Composition for polishing and polishing method

The polishing composition with colloidal silica and a perhalogen oxidizing agent addresses the challenge of polishing gallium nitride semiconductors by achieving a high removal rate and high surface quality.

JP2024141600APending Publication Date: 2024-10-10FUJIMI INCORPORATED
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023053339
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Gallium nitride semiconductors are chemically stable, have low reactivity, and high hardness, making them difficult to polish effectively, while requiring a high polishing removal rate and high surface quality.

Method used

A polishing composition comprising colloidal silica, a pH adjuster, and a perhalogen oxidizing agent, such as periodic acid, is used to improve the polishing removal rate and achieve high surface quality.

Benefits of technology

The composition achieves a high polishing removal rate of 170 nm/hour or more with a surface roughness Ra of less than 0.1 nm, effectively polishing gallium nitride semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141600000001
    Figure 2024141600000001
Patent Text Reader

Abstract

To provide a composition for polishing that is used for polishing of a gallium nitride semiconductor substrate, and can increase polishing and removal speed while obtaining high surface quality.SOLUTION: There is provided a composition for polishing that is used for polishing of a gallium nitride semiconductor substrate. The composition for polishing contains colloidal silica, a pH adjuster, a perchloric acid oxidizing agent, and water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing composition, and more particularly to a polishing composition used for polishing a gallium nitride semiconductor substrate, and a polishing method using the polishing composition. [Background technology]

[0002] Gallium nitride semiconductors are becoming increasingly important as compound semiconductor substrates used in power devices, light-emitting diodes (LEDs), and the like. When manufacturing power devices and the like using a gallium nitride semiconductor substrate, the surface of the semiconductor substrate is generally polished to obtain a smooth surface without processing damage. In polishing a gallium nitride semiconductor substrate, lapping is performed by supplying diamond abrasive grains to a polishing table, and then polishing is performed by supplying a slurry containing abrasive grains between a polishing pad and the object to be polished, or chemical etching is performed using a solution that does not contain abrasive grains. Patent Document 1 is an example of a technical document related to polishing a gallium nitride semiconductor substrate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 2019-535146 Summary of the Invention [Problem to be solved by the invention]

[0004] Gallium nitride semiconductor is chemically very stable, has low reactivity, and has very high hardness, so that it is not easy to process it by polishing.On the other hand, in the embodiment of polishing, particularly polishing, the above-mentioned gallium nitride semiconductor substrate, high polishing removal rate is required, and the polishing composition used in the above-mentioned polishing is required to improve the polishing removal rate while realizing the required surface quality after polishing.

[0005] The present invention has been made in view of the above circumstances, and its main object is to provide a polishing composition that can be used for polishing a gallium nitride semiconductor substrate to improve the polishing removal rate while obtaining high surface quality. Another related object is to provide a method for polishing a gallium nitride semiconductor substrate using the polishing composition. [Means for solving the problem]

[0006] According to the present specification, a polishing composition for use in polishing a gallium nitride semiconductor substrate is provided. The polishing composition contains colloidal silica, a pH adjuster, a perhalogen acid oxidizing agent, and water. With this polishing composition, the polishing removal rate can be improved while achieving high surface quality in polishing a gallium nitride semiconductor substrate.

[0007] In some preferred embodiments, the colloidal silica has a ratio (D90 / D10) of 90% cumulative frequency particle size (D90) to 10% cumulative frequency particle size (D10) of 2.0 or more in a volume-based particle size distribution measured by a dynamic light scattering method. Colloidal silica having such a particle size distribution is likely to achieve a higher polishing removal rate.

[0008] In some preferred embodiments, the content of the perhalogen acid-based oxidizing agent is 0.015 mol / L or more. By setting the concentration of the perhalogen acid-based oxidizing agent to 0.015 mol / L or more, the polishing removal rate can be preferably improved.

[0009] In some embodiments, the perhalogen acid-based oxidizing agent is at least one selected from the group consisting of periodic acid, perchloric acid, and salts thereof. The perhalogen acid-based oxidizing agent preferably exhibits the effects of the technology disclosed herein.

[0010] In some embodiments, the pH of the polishing composition is preferably higher than 0.5 and lower than 2.0. A polishing composition having a low pH range as described above tends to provide a higher polishing removal rate and has good stability.

[0011] This specification also provides a method for polishing a gallium nitride semiconductor substrate. The polishing method includes a step of polishing a gallium nitride semiconductor substrate with any one of the polishing compositions disclosed herein. This polishing method can improve the polishing removal rate for the gallium nitride semiconductor substrate, and can finish the substrate surface after polishing to a high surface quality. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Preferred embodiments of the present invention will be described below. Note that matters other than those specifically mentioned in this specification that are necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field.

