Holding pad and method for manufacturing the same

A photocurable resin-based holding pad with adjustable suction force and chemical resistance addresses the limitations of suede pads, ensuring effective and damage-free polishing by integrating uneven structures and easy release of objects.

JP2024141512APending Publication Date: 2024-10-10FUJIBO HLDG
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023053207
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing holding pads used in chemical mechanical polishing (CMP) are not chemically resistant and have a short lifespan due to the use of suede materials, which deteriorate under acidic conditions, and they lack the ability to adjust suction force and easily release polished objects.

Method used

A holding pad with a holding layer made of photocurable resin, featuring a Shore A hardness of 60-90, a compressive modulus of 60-90%, and a density of 0.5-3.0 kg/m³, which can be formed with uneven structures and integrated convex or concave features, using a manufacturing process involving photocuring and solvent washing to create a chemical-resistant surface.

Benefits of technology

The photocurable resin holding pad provides chemical resistance, allows for adjustable suction force, and facilitates easy release of polished objects, enhancing the polishing process by maintaining the integrity of the surface and preventing damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141512000001_ABST
    Figure 2024141512000001_ABST
Patent Text Reader

Abstract

To provide a holding pad which has chemical resistance, and can impart various uneven structures as a holding pad having a holding layer for holding a polished object, to a holding surface.SOLUTION: A holding pad includes a holding layer for holding a polished object, wherein the holding layer is composed of a photocurable resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The polishing pad of the present invention relates to a holding pad for holding an object to be polished. More specifically, the present invention relates to a holding pad capable of suitably holding an object to be polished when polishing a semiconductor wafer or the like, and a method for manufacturing the same. [Background technology]

[0002] Chemical mechanical polishing (CMP) is commonly used as a polishing method for flattening the surfaces of optical materials, semiconductor wafers, semiconductor devices, substrates for hard disks, silicon wafers, and sapphire glass. The CMP method will be described with reference to Fig. 1. Fig. 1 is a cross-sectional view of a polishing apparatus for carrying out the CMP method, in which an object to be polished W is sandwiched between a polishing pad 3 provided on a polishing platen 4 and a holding pad 10 provided on a holding platen 2, and is rotated while being pressed, thereby polishing the object to be polished W. The holding pad 10 is provided with a frame-shaped member 12, enabling efficient polishing. During polishing, a slurry is supplied between the polishing pad 3 and the workpiece W. The slurry is supplied to the polishing surface through grooves or holes and then discharged. The slurry is a mixture (dispersion liquid) of water, various chemical components, and hard fine abrasive grains, and as the chemical components and abrasive grains are flowed, they move relative to the workpiece W, thereby increasing the polishing effect (see Patent Documents 1, 2, and 3). A typical holding pad is made of suede produced by wet film formation, but a large amount of solvent is used in the manufacturing process. In addition, under polishing conditions where the slurry is highly acidic, materials such as suede cannot withstand the conditions, resulting in a problem of a shortened life of the holding pad. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2009-61524 [Patent Document 2] Patent Publication No. 11-151665 [Patent Document 3] JP 11-151666 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention provides a holding pad and a method for manufacturing the same, which are chemical resistant, can be used as a holding pad to impart various uneven structures to its holding surface, can adjust its adhesive force to an appropriate level, and can facilitate the release of the polished object. [Means for solving the problem]

[0005] The present inventors have found that by using a photocurable resin as the material for the retaining layer, it is possible to produce a retaining pad having a retaining layer that is chemical resistant and capable of imparting various uneven structures to the retaining surface as a retaining pad. [1] A holding pad having a holding layer for holding an object to be polished, the holding layer being made of a photocurable resin. [2] The density of the support layer is 0.5 kg / m 3 More than 3.0kg / m 3 The holding pad described in [1] below. [3] The retaining pad described in [1], wherein the Shore A hardness of the retaining layer is 60 or more and 90 or less. [4] The retention pad described in [1], wherein the retention layer has a compression ratio of 0.1% or more and 10% or less. [5] The holding pad described in [1], wherein the compressive elastic modulus of the holding layer is 60% or more and 90% or less. [6] The holding pad described in [1], wherein the holding layer has an integral holding surface, and the photocurable resin is an ultraviolet curable resin. [7] The holding pad described in [1], wherein the photocurable resin is an acrylic resin. [8] The holding pad described in [1], wherein the holding surface has concave or convex portions formed thereon, and the average height of the concave or convex portions is 0.3 mm or more and 1.5 mm or less. [9] A holder further comprising a frame-shaped member on the outer periphery of the holding surface of the holding pad described in [1], the frame-shaped member being made of glass epoxy or SUS.

