Polishing pad
The polishing pad with optimized abrasive grains and binder composition addresses the challenge of high-pressure polishing by enhancing efficiency and reducing wear, thereby shortening production lead times and costs.
Patent Information
- Application Number
- JP2023052884
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional polishing pads face challenges in achieving high polishing rates without increasing wear and frequency of replacement, leading to longer production lead times and higher costs under high pressure conditions.
A polishing pad with a base material, abrasive grains, and a binder, featuring a polishing layer with specific properties such as a coefficient of dynamic friction of 1.0 or more, abrasive grain sizes between 20 μm and 600 μm, and optimized content of abrasive grains and fillers, enhances polishing efficiency.
The polishing pad achieves improved polishing rates under predetermined pressure, reducing wear and frequency of replacement, thus shortening production lead times and lowering costs.
Smart Images

Figure 2024141307000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad. [Background technology]
[0002] Polishing pads are known that are used as abrasives attached to polishing devices for polishing glass, semiconductors, ceramics, electronic component boards, etc. For example, Patent Document 1 describes a polishing pad for polishing semiconductors, which has a strength of 20 gf / cm 2 Under this pressure, the kinetic friction coefficient μ0 against the silicon oxide film is 0.1 to 0.4, and the kinetic friction coefficient μ N A polishing pad having a surface roughness of 0.5 to 0.7 is disclosed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2021-065619 Summary of the Invention [Problem to be solved by the invention]
[0004] In order to shorten production lead times, polishing using a polishing device may require a large amount of processing in a short time, i.e., a high polishing rate, and therefore there is a demand for the development of polishing pads that can achieve a higher polishing rate.
[0005] In order to improve the polishing rate, it is possible to perform polishing by increasing the pressure at the contact surface between the object to be polished and the polishing pad. However, when polishing is performed under high pressure, the amount of wear on the polishing pad increases, and the frequency of replacing the polishing material increases. As a result, the increase in internal setup required for replacing the polishing material may actually lengthen the production lead time. In addition, the increase in the frequency of replacing the polishing material also leads to an increase in production costs.
[0006] Therefore, an object of the present invention is to provide a polishing pad having an excellent polishing rate under a predetermined pressure. That is, in a polishing process under the same pressure, the polishing pad of the present invention can achieve a higher polishing rate than a conventional polishing pad. [Means for solving the problem]
[0007] (1) The polishing pad of the present invention has a substrate and a polishing layer containing abrasive grains and a binder and laminated on the substrate, and the glass and the polishing layer have a surface roughness of 20 gf / cm 2 When the glass or the polishing layer moves at a uniform velocity in a straight line on the contact surface between the glass and the polishing layer in a state of contact with each other at a pressure of 1.0 or more, the average value of the dynamic friction coefficient for 0.8 seconds from 0.2 seconds to 1.0 second after the start of the uniform velocity in a straight line motion is 1.0 or more. According to the polishing pad described in (1) above, it is possible to achieve an excellent polishing rate in polishing processing under a specified pressure.
[0008] (2) The polishing pad according to (1), wherein the abrasive grains have a median diameter of 20 μm or more and 600 μm or less.
[0009] (3) The polishing pad according to (1) or (2), wherein the content of abrasive grains in the polishing layer is 0.05 volume % or more and less than 20.0 volume %.
[0010] (4) The polishing pad according to any one of (1) to (3), wherein the abrasive grains are diamond abrasive grains.
[0011] According to the polishing pads described in (2) to (4) above, a superior polishing rate can be achieved in polishing under a predetermined pressure.
[0012] (5) The polishing pad according to any one of (1) to (4), wherein the polishing layer further contains a filler.
[0013] (6) The polishing pad according to (5), wherein the filler is an inorganic oxide and the binder is a resin.
[0014] According to the polishing pads described in (5) and (6) above, the polishing rate in polishing under a specified pressure and the wear amount of the polishing pad are further improved.
[0015] (7) The polishing pad according to any one of (1) to (6), wherein the polishing layer is composed of a plurality of polishing portions. According to the polishing pad described in (7) above, it is possible to achieve a more excellent polishing rate under a specified pressure.
