Silencer for vehicle
The vehicle silencer with a fibrous structure layer and sound insulating layers addresses the noise challenge in electric vehicles by creating an anti-resonance point between 500 and 2000 Hz, achieving enhanced noise reduction.
Patent Information
- Application Number
- JP2023052837
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Electric vehicles generate noise in the range of 500 to 2000 Hz due to the location of the sound source and noise frequency changes, requiring effective noise reduction in limited spaces under the rear seat where the battery unit is installed.
A vehicle silencer with a fibrous structure layer having fibers oriented in the thickness direction, a non-breathable sound insulating layer, and a breathable fiber layer, which creates an anti-resonance point between 500 and 2000 Hz by press-molding to reduce noise beyond the mass law.
The silencer effectively reduces noise between 500 and 2000 Hz by generating an anti-resonance point, enhancing sound absorption performance and noise reduction capabilities.
Smart Images

Figure 2024141283000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a silencer for a vehicle that is disposed in contact with a surface of a panel. [Background technology]
[0002] Known silencers installed in automobiles include floor silencers and wheelhouse silencers. In recent years, electric automobiles equipped with electric motors as prime movers have been sold. Electric automobiles are equipped with a battery unit containing a plurality of secondary battery cells (e.g., lithium ion cells) that can be charged by external power, located under the rear seats, and run by a motor installed on the rear side of the vehicle, for example. The position of the sound source and the noise frequency of electric automobiles have changed from gasoline-powered automobiles, and the installation location of silencers has also changed. Patent Document 1 discloses a floor carpet to be installed in gasoline vehicles, etc. The floor carpet includes a design layer in which a concave-convex shape is formed on the passenger compartment side by press molding, and a cushioning material layer in which a concave-convex shape is formed on the panel side by press molding a cushioning material having a fiber structure in which fibers are oriented in the thickness direction. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-173446 A Summary of the Invention [Problem to be solved by the invention]
[0004] For example, in an electric vehicle, the space under the rear seat where the battery unit is installed is limited, and there is a particular need to effectively reduce noise of about 500 to 2000 Hz generated while the electric vehicle is running. [Means for solving the problem]
[0005] The vehicle silencer of the present invention is a vehicle silencer arranged in contact with the surface of a panel, a fiber structure layer having a first surface on the side opposite to the panel and a second surface in contact with the surface of the panel, and a surface layer including at least a non-breathable sound insulation layer adhered to the first surface. The fiber structure layer has a breathable fiber structure in which fibers are oriented in the thickness direction, the basis weight of the surface layer is 250 to 2000 g / m 2 and the basis weight of the fiber structure layer is 400 to 1200 g / m. 2 and the thickness of the fiber structure layer is 8 to 25 mm. In a graph with the 1 / 3 octave band center frequency f (Hz) on the logarithmic scale horizontal axis and the insertion loss IL (dB) on the vertical axis, the vehicle silencer has a specific point (fs, ILs) that is convex upward among a plurality of points (f, IL) connected by a broken line, and a first surrounding point (fa, ILa) and a second surrounding point (fb, ILb) that are convex downward on the broken line are tangent to a straight line with fa < fs < fb, and the distance ILs - ILc between a reference point (fs, ILc) on the straight line and the specific point (fs, ILs) is 4.5 dB or more, and fs is between 500 and 2000 Hz.
Advantages of the Invention
[0006] According to the present invention, it is possible to provide a vehicle silencer capable of effectively reducing noise in the range of about 500 to 2000 Hz generated by the running of a vehicle such as an electric vehicle.
Brief Description of the Drawings
[0007] [Figure 1] A cross-sectional view schematically illustrating a main part of an automobile equipped with a silencer. [Diagram 2] A side view illustrating a main part of a fiber structure. [Diagram 3] FIG. 3A is a perspective view illustrating a main part of a fiber structure, and FIG. 3B is a perspective view illustrating a main part of a fiber structure with a folded-back portion cut away. [Figure 4] 4A and 4B are diagrams showing examples of the "anti-resonance point." [Diagram 5] 1A to 1C are diagrams illustrating an example of a silencer manufacturing method. [Figure 6] 1 is a semi-logarithmic graph showing the difference in the measurement results of insertion loss characteristics depending on whether or not a fiber structure layer is present. [Figure 7] 1 is a semi-logarithmic graph showing the difference in the measurement results of insertion loss characteristics depending on whether or not a fiber structure layer is present. [Figure 8] 1 is a semi-logarithmic graph showing measurement results of insertion loss characteristics according to the basis weight of the surface layer. [Figure 9] 1 is a semi-logarithmic graph showing measurement results of insertion loss characteristics according to the basis weight of the surface layer. [Figure 10] 1 is a semi-logarithmic graph showing the measurement results of insertion loss characteristics according to the basis weight of the fiber structure layer. [Figure 11] 1 is a semi-logarithmic graph showing measurement results of insertion loss characteristics as a function of the thickness of the fiber structure layer. [Figure 12] 1 is a semi-logarithmic graph showing measurement results of insertion loss characteristics as a function of adhesive strength of a sound-insulating layer to a fiber structure layer. [Figure 13] 1 is a semi-logarithmic graph showing the simulation results of the insertion loss characteristics according to the compressive elastic modulus (Young's modulus) of the fiber structure layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following embodiments of the present invention will be described. Of course, the following embodiments are merely illustrative of the present invention, and not all of the features shown in the embodiments are necessarily essential to the solution of the invention.
[0009] (1) Overview of the technology included in this invention: First, the outline of the technology included in the present invention will be described with reference to the examples shown in Figures 1 to 13. Note that the figures in the present application are diagrams showing examples in a schematic manner, and the magnification ratios in each direction shown in these figures may differ, and each figure may not be consistent. Of course, each element of the present technology is not limited to the specific example shown by the symbol. In the present application, the numerical range "Min~Max" means greater than or equal to the minimum value Min and less than or equal to the maximum value Max.
[0010] [Aspect 1] As illustrated in FIG. 1, a vehicle silencer 1 according to one aspect of the present technology is a vehicle silencer 1 disposed in contact with the surface 111 of a panel 110, and includes a fiber structure layer 10 and a surface layer 20. The fiber structure layer 10 has a first surface 11 on the side opposite to the panel 110 and a second surface 12 in contact with the surface 111 of the panel 110. The surface layer 20 has at least a non-breathable sound insulation layer 30 adhered to the first surface 11. The fiber structure layer 10 has air permeability and has a fiber structure 13 in which fibers 64 are oriented in the thickness direction D3 as illustrated in FIG. 2. The basis weight of the surface layer 20 is 250~2000 g / m 2 is. The basis weight of the fiber structure layer 10 is 400~1200 g / m 2 is. The thickness T10 of the fiber structure layer 10 is 8~25 mm. As illustrated in FIGS. 4A and 4B, in the graph with the 1 / 3 octave band center frequency f (Hz) on the logarithmic scale horizontal axis and the insertion loss IL (dB) on the vertical axis, the present vehicle silencer 1 includes a specific point Ps (fs, ILs) that is convex upward among a plurality of points (f, IL) connected by a broken line, and a first surrounding point Pa (fa, ILa) and a second surrounding point Pb (fb, ILb) that are convex downward on the broken line with fa < fs < fb, and a straight line L1 is tangent to them. The distance ILs - ILc between the reference point Pc (fs, ILc) on the straight line L1 and the specific point Ps (fs, ILs) is 4.5 dB or more, and fs is between 500~2000 Hz. In addition, when at least one of the downwardly convex surrounding points Pa and Pb with which the straight line L1 is tangent does not exist between the 1 / 3 octave band center frequencies of 200~5000 Hz, the distance ILs - ILc cannot be calculated, so the distance ILs - ILc is not 4.5 dB or more.
