Resin composition, resin film, laminate, coverlay film, copper foil with resin, metal-clad laminate, and circuit board

The resin composition with a thermoplastic resin and phosphine compound addresses bleed-out and dielectric property deterioration issues, providing excellent flame retardancy and dielectric stability for high-frequency signal transmission in circuit boards, enabling low-temperature processing.

JP2024141761APending Publication Date: 2024-10-10NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023053581
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional resin compositions for circuit boards face issues such as bleed-out of flame retardants, deterioration of dielectric properties due to hygroscopicity and water absorption, and high processing temperatures, which are not suitable for typical flexible printed circuit (FPC) manufacturing processes.

Method used

A resin composition comprising a thermoplastic resin with an aliphatic or alicyclic skeleton and a phosphine compound with a melting point of 250°C or higher and a phosphine oxide group, with a weight ratio of (B/A) between 0.1 to 1, where component (B) has two or more phosphine oxide groups and a linking group, and optionally includes thermoplastic polyimide and polystyrene elastomer.

Benefits of technology

The composition achieves excellent dielectric properties and flame retardancy with low moisture dependence, suitable for high-frequency signal transmission in circuit boards like FPCs, while allowing thermocompression bonding at lower temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141761000009
    Figure 2024141761000009
  • Figure 2024141761000001
    Figure 2024141761000001
  • Figure 2024141761000002
    Figure 2024141761000002
Patent Text Reader

Abstract

To provide a resin composition capable of improving flame retardancy without deteriorating dielectric characteristics of a thermoplastic polyimide, and to provide a resin film.SOLUTION: The resin composition contains: (A) a thermoplastic resin having an aliphatic chain or alicyclic skeleton and having a glass transition temperature (Tg) of 180°C or lower; and (B) a phosphine compound having a melting point of 250°C or higher and having phosphine oxide groups. The weight ratio (B / A) of the component (B) to the component (A) is preferably within the range of 0.1-1. The phosphine compound as the component (B) has two or more phosphine oxide groups and may contain at least one selected from the group consisting of a phenylene group, a xylylene group, a biphenylene group, a naphthylene group, a methylene group and an ethylene group as a linking group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition useful as an adhesive in circuit boards such as printed wiring boards, and to a resin film, a laminate, a coverlay film, a resin-coated copper foil, a metal-clad laminate, and a circuit board each using the same. [Background technology]

[0002] As communication devices have become faster in recent years, development of 5G and even 6G communications is progressing, and there is a demand for materials for circuit boards such as flexible printed circuits (FPCs) to reduce transmission loss of high-frequency signals.

[0003] Thermoplastic resins with an aliphatic skeleton are expected to be used in printed wiring boards because of their excellent dielectric properties and the good handling properties that come with being thermoplastic, but the low flame retardancy derived from the aliphatic skeleton is an issue. In general, the addition of flame retardants is effective in imparting flame retardancy, but from the perspective of environmental impact, it is preferable that the flame retardant be halogen-free, and the use of phosphorus-based flame retardants is being considered.

[0004] Patent Document 1 proposes a resin composition in which a flame-retardant aromatic condensed phosphate ester is blended with a thermoplastic resin. However, because aromatic condensed phosphate esters are soluble in solvents, there is a concern that they may bleed out due to heat treatment during the production process of circuit boards.

[0005] Patent Document 2 proposes a resin composition in which a metal salt of an organic phosphinic acid is blended as a flame retardant in a thermoplastic resin. However, since the metal salt of an organic phosphinic acid has high polarity, there is a concern that the hygroscopicity and water absorption properties are deteriorated and the dielectric properties are deteriorated, and for example, there is a risk of inconvenience such as loss of electrical signals occurring in the transmission of high-frequency signals in the direct conversion method of 5G communication and beyond.

[0006] Patent Document 3 proposes a resin composition containing a thermosetting resin including a modified polyphenylene ether resin and a phosphine compound having a phosphine oxide group. However, the thermosetting resin of Patent Document 3 has a high glass transition temperature (Tg), and requires a high-temperature thermocompression bonding process to exhibit adhesion with other materials, making it difficult to process in the temperature range used in the manufacturing process of general FPCs. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent Publication No. 2021-070824 [Patent Document 2] Patent No. 6267509 [Patent Document 3] Patent No. 6941786 Summary of the Invention [Problem to be solved by the invention]

[0008] Conventional techniques that incorporate flame retardants into thermoplastic resins have problems such as bleed-out and deterioration of dielectric properties due to moisture absorption and water absorption, and there was a need to solve these problems.