[10] The retaining device described in [9], wherein a recess or protrusion is formed in the portion of the retaining surface of the retaining pad described in [1] that includes the frame-shaped member.

[11] A method for manufacturing a holding pad having a holding layer for holding an object to be polished, the holding layer being made of a photocurable resin, comprising: Preparing a mold; placing a photocurable resin in the mold; A step of placing a masking sheet on the photocurable resin so that a concave-convex structure can be imparted; a step of curing the unmasked photocurable resin by irradiating light from above the masking sheet; and washing away the uncured photocurable resin with a solvent to obtain a retaining layer made of cured photocurable resin.

[12] A method for manufacturing a holding pad, comprising: a holding layer for holding an object to be polished, the holding layer being made of a photocurable resin; and a substrate being provided as a separate member on an opposite side to the holding surface, the method comprising: Preparing a mold; providing a substrate in the mold; disposing a photocurable resin on the substrate; a step of irradiating the photocurable resin with light from a substrate side to bond the substrate and the photocurable resin; A step of placing a masking sheet on the opposite side of the substrate from the photocurable resin so that a concave-convex structure can be imparted; a step of curing the unmasked photocurable resin by irradiating light from above the masking sheet; and washing away the uncured photocurable resin using a solvent to obtain a substrate-attached support layer composed of a cured photocurable resin to which the substrate is adhered. Effect of the Invention

[0006] The holding pad has a holding layer for holding the object to be polished, the holding layer having an integral holding surface, and the holding layer being made of a photocurable resin, and is chemical resistant. As a holding pad with a holding layer, it is possible to impart a variety of uneven structures to the holding surface, the adhesive force can be adjusted to an appropriate level, and the object to be polished can be easily peeled off. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic diagram of polishing. [Diagram 2] FIG. 2 is an enlarged view of the supporting surface of supporting layer 11, where FIG. 2(a) shows a first embodiment of the present invention and FIG. 2(b) shows a second embodiment of the present invention. [Diagram 3] FIG. 3 is a front view of the supporting surface of supporting layer 11 (first embodiment). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, a mode for carrying out the invention will be described, however, the present invention is not limited to the mode for carrying out the invention.

[0009] <<Retention pad>> 1, the holding pad 10 is provided on the lower surface of the holding platen 2 and holds the workpiece W to be polished by suction onto a holding surface 110. The holding pad 10 and a frame-shaped member 12 provided on the outer periphery of the holding surface 110 of the holding layer 11 constitute a holder 1. The outer circumferential portion means the inner circumferential portion of the holding surface that is away from the center of rotation when the holding surface rotates and the portion closer to the center of rotation is defined as the inner circumferential portion. The holding pad 10 includes a base material, a double-sided tape (not shown) and the like in addition to the holding layer 11, but may be composed of the holding layer 11 alone.

[0010] (retention layer) The retention layer 11 is composed of a photocurable resin. A photocurable resin is a resin that has the property of being cured by the application of light. The photocurable resin is cured in the portion to which light is applied, and is not cured in the portion to which light is not applied. In this specification, photocurable resin that has not been exposed to light and is not cured is referred to as an uncured photocurable resin, and photocurable resin that has been sufficiently exposed to light and is cured is referred to as a cured photocurable resin.