[0011] When tests were conducted, a fiber structure layer 10 having a fiber structure 13 in which fibers 64 are oriented in the thickness direction D3 was used, and the basis weight of the surface layer 20 was 250~2000 g / m 2and the basis weight of the fiber structure layer 10 is set to 400 to 1200 g / m 2 It was found that, when the thickness T10 of the fiber structure layer 10 is set to 8 to 25 mm, an "upwardly convex point" (hereinafter also referred to as an "anti-resonance point") indicating anti-resonance occurs between 500 and 2000 Hz on the broken line of the above-mentioned graph, as illustrated in Figs. 4A and 4B. Here, the "anti-resonance point" refers to a specific point Ps(fs,ILs) that is upwardly convex and is a specific point Ps(fs,ILs) where the distance ILs-ILc between the reference point Pc(fs,ILc) and the specific point Ps(fs,ILs) on the straight line L1 that is tangent to the first peripheral point Pa(fa,ILa) and the second peripheral point Pb(fb,ILb) that are downwardly convex is 4.5 dB or more. The "anti-resonance point" includes the peak of the broken line. When the fiber structure is not oriented in the thickness direction D3, such as random orientation, the "anti-resonance point" does not appear on the graph between 500 and 2000 Hz, as illustrated in Figs. 6 and 7. In the vehicle silencer 1 of the above-mentioned aspect 1, anti-resonance occurs between 500 and 2000 Hz, so that noise between 500 and 2000 Hz is reduced beyond the mass law. Therefore, the above-mentioned aspect 1 can provide a vehicle silencer that can effectively reduce noise of about 500 to 2000 Hz generated by the running of a vehicle such as an electric vehicle.
[0012] Here, the fiber structure layer may include a plurality of layers, and the surface layer may also include a plurality of layers. The fibers of the fiber structure are oriented in the thickness direction of the fiber structure layer, which means that the fiber arrangement direction is relatively uniform in the thickness direction, and includes having a folded portion for orienting the fibers in the thickness direction. Since the fibers constituting the fiber structure may be bent, the arrangement direction of the fibers of the fiber structure layer may deviate from the direction perpendicular to the front and back surfaces of the fiber structure layer. The fibers of the fiber structure are oriented in the thickness direction, which does not mean that straight fibers are arranged parallel to the thickness direction. From the above, fiber structures in which fibers are oriented in the thickness direction include a wavy fiber structure in which a web is repeatedly folded in the thickness direction, a fiber structure in which the folded-back portion of the wavy fiber structure is removed, and a fiber structure obtained by dividing a wavy fiber structure in two midway in the thickness direction. The fibers constituting the fiber structure may be one type of fiber or a combination of two or more types of fibers, such as a combination of main fibers and adhesive fibers. The fiber structure layer having breathability means that air can pass through the fiber structure layer from the first surface to the second surface. In this application, the terms "first", "second", . . . are terms for distinguishing between components among a plurality of components having similarities, and do not imply an order. The above remarks also apply to the following aspects.
[0013] [Aspect 2] 2 and 3, the fiber structure 13 may have a structure in which webs M1 are repeatedly stacked in a stacking direction D1 along the first surface 11. In a width direction D2 perpendicular to the stacking direction D1, the adhesive strength of the sound insulation layer 30 to the fiber structure layer 10 may be 8.5 N / 50 mm or more in 180-degree peeling of a test piece with a width of 50 mm. The above-mentioned aspect 2 can further effectively reduce noise of about 500 to 2000 Hz.
[0014] [Aspect 3] As illustrated in FIG. 1 , the surface layer 20 may further include a fiber layer 40 that is breathable and contains fibers 41 and a binder 42, and is adhered to a third surface 31 of the sound-insulating layer 30 opposite the fiber structure layer 10. In the above cases, sound heading toward the panel 110 is absorbed by the fiber layer 40, and sound reflected by the sound-insulating layer 30 in a direction away from the panel 110 is reduced. Therefore, the above-mentioned third aspect can provide a vehicle silencer with improved sound absorption performance. Although not included in the above-mentioned embodiment 3, the case where the surface layer 20 does not have the fiber layer 40 is also included in the present technology.
[0015] (2) Examples of vehicle silencers: Fig. 1 shows a schematic diagram of a main part of an automobile 100 (an example of a vehicle) equipped with a vehicle silencer 1. The silencer 1 is shown in the lower part of Fig. 1. In Fig. 1, UP indicates the top, DOWN indicates the bottom, and the symbol D3 indicates the thickness direction of the silencer 1 including the fiber structure layer 10. 1, the automobile 100 may be an electric automobile equipped with a battery unit 120. The electric automobile may be a hybrid vehicle equipped with a driving motor and an engine, and is a vehicle equipped with an electric motor as a prime mover. The battery unit 120 includes, for example, a plurality of secondary battery cells (e.g., lithium ion cells), a blower and duct for air cooling, and the like.
[0016] The body of the automobile 100 is formed of a panel 110 surrounding an interior space SP1, such as a passenger compartment. The panel 110 includes a body panel made of metal, such as a steel plate, but may also be a resin panel or the like. The silencer 1 is disposed in contact with a surface 111 of the non-breathable panel 110. The surface 111 may face the interior space SP1 as shown in FIG. 1, or may face the outside of the vehicle. The silencer 1 shown in FIG. 1 is installed under a seat 130, such as a rear seat, on the panel 110 that covers the battery unit 120. Of course, the silencer 1 may be installed on the surface of the wheel house, or on the surface of the deck floor, or the like.
[0017] In an electric vehicle, the space near the battery unit 120, such as the space under the seat 130 where the battery unit 120 is installed, is limited. In particular, it is required to effectively reduce noise of about 500 to 2000 Hz generated by the running of the electric vehicle. The silencer 1 of this specific example includes a fiber structure layer 10 having a fiber structure 13 in which fibers are oriented in the thickness direction D3 as a layer in contact with the panel 110, and includes a surface layer 20 having at least a non-breathable sound insulation layer 30 bonded to the fiber structure layer 10. The silencer 1 of this specific example can reduce noise between 500 and 2000 Hz beyond the mass law by generating an "anti-resonance point" between 500 and 2000 Hz in cooperation with the panel 110.