[0009] Therefore, an object of the present invention is to provide a resin composition and a resin film that can improve the flame retardancy without deteriorating the dielectric properties of a thermoplastic resin. [Means for solving the problem]

[0010] The resin composition of the present invention comprises the following components (A) and (B); (A) a thermoplastic resin having an aliphatic chain or an alicyclic skeleton and a glass transition temperature (Tg) of 180° C. or lower; And, (B) a phosphine compound having a melting point of 250° C. or higher and having a phosphine oxide group; Contains:

[0011] The resin film of the present invention comprises the following components (A) and (B); (A) a thermoplastic resin having an aliphatic chain or an alicyclic skeleton and a glass transition temperature (Tg) of 180° C. or lower; And, (B) a phosphine compound having a melting point of 250° C. or higher and having a phosphine oxide group; Contains:

[0012] In the resin composition and resin film of the present invention, the weight ratio (B / A) of the component (B) to the component (A) may be within the range of 0.1 to 1.

[0013] In the resin composition and resin film of the present invention, the phosphine compound of the component (B) may have two or more phosphine oxide groups.

[0014] In the resin composition and resin film of the present invention, the phosphine compound of component (B) may have a linking group in the molecule that links two or more phosphine oxide groups, and the linking group may contain at least one selected from the group consisting of a phenylene group, a xylylene group, a biphenylene group, a naphthylene group, a methylene group and an ethylene group.

[0015] In the resin composition and resin film of the present invention, the phosphine compound of the component (B) may be represented by the following general formula.

[0016] [ka]

[0017] In formula (1), X represents a divalent group selected from a phenylene group, a xylylene group, a biphenylene group, a naphthylene group, a methylene group, and an ethylene group, and Ar1 to Ar4 are the same or different and each represents an aryl group.

[0018] In the resin composition and resin film of the present invention, the component (A) may contain a thermoplastic polystyrene elastomer.

[0019] In the resin composition and resin film of the present invention, the thermoplastic polystyrene elastomer may have an acid value of 10 mgKOH / g or less.

[0020] In the resin composition and resin film of the present invention, the component (A) may further contain a thermoplastic polyimide.

[0021] In the resin composition and resin film of the present invention, the thermoplastic polyimide may be a thermoplastic polyimide containing a tetracarboxylic anhydride residue derived from a tetracarboxylic anhydride component and a diamine residue derived from a diamine component, and may contain an aliphatic diamine in an amount of 40 mol % or more relative to the diamine component.

[0022] In the resin composition and resin film of the present invention, the aliphatic diamine may be a dimer diamine composition mainly composed of a dimer diamine in which the two terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups.

[0023] The resin film of the present invention may have a dielectric loss tangent (Tan δ1) at a frequency of 20 GHz measured using a split post dielectric resonator (SPDR) after 24 hours of constant temperature and humidity conditioning at a temperature of 24 to 26°C and a humidity of 45 to 55% RH, and a dielectric loss tangent (Tan δ2) at a frequency of 20 GHz measured using a split post dielectric resonator (SPDR) after 48 hours of immersion in pure water at a temperature of 24 to 26°C, i.e., the difference Tan δ2 - Tan δ1 between these values ​​is less than 0.0020.

[0024] The laminate of the present invention is a laminate having a substrate and an adhesive layer laminated on at least one surface of the substrate, the adhesive layer being made of the above-mentioned resin film.

[0025] The coverlay film of the present invention is a coverlay film having a coverlay film material layer and an adhesive layer laminated on the coverlay film material layer, and the adhesive layer is made of the above-mentioned resin film.

[0026] The resin-coated copper foil of the present invention is a resin-coated copper foil in which an adhesive layer and a copper foil are laminated together, and the adhesive layer is made of the above-mentioned resin film.

