has been formed. In this embodiment, the metallic copper layer forming step S203 includes a seed layer forming step S231 and a copper plating layer forming step S232, similar to the first embodiment. The seed layer and the copper plating layer then form the metallic copper layer 12.
[0058] The film laminate 210 of this embodiment is manufactured by the above-mentioned steps. When forming the metallic copper layers 12 on both sides of the fluororesin film 11, the fluororesin film surface treatment step S201, the intermediate layer formation step S202, and the seed layer formation step S231 may be performed on one side of the fluororesin film 11, and then the fluororesin film surface treatment step S201, the intermediate layer formation step S202, and the seed layer formation step S231 may be performed on the opposite side, followed by the copper plating layer formation step S232.
[0059] According to the manufacturing method of the film laminate of this embodiment configured as described above, the method includes a fluororesin film surface treatment step S201 in which one or more rare earth elements are deposited to a thickness of 0.5 nm or more and 2.0 nm or in which at least one or two of Mg and Al are deposited to a thickness of 0.5 nm or more and 10.0 nm or less on the surface of the fluororesin film 11 by a PVD method, and an intermediate layer formation step S202 in which an intermediate layer 23 is formed on the surface of the fluororesin film 11. This activates the surface of the fluororesin film 11, making it possible to firmly bond the fluororesin film 11 and the intermediate layer 13, and the adhesion between the fluororesin film 11 and the metal copper layer 12 can be significantly improved via this intermediate layer 13.
[0060] In this embodiment, an amorphous oxide layer is formed as the intermediate layer 23, so that a chemical bond is formed via O (oxygen) on the outermost surface of the fluororesin, and a strong bond can be realized. In addition, since the amorphous oxide layer is chemically stable, the reaction between the amorphous oxide layer and the free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin is suppressed, and the decrease in adhesion can be suppressed even when used in a high-temperature environment. Furthermore, since the intermediate layer 23 is an amorphous oxide layer, there is no grain boundary, and it has excellent barrier properties. Therefore, even when used in a high-temperature environment, it is possible to suppress interdiffusion between the fluororesin and the metallic copper layer, and to suppress the decrease in adhesion due to fluorination and oxidation of copper.
[0061] In this embodiment, when the oxide constituting the intermediate layer 23 (amorphous oxide layer) contains one or more selected from Ge, Si, Al, Ti, Ta, Zr, and Cr, the intermediate layer 23 (amorphous oxide layer) is more chemically stable, and it is possible to suppress the reaction between the amorphous oxide layer and the free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin. In addition, it is possible to sufficiently ensure the barrier properties, suppress the interdiffusion between the fluororesin and the metallic copper layer, and appropriately suppress the decrease in adhesion due to the fluorination and oxidation of copper.
[0062] In this embodiment, when the oxide constituting the intermediate layer 23 (amorphous oxide layer) contains In and Zn, the intermediate layer 23 (amorphous oxide layer) is more chemically stable, and it is possible to suppress the reaction between the amorphous oxide layer and the free F (fluorine) or adsorbed O (oxygen) present on the surface of the fluororesin. In addition, it is possible to sufficiently ensure the barrier properties, suppress the interdiffusion between the fluororesin and the metallic copper layer, and appropriately suppress the decrease in adhesion due to the fluorination and oxidation of copper.
[0063] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. EXAMPLES
[0064] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.
[0065] As the fluororesin film, a PFA film (thickness: 50 μm) manufactured by AGC was prepared. As a surface treatment for this fluororesin film, at least one or two of rare earth elements, Mg, and Al were formed by sputtering, as shown in Tables 1 to 3. The degree of vacuum at the start of film formation was 1.0×10 -4 The sputtering gas was high-purity argon, and the pressure was 0.1 Pa or less. In this embodiment, the film formation rate and film formation time were controlled to perform surface treatment to the target film thickness shown in the table. In Comparative Examples 1 and 2, the surface treatment of the fluororesin film was not carried out.