[0018] The silencer 1 including the fiber structure layer 10 and the surface layer 20 is press-molded and has an uneven shape (not shown). The fiber structure layer 10 has a first surface 11 and a second surface 12 on opposite sides. The fiber structure layer 10 is bonded to the sound-insulating layer 30 at the first surface 11, and is in contact with the surface 111 of the panel 110 at the second surface 12. The fiber structure layer 10 is breathable and exhibits sound absorbing performance. The surface layer 20 shown in FIG. 1 includes a non-breathable sound-insulating layer 30 bonded to the fiber structure layer 10, and a fiber layer 40 that is breathable and contains fibers 41 and a binder 42. The sound-insulating layer 30 has a third surface 31 opposite to the fiber structure layer 10. The fiber layer 40 has a surface 21 opposite to the sound-insulating layer 30, and is bonded to the third surface 31 of the sound-insulating layer 30. In addition, breathability means that the air permeability is 0.05cc / cm 2 / sec or more (preferably 1cc / cm 2 / sec or more, more preferably 3cc / cm 2 / sec or more). The air permeability is calculated in cc / cm2 from the air permeability measurement results specified in ASTM C522-03 (2016) (Standard Test Method for Air Permeability of Sound Absorbing Materials) published by ASTM International. 2 The value is expressed in / sec.
[0019] The fiber structure layer 10 is formed from a fiber structure 60 having a fiber structure 62 in which fibers 64 are oriented in a thickness direction D3 as illustrated in FIG. 2 and the like, and has air permeability that allows air to flow from one side to the other side, is lightweight, and has high sound absorption. The fiber structure 60 illustrated in FIGS. 2 and 3A has a corrugated fiber structure 62 in which the web M1 is repeatedly folded and laminated in the thickness direction D3. The fiber structure layer 10 (see FIG. 1) formed from the fiber structure 60 illustrated in FIGS. 2 and 3A has a corrugated fiber structure 13 in which the web M1 is repeatedly folded in the thickness direction D3. The thickness direction D3 of the fiber structure 60 is a direction perpendicular to the front surface 60a and the back surface 60b of the fiber structure 60. The web M1 being folded in the thickness direction D3 of the fiber structure layer 10 means that the folded web M1 is relatively oriented in the thickness direction D3, and the folded web M1 may be shifted from the thickness direction D3. In addition, the fiber structure layer 10 having the corrugated fiber structure 13 can be said to have a fiber structure 13 in which the fibers 64 are oriented in the thickness direction D3. Since the fibers 64 are oriented in the thickness direction D3 in the fiber structure 13, the rigidity in the thickness direction D3 is maintained even if the density of the fiber structure layer 10 is reduced.
[0020] In the fiber structure 60 for forming the fiber structure layer 10, the thickness of the web M1 before folding can be, for example, about 5 to 10 mm, which is about 3 to 30% of the thickness of the fiber structure 60. The number of folds (number of folded ridges) of the web M1 can be, for example, about 1 to 10 times / 20 mm. The fewer the number of folds per unit length, the lower the density and the easier it is to mold, while increasing the number of folds per unit length increases rigidity. Note that the number of folds of the web M1 is defined as the number of ridges, so the number of webs M1 per unit length is twice the number of folds.
[0021] The apparatus for producing a fiber structure in which a continuous web is repeatedly folded back into a corrugated shape and laminated can be appropriately selected from various fiber structure production apparatuses that apply known production methods such as the STRUTO method. Known examples of the fiber structure manufacturing apparatus include a textile wrapping apparatus described in JP-A-2008-538130 and an apparatus that repeatedly folds a continuous web into a corrugated shape using gears.
[0022] In the fiber structure 60, the folded surface of each pleat M2 is aligned with a plane passing through the width direction D2 and thickness direction D3 of the fiber structure 60, and the fibers 64 are oriented in the thickness direction D3 except for the folded portion 67. A boundary line 68 between the pleats M2 appears on the front surface 60a and the back surface 60b of the fiber structure 60. The fibers 64 of the fiber structure 60 shown in FIG. 2 include main fibers 65 and adhesive fibers 66 (an example of a thermoplastic binder). At least a part of the adhesive fibers 66 is melted and bonds the main fibers 65 oriented in a wavy shape. The front surface 60a and the back surface 60b where the folded portions 67 are gathered are formed along the stacking direction D1 of the pleats M2 (web M1). Here, the width direction of the fiber structure 60 is also the width direction of the web M1, and the stacking direction D1 of the web, the width direction D2 of the web, and the thickness direction D3 of the fiber structure are perpendicular to each other. Here, the fibers 64 being oriented in the thickness direction D3 means that the arrangement direction of the fibers 64 is relatively aligned in a direction perpendicular to the front surface 60a and the back surface 60b, and includes having folded-back portions 67 of the fibers.
[0023] The fibers 64 used to form the fiber structure 60 can be synthetic resin (including elastomer) fibers, synthetic resin fibers with additives added, plant fibers, inorganic fibers, reinforcing fibers, combinations of at least some of these fibers, etc., and fibers with a conjugate structure such as a core-sheath structure or a side-by-side structure can also be used.
[0024] The main fibers 65 may be made of thermoplastic resin (including thermoplastic elastomer), thermoplastic resin with additives, vegetable fiber, inorganic fiber, recycled fiber waste, or at least some combination of these fibers. Examples of the main fibers 65 include polyester fibers such as polyethylene terephthalate (PET) fibers, polyolefin fibers such as polypropylene (PP) fibers, polyamide fibers, rayon fibers, glass fibers, clothing fiber waste, recycled cotton fibers, fibers with additives, or at least some combination of these fibers. The diameter of the main fibers may be, for example, about 5 to 60 μm, the thickness of the main fibers may be, for example, about 0.5 to 15 decitex, and the length of the main fibers may be, for example, about 10 to 100 mm. When the main fibers are thermoplastic fibers, the melting point of the thermoplastic fibers may be a high melting point of, for example, about 160 to 260° C.
[0025] The adhesive fiber 66 may be a thermoplastic resin fiber, a fiber in which an additive is added to a thermoplastic resin, or a combination of these fibers. For example, polyester fibers such as PET fibers, polyolefin fibers such as PP fibers and polyethylene (PE) fibers, polyamide fibers, fibers made of materials to which additives are added, or at least a combination of these fibers may be used. When the main fiber is a thermoplastic fiber, it is preferable to use a thermoplastic fiber having a melting point lower than that of the main fiber for the adhesive fiber. For example, when a fiber compatible with the main fiber is used for the adhesive fiber, the adhesion between the main fiber and the adhesive fiber is improved, and sufficient shape retention can be imparted to the fiber structure layer 10. The melting point of the adhesive fiber may be, for example, about 100 to 220°C (preferably about 120°C or less). The fiber 64 may also have a conjugate structure, such as a core-sheath structure including a core of a component usable for the main fiber 65 and a sheath of a component usable for the adhesive fiber 66. When a portion of a component usable for the adhesive fiber 66 appears on the surface of the fiber 64 having a conjugate structure, that portion functions as a thermoplastic binder.