[0013] <Object to be polished> The polishing composition disclosed herein is used to polish a gallium nitride semiconductor substrate. In the present specification, the concept of a gallium nitride semiconductor includes, in addition to gallium nitride (GaN), semiconductors having a composition in which a part of Ga is replaced with other group 13 elements of the periodic table (B, Al, In), such as AlGaN, GaInN, AlGaInN, etc. The polishing composition disclosed herein can be preferably used for polishing a substrate having a surface made of such a gallium nitride semiconductor material. The surface, i.e., the surface to be polished, is typically the gallium surface of the gallium nitride semiconductor material. The gallium nitride semiconductor substrate may be a free-standing gallium nitride semiconductor wafer, or may have a gallium nitride semiconductor crystal on an appropriate underlayer. Examples of such underlayers include a sapphire substrate, a silicon substrate, a SiC substrate, etc. The gallium nitride semiconductor may be doped for the purpose of imparting electrical conductivity, or may be non-doped.

[0014] <Polishing composition> (Abrasive grain) The polishing composition disclosed herein contains colloidal silica as an abrasive. By polishing with a polishing composition containing colloidal silica, scratches generated on the object to be polished in a previous process such as lapping can be removed more efficiently. By using a polishing composition containing colloidal silica, high surface quality is easily obtained, and a high polishing removal rate and good surface quality can be suitably achieved. As an example of an index of surface quality, the surface roughness Ra described below can be used. Examples of the colloidal silica include silica produced using an alkali silicate-containing liquid (e.g., a sodium silicate-containing liquid) containing an alkali metal such as Na or K and SiO2 as a raw material, and silica (alkoxide method silica) produced by a hydrolysis condensation reaction of alkoxysilane such as tetraethoxysilane or tetramethoxysilane. The shape (outer shape) of the colloidal silica may be spherical or non-spherical. In addition, the colloidal silica may be surface-modified. Specifically, the surface modification of the colloidal silica is performed by attaching or bonding a substance having a different electric potential from that of the colloidal silica surface to the colloidal silica surface to change the electric potential of the colloidal silica surface. There is no limitation on the substance used to change the electric potential of the colloidal silica surface, and examples of the substance that can be used include surfactants, inorganic acids, organic acids, etc. The colloidal silica may be used alone or in combination of two or more types that differ in production conditions, physical properties, shapes, surface characteristics, etc.

[0015] The technology disclosed herein can be preferably implemented in an embodiment in which the proportion of colloidal silica in the total weight of the abrasive grains contained in the polishing composition is greater than 70% by weight, from the viewpoint of improving the surface quality after polishing.The proportion of the colloidal silica is more preferably 90% by weight or more, even more preferably 95% by weight or more, and particularly preferably 99% by weight or more.Among them, the polishing composition in which 100% by weight of the abrasive grains contained in the polishing composition are colloidal silica is preferred.

[0016] The particle diameter (Dsa) of the colloidal silica in terms of specific surface area is not particularly limited, and in some embodiments, it is usually preferably 150 nm or less, more preferably 100 nm or less, even more preferably 70 nm or less, even more preferably 60 nm or less, even more preferably 50 nm or less, and particularly preferably 40 nm or less. By using colloidal silica with a small diameter, higher surface quality can be obtained. In some embodiments, the particle diameter (Dsa) of the colloidal silica in terms of specific surface area is preferably, for example, 5 nm or more, more preferably 10 nm or more, even more preferably 20 nm or more, and particularly preferably 30 nm or more. As the particle diameter of colloidal silica increases, the polishing removal rate tends to improve.

[0017] In this specification, the particle size converted to specific surface area (Dsa) is calculated from the specific surface area (BET value) measured by the BET method as follows: BET diameter (nm) = 6000 / (true density (g / cm 3 ) × BET value (m 2 The specific surface area is the particle size calculated by the formula: (1) specific surface area = specific surface area (µm / g) The specific surface area can be measured using, for example, a surface area measuring device manufactured by Micromeritics, Inc., under the trade name "Flow Sorb II 2300".

[0018] The average secondary particle diameter of the colloidal silica contained in the polishing composition is not particularly limited, and in some embodiments, it is usually preferably 10 nm or more, more preferably 20 nm or more, even more preferably 30 nm or more, even more preferably 40 nm or more, even more preferably 50 nm or more, and particularly preferably 60 nm or more. As the average secondary particle diameter of colloidal silica increases, the polishing removal rate tends to improve. In addition, from the viewpoint of obtaining higher surface quality, in some embodiments, the average secondary particle diameter of colloidal silica is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, even more preferably 100 nm or less, and even more preferably 80 nm or less. In this specification, the average secondary particle diameter of colloidal silica refers to the volume average particle diameter (volume average diameter D50) based on dynamic light scattering method.