[0066] Next, in Inventive Examples 2 to 40 and Comparative Examples 2 to 10, an intermediate layer shown in Tables 1 to 3 was formed by sputtering on the surface of the fluororesin film. Note that in Inventive Example 1 and Comparative Example 1, no intermediate layer was formed. Here, the intermediate layer was formed continuously after a film was formed by sputtering as a surface treatment, without being exposed to the atmosphere.
[0067] When an amorphous oxide layer was formed as the intermediate layer, it was formed under the following conditions. (Conditions for forming the amorphous oxide layer) Target material: Ge, Si, Al, Ti, Ta, Zr, Cr, IZO (85at%In-15at%Zn composite oxide) (purity 99.9mass% or more) Deposition start vacuum degree: 1.0×10 -4 Pa or less Sputtering gas: A mixture of high-purity argon and high-purity oxygen Sputtering gas pressure in the chamber: 0.2 Pa DC power density: 7.5W / cm 2 (Si, Al, Ti, Ta, Zr, Cr, IZO) AC power density: 10.0W / cm 2(Ge)
[0068] When a Ta alloy layer was formed as the intermediate layer, it was formed under the following conditions. (Ta alloy layer deposition conditions) Target material: Ta-Ge alloy, Ta-Mg alloy Deposition start vacuum degree: 1.0×10 -4 Pa or less Sputtering gas: High purity argon Sputtering gas pressure in the chamber: 0.2 Pa DC power density: 7.5W / cm 2
[0069] Next, a copper layer was formed to a thickness of 100 nm by sputtering as a seed layer for plating. The sputtering conditions were as follows. In invention example 1, after forming a film by sputtering as a surface treatment, a seed layer was continuously formed without exposing to the atmosphere. In invention examples 2 to 42 and comparative examples 2 to 10, after forming an intermediate layer, a seed layer was continuously formed without exposing to the atmosphere. (Seed layer deposition conditions) Target material: Cu (purity 99.99 mass% or more) Deposition start vacuum degree: 1.0×10 -4 Pa or less Sputtering gas: High purity argon Sputtering gas pressure in the chamber: 0.2 Pa DC power density: 7.5W / cm 2
[0070] Next, a copper plating layer was formed on the seed layer by electrolytic plating under the following conditions: The thickness of the metallic copper layer shown in Table 1 is the total thickness of the seed layer and the copper plating layer. (Electrolytic plating conditions) Pretreatment: Sulfuric acid washing Liquid temperature: 25℃ Anode: phosphorus-containing copper Stirring conditions: Air 12.5L / min Plating conditions: 4A, 45min Plating solution: CuSO4·5H2O 200g / L H2SO4 54g / L 1mol HCl 1.37mL / L
[0071] The film laminate produced as described above was evaluated for the thickness of the intermediate layer, the thickness of the metallic copper layer, the adhesive strength, and the heat resistance as follows.
[0072] (Thickness of middle layer) The thickness of the intermediate layer is the target value based on the deposition rate. The deposition rate was calculated by measuring the film thickness after deposition on a dummy substrate for a certain period of time using a step measurement meter (Dektak-XT by Bruker) and dividing the film thickness by the deposition time. The evaluation results are shown in Tables 1 to 3. Furthermore, the thickness of the intermediate layer was confirmed by observing the cross section of the film laminate with a TEM (transmission electron microscope), and was found to be equivalent to the target value based on the film formation rate.
[0073] (Thickness of metallic copper layer) The thickness of the metallic copper layer (seed layer and copper plating layer) was confirmed by an eddy current method. The evaluation results are shown in Tables 1 to 3.
[0074] (Adhesion strength) As shown in Figure 7, the metallic copper layer (and intermediate layer) formed on the fluororesin film was cut into a width of 5 mm and evaluated using an A&D Tensilon universal testing machine (RTF-1310) at a peel angle of 90 degrees and a peel speed of 50 mm / min. The evaluation results are shown in Tables 4 to 6.
