Sandwich structure
The innovative sandwich structure, featuring a core layer of arranged blocks and a fiber-reinforced skin layer, addresses the challenge of size limitations by enabling large, lightweight structures with enhanced mechanical properties and reduced surface roughness at bends.
Patent Information
- Application Number
- JP2023053085
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing sandwich structures face limitations in increasing size due to the use of a single base material for the core layer.
A sandwich structure comprising a skin layer made of fiber-reinforced resin and a core layer made of discontinuous fiber-reinforced resin, with the core layer formed by arranging multiple blocks in a plane, allowing for a large-sized structure with a bent portion.
Enables the creation of a lightweight sandwich structure with excellent mechanical properties and improved surface quality at bent portions by absorbing wrinkles through seam alignment.
Smart Images

Figure 2024141434000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a sandwich structure made of fiber-reinforced resin. [Background technology]
[0002] In recent years, market demands for lightweight industrial products such as automobiles, aircraft, sports products, and electronic devices have been increasing year by year. To meet such demands, sandwich structures having excellent lightweight properties and excellent mechanical properties have been widely used in various industrial applications. For example, Patent Document 1 discloses a sandwich structure in which a core layer is made of a sheet-like intermediate substrate in which a mat made of reinforcing fibers is impregnated with a thermoplastic resin, and a skin layer is made of a sheet-like intermediate substrate in which continuous reinforcing fibers are impregnated with a thermoplastic resin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2014 / 162873 Summary of the Invention [Problem to be solved by the invention]
[0004] On the other hand, in the structure disclosed in Patent Document 1, a single base material is used for the core layer, so there is a problem in making the sandwich structure larger. An object of the present invention is to provide a sandwich structure that can be made larger. [Means for solving the problem]
[0005] In order to solve the above-mentioned problems, the present invention provides a sandwich structure having a curved portion, which comprises a skin layer (I) made of fiber-reinforced resin and a core layer (II) made of discontinuous fiber-reinforced resin, wherein the core layer (II) is formed by arranging a plurality of blocks in a plane. Effect of the Invention
[0006] According to the present invention, a large sandwich structure that is lightweight and has excellent mechanical properties can be obtained. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic diagram showing one embodiment of a sandwich structure according to the present invention; [Diagram 2] FIG. 1 is a schematic diagram showing one embodiment of a sandwich structure according to the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The sandwich structure of the present invention is a sandwich structure having at least a curved portion, which comprises a skin layer (I) made of fiber-reinforced resin and a core layer (II) made of discontinuous fiber-reinforced resin, and the core layer (II) is formed by arranging a plurality of blocks in a plane.
[0009] In the sandwich structure of the present invention, the core layer (II) is formed by arranging blocks in a plane. Fig. 1 is a schematic cross-sectional view showing a partial structure of a sandwich structure in one embodiment of the present invention. By arranging the blocks in a plane, it becomes possible to mold a large sandwich structure. In addition, in molding having a bent portion, molding can be easily performed by arranging the blocks in accordance with the shape change.
[0010] In the present invention, it is preferable that the joints of the blocks substantially coincide with the ridges of the bent portions. Fig. 2 is a schematic cross-sectional view showing a partial structure of a sandwich structure of this type. By having the joints coincide with the ridges of the bent portions, wrinkles caused by the difference in circumferential length of the skin layers at the bent portions can be captured at the joints, improving the surface quality of the sandwich structure.
[0011] It is preferable to use a thermoplastic resin that melts or flows when heated for the core layer (II). For example, "polyethylene terephthalate (PET), polyamide (PA), polycarbonate (PC), polyphenylene sulfide (PPS), polyetherimide (PEI), polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), and other polyaryletherketones (PAEK)" can be mentioned. From the viewpoint of flame retardancy, a flame-retardant thermoplastic resin having a limiting oxygen index of preferably 25 or more is preferable. The limiting oxygen index is more preferably 30 or more, and even more preferably 35 or more.
[0012] The core layer (II) in the present invention preferably has voids, and the void ratio is preferably 10% by volume or more and 90% by volume or less. The voids in the core layer (II) typically refer to spaces in which neither the discontinuous reinforcing fibers nor the thermoplastic resin exist, formed by bonding overlapping or intersecting discontinuous reinforcing fibers at least at their intersections with a thermoplastic resin to form a support. When the void ratio is 10% by volume or more, the density of the core layer (II) is low, so that light weight can be satisfied. On the other hand, when the void ratio is 90% by volume or less, the thickness of the thermoplastic resin covering the intersections of the discontinuous reinforcing fibers is sufficient, so that the discontinuous reinforcing fibers in the core layer can be sufficiently reinforced, and the mechanical properties are improved.