[0027] The metal-clad laminate of the present invention is a metal-clad laminate having an insulating resin layer and a metal layer laminated on at least one surface of the insulating resin layer, and at least one of the insulating resin layers is made of the above-mentioned resin film.

[0028] The circuit board of the present invention is obtained by wiring the metal layer of the metal-clad laminate. Effect of the Invention

[0029] The resin composition of the present invention contains a thermoplastic resin as component (A) and a phosphine compound as component (B), and therefore has excellent dielectric properties and flame retardancy when made into a film. In addition, the resin film of the present invention has low moisture absorption dependency of the dielectric loss tangent, excellent stability of the dielectric properties, and excellent flame retardancy. Therefore, the resin composition and resin film of the present invention can be particularly suitably used as a material for circuit boards such as FPCs in electronic devices that require the transmission of high-frequency signals in the 1 GHz to 60 GHz band, for example. [Brief description of the drawings]

[0030] [Figure 1] 1 is a schematic diagram showing a cross-sectional configuration of a metal-clad laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Hereinafter, an embodiment of the present invention will be described.

[0032] [Resin composition] The resin composition of the present embodiment comprises the following components (A) and (B); (A) a thermoplastic resin having an aliphatic chain or an alicyclic skeleton and a glass transition temperature (Tg) of 180° C. or lower; And, (B) a phosphine compound having a melting point of 250° C. or higher and having a phosphine oxide group; Contains:

[0033] [Component (A); Thermoplastic resin] Component (A) is a thermoplastic resin. Here, the term "thermoplastic resin" generally refers to a resin that can be softened by heating and solidified by cooling repeatedly, and whose glass transition temperature (Tg) or melting point can be clearly confirmed. Examples of the thermoplastic resin of component (A) include: Condition 1) Having an aliphatic chain or an alicyclic skeleton, and Condition 2) The glass transition temperature (Tg) must be 180°C or lower. Any material that satisfies the above two conditions can be used without particular limitations. By satisfying condition 1, the effect of improving dielectric properties by reducing polar groups, as well as the effect of improving plasticity and adhesiveness, can be obtained. Furthermore, by satisfying condition 2, thermocompression bonding at low temperatures becomes possible in the manufacturing process of circuit boards such as FPCs. The glass transition temperature (Tg) of condition 2 is preferably 160°C or lower, and more preferably 140°C or lower.

[0034] Specific examples of the thermoplastic resin of component (A) include thermoplastic polyimide, thermoplastic polystyrene elastomer, thermoplastic bismaleimide resin, thermoplastic epoxy resin, thermoplastic polyamide, liquid crystal polymer, fluororesin, polyolefin, polyether, polyetherketone, polyester, polypropylene, acrylonitrile-butadiene-styrene, acrylic, etc. Among these, one or more types satisfying conditions 1 and 2 can be selected and used as the thermoplastic resin of component (A). Among these, thermoplastic polyimide and thermoplastic polystyrene elastomer are preferred, and it is particularly preferred to use them in combination because they have a large effect of improving heat resistance, reducing dielectric tangent, and improving adhesion when made into a resin film. Below, thermoplastic polyimide and thermoplastic polystyrene elastomer as representative examples of the thermoplastic resin of component (A) will be described in detail in order.

[0035] <Thermoplastic polyimide> The thermoplastic polyimide as component (A) is obtained by reacting a tetracarboxylic anhydride component with a diamine component, and contains a tetracarboxylic anhydride residue derived from the tetracarboxylic anhydride component and a diamine residue derived from the diamine component. Here, the term "thermoplastic polyimide" generally refers to a polyimide whose glass transition temperature (Tg) can be clearly confirmed, but in the present invention, the term "thermoplastic polyimide" refers to a polyimide whose storage modulus at 30°C measured using a dynamic mechanical analyzer (DMA) is 1.0 x 10 8 Pa or more, and the storage modulus at 300°C is 1.0×10 7 The term "non-thermoplastic polyimide" generally refers to a polyimide that does not soften or exhibit adhesiveness even when heated. In the present invention, however, the term "non-thermoplastic polyimide" refers to a polyimide having a storage modulus of 1.0×10 Pa at 30° C. as measured using a dynamic viscoelasticity measuring device (DMA). 9 Pa or more, and the storage modulus at 300°C is 5.0×10 7 This refers to polyimides with a modulus of tensile strength (MPa) or higher.