[0026] The fiber diameter of the adhesive fiber 66 may be, for example, about 10 to 45 μm, the thickness of the adhesive fiber 66 may be, for example, about 2 to 4 dtex, and the fiber length of the adhesive fiber 66 may be, for example, about 10 to 100 mm. The blending ratio of the main fiber 65 and the adhesive fiber 66 may be about 30 to 95% by weight of the main fiber and about 5 to 70% by weight of the adhesive fiber. It is also possible to form the fibrous structure 60 using a non-fibrous thermoplastic binder instead of adhesive fibers.
[0027] The basis weight of the fiber structure 60 is 400 to 1200 g / m2 in order to generate an anti-resonance point between 500 and 2000 Hz. 2 The density of the fiber structure 60 for forming the fiber structure layer 10 is, for example, 0.006 to 0.15 g / cm 3 The thickness of the fiber structure 60 for forming the fiber structure layer 10 may be, for example, 8 to 30 mm. The thickness T10 of the fiber structure layer 10 formed from the fiber structure 60 is set to 8 to 25 mm in order to generate an anti-resonance point between 500 and 2000 Hz.
[0028] The fiber structure 60 for forming the fiber structure layer 10 may have fibers 64 oriented in the thickness direction D3. As shown in Fig. 3B, it is also possible to use a fiber structure 61 in which the folded-back portions 67 of the front surface 60a and the back surface 60b of the fiber structure 60 shown in Fig. 3A are removed. The concept of the fiber structure 61 is included in the concept of the fiber structure 60 having a fiber structure 62 in which the fibers 64 are oriented in the thickness direction D3. It is also possible to use a fiber structure obtained by dividing a corrugated fiber structure in two midway in the thickness direction as the fiber structure 60. As a result, the fiber structure layer 10 formed from the fiber structures 60, 61 shown in Figures 3A and 3B has a fiber structure 13 in which the web M1 is repeatedly layered in the stacking direction D1 along the first surface 11 and the second surface 12, including a wavy shape in which the web M1 is repeatedly folded in the thickness direction D3.
[0029] The sound insulation layer 30 shown in Fig. 1 may be made of a material that contains at least a synthetic resin (including an elastomer) such as a thermoplastic resin. The thermoplastic resin (including a thermoplastic elastomer) for the film-like sound insulation layer 30 may be a polyolefin resin such as a polyethylene (PE) resin or a polypropylene (PP) resin, a polyamide (PA) resin, an ethylene vinyl acetate (EVA) resin, a polyvinyl chloride (PVC) resin, a modified resin obtained by adding an elastomer to any of these resins, a material obtained by adding an additive such as a colorant or a filler to any of these resins, or a combination of at least some of these. The sound insulation layer 30 may be a single layer of the above-mentioned material, or a layer in which a plurality of layers of the above-mentioned materials are combined.
[0030] The fiber layer 40 shown in Fig. 1 has air permeability that allows air to flow from one side to the other side, and has sound absorbing properties. The fibers 41 contained in the fiber layer 40 may be fibers that can be used for the main fibers 65 described above. The binder 42 contained in the fiber layer 40 may be the adhesive fibers 66 described above, a non-fibrous thermoplastic binder, or the like. The fiber layer 40 may be made of nonwoven fabric, or the like. Even if the fiber layer 40 is not present in the surface layer 20, an anti-resonance point can occur between 500 and 2000 Hz.
[0031] The presence of the breathable fiber structure layer 10 between the breathable sound-insulating layer 30 and the breathable panel 110 means that the panel 110 and the silencer 1 form a vibration system. Theoretically, the anti-resonance frequency depends on the basis weight of the surface layer 20, and when the surface layer 20 includes the sound-insulating layer 30 and the fiber layer 40, the frequency corresponds to the combined basis weight of these layers. The basis weight of the sound-insulating layer 30 and the surface layer 20, which optionally includes the fiber layer 40, is set to 250 to 2000 g / m2 in order to generate an anti-resonance point between 500 and 2000 Hz. 2 (Preferably 480 to 2000 g / m 2 ) is said to be
[0032] Next, an example of the "anti-resonance point" will be described with reference to FIGS. 4A and 4B. Figures 4A and 4B show examples of the frequency characteristics of the insertion loss IL of the silencer 1 installed on the panel 110. In the graphs shown in Figures 4A and 4B, the horizontal axis is the 1 / 3 octave band center frequency f (Hz) on a logarithmic scale, and the vertical axis is the insertion loss IL (dB). The insertion loss IL (dB) is calculated by subtracting the transmission loss (dB) of the iron plate alone from the transmission loss (dB) when the silencer sample is placed on the iron plate according to the SAE J1400_201707 standard. The graphs shown in Figures 4A and 4B are shown as a broken line connecting the points (f, IL) in the coordinate system with line segments.
[0033] Figure 4A includes a specific point Ps (fs, ILs) that is a peak among a plurality of points (f, IL) connected by a broken line. Here, the peak corresponds to the maximum value of the insertion loss IL (f) with the center frequency f as a variable. The insertion loss ILs at the specific point Ps (fs, ILs) is greater than the insertion losses IL of two points immediately before and after the specific point Ps (fs, ILs) in the horizontal axis direction. Also, let fa < fs < fb, and assume that the straight line L1 is tangent to the first surrounding point Pa (fa, ILa) and the second surrounding point Pb (fb, ILb) that are convex downward on the broken line. Here, the point that is convex downward corresponds to the point where the second derivative IL''(f) of the insertion loss IL (f) with the center frequency f as a variable is positive. The straight line L1 does not intersect the broken line in the part where the center frequency f is greater than fa and less than fb, and is always below the specific point Ps (fs, ILs). When the specific point Ps (fs, ILs) is a peak, the specific point Ps (fs, ILs) is an anti-resonance point, and the distance ILs - ILc between the reference point Pc (fs, ILc) on the straight line L1 and the specific point Ps (fs, ILs) is 4.5 dB or more. In the silencer 1 of this specific example, the frequency fs of the specific point Ps (fs, ILs) is between 500 and 2000 Hz.
[0034] FIG. 4B includes a non-peak but upwardly convex specific point Ps (fs, ILs) among a plurality of points (f, IL) connected by a broken line. Here, the upwardly convex point corresponds to a point where the second derivative IL''(f) of the insertion loss IL(f) with the center frequency f as a variable is negative. Also, assuming fa < fs < fb, let a straight line L1 be tangent to a first surrounding point Pa (fa, ILa) and a second surrounding point Pb (fb, ILb) that are downwardly convex on the broken line. The straight line L1 does not intersect the broken line in a portion where the center frequency f is greater than fa and less than fb, and is always below the specific point Ps (fs, ILs). The anti-resonance point of this specific example means a specific point Ps (fs, ILs) where the distance ILs - ILc between a reference point Pc (fs, ILc) on the straight line L1 and the specific point Ps (fs, ILs) is 4.5 dB or more. Since the distance ILs - ILc where ILs - ILc > 0 may be calculated due to measurement errors or the like, the point (f, IL) at which the distance ILs - ILc, which is the error level, is obtained is not an anti-resonance point. The point (f, IL) where the distance ILs - ILc is less than 4.5 dB is not the specific point Ps (fs, ILs), and thus is not the anti-resonance point of this specific example. In the silencer 1 of this specific example, the frequency fs of the specific point Ps (fs, ILs) that is the anti-resonance point is between 500 and 2000 Hz.