[0011] The photocurable resin is not particularly limited as long as it is a resin that is polymerized and cured by light of a specific wavelength, but examples thereof include photosensitive resins, ultraviolet-curable resins, and visible-light-curable resins. In addition, examples of the photocurable resin include radical-polymerizable resins that are cured by radicals activated by light, and cationic-polymerizable resins that are cured by cations generated by light. Preferable embodiments of the retaining layer 11 include polyester-based resins, unsaturated polyester-based resins, vinyl ether resins, vinyl ester resins, acrylic resins, and epoxy-based resins. More preferably, acrylic resins and epoxy resins are used. The resins may be used alone or in combination of two or more. By using these resins, the surface shape can be easily manufactured, and the resin has chemical resistance, improving resistance to strongly acidic and strongly alkaline polishing solutions.

[0012] During polishing, a slurry is supplied between the polishing pad 3 and the workpiece W. The slurry is a mixture (dispersion) of water, various chemical components, and hard fine abrasive grains, and may chemically deteriorate the retaining layer 11. Therefore, the retaining layer 11 is preferably made of an acrylic ultraviolet curing resin, which has a higher crosslink density and better chemical resistance than thermosetting resins and room temperature curing resins.

[0013] Since the retaining layer 11 is made of a photocurable resin, it is easy to manufacture a retaining layer 11 having an integral retaining surface 110 on which recesses or protrusions are formed, and it is easy to adjust the height and position of the recesses or protrusions, and as a result, it is easy to adjust the adhesiveness and releasability of the retaining surface 110 to the polished object W. The term "integral" used here means that the retaining surface of the retaining layer is entirely made of the same material, and that the protrusions 110A are formed in a state in which they cannot be separated from the portions of the retaining surface other than the protrusions 110A.

[0014] The density of the support layer 11 is 0.5 kg / m 3 More than 3.0kg / m 3 Less than 1.0 kg / m is preferable. 3 More than 2.0kg / m 3 The following is more preferable. When the density is within the above range, the attachment and detachment property of the object to be polished is excellent.

[0015] In this specification, the Shore A hardness refers to a value measured in accordance with Japanese Industrial Standards (JIS K7311). The Shore A hardness of the retaining layer 11 is preferably not less than 60 and not more than 90, and more preferably not less than 70 and not more than 80. When the Shore A hardness is within the above range, the polished state of the object to be polished is good.

[0016] In this specification, the compressibility is an index of softness, and the compressive elastic modulus is an index of the ease of return to normal after compressive deformation. The compressibility and compressive elasticity can be determined using a Shopper type thickness gauge (pressure surface: circular with a diameter of 1 cm) in accordance with the Japanese Industrial Standards (JIS L1021). Specifically, the method is as follows. The thickness t0 is measured after applying the initial load for 30 seconds from the no-load state, and then the thickness t1 is measured after applying the final load for 5 minutes from the thickness t0 state. Next, all loads are removed from the thickness t1 state, and the specimen is left for 5 minutes (to be in a no-load state), after which the initial load is again applied for 30 seconds and the thickness t0' is measured. The compression ratio can be calculated using the formula: Compression ratio (%) = 100 × (t0-t1) / t0 (initial load is 100 g / cm 2 , final load is 1120g / cm2 (It is.) The compressive elastic modulus can be calculated using the formula: Compressive elastic modulus (%) = 100 × (t0'-t1) / (t0-t1) (initial load is 100 g / cm 2 , final load is 1120g / cm 2 (It is.)

[0017] The compressibility of the support layer 11 is preferably 0.1% or more and 10% or less, and more preferably 0.5% or more and 5% or less. The compressive elastic modulus of the retaining layer 11 is preferably 60% or more and 90% or less, and more preferably 70% or more and 80% or less. When the compressive modulus and the compressive elastic modulus are within the above ranges, the polished state of the object to be polished is good.

[0018] The thickness of the support layer 11 can be adjusted within the range of 0.5 to 1.7 mm, and is more preferably 0.7 to 1.5 mm. When the thickness of the support layer 11 is within the above range, the workability when replacing the support layer 11 is good.

[0019] The support surface 110 of the support layer 11 has recesses or protrusions formed thereon. As an example, the support layer 11, as shown in FIG. 2(a) and FIG. 3, is integrally provided with a support surface 110 on which a plurality of protrusions 110A are arranged in a dot pattern. As shown in FIG. 3, a plurality of protrusions 110A are arranged on the holding surface 110 at approximately equal intervals.