[0019] In some embodiments, the colloidal silica preferably has a ratio (D90 / D10) of the cumulative frequency 90% particle size (D90) to the cumulative frequency 10% particle size (D10) in the volume-based particle size distribution by dynamic light scattering method greater than 1.5, more preferably 1.8 or more. By using colloidal silica having a broad particle size distribution in which the ratio (D90 / D10) is a predetermined value or more, it is easy to obtain an effect of improving the polishing removal rate in polishing a gallium nitride semiconductor substrate while obtaining high surface quality. In some preferred embodiments, the ratio (D90 / D10) is 2.0 or more, more preferably 2.2 or more, even more preferably 2.4 or more, and particularly preferably 2.5 or more. Colloidal silica having such a particle size distribution is easy to obtain a higher polishing removal rate.

[0020] The average secondary particle diameter (volume average diameter D50) and ratio (D90 / D10) of colloidal silica can be measured using a commercially available dynamic light scattering particle size analyzer, for example, a Microtrac model "UPA-UT151" or an equivalent. The measurement conditions are appropriately adjusted, but as an example, the measurement can be performed under the conditions described in the Examples.

[0021] The concentration of colloidal silica in the polishing composition is not particularly limited. In some embodiments, the concentration of colloidal silica is, for example, preferably 5% by weight or more, more preferably 12% by weight or more, even more preferably 17% by weight or more, and particularly preferably 22% by weight or more. As the concentration of colloidal silica increases, the polishing removal rate tends to improve. In addition, from the viewpoint of achieving both a high level of polishing removal rate and a high level of surface quality after polishing, in some embodiments, the concentration of colloidal silica is usually preferably about 50% by weight or less, more preferably 40% by weight or less. In some preferred embodiments, the concentration of colloidal silica is 35% by weight or less.

[0022] The polishing composition disclosed herein may contain silica particles other than the colloidal silica (e.g., dry process silica, fumed silica, precipitated silica, etc.) as abrasive grains, or may not substantially contain silica particles other than the colloidal silica, as long as the effects of the present invention are not significantly impaired. In addition, the polishing composition may contain abrasive grains made of a material other than silica (hereinafter also referred to as non-silica particles), or may not substantially contain non-silica particles, as long as the effects of the present invention are not significantly impaired. Examples of the constituent materials of such non-silica particles include oxides such as aluminum oxide, cerium oxide, chromium oxide, titanium dioxide, zirconium oxide, magnesium oxide, manganese oxide, zinc oxide, and iron oxide particles; nitrides such as silicon nitride and boron nitride; carbides such as silicon carbide and boron carbide particles; diamond; and the like.

[0023] In addition, the polishing composition disclosed herein can be preferably implemented in an embodiment that does not substantially contain alumina particles. Examples of alumina particles include α-alumina, intermediate alumina other than α-alumina, and composites thereof. Intermediate alumina is a general term for alumina particles other than α-alumina, and specific examples include γ-alumina, δ-alumina, θ-alumina, η-alumina, κ-alumina, and composites thereof. By using such a polishing composition that does not substantially contain alumina particles, the deterioration of surface quality after polishing is prevented.

[0024] In this specification, "substantially not containing silica particles other than colloidal silica, non-silica particles, for example, alumina particles" means that the proportion of the particles in the total solid content of the polishing composition is 1% by weight or less, more preferably 0.5% by weight or less, for example 0.1% by weight or less.For example, a polishing composition with alumina particles of 0% by weight, that is, a polishing composition that does not contain alumina particles, is particularly preferred.

[0025] (pH adjuster) The polishing composition disclosed herein contains a pH adjuster. By adding an appropriate amount of a suitable pH adjuster to the polishing composition, the pH of the polishing composition can be adjusted to a desired range. The concentration of the pH adjuster is not particularly limited, and an appropriate amount is used so that the pH of the polishing composition is in the desired range.

[0026] In some preferred embodiments, the polishing composition contains one or more acids as a pH adjuster. Specific examples of the acid include inorganic acids such as sulfuric acid, nitric acid, hydrochloric acid, chloric acid, bromic acid, phosphoric acid, phosphonic acid, phosphinic acid, and boric acid; and organic acids such as acetic acid, itaconic acid, succinic acid, tartaric acid, citric acid, maleic acid, glycolic acid, malonic acid, methanesulfonic acid, formic acid, malic acid, gluconic acid, alanine, glycine, lactic acid, trifluoroacetic acid, and trifluoromethanesulfonic acid; and the like. The acid may be used in the form of a salt of the acid. The salt of the acid may be, for example, an alkali metal salt such as a sodium salt or a potassium salt, or an ammonium salt. In some embodiments, the acid as a pH adjuster is added to the polishing composition in the form of a compound other than an acid salt (particularly a metal salt). In some other embodiments, the polishing composition may contain one or more alkalis as a pH adjuster. Specific examples of alkali include inorganic alkali compounds derived from alkali metals such as sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, and potassium hydrogen carbonate, and organic alkali compounds such as ammonia and amines. Acids and alkalis may be used in combination. As pH adjusters, inorganic acids such as nitric acid, hydrochloric acid, sulfuric acid, and phosphoric acid are preferably used.