[0035] FIGS. 6 and 7 are semi-logarithmic graphs showing the difference in the measurement results of the insertion loss characteristics depending on the presence or absence of the fiber structure layer 10. When the test was conducted, as shown in FIGS. 6 and 7, no anti-resonance point appeared in the silencer using a felt layer formed of felt in which the fibers were randomly oriented instead of the fiber structure layer 10, and an anti-resonance point appeared between 500 and 2000 Hz in the silencer 1 using the fiber structure layer 10. This is presumably because the fiber structure layer 10 has a fiber structure 13 in which the fibers are oriented in the thickness direction D3, and thus is highly elastic and highly viscous in the thickness direction D3, vibration is easily transmitted to the fiber structure layer 10, and anti-resonance is likely to occur in the silencer 1. In this specific example, the fiber structure layer 10 is used in the silencer 1, the basis weight of the surface layer 20 is 250 to 2000 g / m 2 and the basis weight of the fiber structure layer 10 is 400 to 1200 g / m 2By setting the thickness T10 of the fiber structure layer 10 to 8 to 25 mm, an anti-resonance point is generated between 500 and 2000 Hz. This effectively reduces noise of about 500 to 2000 Hz generated by running vehicles such as electric cars, exceeding the mass law.
[0036] 12, the central frequency fs of the anti-resonance point increases when the adhesive strength of the sound-insulating layer 30 to the fiber structure layer 10 is increased, and the central frequency fs of the anti-resonance point decreases when the adhesive strength of the sound-insulating layer 30 to the fiber structure layer 10 is decreased. Here, the adhesive strength is defined as the measured value (N / 50 mm) when the surface layer 20 is pulled under the test conditions of JIS (Japanese Industrial Standards) K6854-2:1999 (Adhesives-Test method for peel adhesion strength-Part 2: 180 degree peeling) with a test piece width of 50 mm, a test piece length of 200 mm, a test piece total thickness of 10 mm, a tensile speed of 20 mm / min, a gap between the upper and lower grippers of 100 mm, and a test temperature of 23°C±2°C. When the surface layer 20 peels off at the interface between the fiber structure layer 10 and the sound insulation layer 30, the adhesive strength is the arithmetic mean value of the peel strengths of the surface layer 20 against the pulling distance, excluding the maximum and minimum peaks. When the test piece breaks, the adhesive strength is equal to or greater than the maximum peak of the peel strength of the surface layer 20 against the pulling distance.
[0037] 2, 3A, and 3B, the adhesive strength in the width direction D2 perpendicular to the lamination direction D1 of the web M1 is higher than the adhesive strength in the lamination direction D1. In this specific example, the adhesive strength in the width direction D2 is used to adjust the central frequency fs of the anti-resonance point. Fig. 12 shows that the adhesive strength in the width direction D2 of the sound insulation layer 30 to the fiber structure layer 10 is 8.5 N / 50 mm or more in 180-degree peeling of a test piece width of 50 mm.
[0038] Furthermore, as shown in the simulation results in Fig. 13, increasing the compressive elastic modulus (Young's modulus) of the fiber structure layer 10 increases the center frequency fs of the anti-resonance point, and decreasing the compressive elastic modulus of the fiber structure layer 10 decreases the center frequency fs of the anti-resonance point. Here, the compressive elastic modulus is the compressive elastic modulus obtained in accordance with JIS L1913:2010 (general nonwoven fabric testing method). Fig. 13 shows that the compressive elastic modulus of the fiber structure layer 10 is 30 to 300 kPa.
[0039] (3) Specific examples of manufacturing methods for vehicle silencers: Fig. 5 shows a schematic example of a method for manufacturing the vehicle silencer 1. The manufacturing method shown in Fig. 5 includes a setting step ST1 and a press molding step ST2 that is performed after the setting step ST1. 5 shows a press molding machine 200 suitable for press molding of the laminate material LM1 that becomes the silencer 1. In the press molding machine 200, an upper die 212 and a lower die 214 that constitute a press molding die 210 are provided so as to be able to approach and separate from each other. In FIG. 5, the upper die 212 is a die having a die surface aligned with the front surface 21, and the lower die 214 is a die having a die surface aligned with the second surface 12. Of course, the upper die 212 may have a die surface aligned with the second surface 12, and the lower die 214 may have a die surface aligned with the front surface 21.
[0040] First, a setting step ST1 is performed in which the laminate material LM1 is set in the press mold 210. In the laminate material LM1 shown in Fig. 5, a fiber structure 60 or 61 which becomes the fiber structure layer 10, a thermoplastic resin sheet 70 which becomes the sound insulation layer 30, and a fiber material 80 which becomes the fiber layer 40 are layered in this order from the second surface 12 toward the front surface 21. The fiber material 80 is a fibrous material such as a nonwoven fabric, and has air permeability. The fiber structures 60, 61 and the fiber material 80 contain a thermoplastic binder. The laminate material LM1 does not necessarily need to have the fiber material 80. The laminate material LM1 can be heated by radiant heating using an infra-heater (infrared heater), hot air heating using a suction heater (hot air circulation heater), a combination of these, etc. The laminate material LM1 may be heated before the laminate material LM1 is set in the press mold 210, or may be heated after the laminate material LM1 is set in the press mold 210 if the press mold 210 is provided with a heater. The heating temperature of the laminate material LM1 is a temperature higher than the melting point of the thermoplastic binder contained in the laminate material LM1, and can be, for example, about 110 to 200°C.
[0041] After the setting step ST1, a press molding step ST2 is performed in which the lower mold 214 and the upper mold 212 are brought close to each other to press-mold the laminate material LM1 in the thickness direction D3. The resin sheet 70 may be melted and partially impregnated into the fiber structure layer 10 and the fiber layer 40. The fiber structure layer 10 is formed from the fiber structure 60 or 61, the non-breathable sound insulation layer 30 is formed from the resin sheet 70, and the fiber layer 40 is formed from the fiber material 80. The sound insulation layer 30 is integrated with both the fiber structure layer 10 and the fiber layer 40. When the thermoplastic component in the laminate material LM1 solidifies, the uneven shape of the silencer 1 is maintained. The molded silencer 1 is cut into a product shape as necessary. The silencer 1 may be cut by a cutting machine (not shown). The cutting machine may be a cutting machine equipped with a cutting blade, a cutting machine that cuts by a water jet, or the like. The silencer 1 can also be cut by hand using a cutter.
[0042] (4) Examples and simulations: The present invention will be specifically described below with reference to examples and simulation examples, but the present invention is not limited to the following examples.