[0016] (8) The polishing pad according to any one of (1) to (7), which is used for polishing glass. The polishing pad described in (8) above can be suitably used in polishing glass, which requires a high polishing rate. Effect of the Invention
[0017] According to the present invention, it is possible to improve the polishing rate in polishing under a predetermined pressure, as compared with the conventional case, which results in a reduction in production lead time and production costs. [Brief description of the drawings]
[0018] [Figure 1] 1 is a cross-sectional view showing a schematic view of a portion of an abrasive 10. FIG. [Diagram 2] 2 is a surface view showing a schematic view of a portion of a first surface 21 of a polishing pad 11. FIG. [Diagram 3] FIG. 1 is a schematic diagram of a surface property tester 1000. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0020] FIG. 1 is a cross-sectional view showing a schematic view of a part of the polishing material 10. As shown in FIG. 1, the polishing material 10 is composed of a polishing pad 11 and a support 12 laminated together. The polishing material 10 is attached to a polishing device equipped with a rotary drive device and used to polish a plate material. The polishing device is not particularly limited as long as it is a known polishing device, including a double-sided polishing machine and a single-sided polishing machine. The polishing pad 11 has a plurality of convex polishing parts 23. In this embodiment, each polishing part 23 of the polishing pad 11 is configured to have abrasive grains 24, a filler 26, and a binder 25. The filler 26 is an optional component, and the polishing part 23 may be configured not to include the filler 26. Examples of the material of the plate material to be polished include metal, resin, silicon, silicon carbide, glass, and sapphire. The polishing material 10 of this embodiment can be suitably used in a glass polishing process that requires a high polishing rate.
[0021] The polishing process using the above-mentioned polishing apparatus is performed in a state where the polishing material 10 is in contact with the above-mentioned plate material at a predetermined pressure (hereinafter, may be referred to as "polishing pressure"). The area where the polishing pad 11 of the polishing material 10 and the plate material are in contact with each other is the polishing region. In the polishing region, the polishing pad 11 and the plate material are in contact with each other at a predetermined pressure (hereinafter, may be referred to as "polishing pressure"). The polishing apparatus has a mechanism for adjusting the polishing pressure. The polishing pressure may be adjusted appropriately depending on the polishing process, and is not particularly limited, but is preferably 10 gf / cm. 2 More than 400gf / cm 2 The polishing pressure is preferably 10 gf / cm or less. 2 If the polishing pressure is 400 gf / cm or more, the polishing rate in the polishing process can be secured. 2 If it is equal to or less than this, the amount of wear of the polishing pad 11 is suppressed, and the frequency of replacing the abrasive 10 can be reduced.
[0022] 1, the abrasive 10 includes a first adhesive layer 13 and a second adhesive layer 14. The first adhesive layer 13 bonds a second surface 22, which is the back surface of the polishing pad 11, to a front surface 16 of the support 12. The second adhesive layer 14 bonds a back surface 17 of the support 12 to a platen SP of a polishing device. The polishing pad 11 includes a base material 20 and a plurality of polishing portions 23 provided on a first surface 21, which is the front surface of the base material 20. The polishing portions 23 on the first surface 21 constitute a polishing layer of the polishing pad 11.
[0023] When the plate material to be polished is glass, the polishing pressure is 20gf / cm 2 The average value of the dynamic friction coefficient in the polishing region under the above conditions is 1.0 or more. The dynamic friction coefficient is the dynamic friction coefficient when the plate material or the polishing layer moves linearly at a constant speed on the contact surface between the plate material and the polishing layer. The average value of the dynamic friction coefficient is the average value of the dynamic friction coefficient for 0.8 seconds from 0.2 seconds to 1.0 seconds after the start of the uniform linear motion. The polishing pad 11 having the average dynamic friction coefficient of 1.0 or more has an excellent polishing rate. The average value of the dynamic friction coefficient is preferably 1.5 to 4.0. The polishing material 10 having the polishing pad 11 having the average dynamic friction coefficient of 1.5 or more can meet the demand for a high polishing rate in the polishing of glass. The polishing material 10 having the polishing pad 11 having the average dynamic friction coefficient of 4.0 or less can precisely adjust the polishing amount of the plate material in the polishing process.
[0024] FIG. 2 is a surface view showing a schematic view of a part of the first surface 21 of the polishing pad 11 as viewed from the direction of the arrow A in FIG. 1. As shown in FIG. 2, a plurality of polishing parts 23 are uniformly scattered along the first surface 21. This improves the uniformity of the polishing pressure in the polishing region. Therefore, the flattening accuracy in the polishing process is improved. As shown in FIG. 1, the polishing layer is composed of these polishing parts 23. The average thickness of the polishing layer is preferably 500 μm or more and 2000 μm or less, and particularly preferably 800 μm or more and 1500 μm or less. If the average thickness of the polishing layer is 500 μm or more, particularly 800 μm or more, the frequency of replacing the polishing material 10 due to wear of the polishing layer in the polishing process can be reduced. If the average thickness of the polishing layer is 2000 μm or less, particularly 1500 μm or less, the load applied to the interface between the polishing parts 23 and the substrate 20 during the polishing process can be reduced. This suppresses the occurrence of breakage of the polishing parts 23, and improves the durability of the polishing pad 11. The average thickness of the polishing layer is synonymous with the average height of the polishing portion 23.