[0027] (Oxidizing agent) The polishing composition disclosed herein contains a perhalogen acid compound (i.e., a perhalogen acid oxidizing agent) as an oxidizing agent. The polishing composition containing a perhalogen acid oxidizing agent can improve the polishing removal rate while realizing high surface quality in polishing a gallium nitride semiconductor substrate. It is considered that the perhalogen acid compound exerts a superior oxidizing effect on the surface of a gallium nitride semiconductor substrate compared with other oxidizing agents, and improves the polishing removal rate. Therefore, although not particularly limited, the perhalogen acid oxidizing agent can obtain a desired polishing removal rate improvement effect without relying on other oxidizing agents such as peracids or polishing assistants. As the perhalogen acid oxidizing agent, periodic acid, perchloric acid, and salts thereof (e.g., sodium salt, potassium salt, etc.) are preferably used. Among them, periodic acid or its salt is more preferable, and periodic acid is particularly preferable. The perhalogen acid oxidizing agent can be used alone or in combination of two or more kinds. When the perhalogen acid-based oxidizing agent is a salt (for example, a periodate), the salt may be present in the polishing composition in the form of ions.

[0028] The concentration of the perhalogen acid-based oxidizing agent in the polishing composition is not particularly limited. In some embodiments, the concentration of the perhalogen acid-based oxidizing agent is usually preferably 0.0001 mol / L or more, more preferably 0.001 mol / L or more, even more preferably 0.005 mol / L or more, even more preferably 0.008 mol / L or more, even more preferably 0.01 mol / L or more. In some preferred embodiments, the concentration of the perhalogen acid-based oxidizing agent is 0.015 mol / L or more, more preferably 0.02 mol / L or more, even more preferably 0.03 mol / L or more. By increasing the concentration of the perhalogen acid-based oxidizing agent, the polishing removal rate can be preferably improved in polishing the gallium nitride semiconductor substrate. In some embodiments, the concentration of the perhalogen acid-based oxidizing agent is usually preferably 10 mol / L or less, and from the viewpoint of maintaining high surface quality, is preferably 1 mol / L or less, more preferably 0.5 mol / L or less, even more preferably 0.1 mol / L or less, even more preferably 0.08 mol / L or less, and particularly preferably 0.05 mol / L or less.

[0029] The polishing composition disclosed herein may contain an oxidizing agent other than a perhalogen acid-based oxidizing agent, or may not substantially contain an oxidizing agent other than the perhalogen acid-based oxidizing agent, as long as the effect of the present invention is not significantly impaired. Examples of oxidizing agents other than perhalogen acid-based oxidizing agents include hydrogen peroxide; nitric acid compounds, such as nitrates such as iron nitrate, silver nitrate, and aluminum nitrate, and nitric acid complexes such as cerium ammonium nitrate; persulfates, such as metal persulfates such as sodium persulfate and potassium persulfate, and persulfates such as ammonium persulfate; chloric acids, such as chlorates; bromic acids, such as bromates such as potassium bromate; iodic acids, such as iodates such as ammonium iodate; dichloroisocyanurates such as sodium dichloroisocyanurate and potassium dichloroisocyanurate; ferric acids, such as ferrates such as potassium ferrate; persulfates, such as ammonium iodate; Examples of the acid salts include manganic acids, such as permanganates such as sodium permanganate and potassium permanganate; chromic acids, such as chromates such as potassium chromate and potassium dichromate; vanadic acids, such as metavanadates such as ammonium metavanadate, sodium metavanadate and potassium metavanadate; perruthenic acids, such as perruthenate; molybdic acids, such as molybdates such as ammonium molybdate and disodium molybdate; perrhenic acids, such as perrhenate; and tungstic acids, such as tungstates such as disodium tungstate. These may be used alone or in appropriate combination of two or more.

[0030] Although not particularly limited, the technology disclosed herein can be preferably implemented in an embodiment in which the ratio of the perhalogen acid-based oxidizing agent in the oxidizing agent contained in the polishing composition is greater than 50% by weight, from the viewpoint of effectively exerting the effect of the perhalogen acid-based oxidizing agent (improving the polishing removal rate). In some embodiments, the ratio of the perhalogen acid-based oxidizing agent is more preferably greater than 70% by weight, even more preferably 80% by weight or more, even more preferably 90% by weight or more, even more preferably 95% by weight or more, and particularly preferably 99% by weight or more. Among them, a polishing composition in which 100% by weight of the oxidizing agent contained in the polishing composition is a perhalogen acid-based oxidizing agent is preferred.