[0036] The thermoplastic polyimide used as component (A) has an aliphatic chain or alicyclic skeleton in the tetracarboxylic anhydride residue or diamine diamine residue. The thermoplastic polyimide as component (A) has an aliphatic chain or alicyclic skeleton, which allows the resin film to have a low dielectric tangent. The thermoplastic resin having an aliphatic chain or alicyclic skeleton will be described below with reference to preferred specific examples of the tetracarboxylic anhydride component and the diamine component.

[0037] (Tetracarboxylic acid anhydride component) The thermoplastic polyimide as component (A) may be made of any tetracarboxylic anhydride generally used for thermoplastic polyimides as a raw material, without any particular limitations. However, it is preferable to use a raw material containing 90 mol % or more of tetracarboxylic anhydrides represented by the following general formula (2) and / or (3) in total relative to the total tetracarboxylic anhydride components. In other words, the thermoplastic polyimide as component (A) preferably contains 90 mol % or more of tetracarboxylic acid residues derived from tetracarboxylic anhydrides represented by the following general formula (2) and / or (3) in total relative to the total tetracarboxylic acid residues. By containing 90 mol % or more of tetracarboxylic acid residues derived from tetracarboxylic anhydrides represented by the following general formula (2) and / or (3) in total relative to the total tetracarboxylic acid residues, it is preferable that the thermoplastic polyimide as component (A) easily achieves both flexibility and heat resistance. If the total amount of tetracarboxylic acid residues derived from tetracarboxylic anhydrides represented by the following general formula (2) and / or (3) is less than 90 mol %, the solvent solubility of the thermoplastic polyimide as component (A) tends to decrease.

[0038] [ka]

[0039] In general formula (2), X1 represents a single bond or a divalent group selected from the following formulas, and in general formula (3), the cyclic portion represented by Y represents a cyclic saturated hydrocarbon group selected from a 4-membered ring, a 5-membered ring, a 6-membered ring, a 7-membered ring, or an 8-membered ring.

[0040] [ka]

[0041] In the above formula, Z represents -C6H4-, -(CH2)n-, or -CH2-CH(-OC(=O)-CH3)-CH2-, where n represents an integer of 1 to 20.

[0042] Examples of the tetracarboxylic acid anhydride represented by the above general formula (2) include 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA), 4,4'-oxydiphthalic anhydride (ODPA), 4,4'-(hexafluoroisopropylidene)diphthalic anhydride (6FDA), 2,2-bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), p-phenylenebis(trimellitic acid monoester anhydride) (TAHQ), ethylene glycol bisanhydrotrimellitate (TMEG), etc. Among these, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) is particularly preferred. When BTDA is used, the carbonyl group (ketone group) contributes to adhesion, and therefore the adhesion of the thermoplastic polyimide as component (A) can be improved. In addition, the ketone group present in the molecular skeleton of BTDA may react with the amino group of an amino compound for crosslinking, which will be described later, to form a C=N bond, which is likely to produce an effect of improving heat resistance. From this viewpoint, it is preferable that the tetracarboxylic acid residue derived from BTDA is contained in an amount of preferably 50 mol % or more, more preferably 60 mol % or more, of the total tetracarboxylic acid residues.

[0043] Examples of the tetracarboxylic acid anhydride represented by the general formula (3) include 1,2,3,4-cyclobutane tetracarboxylic acid dianhydride, 1,2,3,4-cyclopentane tetracarboxylic acid dianhydride, 1,2,4,5-cyclohexane tetracarboxylic acid dianhydride, 1,2,4,5-cycloheptane tetracarboxylic acid dianhydride, and 1,2,5,6-cyclooctane tetracarboxylic acid dianhydride.