[0020] The shape of the convex portion 110A is a truncated cone in this example, but it may also be an approximately truncated cone, a truncated elliptical cone, a truncated polygonal pyramid, a cylinder, an elliptical cylinder, or a polygonal cylinder. A truncated cone is preferred because it is easy to manufacture and is less likely to damage the object to be polished. A truncated cone is preferable from the viewpoints of ease of manufacture and of preventing damage to the workpiece to be polished.

[0021] 2(b), the support layer 11 can have recesses on the support surface 110. The shape of the recesses is not particularly limited and can be a truncated cone or the like, and like the above-mentioned protrusions, they can be arranged in a dot pattern or linear recesses (linear grooves).

[0022] The average height of the recesses or protrusions is preferably 0.3 mm or more and 1.5 mm or less, more preferably 0.5 mm or more and 1.3 mm or less. The recesses or protrusions are preferably 18% to 88% of the total height of the retaining layer, more preferably 33% to 66%. In this specification, the height of the recesses refers to the depth of the recesses. That is, in this specification, in the case of the protrusions, α in FIG. 2(a) is referred to as the height of the protrusions, and in the case of the recesses, α in FIG. 2(b) is referred to as the height of the recesses. When the average height of the recesses or protrusions is within the above range, the adhesion and releasability of the polished object are good.

[0023] The retaining layer 11 has a frame-shaped member 12 on the outer periphery of the retaining surface 110, and the retaining pad 10 and the frame-shaped member 12 form the retainer 1. The frame-shaped member 12 surrounds the workpiece W to prevent the workpiece W from shifting sideways or falling off during polishing. A recess or protrusion may be formed in the portion of the retaining surface 110 that is provided with the frame-shaped member 12 (13 in FIG. 2). The frame-shaped member 12 is attached to the retaining surface 110 with an adhesive layer. If the retaining surface 110 of the retaining layer 11 becomes too smooth, the adhesion between the frame-shaped member 12 and the retaining surface 110 decreases. However, if a recess or protrusion is formed in the portion of the retaining surface 110 of the retaining layer 11 that is provided with the frame-shaped member 12, peeling between the frame-shaped member 12 and the retaining layer 11 can be suppressed, and the infiltration of slurry between them can be suppressed. The frame member 12 is made of glass epoxy or SUS. Glass epoxy is a glass epoxy resin plate obtained by impregnating or coating glass woven fabric with epoxy resin. SUS is stainless used steel. It is preferable that the frame member 12 has excellent heat resistance, taking into consideration the frictional heat and wear generated by contact with the polishing pad 3 during polishing.

[0024] <<Method of manufacturing the holding pad>> The method for manufacturing the holding pad 10 of the present invention is not particularly limited as long as a photocurable resin is used as the material for the holding layer 11, but an example is as follows. Note that this example will be described using a holding pad in which a base material is disposed on the holding layer 11. Namely; A method for manufacturing a holding pad, comprising: a holding layer 11 for holding a workpiece W, the holding layer 11 being made of a photocurable resin; and a substrate being provided as a separate member on an opposite side to the holding surface, the method comprising: The process of preparing the mold (Step 1), Step 2: placing a substrate in the mold; A step (Step 3) of disposing a photocurable resin on the substrate; a step of irradiating the photocurable resin with light from the substrate side to bond the substrate and the photocurable resin (Step 4); A step of placing a masking sheet on the opposite side of the substrate to the photocurable resin so that a concave-convex structure can be imparted (Step 5); A step of curing the unmasked photocurable resin by irradiating light from above the masking sheet (Step 6); The method for manufacturing the retaining pad 10 includes a step (Step 7) of obtaining a retaining layer 11 made of cured photocurable resin to which the substrate is adhered by washing away the uncured photocurable resin with a solvent.