[0025] The polishing portion 23 includes abrasive grains 24. The polishing material 10 rotates and polishes the surface of the plate material to be polished. The polishing layer of the polishing material 10 slides against the surface of the plate material in the above-mentioned polishing region. The polishing layer of this embodiment is composed of a plurality of convex polishing portions 23, but is not limited thereto. For example, the polishing layer can be composed of a polishing portion 23 that covers the entire first surface 21. From the viewpoint of achieving a better polishing rate, it is preferable that the polishing layer is composed of a plurality of polishing portions 23. D shown in FIG. 2 indicates the minimum distance between adjacent polishing portions 23. Each minimum distance D is approximately the same. In addition, when any one polishing portion 23 is taken as the center, the central polishing portion 23 is surrounded by five adjacent polishing portions 23. This further improves the uniformity of the polishing pressure in the above-mentioned polishing region. As a result, the polishing material 10 of this embodiment can achieve a better polishing rate in polishing processing.
[0026] The minimum distance D is not particularly limited, but is preferably 0.3 mm or more and 2.5 mm or less, and particularly preferably 0.5 mm or more and 2.0 mm or less. If the minimum distance D is 0.3 mm or more, particularly 0.5 mm or more, the flattening accuracy in the polishing process can be improved. If the minimum distance D is 2.5 mm or less, particularly 2.0 mm or less, the area of the polishing layer on the first surface 21 (hereinafter, sometimes referred to as the "occupied area") can be secured. The occupied area is synonymous with the sum of the top surface areas of the polishing parts 23 present on the first surface 21. The ratio of the occupied area to the first surface 21 (hereinafter, sometimes referred to as the "occupied area ratio") is preferably 20% or more and 60% or less, and particularly preferably 30% or more and 50% or less. If the occupied area ratio is 20% or more, particularly 30% or more, the contact area between the top surface of the polishing part 23 and the plate material in the above-mentioned polishing region can be secured. If the occupied area ratio is 60% or less, particularly 50% or less, the polishing pressure is sufficiently concentrated on the occupied area. As a result, the abrasive material 10 of this embodiment can achieve a superior polishing rate in polishing. The average area of the top surface of one abrasive portion 23 is 6 mm 2 More than 100mm 2 Less than 8mm is preferable 2 More than 30mm 2 The following is particularly preferred: The average area of the top surface of the polishing portion 23 is 6 mm 2 Above, especially 8mm 2 If the average area of the top surface of the polishing portion 23 is 100 mm or more, the occurrence of breakage of the polishing portion 23 can be suppressed, and the durability of the polishing pad 11 can be improved. 2 Below, especially 30mm 2 If it is equal to or less than this, the polishing pressure is sufficiently concentrated on the top surface of the polishing portion 23. As a result, the abrasive 10 of this embodiment can achieve a superior polishing rate in polishing processing.
[0027] <About each part of the abrasive 10> [Base material 20] The substrate 20 of the polishing pad 11 is not particularly limited, but examples thereof include polycarbonate, polyethylene terephthalate, polypropylene, polyethylene, polyimide, polyethylene naphthalate, aramid, aluminum, and copper. The average thickness of the substrate 20 in this embodiment is preferably 0.1 mm or more and 3.0 mm or less, and particularly preferably 0.3 mm or more and 1.0 mm or less. If the average thickness of the substrate 20 is 0.5 mm or more, particularly 0.3 mm or more, the strength and flatness of the polishing pad 11 can be ensured. If the average thickness of the substrate 20 is 3 mm or less, particularly 1.0 mm or less, the handleability of the polishing pad 11 can be improved.
[0028] [Polishing section 23 (polishing layer)] Each polishing portion 23 of the polishing pad 11 has abrasive grains 24, a filler 26, and a binder 25. The polishing portions 23 are provided so as to protrude from the first surface 21 of the substrate 20. Each polishing portion 23 is columnar, and in this embodiment, is cylindrical. The sizes of the polishing portions 23 may all be the same or may be different. In this embodiment, all the polishing portions 23 have the same shape and size.
[0029] (Grain 24) Examples of the abrasive grains 24 include diamond abrasive grains, alumina abrasive grains, silica abrasive grains, ceria abrasive grains, silicon carbide abrasive grains, and the like. The abrasive grains 24 preferably have a Mohs hardness of 8 or more, and diamond abrasive grains with a Mohs hardness of 10 are particularly preferred. Abrasive grains 24 with a Mohs hardness of 8 or more can achieve a better polishing rate in polishing with the polishing pad 11. If the abrasive grains 24 are diamond abrasive grains, they can meet the demand for a high polishing rate in polishing glass.