[0013] The precursor of the core layer (II) preferably has thermal expansion properties. The method of expanding the precursor of the core layer is not particularly limited, and can be performed by existing expansion methods such as releasing the residual stress of discontinuous reinforcing fibers, expanding particles, and foaming resins. Here, releasing the residual stress of discontinuous reinforcing fibers refers to softening the matrix resin by heating, so that the reinforcing fibers that have been compressed by pressure expand due to the raising force derived from the elastic modulus of the reinforcing fibers. This allows the thickness of the core layer (II) to be freely controlled within the range allowed by the properties of the reinforcing fibers and the matrix resin.
[0014] In the present invention, the discontinuous reinforcing fiber used in the core layer (II) refers to a reinforcing fiber having a fiber length of 1 mm or more and 15 mm or less. When the fiber length is 1 mm or more, the reinforcing effect of the reinforcing fiber satisfies the mechanical properties, and when the fiber length is 15 mm or less, the fiber is easily dispersed and isotropic. As a method for measuring the fiber length of the reinforcing fiber, for example, there is a method in which the reinforcing fiber is directly extracted from the reinforcing fiber group and measured by observation under a microscope. When resin is attached to the reinforcing fiber group, the resin is dissolved from the reinforcing fiber group using a solvent that dissolves only the resin contained therein, and the remaining reinforcing fiber is filtered and measured by observation under a microscope (dissolution method). When there is no solvent that dissolves the resin, there is a method in which only the resin is burned off in a temperature range in which the reinforcing fiber does not oxidize and lose weight, and the reinforcing fiber is separated and measured by observation under a microscope (burn-off method).
[0015] In addition, the discontinuous reinforcing fibers are preferably dispersed randomly in an approximately monofilament shape in the core layer (II). By distributing the fibers in an approximately monofilament shape, the number of discontinuous reinforcing fibers present as fiber bundles is reduced, so that weak parts at the ends of the fiber bundles can be minimized, and in addition to excellent reinforcing efficiency and reliability, isotropy can also be imparted. Dispersing the fibers randomly can further impart isotropy.
[0016] On the other hand, for the fiber-reinforced resin used in the skin layer (I), from the viewpoint of strength, the reinforcing fiber is preferably a continuous reinforcing fiber. Here, the continuous reinforcing fiber refers to a reinforcing fiber that is continuous in at least one direction with a length of 100 mm or more. The form of the continuous fiber includes a fiber fabric composed of a reinforcing fiber bundle composed of a large number of continuous fibers, and a unidirectional continuous fiber in which a large number of continuous fibers are arranged in one direction. Among them, from the viewpoint of enhancing the reinforcing effect of the molded body, a unidirectional continuous fiber is preferable, and when the molded body is to have a complex shape, a fiber fabric having excellent shapeability is preferable.
[0017] The type of reinforcing fiber used in the skin layer (I) and the core layer (II) is not particularly limited, and examples thereof include metal fibers such as aluminum fibers, brass fibers, and stainless steel fibers; carbon fibers (including graphite fibers) such as polyacrylonitrile (PAN)-based carbon fibers, rayon-based carbon fibers, lignin-based carbon fibers, and pitch-based carbon fibers; insulating fibers such as glass fibers; organic fibers such as aramid fibers, polyparaphenylenebenzoxazole (PBO) fibers, polyphenylene sulfide fibers, polyester fibers, acrylic fibers, nylon fibers, polyethylene fibers, and cellulose fibers; and inorganic fibers such as silicon carbide fibers and silicon nitride fibers. These fibers may also be surface-treated. Examples of surface treatments include, in addition to deposition of metals that are conductors, treatment with a coupling agent, treatment with a sizing agent, treatment with a bundling agent, and deposition of additives. These reinforcing fibers may be used alone or in combination of two or more types.