[0044] The thermoplastic polyimide as component (A) may contain tetracarboxylic acid residues derived from acid anhydrides other than the tetracarboxylic acid anhydrides represented by the above general formulas (2) and (3), within the scope of the invention.Such a tetracarboxylic acid residue is not particularly limited, and examples thereof include pyromellitic dianhydride, 2,3',3,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'- or 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 2,3',3,4'-diphenylethertetracarboxylic dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, 3,3'',4,4''-, 2,3,3'',4''- or 2,2'',3,3''-p-terphenyltetracarboxylic dianhydride, 2,3',3,4''- ... ,2-Bis(2,3- or 3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3- or 3,4-dicarboxyphenyl)methane dianhydride, bis(2,3- or 3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3- or 3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-, 1,2,6,7- or 1,2,9,10-phenanthrene-tetracarboxylic acid dianhydride, 2,3,6,7-anthracene tetracarboxylic acid dianhydride, 2,2-bis(3,4-dicarboxyphenyl) ) tetrafluoropropane dianhydride, 1,2,5,6-naphthalene tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 2,6- or 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-(or 1,4,5,8-)tetrachloronaphthalene-1,4,5,8-(or 2, 3,6,7-tetracarboxylic acid dianhydride, 2,3,8,9-, 3,4,9,10-, 4,5,10,11- or 5,6,11,12-perylene-tetracarboxylic acid dianhydride, pyrazine-2,3,5,6-tetracarboxylic acid dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic acid dianhydride, thiophene-2,3,4,5-tetracarboxylic acid dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride and other aromatic tetracarboxylic acid dianhydrides.

[0045] (Diamine component) The thermoplastic polyimide as component (A) can be made of any diamine compound generally used for thermoplastic polyimides as a raw material, but it is preferable to use a dimer diamine composition as the main component of the aliphatic diamine, in which two terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl groups or amino groups, in an amount of 40 mol% or more, more preferably 60 mol% or more, based on the total diamine components. In other words, the thermoplastic polyimide as component (A) preferably contains 40 mol% or more, more preferably 60 mol% or more of diamine residues derived from the dimer diamine composition based on the total diamine residues. By using the dimer diamine composition in the above amount, the dielectric properties of the thermoplastic polyimide as component (A) can be improved, and the thermocompression bonding properties can be improved by lowering the glass transition temperature (lowering Tg), and the internal stress can be relaxed by lowering the elastic modulus.

[0046] (Dimer diamine composition) The dimer diamine composition contains the following component (a) as a main component, with the amounts of components (b) and (c) being controlled.

[0047] (a) dimer diamine; The dimer diamine of the component (a) means a diamine in which two terminal carboxylic acid groups (-COOH) of a dimer acid are replaced by primary aminomethyl groups (-CH2-NH2) or amino groups (-NH2). Dimer acid is a known dibasic acid obtained by intermolecular polymerization of unsaturated fatty acids, and its industrial production process is almost standardized in the industry, and is obtained by dimerizing unsaturated fatty acids having 11 to 22 carbon atoms using a clay catalyst or the like. Industrially obtained dimer acid is mainly composed of a dibasic acid having 36 carbon atoms obtained by dimerizing unsaturated fatty acids having 18 carbon atoms, such as oleic acid, linoleic acid, and linolenic acid, but contains any amount of monomer acid (having 18 carbon atoms), trimer acid (having 54 carbon atoms), and other polymerized fatty acids having 20 to 54 carbon atoms depending on the degree of purification. In addition, although double bonds remain after the dimerization reaction, in the present invention, those which have been further subjected to a hydrogenation reaction to reduce the degree of unsaturation are also included in the dimer acid. The dimer diamine of component (a) can be defined as a diamine compound obtained by substituting the terminal carboxylic acid group of a dibasic acid compound having 18 to 54 carbon atoms, preferably 22 to 44 carbon atoms, with a primary aminomethyl group or an amino group.

[0048] As a feature of dimer diamine, it is possible to impart characteristics derived from the skeleton of dimer acid. That is, since dimer diamine is an aliphatic macromolecule with a molecular weight of about 560 to 620, it is possible to increase the molar volume of the molecule and relatively reduce the polar group of the thermoplastic polyimide. It is considered that such a feature of dimer acid type diamine contributes to improving the dielectric properties by reducing the relative dielectric constant and dielectric loss tangent while suppressing the deterioration of the heat resistance of the thermoplastic polyimide. In addition, since it has two freely moving hydrophobic chains with 7 to 9 carbon atoms and two chain-like aliphatic amino groups with a length close to 18 carbon atoms, it is not only possible to impart flexibility to the thermoplastic polyimide, but also possible to make the thermoplastic polyimide have an asymmetric chemical structure or a non-planar chemical structure, and therefore it is considered that it is possible to reduce the dielectric constant and dielectric loss tangent of the thermoplastic polyimide.