[0030] The median diameter of the abrasive grains 24 is 20 μm or more and 600 μm or less, and the median diameter is specifically measured by a laser diffraction method. Specifically, the median diameter is calculated by appropriately setting the particle refractive index, the dispersion solvent refractive index, the selection of whether the particles are spherical or non-spherical, and whether the particles are transparent or not, by using a laser diffraction particle size distribution meter (Microtrac MT3300EX II manufactured by Nikkiso Co., Ltd.) and performing wet measurement using water as a dispersion solvent or other dispersion solvent suitable for particle dispersion. If the median diameter of the abrasive grains 24 is 20 μm or more, a better polishing rate can be achieved. If the median diameter of the abrasive grains 24 is 600 μm or less, the abrasive grains 24 can be uniformly dispersed in the polishing portion 23, and the quality of the polishing pad 11 is stabilized. The median diameter of the abrasive grains 24 is preferably 30 μm or more and 450 μm or less. If the median diameter of the abrasive grains 24 is 30 μm or more, the demand for a high polishing rate in glass polishing can be met. If the median diameter of the abrasive grains 24 is 450 μm or less, the quality of the polishing pad 11 becomes more stable.
[0031] The content of the abrasive grains 24 contained in the polishing layer is 0.05 vol% or more and less than 20.0 vol%. If the content of the abrasive grains 24 contained in the polishing layer is 0.05 vol% or more, an excellent polishing rate can be realized and the amount of wear of the polishing pad in the polishing process can be reduced. This reduces the frequency of replacing the abrasive 10, improving the productivity of the polishing process and reducing the production cost. If the content of the abrasive grains 24 contained in the polishing layer is less than 20.0 vol%, an excellent polishing rate can be realized and the abrasive grains 24 can be uniformly dispersed in the polishing part 23. This stabilizes the quality of the polishing pad 11. The content of the abrasive grains 24 contained in the polishing layer is preferably 0.08 vol% or more and 13.0 vol% or less, particularly preferably 0.1 vol% or more and 10.0 vol% or less. The polishing pad 11 having the content of the abrasive grains 24 contained in the polishing layer of 0.08 vol% or more and 13.0 vol% or less can meet the demand for a high polishing rate in the polishing process. If the content of the abrasive grains 24 in the polishing layer of the polishing pad 11 is 0.1 volume % or more and 10.0 volume % or less, the demand for a higher polishing rate in polishing glass can be met. In addition, if the content of the abrasive grains 24 can be suppressed to 10.0 volume % or less, the cost of the polishing material 10 can be reduced.
[0032] (Filler 26) The filler 26 may be an organic or inorganic powder that is generally used as a filler for polishing pads, and is not particularly limited. An example of an organic powder is wood powder. An example of an inorganic powder is an inorganic oxide or a composite oxide. Examples of inorganic oxides include aluminum oxide, silica, cerium oxide, magnesium oxide, zirconia, and titanium oxide. Examples of composite oxides include silica-alumina, silica-zirconia, and silica-magnesia. The Mohs hardness of the filler 26 is preferably lower than the Mohs hardness of the abrasive grains 24. This can further reduce the interference of the filler 26 with the polishing force of the abrasive grains 24. As a result, the abrasive material 10 of this embodiment can achieve a better polishing rate in the polishing process. In addition, the polishing portion 23 containing the filler 26 has an improved elastic modulus of the binder 25, and a better polishing rate is achieved. As the filler 26, an inorganic oxide is preferable, and aluminum oxide is particularly preferable. The polishing pad 11 containing aluminum oxide as the filler 26 can meet the demand for a high polishing rate in the polishing of glass.
[0033] The median diameter of the filler 26 is preferably smaller than the median diameter of the abrasive grains 24. This reduces the interference of the filler 26 with the polishing force of the abrasive grains 24. As a result, the abrasive 10 of this embodiment can achieve a better polishing rate in the polishing process. The median diameter of the filler 26 is preferably 0.01 μm or more and less than 20 μm. If the median diameter of the filler 26 is 0.01 μm or more, the elastic modulus of the binder 25 is ensured. If the median diameter of the filler 26 is less than 20 μm, the interference of the filler 26 with the polishing force of the abrasive grains 24 is further reduced. This allows the abrasive 10 of this embodiment to achieve a further better polishing rate in the polishing process. The median diameter of the filler 26 is particularly preferably 2 μm or more and 15 μm or less. Polishing pad 11 containing filler 26 with a median diameter of 2 μm or more and 15 μm or less can meet the demand for a high polishing rate in glass polishing.
[0034] The content of the filler 26 contained in the polishing layer is appropriately adjusted based on the content of the abrasive grains 24 and the content of the binder 25. In this embodiment, the content of the filler 26 contained in the polishing layer is preferably 15 volume % or more and 75 volume % or less, and particularly preferably 30 volume % or more and 72 volume % or less. If the content of the filler 26 contained in the polishing layer is 15 volume % or more, particularly 30 volume % or more, the elastic modulus of the binder 25 is ensured. If the content of the filler 26 contained in the polishing layer is 75 volume % or less, particularly 72 volume % or less, the interference of the filler 26 with the polishing force of the abrasive grains 24 is reduced. As a result, the polishing material 10 of this embodiment can achieve a better polishing rate in polishing processing.