[0043] [Example 1] The fiber structure 60 has a corrugated fiber structure 62 including PET fiber (main fiber 65), remnant fiber (main fiber 65), and low melting point PET fiber (adhesive fiber 66) (weight: 800 g / m 2The weight ratio of the PET fiber to the regenerated fiber was 1:1. The resin sheet 70 was a PE resin sheet (weight 800 g / m 2 The fiber material 80 was a needle-punched nonwoven fabric (200 g / m2) made of PET fiber containing low-melting-point PET fiber. 2 ) was used. A laminated material LM1 in which the fiber structure 60, the resin sheet 70, and the fiber material 80 are layered in this order was heated and press molded to produce a silencer sample having a thickness of 13 mm. The thickness T10 of the fiber structure layer 10 was 11 mm, and the basis weight of the fiber structure layer 10 was 800 g / m 2 The sound-insulating layer 30 has a basis weight of 800 g / m 2 The fiber layer 40 has a basis weight of 200 g / m 2 It is.
[0044] [Comparative Example 1] Instead of the fiber structure 60, a felt (basis weight 800 g / m) in which PET fibers including low melting point PET fibers are oriented perpendicular to the thickness direction D3 is used. 2 A silencer sample having a thickness of 13 mm was produced in the same manner as in Example 1, except that a felt layer having a thickness of 11 mm and a weight per unit area of 800 g / m 2 The sound-insulating layer 30 has a basis weight of 800 g / m 2 The fiber layer 40 has a basis weight of 200 g / m 2 It is.
[0045] [Example 2] The fiber structure 60 has a corrugated fiber structure 62 including PET fiber (main fiber 65), remnant fiber (main fiber 65), and low melting point PET fiber (adhesive fiber 66). 2 The weight ratio of the PET fiber to the regenerated fiber was 1:1. The resin sheet 70 was a PE resin sheet (weight per unit area: 500 g / m 2 The fiber material 80 was a needle-punched nonwoven fabric made of PET fiber containing low-melting-point PET fiber (weight: 230 g / m 2 ) was used. A laminated material LM1 in which the fiber structure 60, the resin sheet 70, and the fiber material 80 are layered in this order is heated and press-molded to produce a silencer sample having a thickness of 23 mm. The thickness T10 of the fiber structure layer 10 is 20 mm, and the basis weight of the fiber structure layer 10 is 1200 g / m 2 The sound-insulating layer 30 has a basis weight of 500 g / m 2 The fiber layer 40 has a basis weight of 230 g / m 2 It is.
[0046] [Comparative Example 2] Instead of the fiber structure 60, a felt (basis weight 1100 g / m) in which PET fibers including low melting point PET fibers are oriented perpendicular to the thickness direction D3 is used. 2 A silencer sample having a thickness of 23 mm was produced in the same manner as in Example 2, except that a felt layer having a thickness of 20 mm and a weight per unit area of 1100 g / m 2 The sound-insulating layer 30 has a basis weight of 500 g / m 2 The fiber layer 40 has a basis weight of 230 g / m 2 It is.
[0047] 6 is a semi-logarithmic graph showing the insertion loss characteristics of Example 1 and Comparative Example 1. FIG. 7 is a semi-logarithmic graph showing the insertion loss characteristics of Example 2 and Comparative Example 2. 6, the graph of Example 1 has a peak at 1600 Hz, the specific point Ps(fs,ILs) is (1600,19.82), the first surrounding point Pa(fa,ILa) is (500,-6.32), and the second surrounding point Pb(fb,ILb) is (2500,19.45). Therefore, the insertion loss ILc of the reference point Pc(fs,ILc) of the straight line L1 passing through Pa and Pb is -6.32+(19.45+6.32)×(5 / 7)=12.09 dB, and the distance ILs-ILc is 7.4 dB. 7, the graph of Example 2 has a peak at 630 Hz, the specific point Ps(fs,ILs) is (630,14.74), the first surrounding point Pa(fa,ILa) is (315,-3.76), and the second surrounding point Pb(fb,ILb) is (1000,12.66). Therefore, the insertion loss ILc of the reference point Pc(fs,ILc) is -3.76+(12.66+3.76)×(3 / 5)=6.09 dB, and the distance ILs-ILc is 6.6 dB. From the above, it has been shown that a silencer 1 including a fiber structure layer 10 having a fiber structure 13 in which fibers are oriented in the thickness direction D3 reduces noise in the range of 500 to 2000 Hz beyond the mass law by generating anti-resonance in the range of 500 to 2000 Hz.
[0048] On the other hand, there is no specific point Ps(fs,ILs) where the distance ILs-ILc is 4.5 dB or more in the graphs of Comparative Examples 1 and 2. This indicates that if the silencer does not have a fiber structure layer 10 having a fiber structure 13 in which fibers are oriented in the thickness direction D3, anti-resonance does not occur between 500 and 2000 Hz, and sound absorption performance exceeding the mass law cannot be obtained. As described above, it has been confirmed that a silencer 1 including a fiber structure layer 10 having a fiber structure 13 in which fibers 64 are oriented in the thickness direction D3 exhibits sound absorption performance that exceeds the mass law for noise in the range of 500 to 2000 Hz.
[0049] [Example 3] The surface layer 20 has a basis weight of 480g / m 2 (Test area 1), 730 g / m 2 (Test area 2), 1000g / m 2 (Test area 3), 1200g / m 2 (Test area 4), 1600g / m 2 (Test area 5), 2600g / m 2 (Comparative test area 6), 3200g / m 2 (Comparative Test Area 7) and the insertion loss characteristics were measured. The fiber structure 60 has a corrugated fiber structure 62 including PET fiber (main fiber 65), remnant fiber (main fiber 65), and low melting point PET fiber (adhesive fiber 66) (weight: 800 g / m 2 The weight ratio of PET fiber to regenerated fiber was 1:1. The resin sheet 70 in the test area 1 was a PE resin sheet (basis weight 250 g / m 2 For the resin sheet 70 in the test area 2, a PE resin sheet (basis weight 500 g / m 2 The fiber material 80 in the test areas 1 and 2 was a needle-punched nonwoven fabric made of PET fiber containing low-melting-point PET fiber (basis weight 230 g / m 2 For the resin sheet 70 in the test area 3, a PE resin sheet (basis weight 800 g / m 2 For the resin sheet 70 in test area 4, a PE resin sheet (1000 g / m 2 The fiber material 80 in test areas 3 and 4 was a needle-punched nonwoven fabric made of PET fiber containing low-melting-point PET fiber (basis weight 200 g / m 2 For the resin sheet 70 in test area 5, a PVC resin sheet (basis weight 1600 g / m 2 For the resin sheet 70 in test area 6, a PVC resin sheet (weight 2600 g / m 2 For the resin sheet 70 in test area 7, a PVC resin sheet (basis weight 3200 g / m 2 In test plots 5 to 7, fiber material 80 was not used.
[0050] A laminated material LM1 in which the fiber structure 60, the resin sheet 70, and the fiber material 80 were layered in this order was heated and press molded to produce silencer samples. The thickness of the silencer samples in test plots 1, 2, and 4 was 15 mm, the thickness T10 of the fiber structure layer 10 in test plots 1, 2, and 4 was 12 mm, the thickness of the silencer samples in test plots 3, 5, 6, and 7 was 10 mm, and the thickness T10 of the fiber structure layer 10 in test plots 3, 5, 6, and 7 was 8 mm. The basis weight of the fiber structure layer 10 was 800 g / m 2 and the basis weight of the surface layer 20 is as described above.