[0025] (Step 1) First, a mold is prepared. The mold is not particularly limited as long as it can form the retaining layer 11, but it is preferable that the mold has a shape that can form the shape of the retaining layer 11. The material of the mold is not particularly limited as long as it can form the retaining layer 11, and examples of the material include a metal mold, a plastic mold, and a resin mold.

[0026] (Step 2) Next, a substrate is placed in the mold. The substrate is not particularly limited as long as it is a substrate on which the photocurable resin can be placed and does not block light, and flexible films, nonwoven fabrics, woven fabrics, etc. can be used. The placement of the substrate is not essential as a step of the manufacturing method, but it is preferable to use it because it allows the photocurable resin to be stably cured.

[0027] (Step 3) A photocurable resin is placed on the substrate. The photocurable resin may be a commercially available resin such as "Cosmolite" manufactured by Toyobo Co., Ltd., "PG Plate" manufactured by Toray Industries, Inc., or "Fuji Torelief" manufactured by Fujifilm Corporation, or a resin having desired properties may be manufactured by oneself. The photocurable resin may be used in either a liquid or solid state at room temperature, but it is preferable to use a resin that is solid at room temperature from the viewpoint of workability.

[0028] (Step 4) Next, the photocurable resin is irradiated with light from the substrate side to bond the substrate and the photocurable resin. "Irradiating light from the substrate side" means that in Step 3, in a state where the photocurable resin is placed on the substrate inside the mold, light is irradiated from below the substrate (from the bottom of the mold). As described above, by using a substrate that transmits light, the photocurable resin placed on the substrate can be cured. This process allows the photocurable resin on the substrate side to be cured uniformly, so that in the subsequent process, the convex parts 110A located on the opposite side to the substrate are not independent of each other, and are not independently separable, but the entire holding layer and holding surface are formed as an integral body. The substrate is not exposed from the supporting surface 110 of the supporting layer 11 .

[0029] The light irradiating device is not particularly limited as long as it is a device that emits light in a wavelength range including the wavelength of light at which the photocurable resin is cured, and examples thereof include ultraviolet ray irradiating devices, and more specifically, high pressure mercury lamps, UV-LED lamps, and black light blue fluorescent lamps (BLB), with BLB being preferred. The wavelength of the ultraviolet ray irradiation is preferably 315 nm to 400 nm, and the irradiation time is preferably 1 minute to 15 minutes.

[0030] (Step 5) A masking sheet that can impart a concave-convex structure is placed on the side of the photocurable resin opposite to the substrate. That is, the masking sheet is placed on the side where the photocurable resin is exposed, not on the side where the substrate and the photocurable resin are in contact. The substrate and the photocurable resin are bonded by the above-mentioned photocuring, but the side where the substrate is not bonded is in an uncured state at this point. A masking sheet is placed on the uncured photocurable resin. The masking sheet is not particularly limited as long as it is a sheet made of a material that blocks light, and cellulose triacetate (TAC) or polyethylene terephthalate (PET) can be used.

[0031] (Step 6) By irradiating light from above the masking sheet, the unmasked photocurable resin is cured, and this curing determines the shape of the holding surface 110. The same ultraviolet irradiating device as that used in the process of bonding the base material and the photocurable resin can be used, and the wavelength, illuminance, and irradiation time of the ultraviolet irradiation are adjusted according to the type of photocurable resin and the desired shape of the holding surface 110.

[0032] (Step 7) Next, the uncured photocurable resin is washed away using a solvent. The substrate is bonded to the support layer 11, which is made of photocurable resin cured by light. The solvent is not particularly limited as long as it can remove the uncured photocurable resin, but it is preferable to use water. The retaining layer 11 is environmentally friendly because the amount of solvent used in the manufacturing process can be reduced or eliminated. The obtained retaining layer 11 is connected to a retaining platen 2 to which the substrate is bonded, as shown in Fig. 1, and is subjected to a polishing process. If necessary, an adhesive layer such as a double-sided tape may be further provided on the surface of the substrate opposite to the surface to which the photocurable resin is bonded, and the retaining layer 11 may be connected to the retaining platen via this adhesive layer. EXAMPLES

[0033] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0034] In each of the examples and comparative examples, unless otherwise specified, "parts" means "parts by mass".