[0031] Although not particularly limited, in some embodiments, the polishing composition can be preferably implemented in an embodiment that does not substantially contain a complex metal oxide as an oxidizing agent, which is a salt of a cation selected from alkali metal ions and an anion selected from transition metal oxoacid ions. According to the technology disclosed herein, a high polishing removal rate can be achieved with a composition that does not use the complex metal oxide as an oxidizing agent. Such a composition is also preferable from the viewpoint of achieving both a polishing removal rate and dispersion stability of colloidal silica. Specific examples of the transition metal oxoacid ions in the complex metal oxide include permanganate ions, ferrate ions, chromate ions, dichromate ions, vanadate ions, ruthenate ions, molybdate ions, rhenate ions, tungstate ions, etc. The alkali metal ions in the complex transition metal oxide include Na + K may be + may be also possible.

[0032] In some embodiments, the polishing composition is preferably substantially free of permanganic acids as an oxidizing agent. A polishing composition that is substantially free of permanganic acids as an oxidizing agent can reduce the risk of corrosion of the substrate support material and the polishing pad.

[0033] In some embodiments, the polishing composition is preferably substantially free of molybdic acids, vanadic acids, and tungstic acids as oxidizing agents. According to the technology disclosed herein, a high polishing removal rate can be achieved with a composition that does not use molybdic acids, vanadic acids, and tungstic acids as oxidizing agents. Such a composition is also preferable from the viewpoint of achieving both the polishing removal rate and the dispersion stability of colloidal silica.

[0034] In the embodiment in which an oxidizing agent other than a perhalogen acid-based oxidizing agent is used, the oxidizing agent other than a perhalogen acid-based oxidizing agent may be substantially free of metal salts (specifically, alkali metal salts such as potassium and sodium, and alkaline earth metal salts). According to the technology disclosed herein, it is possible to improve the polishing removal rate without containing metals derived from the oxidizing agent (specifically, alkali metals and alkaline earth metals). This is advantageous in that it is easy to obtain dispersion stability of colloidal silica, etc.

[0035] In some embodiments, the polishing composition is substantially free of hydrogen peroxide as an oxidizing agent. According to the technology disclosed herein, a high polishing removal rate can be achieved with a composition that does not use hydrogen peroxide as an oxidizing agent.

[0036] In this specification, "substantially free of oxidizing agents other than perhalogen acid-based oxidizing agents (for example, composite metal oxides, permanganic acids, molybdic acids, vanadic acids, tungstic acids, metal salts, or hydrogen peroxide)" means that such oxidizing agents are not blended at least intentionally, and it is acceptable for a trace amount of oxidizing agent to be inevitably contained due to the raw materials, manufacturing method, etc. For example, the concentration of the oxidizing agent other than the perhalogen acid-based oxidizing agent in the polishing composition (for example, it may be each or all of a complex metal oxide, permanganic acid, molybdic acid, vanadic acid, and tungstic acid. In some embodiments, it may be an oxidizing agent other than the perhalogen acid-based oxidizing agent in the form of a metal salt. Or hydrogen peroxide.) is preferably less than 0.003 mol / L, more preferably less than 0.001 mol / L, even more preferably less than 0.0005 mol / L, even more preferably less than 0.0001 mol / L, even more preferably less than 0.00001 mol / L, and particularly preferably less than 0.000001 mol / L. The concentration of the oxidizing agent may be zero or below the detection limit.

[0037] (water) The polishing composition disclosed herein contains water as an essential component. As the water, ion-exchanged water (deionized water), pure water, ultrapure water, distilled water, etc. can be preferably used. The polishing composition disclosed herein may further contain an organic solvent (lower alcohol, lower ketone, etc.) that can be uniformly mixed with water, if necessary. Usually, it is preferable that 90% by volume or more of the solvent contained in the polishing composition is water, and more preferably 95% by volume or more (typically 99 to 100% by volume) is water.

[0038] (Other Ingredients) The polishing composition disclosed herein may contain an alkali metal salt and an alkaline earth metal salt as an optional component different from the oxidizing agent, or may be substantially free of the metal salt from the viewpoint of dispersion stability, etc. Although not particularly limited, in some embodiments, the concentration of the alkali metal salt and the alkaline earth metal salt in the polishing composition is preferably less than 0.001 mol / L, more preferably less than 0.0005 mol / L, even more preferably less than 0.0001 mol / L, even more preferably less than 0.00001 mol / L, and particularly preferably less than 0.000001 mol / L.

[0039] The polishing composition disclosed herein may further contain, as necessary, known additives that can be used in polishing compositions (for example, polishing compositions for gallium nitride substrates), such as chelating agents, thickeners, dispersants, surface protective agents, wetting agents, surfactants, rust inhibitors, preservatives, and fungicides, within the scope that does not impair the effects of the present invention. The content of the above additives may be appropriately set according to the purpose of their addition.