[0035] (Binder 25) The binder 25 may be any component known as a binder for the polishing layer of the polishing pad, and is not particularly limited. The main component of the binder may be a resin or an inorganic substance. In the case of a resin, for example, polyurethane, polyphenol, epoxy resin, polyester, cellulose, ethylene copolymer, polyvinyl acetal, acrylic resin, polyvinyl alcohol, polyvinyl chloride, polyvinyl acetate, polyamide, etc. may be mentioned. In the case of an inorganic substance, for example, silicate, phosphate, polyvalent metal alkoxide, etc. may be mentioned. As the binder 25 in this embodiment, a resin, particularly an epoxy resin, is preferable. The polishing part 23 containing a resin as the binder 25 ensures a moderate elastic modulus and realizes a better polishing rate. The polishing part 23 containing an epoxy resin as the binder 25 can meet the demand for a high polishing rate in the polishing process of glass. In addition, when the binder 25 is a resin, the resin may be partially crosslinked. The curing agent used for crosslinking the resin can be appropriately set according to the resin used for the binder 25.
[0036] In FIG. 1 and FIG. 2, the binder 25 including the abrasive grains 24 and the filler 26 is shown in a schematic manner, but the binder 25 may also include other additives. The additives may be any known additives added to the polishing layer of the polishing pad, and are not particularly limited. Examples of the additives include dispersants, coupling agents, surfactants, lubricants, antifoaming agents, colorants, and other granular materials. Examples of the other granular materials include silica, wollastonite, calcium carbonate, and barium sulfate. The Mohs hardness of the other granular materials is preferably lower than the Mohs hardness of the filler 26. This reduces the interference of the other granular materials with the polishing force of the abrasive grains 24, and achieves a better polishing rate. The median diameter of the other granular materials is preferably smaller than the median diameter of the filler 26. The median diameter of the other granular materials is preferably 10 nm or more and 50 nm or less, and particularly preferably 20 nm or more and 30 nm or less. The polishing portion 23 contains other granular matter having the above median diameter, so that the demand for a high polishing rate in glass polishing can be met. The content of the binder 25 contained in the polishing layer is appropriately adjusted based on the contents of the abrasive grains 24, the filler 26, and the above additives.
[0037] (Support 12) The support 12 is not particularly limited, but examples of the main component thereof include thermoplastic resins such as polypropylene, polyethylene, polytetrafluoroethylene, and polyvinyl chloride, and engineering plastics such as polycarbonate, polyamide, and polyethylene terephthalate.
[0038] (First adhesive layer 13) The first adhesive layer 13 bonds the substrate 20 and the support 12. The first adhesive layer 13 has an adhesive. The adhesive is not particularly limited, but examples thereof include a reactive adhesive, an instant adhesive, a hot melt adhesive, and a repositionable adhesive.
[0039] (Second adhesive layer 14) The second adhesive layer 14 bonds the support 12 to the platen SP of the polishing apparatus. The second adhesive layer 14 has an adhesive layer provided along the back surface 17 of the support 12 and a release sheet covering the adhesive layer. By peeling off the release sheet, the support 12 can be fixed to the platen SP of the polishing apparatus.
[0040] <Method of Manufacturing Polishing Pad 11> The polishing pad 11 can be manufactured by a known manufacturing method of a polishing pad. For example, the manufacturing method of the polishing pad 11 includes a manufacturing method including a preparation step, a polishing layer forming step, and an adhesive layer attaching step. In the preparation step, the abrasive grains 24, the filler 26, and the binder 25 are mixed to prepare a composition for the polishing part (coating liquid). In the polishing layer forming step, the first surface 21 of the substrate 20 is coated with the coating liquid, and then dried to form a polishing layer. In the manufacturing method of this embodiment, the formation step is performed in a state in which a mask corresponding to a plurality of polishing parts 23 is arranged on the first surface 21. As a result, a polishing layer having a plurality of polishing parts 23 is formed on the first surface 21 of the substrate 20. In the adhesive layer attaching step, the first adhesive layer 13 is laminated on the second surface 22 of the substrate 20. As a result, the polishing pad 11 on which the first adhesive layer 13 is laminated can be adhered to the surface 16 of the support 12.
[0041] The above-described embodiment is illustrative in all respects and is not restrictive. The scope of the present invention is indicated by the claims, not by the above-described embodiment, and includes all modifications within the scope equivalent to the configurations described in the claims. Furthermore, the upper and lower limit values in the combinations of upper and lower limits illustrated in the above-described embodiment can be individually changed to the upper and lower limit values in the corresponding combinations of other upper and lower limits. EXAMPLES
[0042] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0043] [Example 1] Diamond abrasive grains (median diameter: approximately 30 μm, Mohs hardness: 10) were prepared as abrasive grains. Aluminum oxide grains (median diameter: approximately 4 μm, Mohs hardness: 9) were prepared as a filler. Epoxy resin was prepared as a binder. Furthermore, silica grains (median diameter: approximately 4 μm, Mohs hardness: 9) were prepared as other granular materials.