[0018] Among them, from the viewpoint of weight reduction effect, carbon fibers such as PAN-based carbon fibers, pitch-based carbon fibers, and rayon-based carbon fibers, which are excellent in specific strength and specific rigidity, are preferably used, and PAN-based carbon fibers, which are excellent in mechanical properties such as strength and elastic modulus, are particularly preferably used. From the viewpoint of improving the economic efficiency of the obtained molded product, glass fibers are preferably used, and it is particularly preferable to use carbon fibers and glass fibers in combination from the viewpoint of the balance between mechanical properties and economic efficiency. Furthermore, from the viewpoint of improving the impact absorption and formability of the obtained molded product, aramid fibers are preferably used, and it is particularly preferable to use carbon fibers and aramid fibers in combination from the viewpoint of the balance between mechanical properties and impact absorption. From the viewpoint of improving the conductivity of the obtained molded product, reinforced fibers coated with metals such as nickel, copper, and ytterbium can also be used.
[0019] The carbon fiber may be a recycled carbon fiber obtained by recycling a carbon fiber reinforced plastic containing carbon fiber and a matrix resin. The recycling method may include, for example, removing the matrix resin by a treatment method such as a normal pressure dissolution method, a subcritical decomposition method, a supercritical decomposition method, an electrolysis method, a thermal decomposition method, or a superheated steam method.
[0020] Cellulosic materials for cellulose fibers include vegetable pulp, solvent-spun cellulose, semi-synthetic cellulose, etc. Vegetable pulp includes wood-based pulp such as kraft pulp (KP), dissolving pulp (DP), and dissolving kraft pulp (DKP) made from hardwood (L-wood) and softwood (N-wood). Other examples include non-wood-based pulp such as straw pulp, hemp pulp, cotton pulp, cotton linter pulp, and kenaf pulp.
[0021] As the matrix resin of the fiber reinforced resin used in the skin layer (I), those generally used in FRP, such as thermoplastic resin, thermosetting resin, and photocurable resin, can be used.
[0022] The sandwich structure can be manufactured, for example, by a manufacturing method including a step of heating and expanding a plurality of blocks of a precursor of the core layer (II) made of a mat-like base material in which thermoplastic resin fibers and / or thermoplastic resin particles and discontinuous reinforcing fibers are mixed. According to such a method, the thermoplastic resin fibers and / or thermoplastic resin particles are uniformly dispersed with the discontinuous reinforcing fibers, so that the impregnation of the thermoplastic resin can be performed quickly. There is no particular limitation on the method for manufacturing the precursor of the core layer made of the mat-like base material, and examples thereof include the spunlace method, the needle punch method, the steam jet method, the airlaid method, the dry papermaking method, and the wet papermaking method.
[0023] Regarding the diameter of the thermoplastic resin fiber, it is possible to use a fiber diameter that is generally available on the market, but when the reinforcing fiber and the resin fiber are mixed to form a mixed mat, it is preferable to select and use a fiber diameter that is equal to or larger than the diameter of the reinforcing fiber from the viewpoint of the stability of the process. In addition, in the case of the thermoplastic resin particles, no particular restriction is imposed on the particle diameter, but it is preferable to appropriately adjust the particle diameter from the viewpoint of preventing the particles from falling off during the process when the mixed mat is formed by mixing with the reinforcing fiber mat.
[0024] There is no particular limitation on the method for joining the core layer (II) and the skin layer (I). They may be joined by integral molding, or the core layer (II) may be molded and then the skin layer (I) may be bonded with an adhesive.
[0025] The sandwich structure of the present invention is particularly suitable for use as a structural member for a large-scale mobile body that must have both advanced properties and light weight. Here, "mobile body" refers to automobiles, railroad cars, aircraft, ships, drones, UAM (Urban Air Mobility), etc. EXAMPLES
[0026] The present invention will now be described in more detail with reference to examples.
[0027] <Measurement methods for various physical properties> (1) Measurement of porosity of the core layer A test piece measuring 10 mm in length and 10 mm in width was cut from the flat surface of the fiber-reinforced resin structure, and the cross section was observed using a scanning electron microscope (SEM) (S-4800 model, manufactured by Hitachi High-Technologies Corporation). Ten equally spaced locations on the surface of the structure were photographed at 1000x magnification. The area of the voids in each image was determined. Furthermore, the void area was divided by the area of the entire image to calculate the void ratio. The volumetric content of the voids in the structure was calculated by arithmetic average of the void ratios of a total of 50 locations, 10 locations of which were photographed on each of the five test pieces.