[0035] (Manufacture of holding pads) <Example 1> A mold was prepared and a PET film substrate was placed on the bottom side of the mold. Cosmolite (Toyobo Co., Ltd.), a photocurable resin, was placed on top of the PET film substrate, and the substrate and photocurable resin were bonded by irradiating the BLB from the substrate side for 3 minutes. A masking sheet with multiple holes so that convex parts could be formed was placed on the surface of the photocurable resin opposite the substrate, and the unmasked photocurable resin was cured by irradiating it with the BLB from above the masking sheet for 3 minutes. The uncured photocurable resin was washed away with water to obtain a holding layer 11 made of cured photocurable resin. Note that since water was used for washing away, no solvent was used. A double-sided tape was attached to the surface of the substrate opposite to the surface to which the photocurable resin was attached to obtain a holding pad 10.

[0036] <Example 2> A mold was prepared and a PET film substrate was placed on it. A photocurable resin, Shikou (UV-curable urethane acrylate, manufactured by Mitsubishi Chemical Corporation), was placed on top of the PET film substrate, and the substrate and photocurable resin were bonded by irradiating the BLB onto the photocurable resin from the substrate side for 3 minutes. A masking sheet with multiple holes so that convex parts could be formed was placed on the surface of the photocurable resin opposite the substrate, and the unmasked photocurable resin was cured by irradiating it with the BLB from above the masking sheet for 3 minutes. The uncured photocurable resin was washed away with water to obtain a holding layer 11 made of cured photocurable resin. A double-sided tape was attached to the surface of the substrate opposite to the surface to which the photocurable resin was attached to obtain a holding pad 10.

[0037] <Comparative Example 1> A resin solution was obtained by adding and mixing 50 parts of DMF, 5 parts of water, 2 parts of carbon black, and 1 part of surfactant to 100 parts of a DMF solution containing 30 mass % of polyester polyurethane resin having a 100% modulus of 6 MPa. The obtained resin solution was cast onto a polyester film to a thickness of 1.2 mm using a reverse coater set to a clearance of 1.5 mm. Thereafter, the polyester film onto which the resin solution had been cast was immersed in a coagulation bath (water) (at 20°C for 60 minutes) to coagulate the resin solution, and then peeled off, washed and dried to obtain a wet resin sheet. The skin layer of the resin sheet was buffed, and then a double-sided tape was attached to the surface opposite to the buffed surface to obtain a holding pad. Note that a large amount of DMF was used in the manufacturing process of Comparative Example 1.

[0038] <Comparative Example 2> Acrylic phenol resin (Arakawa Kogyo Co., Ltd.) was placed on a PET film substrate and cured by heating. The cured resin surface was cut into a lattice pattern. Double-sided tape was attached to the opposite side of the cut surface of the resin to obtain a holding pad.

[0039] Table 1 shows the materials and manufacturing methods of the holding pads of Examples 1 and 2 and Comparative Examples 1 and 2, as well as the results of the following evaluation of each holding pad.

[0040] [Table 1]

[0041] (Surface shape formation) Using the holding pads of Examples 1 and 2 and Comparative Examples 1 and 2, a wafer was adsorbed as the workpiece to be polished, and a polishing test was carried out under the following conditions. After the polishing test, the surface of the workpiece that was in contact with the holding pad was visually checked, and if there was no damage, it was rated as ◯, and if there was damage, it was rated as ×. In Comparative Example 2, cutting was performed to create an uneven surface shape, and burrs from this process caused scratches on the workpiece during the polishing test.

[0042] (Chemical resistance) A polishing test was carried out under the following conditions. If the holding pad peeled off within 10 hours, it was rated as ×, if it peeled off within 18 hours, it was rated as △, and if it withstood 18 hours or more, it was rated as ◯.

[0043] (Polishing effect) If both the surface shape formation and chemical resistance were rated as ◯, polishing could be performed without any problems, and the polishing effect was rated as ◯. If either was rated as △, the polishing effect was rated as △, since it had a greater effect on polishing than the polishing effect rated as ◯. If either was rated ×, the material could not be used for polishing, and the polishing effect was rated ×.