[0051] 8 is a semi-logarithmic graph showing the insertion loss characteristics of test plots 1, 2, and 4 of Example 3. FIG. 9 is a semi-logarithmic graph showing the insertion loss characteristics of test plots 3, 5, 6, and 7 of Example 3. In the graphs of test plots 1, 2, and 4 shown in FIG. 8, there is a peak at 800 Hz, and in the graph of test plot 3 shown in FIG. 9, there is a peak at 1000 Hz. 2 The distance ILs-ILc in test plots 1 to 4 is 4.5 dB or more. The surface layer 20 has a basis weight of 1600g / m 2 In the graph of test area 5 (see Figure 9), there is a specific point Ps(fs,ILs)=(800,11.18) at 800Hz. The first surrounding point Pa(fa,ILa) is (500,-4.70), and the second surrounding point Pb(fb,ILb) is (1250,12.11). Therefore, the insertion loss ILc of the reference point Pc(fs,ILc) of the straight line L1 passing through Pa and Pb is -4.70+(12.11+4.70)×(2 / 4)=3.71dB, and the distance ILs-ILc is 7.5dB. The surface layer 20 has a basis weight of 2600g / m 2 In the graphs of the comparative test plots 6 and 7 (see FIG. 9) described above, there is no specific point Ps(fs, ILs) where the distance ILs-ILc is 4.5 dB or more. Although not shown in Figs. 8 and 9, the surface layer 20 has a basis weight of 2000 g / m 2 In this case, the distance ILs-ILc is 4.5 dB or more.
[0052] [Simulation example] The compression modulus (Young's modulus) of the fiber structure layer 10 was changed to 30 kPa (Test 1), 65 kPa (Test 2), 130 kPa (Test 3), and 300 kPa (Test 4) to simulate the insertion loss characteristics. The fiber structure layer 10 had a basis weight of 600 g / m 2 The surface layer 20 has a basis weight of 250 g / m 2 It is.
[0053] 13 is a semi-logarithmic graph showing the simulation results of the insertion loss characteristics according to the compressive modulus of the fiber structure layer 10. The graph for test area 1, where the compressive modulus is 30 kPa, has a peak at 500 Hz, the graph for test area 2, where the compressive modulus is 65 kPa, has a peak at 800 Hz, the graph for test area 3, where the compressive modulus is 130 kPa, has a peak at 1000 Hz, and the graph for test area 4, where the compressive modulus is 300 kPa, has a peak at 1600 Hz. In test areas 1 to 4, the surface layer 20 had a basis weight of 250 g / m 2 Even if the compression modulus is 100, the noise level between 500 and 2000 Hz is reduced beyond the mass law by the occurrence of a clear peak between 500 and 2000 Hz as the anti-resonance point. It can also be seen that the higher the compression modulus, the higher the center frequency fs of the specific point Ps(fs,ILs), and the lower the compression modulus, the lower the center frequency fs of the specific point Ps(fs,ILs). Therefore, it is presumed that the center frequency fs of the anti-resonance point can be adjusted by adjusting the compression modulus.
[0054] [Example 4] The fiber structure layer 10 has a basis weight of 400 g / m 2 (Test area 1), 600 g / m 2 (Test area 2), 800g / m 2 (Test area 3), 1000g / m 2 (Test area 4), 1200g / m 2 (Test area 5) and the insertion loss characteristics were measured. The fiber structure 60 used had a corrugated fiber structure 62 including PET fibers (main fibers 65), revert fibers (main fibers 65), and low melting point PET fibers (adhesive fibers 66). The weight ratio of the PET fibers to the revert fibers was 1:1. The fiber structure 60 had a basis weight as described above. The resin sheet 70 used was a PE resin sheet (basis weight 500 g / m 2 The fiber material 80 was a needle-punched nonwoven fabric made of PET fiber containing low-melting-point PET fiber (weight: 230 g / m 2 ) was used.
[0055] A laminated material LM1, in which the fiber structure 60, the resin sheet 70, and the fiber material 80 are layered in this order, was heated and press molded to produce a silencer sample having a thickness of 15 mm. The thickness T10 of the fiber structure layer 10 was 12 mm, the basis weight of the fiber structure layer 10 was as described above, and the basis weight of the sound insulation layer 30 was 500 g / m 2 The fiber layer 40 has a basis weight of 230 g / m 2 It is.
[0056] 10 is a semi-logarithmic graph showing the insertion loss characteristics of test plots 1 to 5 in Example 4. The graph for test plot 1 has a peak at 630 Hz, and the graphs for test plots 2 to 5 have a peak at 800 Hz. 2 The distance ILs-ILc in test plots 1 to 5 is 4.5 dB or more.
[0057] [Example 5] The thickness T10 of the fiber structure layer 10 was changed to 8 mm (test section 1), 12 mm (test section 2), 16 mm (test section 3), 20 mm (test section 4), and 25 mm (test section 5), and the insertion loss characteristics were measured. The fiber structure 60 has a corrugated fiber structure 62 including PET fiber (main fiber 65), remnant fiber (main fiber 65), and low melting point PET fiber (adhesive fiber 66) (weight: 800 g / m 2 The weight ratio of the PET fiber to the regenerated fiber was 1:1. The resin sheet 70 was a PE resin sheet (weight 800 g / m 2 The fiber material 80 was a needle-punched nonwoven fabric (200 g / m2) made of PET fiber containing low-melting-point PET fiber. 2 ) was used.
[0058] A laminated material LM1, in which the fiber structure 60, the resin sheet 70, and the fiber material 80 were layered in this order, was heated and press-molded to produce a silencer sample. The thicknesses of the silencer samples in test plots 1, 2, 3, 4, and 5 were 11 mm, 15 mm, 19 mm, 23 mm, and 28 mm, respectively. The thickness T10 of the fiber structure layer 10 in test plots 1 to 5 was as described above. The basis weight of the sound-insulating layer 30 was 800 g / m2 The fiber layer 40 has a basis weight of 200 g / m 2 It is.
[0059] 11 is a semi-logarithmic graph showing the insertion loss characteristics of test plots 1 to 5 of Example 5. The graph for test plot 1 has a peak at 1000 Hz, the graphs for test plots 2 and 3 have a peak at 800 Hz, and the graphs for test plots 4 and 5 have a peak at 630 Hz. The distance ILs-ILc of test plots 1 to 5, in which the thickness T10 of the fiber structure layer 10 is 8 to 25 mm, is 4.5 dB or more.