[0028] (2) Surface roughness of the bent part Using a surface roughness meter, the cutoff value and reference length were selected based on JIS-B-0601 (2001), and the surface roughness Ra of the bent portion of the skin layer was obtained. <Material> [Carbon fiber] A polymer mainly composed of polyacrylonitrile was spun and sintered to obtain continuous carbon fibers with a total of 12,000 filaments. The continuous carbon fibers were then electrolytically surface-treated and dried in heated air at 120°C to obtain carbon fibers. The properties of the carbon fibers were as follows:
[0029] Density: 1.80g / cm 3 Single fiber diameter: 7μm Tensile strength: 4.9GPa Tensile modulus: 230GPa [Recycled carbon fiber] A predetermined number of carbon fiber prepregs "TORAYCA (registered trademark) prepreg" P2352W-19 manufactured by Toray Industries, Inc. were laminated, and then cured at 180°C for 10 hours to produce carbon fiber reinforced plastic waste material of 100mm x 100mm x 5mm. The carbon fiber reinforced plastic waste material was crushed and passed through a screen to obtain carbon fiber reinforced plastic crushed pieces of a predetermined fiber length. The material was then placed in a pyrolysis furnace and subjected to a pyrolysis treatment process under conditions of an oxygen concentration of 5%, a heat treatment temperature of 550°C, and a heat treatment time of 20 minutes to obtain recycled carbon fiber.
[0030] [Epoxy resin] As epoxy resins, 30 parts by mass of "jER (registered trademark)" 828 (manufactured by Mitsubishi Chemical Corporation), 35 parts by mass of "jER (registered trademark)" 1001, and 35 parts by mass of "jER (registered trademark)" 154 were put into a kneader, and the temperature was raised to 150 ° C. while kneading, and kneaded at 150 ° C. for 1 hour to obtain a transparent viscous liquid. After lowering the temperature of the viscous liquid to 60 ° C. while kneading, 3.7 parts by mass of DYCY7 (manufactured by Mitsubishi Chemical Corporation) as a curing agent, 3 parts by mass of DCMU99 (manufactured by Hodogaya Chemical Co., Ltd.) as a curing accelerator, and 3 parts by mass of "Matsumoto Microsphere (registered trademark)" M (manufactured by Matsumoto Yushi Seiyaku Co., Ltd.) as particles were blended, and the mixture was kneaded at 60 ° C. for 30 minutes to prepare a thermosetting resin composition. From this, a resin film with a basis weight of 132 g / m2 was produced using a knife coater.
[0031] [PA resin fiber] Resin fibers having an average fiber diameter of 15 μm were produced using nylon 66 resin (manufactured by Toray Industries, Inc., "Amilan" (registered trademark) CM3006, melting temperature 265° C.).
[0032] [PEI resin] A resin film having a basis weight of 132 g / m2 was produced using a polyetherimide resin (GE Plastics, "URTEM1000" (registered trademark), melting temperature 220°C) with a knife coater.
[0033] [PEI resin fiber] Resin fibers having an average fiber diameter of 15 μm were produced using a polyetherimide resin (GE Plastics, "URTEM1000" (registered trademark), melting temperature 220° C.).
[0034] [PC resin] A resin film with a basis weight of 132 g / m2 was produced using a knife coater using polycarbonate resin ("Iupilon" (registered trademark) H-4000, manufactured by Mitsubishi Engineering Plastics Corporation, melting temperature 160°C).
[0035] [PC resin particles] Resin particles made of polycarbonate resin ("Iupilon" (registered trademark) H-4000, manufactured by Mitsubishi Engineering Plastics Corporation, melting temperature 160°C) with an average particle size of 300 µm were prepared.