[0044] The above-mentioned abrasive grains, filler, binder, and other granular materials were mixed to prepare a composition for polishing part (coating liquid). The content of each material in the composition for polishing part was 2.5 vol% abrasive grains, 58.5 vol% filler, 35 vol% binder, and 4 vol% other granular materials.
[0045] A SUS mask was prepared, which was composed of a pattern of a polishing layer having multiple polishing parts, each of which had a diameter of 4 mm, an average thickness of 1000 μm, and an occupation area ratio of 43%, which was the minimum.A substrate with an average thickness of 0.5 mm and mainly composed of polycarbonate was prepared.
[0046] The substrate was covered with the mask. The substrate covered with the mask was coated with the prepared composition for polishing parts. The substrate coated with the composition for polishing parts was dried at 80 to 160°C to harden the composition for polishing parts. As a result, a polishing pad was obtained in which a polishing layer having a plurality of polishing parts was formed on the substrate.
[0047] A support having an average thickness of 1.0 mm and mainly made of polyvinyl chloride was prepared. The polishing pad and the support were bonded together using a tape-like adhesive layer. This resulted in the production of an abrasive having the polishing pad.
[0048] [Example 2] An abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter: approximately 90 μm, Mohs hardness: 10) were used as the abrasive grains.
[0049] [Example 3] An abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter: approximately 150 μm, Mohs hardness: 10) were used as the abrasive grains.
[0050] [Example 4] An abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter: approximately 300 μm, Mohs hardness: 10) were used as the abrasive grains.
[0051] [Example 5] An abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter: approximately 450 μm, Mohs hardness: 10) were used as the abrasive grains.
[0052] [Example 6] The abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter approximately 90 μm, Mohs hardness 10) were used as the abrasive grains, and the content of each material in the composition for the polishing part was 0.1 volume % abrasive grains, 60.9 volume % filler, 35 volume % binder, and 4 volume % other granular materials.
[0053] [Example 7] The abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter approximately 90 μm, Mohs hardness 10) were used as the abrasive grains, and the content of each material in the composition for the polishing part was 10.0 volume % abrasive grains, 51.0 volume % filler, 35 volume % binder, and 4 volume % other granular materials.
[0054] [Example 8] The abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter approximately 300 μm, Mohs hardness 10) were used as the abrasive grains, and the content of each material in the composition for the polishing part was 10.0 volume % abrasive grains, 51.0 volume % filler, 35 volume % binder, and 4 volume % other granular materials.
[0055] [Example 9] An abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter: approximately 90 μm, Mohs hardness: 10) were used as the abrasive grains and acrylic resin was used as the binder.
[0056] [Comparative Example 1] An abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter: approximately 10 μm, Mohs hardness: 10) were used as the abrasive grains.
[0057] [Comparative Example 2] An abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter: approximately 15 μm, Mohs hardness: 10) were used as the abrasive grains.
[0058] [Comparative Example 3] The abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter approximately 90 μm, Mohs hardness 10) were used as the abrasive grains, and the content of each material in the composition for the polishing part was 20.0 volume % abrasive grains, 41.0 volume % filler, 35 volume % binder, and 4 volume % other granular materials.
[0059] [Comparative Example 4] An abrasive was obtained in the same manner as in Example 1, except that diamond abrasive grains (median diameter: approximately 10 μm, Mohs hardness: 10) were used as the abrasive grains, and acrylic resin was used as the binder.
[0060] [Measurement of polishing rate] Aluminosilicate glass plates (Corning Golllira3) measuring 58 mm in length, 33 mm in width, and having a specific gravity of about 2.4 were polished using the polishing materials of Examples 1 to 9 and Comparative Examples 1 to 4. The polishing was performed using a double-sided polishing machine (Engis Japan EDJ-6BY) at a polishing pressure of 100 g / cm. 2The test was performed under the conditions of: upper and bottom plate rotation speed 30 rpm, lower plate rotation speed 60 rpm, and coolant supply rate 50 ml / min. The coolant used was a 30-fold diluted aqueous solution of Noritake Cool CG-50P (manufactured by Noritake Company Limited). The weight change (g) of the aluminosilicate glass before and after polishing was calculated based on the surface area (cm2) of the polished portion. 2 ), specific gravity of aluminosilicate glass (g / cm 3 The polishing rate (μm / min) was calculated by dividing the polishing rate (μm / min) by the polishing time (min). Table 1 shows the calculation results of the polishing rate.