[0040] (pH) The pH of the polishing composition disclosed herein can be set in an appropriate range that can realize a desired polishing removal rate. In some embodiments, the pH of the polishing composition is, for example, preferably less than 7.0, more preferably less than 6.0, even more preferably less than 5.0, and even more preferably less than 4.0. By using a polishing composition with a lower pH, the polishing removal rate tends to improve. In some preferred embodiments, the pH of the polishing composition is, for example, less than 3.0, more preferably less than 2.5, even more preferably less than 2.0, even more preferably less than 1.5, and particularly preferably less than 1.3. A polishing composition that contains a perhalogen acid-based oxidizing agent and has a low pH range as described above can realize a particularly excellent polishing removal rate. The lower limit of the pH of the polishing composition is not particularly limited, but from the viewpoints of dispersion stability of colloidal silica, corrosion inhibition of equipment, environmental hygiene, etc., it is usually appropriate to be greater than 0.5, and may be 0.7 or more, or may be 0.9 or more. In this specification, the pH can be determined by using a pH meter and performing three-point calibration using standard buffer solutions (phthalate pH buffer solution, pH: 4.01 (25°C), neutral phosphate pH buffer solution, pH: 6.86 (25°C), carbonate pH buffer solution, pH: 10.01 (25°C)), then placing a glass electrode in the composition to be measured and measuring the value after 2 minutes or more have elapsed and the value has stabilized. As the pH meter, for example, a glass electrode type hydrogen ion concentration indicator (model number F-23) manufactured by Horiba, Ltd. or an equivalent product can be used.

[0041] <Production of Polishing Composition> The method for producing the polishing composition disclosed herein is not particularly limited.For example, it is advisable to use a well-known mixing device such as a blade type agitator, an ultrasonic disperser, a homomixer, etc. to mix each component contained in the polishing composition.The manner of mixing these components is not particularly limited, and for example, all components may be mixed at once, or may be mixed in a suitably set order.

[0042] The polishing composition disclosed herein may be a one-component type, or may be a multi-component type including a two-component type.For example, the polishing composition may be configured such that the A liquid containing some of the components (typically components other than solvent) of the polishing composition and the B liquid containing the remaining components are mixed together and used for polishing the object to be polished.

[0043] The polishing composition disclosed herein may be in a concentrated form (i.e., in the form of a concentrated polishing liquid) before being supplied to an object to be polished. Such a concentrated polishing composition is advantageous from the viewpoints of convenience and cost reduction during production, distribution, storage, etc. The concentration ratio can be, for example, about 1.2 to 5 times in volume.

[0044] The polishing composition in the form of a concentrated liquid can be used in such a manner that the polishing liquid is prepared by diluting at a desired time and the polishing liquid is supplied to the object to be polished. The dilution can typically be performed by adding the above-mentioned solvent to the concentrated liquid and mixing. In addition, when the solvent is a mixed solvent, dilution can be performed by adding only a part of the components of the solvent, or by adding a mixed solvent containing the components in a different amount ratio from the solvent. In the case of a multi-agent type polishing composition, a part of the agents may be diluted and then mixed with other agents to prepare a polishing liquid, or a plurality of agents may be mixed and then the mixture may be diluted to prepare a polishing liquid.

[0045] <Polishing method> The polishing composition disclosed herein can be used for polishing an object to be polished, for example, in an embodiment including the following steps. That is, prepare a polishing liquid (slurry) containing any of the polishing compositions disclosed herein. The preparation of the polishing liquid may include adjusting the concentration (e.g., dilution), adjusting pH, etc., of the polishing composition to prepare the polishing liquid. Alternatively, the polishing composition may be used as it is as the polishing liquid. In addition, in the case of a multi-agent type polishing composition, the preparation of the polishing liquid may include mixing the agents, diluting one or more agents before the mixing, diluting the mixture after the mixing, etc. Next, the polishing liquid is supplied to the surface of the object to be polished, and the object is polished by a conventional method (a method normally used by a person skilled in the art). For example, the object to be polished is set in a general polishing device, and the polishing liquid is supplied to the surface of the object to be polished (the surface to be polished) through the polishing pad of the polishing device. Typically, the polishing liquid is continuously supplied, and the polishing pad is pressed against the surface of the object to be polished, and the two are moved relatively (for example, rotated). Through this polishing process, the polishing of the object to be polished is completed.

[0046] According to the present specification, a polishing method for polishing a material to be polished and a method for manufacturing a polished product using the polishing method are provided. The polishing method is characterized by including a step of polishing an object to be polished using the polishing composition disclosed herein. Some preferred embodiments of the polishing method include a step of performing pre-polishing (pre-polishing step) and a step of performing finish polishing (finish polishing step). In a typical embodiment, the pre-polishing step is a polishing step arranged immediately before the finish polishing step. The finish polishing step referred to here is a step of performing finish polishing on an object to be polished that has been pre-polished, and refers to a polishing step arranged at the end (i.e., the most downstream side) of the polishing steps performed using a polishing slurry containing abrasive grains. In the polishing method including the pre-polishing step and the finish polishing step, the polishing composition disclosed herein may be used in the pre-polishing step, may be used in the finish polishing step, or may be used in both the pre-polishing step and the finish polishing step.