[0060] As described above, it is required to effectively reduce noise of about 500 to 2000 Hz generated by running an electric vehicle in a limited space. When the fiber structure layer 10 has a fiber structure 13 in which the fibers are oriented in the thickness direction D3, the weight of the surface layer 20 is set to 250 to 2000 g / m 2 The fiber structure layer 10 has a basis weight of 400 to 1200 g / m 2 By setting the thickness T10 of the fiber structure layer 10 to 8 to 25 mm, it is possible to easily obtain a silencer 1 having a center frequency fs between 500 and 2000 Hz, which indicates the anti-resonance point where the distance ILs-ILc is 4.5 dB or more. Therefore, it was confirmed from Examples 1 to 5 and the simulation example that the above-mentioned silencer 1 can effectively reduce noise of about 500 to 2000 Hz generated by the running of a vehicle.
[0061] [Example 6] The adhesive strength of the sound-insulating layer 30 to the fiber structure layer 10 in the width direction D2 perpendicular to the lamination direction D1 of the web M1 (180-degree peeling with a test piece width of 50 mm) was changed to 8.5 N / 50 mm (test section 1), 24.0 N / 50 mm (test section 2), 87.6 N / 50 mm or more (test section 3), and 100.0 N / 50 mm or more (test section 4), and the insertion loss characteristics were measured. As a comparative test section 5, the insertion loss characteristics of a silencer sample in which the sound-insulating layer 30 was not adhered to the fiber structure layer 10 was also measured. The fiber structure 60 has a corrugated fiber structure 62 including PET fiber (main fiber 65), remnant fiber (main fiber 65), and low melting point PET fiber (adhesive fiber 66) (weight: 800 g / m 2 The weight ratio of the PET fiber to the regenerated fiber was 1:1. The resin sheet 70 was a PE resin sheet (weight 800 g / m 2 The fiber material 80 was a needle-punched nonwoven fabric (200 g / m2) made of PET fiber containing low-melting-point PET fiber. 2 ) was used.
[0062] In test section 1, a surface layer 20 in which a fiber layer 40 was bonded to a sound-insulating layer 30 was prepared, and the sound-insulating layer 30 of the surface layer 20 was bonded to the fiber structure layer 10 by spraying a liquid adhesive. In test sections 2 to 4, a laminate material LM1 in which a fiber structure 60, a resin sheet 70, and a fiber material 80 were layered in this order was heated and press-molded to prepare silencer samples. In test section 3, the heating temperature before press molding was set higher than in test section 2 in order to increase the adhesive strength compared to test section 2. In test section 4, the heating temperature before press molding was set higher than in test section 3 in order to increase the adhesive strength compared to test section 3. The thickness of the silencer sample was 11 mm, the thickness T10 of the fiber structure layer 10 was 8 mm, and the basis weight of the fiber structure layer 10 was 800 g / m 2 The sound-insulating layer 30 has a basis weight of 800 g / m 2 The fiber layer 40 has a basis weight of 200 g / m 2 It is.
[0063] 12 is a semi-logarithmic graph showing the insertion loss characteristics of test sections 1 to 5 of Example 6. The graph of test section 1, where the adhesive strength is 8.5 N / 50 mm, has a peak at 800 Hz, the graph of test section 2, where the adhesive strength is 24.0 N / 50 mm, has a peak at 1600 Hz, the graph of test section 3, where the adhesive strength is 87.6 N / 50 mm or more, has a specific point Ps (1600, 19.44) where the distance ILs-ILc is 4.5 dB or more, and the graph of test section 4, where the adhesive strength is 100.0 N / 50 mm or more, has a specific point Ps (2000, 22.81) where the distance ILs-ILc is 4.5 dB or more. The distance ILs-ILc of test sections 1 to 4, where the adhesive strength is 8.5 N / 50 mm or more, is 4.5 dB or more. In the graph for Comparative Test Area 5, there is no specific point Ps(fs, ILs) where the distance ILs-ILc is 4.5 dB or more. From the test sections 1 to 4, it can be seen that the higher the adhesive strength, the higher the center frequency fs of the specific point Ps (fs, ILs), and the lower the adhesive strength, the lower the center frequency fs of the specific point Ps (fs, ILs). Therefore, it was found that the center frequency fs of the anti-resonance point can be adjusted by adjusting the adhesive strength.
[0064] (5) Conclusion: As described above, according to the present invention, it is possible to provide a technology such as a vehicle silencer that can effectively reduce noise of about 500 to 2000 Hz generated by the running of a vehicle through various aspects. Of course, even if the technology is composed only of the constituent elements according to the independent claims, the basic actions and effects described above can be obtained. In addition, configurations in which the configurations disclosed in the above examples are substituted with each other or the combination is changed, configurations in which the configurations disclosed in the publicly known techniques and the above examples are substituted with each other or the combination is changed, etc. The present invention also includes these configurations. [Explanation of symbols]
[0065] 1…silencer, 10... fiber structure layer, 11... first surface, 12... second surface, 13... fiber structure, 20...surface layer, 21...surface, 30...sound insulation layer, 31...third surface, 40...fiber layer, 41...fiber, 42...binder, 60, 61... fiber structure, 60a... surface, 60b... back surface, 62... fiber structure, 64...fiber, 65...main fiber, 66...adhesive fiber (example of thermoplastic binder), 70: Resin sheet, 80: Fiber material, 100... automobile, 110... panel, 111... surface, 120... battery unit, D1: stacking direction, D2: width direction, D3: thickness direction, L1...straight line, M1...web, M2...fold.
Claims
1. A silencer for a vehicle that is disposed in contact with a surface of a panel, a fibrous structure layer having a first surface opposite the panel and a second surface adjacent to a surface of the panel; a surface layer having at least a non-breathable sound insulating layer adhered to the first surface; The fiber structure layer has air permeability and a fiber structure in which fibers are oriented in a thickness direction, The surface layer has a basis weight of 250 to 2000 g / m 2 and The fiber structure layer has a basis weight of 400 to 1200 g / m 2 and The thickness of the fiber structure layer is 8 to 25 mm; This vehicle silencer is a vehicle silencer in which, in a graph with a 1 / 3 octave band center frequency f (Hz) on a logarithmic scale on the horizontal axis and insertion loss IL (dB) on the vertical axis, a specific point (fs, ILs) that is upwardly convex is included among a plurality of points (f, IL) connected by a broken line, fa<fs<fb, and the broken line is tangent to a first peripheral point (fa, ILa) and a second peripheral point (fb, ILb) that are downwardly convex, and the distance ILs-ILc between a reference point (fs, ILc) on the line and the specific point (fs, ILs) is 4.5 dB or more, and fs is between 500 and 2000 Hz.
2. The fiber structure has a structure in which webs are repeatedly stacked in a stacking direction along the first surface, 2. The vehicle silencer according to claim 1, wherein an adhesive strength of the sound-insulating layer to the fiber structure layer in a width direction perpendicular to the lamination direction is 8.5 N / 50 mm or more in a 180 degree peel test using a test piece having a width of 50 mm.
3. 3. The vehicle silencer according to claim 1, wherein the surface layer further includes a fiber layer having breathability, containing fibers and a binder, and adhered to a third surface of the sound-insulating layer opposite the fiber structure layer.
Citation Information
Patent Citations
Ultralightweight soundproof material
JP2005227747A
Soundproof material for vehicle
JP2012192751A
Molded laying interior material for vehicle
JP2011173446A