[0075] (Heat resistance test) As a heat resistance test, the film laminate was stored in a clean oven under the conditions of 150°C x 240h. After storage, the adhesion strength of the film laminate was measured as described above. Then, the rate of change in adhesion strength before and after the heat resistance test was calculated. The evaluation results are shown in Tables 4 to 6. (Change rate) = (Adhesion strength after test - Adhesion strength before test) / Adhesion strength before test × 100 (%)
[0076] [Table 1]
[0077] [Table 2]
[0078] [Table 3]
[0079] [Table 4]
[0080] [Table 5]
[0081] [Table 6]
[0082] In Comparative Examples 1 and 2, no surface treatment was performed, and therefore the adhesion was reduced. In Comparative Examples 3 to 10, the target thickness of the metal film formed as the surface treatment was outside the range of the present invention, and therefore the adhesion was reduced.
[0083] In contrast, in Examples 1 to 42 of the present invention, in which the surface treatment of the fluororesin film was carried out by forming a film of one or more rare earth elements in a thickness range of 0.5 nm to 2.0 nm on the surface of the fluororesin film using a PVD method, or a film of at least one or two of Mg and Al in a thickness range of 0.5 nm to 10.0 nm, the adhesion strength was significantly improved. In addition, in Examples 2 to 42 of the present invention in which an intermediate layer was formed, the adhesive strength did not decrease significantly even after the heat resistance test, and the heat resistance was particularly excellent. Therefore, in applications in which the film is used in a high-temperature environment, it is preferable to form an intermediate layer.
[0084] From the above, it was confirmed that the present invention can provide a method for producing a film laminate that has particularly excellent adhesion between a fluororesin film and a metallic copper layer, which has low transmission loss in the high frequency range, and can stably produce a film laminate that can be used for wiring boards for high frequency signal transmission, etc.
Claims
1. A method for producing a film laminate in which a metallic copper layer is laminated on one or both sides of a fluororesin film, comprising the steps of: a fluororesin film surface treatment step of forming a film of one or more rare earth elements having a thickness of 0.5 nm to 2.0 nm on the surface of the fluororesin film by a PVD method, or forming a film of at least one or two of Mg and Al having a thickness of 0.5 nm to 10.0 nm on the surface of the fluororesin film; a metallic copper layer forming step of forming the metallic copper layer on the surface of the fluororesin film after the fluororesin film surface treatment step; A method for producing a film laminate, comprising:
2. 2. The method for producing a film laminate according to claim 1, further comprising, after the fluororesin film surface treatment step, an intermediate layer formation step of forming an intermediate layer on the surface of the fluororesin film, and in the metallic copper layer formation step, the metallic copper layer is formed on the intermediate layer.
3. 3. The method for producing a film laminate according to claim 2, wherein the thickness of the intermediate layer is set within a range of 10 nm to 100 nm.
4. The method for producing a film laminate described in claim 2, characterized in that the intermediate layer is a Ta alloy layer consisting of a Ta alloy containing at least one or two of Mg and Ge in a total amount of 0.5 atomic % to 50.0 atomic % and the remainder being Ta and unavoidable impurities.
5. 3. The method for producing a film laminate according to claim 2, wherein the intermediate layer is an amorphous oxide layer.
6. 6. The method for producing a film laminate according to claim 5, wherein the oxide constituting the amorphous oxide layer contains one or more elements selected from the group consisting of Ge, Si, Al, Ti, Ta, Zr, and Cr.
7. 6. The method for producing a film laminate according to claim 5, wherein the oxide constituting the amorphous oxide layer contains In and Zn.
8. 2. The method for producing a film laminate according to claim 1, wherein the metallic copper layer forming step includes a seed layer forming step of forming a copper seed layer by a PVD method, and a copper plating layer forming step of forming copper plating on the seed layer.
Citation Information
Patent Citations
Ag ALLOY FILM AND METHOD OF MANUFACTURING THE SAME
JP2014019932A
Metalized film and production method therefor
WO2018179904A1