[0061] [Table 1]
[0062] The polishing materials of Examples 1 to 9 and Comparative Examples 1 to 4 all use diamond abrasive grains as abrasive grains. However, as is clear from Table 1, it can be seen that the polishing materials of Examples 1 to 9 have a higher polishing rate than the polishing materials of Comparative Examples 1 to 4. The median diameter of the diamond abrasive grains is different between Examples 1 to 9 and Comparative Examples 1, 2, and 4. More specifically, the median diameter of the diamond abrasive grains of Examples 1 to 9 is 30 μm or more. On the other hand, the median diameter of the diamond abrasive grains of Comparative Examples 1, 2, and 4 is 15 μm or less. This suggests that the polishing material having a polishing pad containing abrasive grains with a median diameter of 20 μm or more has a superior polishing rate. In addition, it was shown that the polishing material having a polishing pad containing abrasive grains with a median diameter of 30 μm or more and 450 μm or less has a superior polishing rate of 70 μm / min or more. Furthermore, it was shown that a polishing material having a polishing pad containing abrasive grains having a median diameter of 90 μm or more and 450 μm or less has an even better removal rate of 140 μm / min or more.
[0063] The abrasive of Example 2 and the abrasive of Example 9 have different types of binders, but both have excellent polishing rates of 140 μm / min or more. The abrasive of Example 9 and the abrasive of Comparative Example 4 both use acrylic resin as the binder. However, as described above, the abrasive of Example 9 has a higher polishing rate than the abrasive of Comparative Example 4. This suggests that the type of binder does not have a significant effect on the polishing rate.
[0064] The abrasive of Example 6 and the abrasive of Comparative Example 3 have different content (volume %) of diamond abrasive grains in the composition for polishing part. More specifically, the content of diamond abrasive grains in the composition for polishing part of Example 6 is 0.1 volume %. On the other hand, the content of diamond abrasive grains in the composition for polishing part of Comparative Example 3 is 20.0 volume %. From this, it was suggested that the abrasive having a polishing pad with a content of abrasive grains contained in the polishing layer of 0.1 volume % or more and less than 20.0 volume % has an excellent polishing rate. In addition, it was suggested that the abrasive having a polishing pad containing abrasive grains with a median diameter of 20 μm or more and a content of abrasive grains contained in the polishing layer of 0.1 volume % or more and 10.0 volume % or less has a higher polishing rate.
[0065] It is believed that the increase in the content of abrasive grains contributes to the improvement of the polishing rate. However, from the experimental results of Example 6 and Comparative Example 3, it has surprisingly become clear that the increase in the content of abrasive grains may cause the decrease in the polishing rate. More specifically, it has been shown that the polishing rate of a polishing pad containing diamond abrasive grains with a median diameter of 90 μm decreases when the content of diamond abrasive grains contained in the polishing layer becomes 20.0 volume % or more. From this, it is suggested that in the case of a polishing pad containing abrasive grains with a median diameter of 20 μm or more, the polishing rate decreases when the content of abrasive grains contained in the polishing layer becomes 20.0 volume % or more.
[0066] The measurement results of the polishing rate using the polishing materials of Examples 1-9 and Comparative Examples 1-4 suggest that the polishing rate of the polishing pad containing the abrasive grains with a median diameter of 20 μm or more and 600 μm or less can be improved by making the content of the abrasive grains contained in the polishing layer 0.05 volume % or more and less than 20.0 volume %.In particular, it has been experimentally shown that the polishing rate of the polishing pad containing the diamond abrasive grains with a median diameter of 30 μm or more and 450 μm or less can be significantly improved by making the content of the diamond abrasive grains contained in the polishing layer 0.1 volume % or more and 10.0 volume % or less.
[0067] [Measurement of dynamic friction coefficient μ0] The dynamic friction coefficient μ0 against glass was measured using a surface property tester (Tribogear HEIDON 14DR, manufactured by Shinto Scientific Co., Ltd.) for the abrasives obtained in Examples 1 to 9 and Comparative Examples 1 to 4. The glass used was an aluminosilicate glass (Gollira3, manufactured by Corning) measuring 10 mm in length, 10 mm in width, and with a specific gravity of approximately 2.4.
[0068] FIG. 3 is a schematic diagram of a commercially available surface property tester 1000 including Tribogear HEIDON 14DR manufactured by Shinto Scientific Co., Ltd. The surface property tester 1000 includes a detector 1100, an arm unit 1200, a pedestal 1300, and a main body base 1400. The pedestal 1300 can move linearly at a constant speed on the main body base 1400 in the pedestal scanning direction indicated by the arrow in FIG. 3. The abrasive 1010 is detachably fixed on the pedestal 1300. In this embodiment, the abrasive 1010 is each of the abrasives of Examples 1 to 5 and Comparative Examples 1 to 3. The arm unit 1200 is connected to the detector 1100. A tip portion 1210 is provided at the tip of the arm unit 1200 opposite to the connection side with the detector 1100. A plate material 1030 and a weight 1040 are detachably fixed to the tip portion 1210. In this embodiment, the plate material 1030 is the above-mentioned aluminosilicate glass. By changing the load of the weight 1040, it is possible to adjust the pressure on the contact surface between the abrasive 1010 and the plate material 1030 in measuring the dynamic friction coefficient. With the plate material 1030 in contact with the abrasive 1010 at a predetermined pressure, the base 1300 moves linearly at a constant speed in the base scanning direction. At this time, the dynamic friction coefficient on the contact surface between the plate material 1030 and the abrasive 1010 is measured by the detector 1100.