[0049] The dimer diamine composition used may be one in which the dimer diamine content of component (a) is increased to 96% by weight or more, preferably 97% by weight or more, more preferably 98% by weight or more by a purification method such as molecular distillation. By increasing the dimer diamine content of component (a) to 96% by weight or more, the broadening of the molecular weight distribution of the thermoplastic polyimide can be suppressed. If technically possible, it is best that the entire dimer diamine composition (100% by weight) is composed of component (a) dimer diamine.

[0050] (b) a monoamine compound obtained by substituting a terminal carboxylic acid group of a monobasic acid compound having 10 to 40 carbon atoms with a primary aminomethyl group or an amino group; The monobasic acid compound having 10 to 40 carbon atoms is a mixture of a monobasic unsaturated fatty acid having 10 to 20 carbon atoms derived from the raw material of dimer acid, and a monobasic acid compound having 21 to 40 carbon atoms which is a by-product during the production of dimer acid. The monoamine compound is obtained by substituting the terminal carboxylic acid group of these monobasic acid compounds with a primary aminomethyl group or an amino group.

[0051] The monoamine compound of component (b) is a component that suppresses an increase in the molecular weight of the thermoplastic polyimide. During polymerization of the polyamic acid or thermoplastic polyimide, the monofunctional amino group of the monoamine compound reacts with the terminal acid anhydride group of the polyamic acid or thermoplastic polyimide to cap the terminal acid anhydride group, thereby suppressing an increase in the molecular weight of the polyamic acid or thermoplastic polyimide.

[0052] (c) an amine compound obtained by substituting a terminal carboxylic acid group of a polybasic acid compound having a hydrocarbon group having 41 to 80 carbon atoms with a primary aminomethyl group or an amino group (excluding the above-mentioned dimer diamine); The polybasic acid compound having a hydrocarbon group having 41 to 80 carbon atoms is a polybasic acid compound mainly composed of a tribasic acid compound having 41 to 80 carbon atoms, which is a by-product during the production of dimer acid. It may also contain a polymerized fatty acid other than dimer acid having 41 to 80 carbon atoms. The amine compound is obtained by substituting the terminal carboxylic acid group of these polybasic acid compounds with a primary aminomethyl group or an amino group.

[0053] The amine compound (c) is a component that promotes an increase in the molecular weight of the thermoplastic polyimide. The trifunctional or higher amino group, the main component of which is a triamine derived from a trimer acid, reacts with the terminal acid anhydride group of the polyamic acid or thermoplastic polyimide, rapidly increasing the molecular weight of the thermoplastic polyimide. In addition, amine compounds derived from polymerized fatty acids other than dimer acids having 41 to 80 carbon atoms also increase the molecular weight of the thermoplastic polyimide, causing gelation of the polyamic acid or thermoplastic polyimide.

[0054] When the above dimer diamine composition is subjected to quantitative analysis of each component by gel permeation chromatography (GPC), in order to facilitate confirmation of the peak start, peak top and peak end of each component of the dimer diamine composition, a sample of the dimer diamine composition treated with acetic anhydride and pyridine is used, and cyclohexanone is used as an internal standard. Using the sample thus prepared, each component is quantified by the area percentage of the GPC chromatogram. The peak start and peak end of each component are the minimum values ​​of each peak curve, and the area percentage of the chromatogram can be calculated based on this.

[0055] In the dimer diamine composition used in the present invention, the total area percentage of components (b) and (c) is 4% or less, preferably less than 4%, in the chromatogram obtained by GPC measurement. By keeping the total area percentage of components (b) and (c) at 4% or less, the broadening of the molecular weight distribution of the thermoplastic polyimide can be suppressed.