[0044] (polishing conditions) Polishing machine used: 15inch single-sided polishing machine Abrasive temperature: 50~120 degrees Polishing platen rotation speed: 60~100rpm Polishing head rotation speed: 30~50rpm Grinding pressure: 350~500g / cm 2 Polishing slurry (metal film): Potassium permanganate + lubricant liquid Polishing slurry flow rate: 5 cc / min Polishing time: 3 to 20 hours Polished object (metal film): SiC WF [Industrial Applicability]

[0045] The present invention provides a holding pad that is chemical resistant, has an integral holding layer, and can be given a variety of uneven structures on its holding surface, has an appropriate adhesive force that can be adjusted, and can facilitate the release of the polished object. Therefore, the present invention contributes to the manufacture and sale of holding pads, and has industrial applicability.

[0046] 1 Holder 10 Retaining Pad 11 Retention layer 110 Holding surface 110A Convex 110B Recess 13 Part of the holding surface having a frame-shaped member (joint part between the holding surface and the frame-shaped member) 12 Frame-shaped member 2 Holding plate 3 Polishing Pads 4 Polishing plate W Object to be polished

Claims

1. A holding pad having a holding layer for holding an object to be polished, The holding pad, wherein the holding layer is made of a photocurable resin.

2. The density of the support layer is 0.5 kg / m 3 Above, 3.0kg / m 3 2. The support pad of claim 1, wherein:

3. The support pad of claim 1 , wherein the support layer has a Shore A hardness of 60 or more and 90 or less.

4. The support pad according to claim 1 , wherein the support layer has a compressibility of 0.1% or more and 10% or less.

5. The support pad according to claim 1 , wherein the support layer has a compressive elastic modulus of 60% or more and 90% or less.

6. The support pad of claim 1 , wherein the support layer is integrally provided with a support surface, and the photocurable resin is an ultraviolet curable resin.

7. The support pad of claim 1 , wherein the photocurable resin is an acrylic resin.

8. 2. The holding pad according to claim 1, wherein said holding surface is formed with recesses or protrusions, and the average height of said recesses or protrusions is 0.3 mm or more and 1.5 mm or less.

9. 2. A holder, further comprising a frame member on an outer periphery of the holding surface of the holding pad according to claim 1, the frame member being made of glass epoxy or SUS.

10. The holder according to claim 9 , wherein a recess or a protrusion is formed on the holding surface of the holding pad according to claim 1 in a portion that includes the frame member.

11. A method for manufacturing a holding pad, comprising: Preparing a mold; placing a photocurable resin in the mold; A step of placing a masking sheet on the photocurable resin so that a concave-convex structure can be imparted; a step of curing the unmasked photocurable resin by irradiating light from above the masking sheet; and washing away the uncured photocurable resin with a solvent to obtain a retaining layer made of cured photocurable resin.

12. A method for manufacturing a holding pad, comprising: a holding layer for holding an object to be polished, the holding layer being made of a photocurable resin; and a substrate being provided as a separate member on an opposite side to the holding surface, the method comprising: Preparing a mold; providing a substrate in the mold; disposing a photocurable resin on the substrate; a step of irradiating the photocurable resin with light from a substrate side to bond the substrate and the photocurable resin; A step of placing a masking sheet on the opposite side of the substrate from the photocurable resin so that a concave-convex structure can be imparted; a step of curing the unmasked photocurable resin by irradiating light from above the masking sheet; and washing away the uncured photocurable resin using a solvent to obtain a substrate-attached support layer composed of a cured photocurable resin to which the substrate is adhered.

Citation Information

Patent Citations

  • Manufacture for work holding block

    JP2000190209A

  • Conditioning free CMP pad, its manufacturing method, and polishing method of substrate

    JP2004119875A

  • Holder and manufacturing method for holder

    JP2018161732A

  • Elastic film for holding wafer of CMP device

    JP2018182064A

  • Head assembly for edge polishing apparatus of wafer

    KR1020100081695A