[0036] Example 1 The skin layer (I) was reinforced with carbon fiber, the matrix resin was epoxy resin, the core layer (II) was reinforced with chopped carbon fiber cut to 6 mm with a cartridge cutter, and the matrix resin was PA resin fiber. The sandwich structure was obtained under the following molding conditions. (First step) The chopped carbon fibers and PA resin fibers to be used for the core layer (II) are mixed by a wet papermaking method to prepare a mat-like substrate. (Second step) Next, a plurality of mat-like substrates are arranged in the planar direction, and prepregs in which reinforcing fibers are impregnated with a matrix resin are laminated on both sides as precursors of the skin layers (I). (Third step) The laminate is placed in a press molding die cavity having a bent portion preheated to 280°C, which is higher than the melting temperature of the matrix resin used in the core layer, and the die is closed. At this time, the mat-like substrate is placed so that the seam does not overlap with the bent portion. (Fourth step) A pressure of 5 MPa is applied and maintained for an additional 60 seconds. (5th step) The mold cavity is opened and metal spacers are inserted into its ends to adjust the void ratio to 50%. (Sixth step) After that, the cavity temperature is cooled to 50°C while maintaining the pressure, and then the mold is opened to remove the sandwich structure. The properties of the resulting sandwich structure are shown in Table 1.
[0037] Example 2 A sandwich structure was prepared in the same manner as in Example 1, except that the matrix resin used for the skin layer was PC resin, the matrix resin used for the core layer (II) was PC resin particles, a mat-like substrate was prepared by a dry papermaking method in the first step, and the preheating temperature in the third step was 300°C. The properties of the resulting sandwich structure are shown in Table 1.
[0038] Example 3 In the third step, a sandwich structure was produced in the same manner as in Example 1, except that the mat-like substrate was placed in the mold so that the seam coincided with the bent portion. The properties of the resulting sandwich structure are shown in Table 1.
[0039] Comparative Example 1 In the second step, a sandwich structure was prepared in the same manner as in Example 2, except that a single mat-like substrate was used instead of arranging the mat-like substrates. The properties of the resulting sandwich structure are shown in Table 1.
[0040] Comparative Example 2 A sandwich structure was prepared in the same manner as in Comparative Example 1, except that the matrix resin used for the skin layer was PEI resin, the matrix resin used for the core layer (II) was PEI resin fiber, a mat-like substrate was prepared by the needle punch method in the first step, and the preheating temperature in the third step was 360°C. The properties of the resulting sandwich structure are shown in Table 1.
[0041] Comparative Example 3 A sandwich structure was prepared in the same manner as in Example 1, except that recycled carbon fibers were used as the reinforcing fibers for the core layer (II) and a single mat-like substrate was used in the second step instead of arranging the mat-like substrates. The properties of the resulting sandwich structure are shown in Table 1.
[0042] [Table 1]
[0043] In both Examples 1 and 2, the core layer was composed of multiple blocks arranged in a plane, so that a large sandwich panel could be formed. In Example 3, the joints of the blocks coincided with the ridges of the bent parts, so that the joints absorbed the wrinkles in the skin layer caused by the difference in circumferential length at the bent parts, and a sandwich structure with good surface quality and small surface roughness at the bent parts was obtained. On the other hand, in Comparative Examples 1 to 3, a single core was used, so that a large panel could not be produced. [Explanation of symbols]
[0044] 1. Skin Layer 2. Core layer 3. Bends 4. Block 5. Seams
Claims
1. A sandwich structure having a bent portion, comprising a skin layer (I) made of fiber-reinforced resin and a core layer (II) made of discontinuous fiber-reinforced resin, wherein the core layer (II) is formed by arranging a plurality of blocks in a plane.
2. 2. The sandwich structure of claim 1, wherein the block seams are substantially aligned with the ridges of the bends.
3. The sandwich structure according to claim 1 or 2, wherein the core layer (II) comprises a thermoplastic resin.
4. The sandwich structure according to claim 1 or 2, wherein the core layer (II) has 10 to 90 volume % of continuous voids.
5. The sandwich structure according to claim 1 or 2, wherein the precursor of the core layer (II) has thermal expansion properties.
6. A method for producing a sandwich structure as described in claim 1 or 2, characterized in that a core layer (II) is formed by heating and expanding multiple blocks of a precursor of a core layer consisting of a mat-like substrate in which thermoplastic resin fibers and / or thermoplastic resin particles are mixed with discontinuous reinforcing fibers by any one of needle punching, wet papermaking, and dry papermaking, to a temperature above the melting point of the thermoplastic resin constituting the thermoplastic resin fibers and / or thermoplastic resin particles.
7. A structural member for a moving body, comprising the sandwich structure according to claim 1 or 2.
8. The movable body structural member according to claim 7 , wherein the movable body is a vehicle, a ship, or an aircraft.
Citation Information
Patent Citations
Sandwich laminate, sandwich structure and unified molded product using same and processes for producing both
WO2014162873A1