[0069] In this embodiment, the aluminosilicate glass plate 1030 was fixed to the tip 1210 of the surface property tester using paraffin-based wax as an adhesive. A weight 1040 was used to apply pressure of the plate 1030 to the abrasive 1010 at 20 gf / cm 2The temperature was adjusted to 0.05° C. Furthermore, a 30-fold diluted aqueous solution of coolant (Noritake Cool CG-50P manufactured by Noritake Company Limited) was dripped onto the contact surface between the plate material 1030 and the abrasive 1010. With the coolant dripped, the abrasive 1010 fixed to the base 1300 was scanned in a uniform linear motion in the horizontal direction, and the dynamic friction coefficient μ0 was measured. During the measurement, the scanning speed of the uniform linear motion was 50 mm / sec, the scanning distance was 50 mm, and the measurement time was 1.0 sec. The dynamic friction coefficient μ0 was calculated as an average value for 0.8 sec from 0.2 to 1.0 sec after the start of the scanning of the uniform linear motion. This suppressed the influence of the acceleration at the start of the surface property tester and the influence of the static friction coefficient on the dynamic friction coefficient μ0 from 0 to 0.2 sec after the start of the scanning of the uniform linear motion. Table 3 shows the measurement results of the dynamic friction coefficient μ0.
[0070] [Table 2]
[0071] From Table 3, it can be seen that the abrasives of Examples 1 to 9 have a higher dynamic friction coefficient μ0 than the abrasives of Comparative Examples 1 to 4. That is, in the above-mentioned measurement of the polishing rate, the abrasives of Examples 1 to 9, which were confirmed to have excellent polishing rates, were shown to have a dynamic friction coefficient μ0 of 1.54 or more under the above-mentioned measurement conditions of the dynamic friction coefficient μ0. This suggests that abrasives with an average dynamic friction coefficient of 1.0 or more under the above-mentioned measurement conditions of the dynamic friction coefficient μ0 have an excellent polishing rate. In particular, it is suggested that abrasives with an average dynamic friction coefficient of 1.5 or more and 4.0 or less have a better polishing rate. [Explanation of symbols]
[0072] 10, 1010 Abrasive material 11 Polishing Pad 12 Support 13 First adhesive layer 14 Second adhesive layer 16 Surface 17 Back side 20 Base material 21 Front page 22 Second side 23 Polishing section 24 Abrasive grain 25 Binder 26 Fillers 1030 Board material 1000 Surface Property Tester 1100 Detector 1200 Arm section 1210 Tip 1300 Pedestal 1400 Body base SP Polishing machine surface plate
Claims
1. A substrate; a polishing layer including abrasive grains and a binder and laminated on the substrate; having The glass and the polishing layer have a strength of 20 gf / cm 2 When the glass or the polishing layer moves linearly at a uniform velocity on the contact surface between the glass and the polishing layer in a state of contact with each other under a pressure of 0.2 to 1.0 seconds, the average value of the dynamic friction coefficient for 0.8 seconds from the start of the uniform linear motion to the start of the uniform linear motion is 1.0 or more. Polishing pad.
2. 2. The polishing pad according to claim 1, wherein the abrasive grains have a median diameter of 20 μm or more and 600 μm or less.
3. 2. The polishing pad according to claim 1, wherein the content of abrasive grains in the polishing layer is 0.05 vol. % or more and less than 20.0 vol. %.
4. The polishing pad according to any one of claims 1 to 3, wherein the abrasive grains are diamond abrasive grains.
5. The polishing pad according to any one of claims 1 to 3, wherein the polishing layer further comprises a filler.
6. The polishing pad of claim 5 , wherein the filler is an inorganic oxide and the binder is a resin.
7. The polishing pad according to any one of claims 1 to 3, wherein the polishing layer is composed of a plurality of polishing portions.
8. The polishing pad according to any one of claims 1 to 3, which is used for polishing glass.
Citation Information
Patent Citations
Polishing pad and its manufacturing method
JP2005324302A
Polishing pad
JP2022098876A
Abrasive article with Anti-slip polymeric layer
US20090035519A1
Polishing pad and method for manufacturing polished product
WO2021065619A1
Cited By
Polishing pad and method of use thereof
JP7850874B1
Polishing pad
WO2026167953A1