[0047] In some preferred embodiments, the polishing step using the polishing composition is a finish polishing step. The polishing composition disclosed herein and the polishing method using the polishing composition can realize a high-quality surface with a small surface roughness Ra after polishing, and therefore can be particularly preferably used in the finish polishing step of the surface of a gallium nitride semiconductor substrate. Although not particularly limited, the polishing composition disclosed herein and the polishing method using the polishing composition can realize a surface roughness Ra of less than 0.1 nm after polishing at a polishing removal rate of 170 nm / hour or more (preferably 200 nm / hour or more, more preferably 220 nm / hour or more, and even more preferably 240 nm / hour or more) in the finish polishing of a gallium nitride semiconductor substrate. The polishing removal rate and surface roughness Ra can be measured, for example, by the method described in the Examples below.

[0048] Preliminary polishing and finish polishing can be applied to both polishing using a single-sided polishing machine and polishing using a double-sided polishing machine. In a single-sided polishing machine, the object to be polished is attached to a ceramic plate with wax or held using a holding device called a carrier, and one side of the object to be polished is polished by pressing a polishing pad against one side of the object to be polished while supplying a polishing composition, and moving the two relatively (for example, rotating). In a double-sided polishing machine, the object to be polished is held using a holding device called a carrier, and while supplying a polishing composition from above, a polishing pad is pressed against the opposing side of the object to be polished, and they are rotated in the relative direction to polish both sides of the object to be polished simultaneously.

[0049] The polishing pad used in each polishing step is not particularly limited. For example, any of nonwoven fabric type, suede type, and hard foam polyurethane type may be used. It is preferable that the polishing pad does not contain abrasive grains.

[0050] The polished object polished by the method disclosed herein is typically washed after polishing. This washing can be performed using a suitable washing liquid. The washing liquid to be used is not particularly limited, and a known or commonly used one can be appropriately selected and used.

[0051] The polishing method disclosed herein may include any other steps in addition to the above-mentioned preliminary polishing step and finish polishing step. Such steps include a lapping step performed before the preliminary polishing step. The lapping step is a step of polishing the object to be polished by pressing the surface of a polishing platen (e.g., a cast iron platen) against the object to be polished. Therefore, a polishing pad is not used in the lapping step. The lapping step is typically performed by supplying abrasive grains (typically diamond abrasive grains) between the polishing platen and the object to be polished. The polishing method disclosed herein may also include an additional step (cleaning step or polishing step) before the preliminary polishing step or between the preliminary polishing step and the finish polishing step.

[0052] <Method of manufacturing polished object> The technology disclosed herein may include a method for producing a polished object (specifically, a method for producing a gallium nitride semiconductor substrate) including a polishing step using the above-mentioned polishing composition, and a method for producing a polished object produced by the method. That is, the technology disclosed herein provides a method for producing a polished object, which includes supplying any of the polishing compositions disclosed herein to a polished object made of a material to be polished, and a polished object produced by the method. The above-mentioned production method can be carried out by preferably applying the contents of any of the polishing methods disclosed herein. The above-mentioned production method can efficiently provide a polished object (specifically, a gallium nitride semiconductor substrate) having a high-quality surface. EXAMPLES

[0053] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in the examples. In the following description, "%" is based on weight unless otherwise specified.

[0054] <Preparation of Polishing Composition> For each example, a polishing composition having the composition shown in Table 1 was prepared. Table 1 also shows the pH of the polishing composition for each example. The colloidal silica used had a specific surface area converted average particle size (Dsa) of 33 nm, and the ratio (D90 / D10) of the 90% cumulative frequency particle size (D90) to the 10% cumulative frequency particle size (D10) in the volume-based particle size distribution measured by dynamic light scattering was 2.6. A pH adjuster was used in a predetermined amount to give the pH shown in Table 1. The balance of the polishing composition for each example was water. The particle size distribution ratio (D90 / D10) was measured using a Microtrac model "UPA-UT151" with 3 measurements and a measurement time of 120 seconds. The colloidal silica concentration in the measurement sample was adjusted so that the loading index, which indicates the total amount of scattered light detected by the device, was 0.03 to 0.05.

[0055] <Polishing removal speed> The polishing composition according to each example was used as a polishing liquid to polish the gallium surface of a commercially available non-doped (n-type) freestanding GaN wafer under the following polishing conditions. All of the GaN wafers used were circular and had a diameter of 2 inches. [Policing conditions] Polishing device: Single-sided polishing device manufactured by Engis Japan, model number "EJ-380IN" Polishing pad: Nitta DuPont, non-woven fabric type, product name "SUBA400 (XA250)" Polishing load: 500gf / cm 2 Rotation speed of the plate: 80 rpm Average linear velocity: 55m / min Polishing fluid supply rate: 10mL / min Polishing time: 60 minutes

[0056] Based on the weight of the wafer before and after the above polishing, the polishing removal rate was calculated according to the following formulas (1) to (3). The results are shown in Table 1. (1) ΔV=(W0-W1) / ρ (2) Δx=ΔV / S (3) R=Δx / t Where: W0: weight of the wafer before polishing, W1: weight of the wafer after polishing, ρ: Specific gravity of GaN (6.15 g / cm 3 ), ΔV: Volume change of the wafer due to polishing, S: surface area of ​​the wafer, Δx: thickness change of the wafer due to polishing, t: polishing time, R: Polishing removal rate.

[0057] <Surface roughness Ra> After the above-mentioned polishing was performed using the polishing composition of each example, the surface roughness Ra of the wafer surface was measured under the following conditions. [Ra measurement conditions] Evaluation equipment: Bruker atomic force microscope (AFM) Device model: nanoscope V Viewing angle: 10μm square Scanning speed: 1Hz (20μm / sec) Number of measurement points per scan: 256 (points) Number of scans: 256 Measurement points: 5 (measurements were taken at one point in the center of the wafer and four points at 90° intervals around the circumference of the 1 / 2 radius of the wafer, and the average of the measurement results at the above five points was recorded as Ra.)

[0058] [Table 1]

[0059] As shown in Table 1, in Examples 1 to 3, in which a polishing composition containing colloidal silica, phosphoric acid as a pH adjuster, and orthoperiodic acid, sodium periodate, or perchloric acid as an additive was used, the polishing removal rate was 177 nm / hour or more. The polishing removal rate of Examples 1 and 2, in which orthoperiodic acid or sodium periodate was used as an additive, was particularly excellent. In Examples 1 to 3, the surface roughness Ra after polishing was smaller than 0.1 nm. On the other hand, in Comparative Examples 1 to 5, in which an additive that does not fall under the category of perhalogen acid was used, no effect of improving the polishing removal rate was observed in comparison with the reference example in which no additive was used. In Comparative Example 3, in which potassium permanganate was used as an additive, the substrate holder and polishing pad were damaged by corrosion, and the polishing removal rate could not be measured. It was found that permanganic acids are difficult to use in a low pH range. In addition, from the comparison of the above-mentioned Examples 1-2 and Comparative Example 4, and from the comparison of the above-mentioned Example 3 and Comparative Example 5, it is considered that the presence of a perhalogen acid structure, rather than the presence of a halogen (iodine, chlorine) as an additive, contributes to the improvement of the polishing removal rate. In addition, from the results of the above-mentioned Examples, it is considered that the above-mentioned effect of improving the polishing removal rate is not due to the aggregation effect of metal (sodium). When the same evaluation as in the above-mentioned Examples was carried out using a polishing composition consisting of 10% calcined alumina, phosphoric acid, and water and having a pH of 1.0, the surface roughness Ra was as high as 0.3 nm, and good surface quality could not be obtained. The above results show that a polishing composition containing colloidal silica, a pH adjuster, a perhalogen acid-based oxidizing agent, and water can improve the polishing removal rate while achieving high surface quality in polishing a gallium nitride semiconductor substrate.

[0060] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.

Claims

1. A polishing composition used for polishing a gallium nitride semiconductor substrate, comprising: A polishing composition comprising colloidal silica, a pH adjuster, a perhalogen acid-based oxidizing agent, and water.

2. 2. The polishing composition according to claim 1, wherein the colloidal silica has a ratio (D90 / D10) of a cumulative frequency 90% particle size (D90) to a cumulative frequency 10% particle size (D10) in a volume-based particle size distribution measured by a dynamic light scattering method of 2.0 or more.

3. 3. The polishing composition according to claim 1, wherein the content of the perhalogen acid-based oxidizing agent is 0.015 mol / L or more.

4. 3. The polishing composition according to claim 1, wherein the perhalogen acid-based oxidizing agent is at least one selected from the group consisting of periodic acid, perchloric acid, and salts thereof.

5. 3. The polishing composition according to claim 1, having a pH greater than 0.5 and less than 2.

0.

6. A polishing method comprising the step of polishing a gallium nitride semiconductor substrate with the polishing composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Polishing agent composition for nitride semiconductor substrate

    JP2018067591A

  • Polishing composition, polishing method of substrate, and manufacturing method of substrate

    JP2020055914A

  • Aqueous dispersion for chemical mechanical polishing and chemical mechanical polishing method using same

    WO2011016323A1

  • Polishing agent and polishing method

    WO2012036087A1

  • Polishing composition production method and polishing method

    WO2020203568A1