[0056] The area percentage of the chromatogram of the (b) component is preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. By setting it in such a range, it is possible to suppress the decrease in the molecular weight of the thermoplastic polyimide, and further to widen the range of the molar ratio of the tetracarboxylic anhydride component and the diamine component. It is not necessary for the (b) component to be contained in the dimer diamine composition.

[0057] The area percentage of the chromatogram of component (c) is 2% or less, preferably 1.8% or less, and more preferably 1.5% or less. By setting it in such a range, it is possible to suppress a sudden increase in the molecular weight of the thermoplastic polyimide, and further to suppress an increase in the dielectric tangent of the resin film over a wide frequency range. Note that component (c) does not have to be contained in the dimer diamine composition.

[0058] Furthermore, when the ratio (b / c) of the area percentages of the chromatograms of the components (b) and (c) is 1 or more, the molar ratio of the tetracarboxylic anhydride component and the diamine component (tetracarboxylic anhydride component / diamine component) is preferably 0.97 or more and less than 1.0. By setting such a molar ratio, it becomes easier to control the molecular weight of the thermoplastic polyimide.

[0059] Furthermore, when the ratio (b / c) of the area percentages of the components (b) and (c) in the chromatograms is less than 1, the molar ratio of the tetracarboxylic anhydride component and the diamine component (tetracarboxylic anhydride component / diamine component) is preferably 0.97 or more and 1.1 or less. By setting such a molar ratio, it becomes easier to control the molecular weight of the thermoplastic polyimide.

[0060] The dimer diamine composition used in the present invention is preferably purified in order to reduce the amount of components other than the dimer diamine of the component (a). The purification method is not particularly limited, but known methods such as distillation and precipitation purification are suitable. The dimer diamine composition before purification is commercially available, and examples thereof include PRIAMINE 1073 (trade name), PRIAMINE 1074 (trade name), and PRIAMINE 1075 (trade name) manufactured by Croda Japan.

[0061] Examples of diamine compounds other than dimer diamine used in the thermoplastic polyimide as component (A) include aromatic diamine compounds, aliphatic diamine compounds, etc. Specific examples thereof include 1,4-diaminobenzene (p-PDA; paraphenylenediamine), 2,2'-dimethyl-4,4'-diaminobiphenyl (m-TB), 2,2'-n-propyl-4,4'-diaminobiphenyl (m-NPB), 4-aminophenyl-4'-aminobenzoate (APAB), 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)biphenyl, bis[1 ... aminophenoxy)]biphenyl, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)]benzophenone, 9,9-bis[4-(3-aminophenoxy)phenyl]fluorene, 2,2-bis-[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis-[4-(3-aminophenoxy)phenyl]hexafluoropropane, 3,3'-dimethyl-4,4'-diaminobiphenyl , 4,4'-methylenedi-o-toluidine, 4,4'-methylenedi-2,6-xylidine, 4,4'-methylene-2,6-diethylaniline, 3,3'-diaminodiphenylethane, 3,3'-diaminobiphenyl, 3,3'-dimethoxybenzidine, 3,3''-diamino-p-terphenyl, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, bis(p-aminocyclohexyl)methane, biphenyl Bis(p-β-amino-t-butylphenyl)ether, bis(p-β-methyl-δ-aminopentyl)benzene, p-bis(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,4-bis(β-amino-t-butyl)toluene, 2,4-diaminotoluene, m-xylene-2,5-diamine, p-xylene-2,5-diamine, m-xylylenediamine, p-xylylenediamine, 2,Examples of diamine compounds include 6-diaminopyridine, 2,5-diaminopyridine, 2,5-diamino-1,3,4-oxadiazole, piperazine, 2'-methoxy-4,4'-diaminobenzanilide, 4,4'-diaminobenzanilide, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 6-amino-2-(4-aminophenoxy)benzoxazole, and 1,3-bis(3-aminophenoxy)benzene.

[0062] The thermoplastic polyimide as component (A) can be produced by reacting the above-mentioned tetracarboxylic anhydride component and diamine component in a solvent to generate polyamic acid, which is then subjected to ring closure by heating. For example, the tetracarboxylic anhydride component and the diamine component are dissolved in an organic solvent in approximately equimolar amounts, and the mixture is stirred at a temperature in the range of 0 to 100°C for 30 minutes to 24 hours to cause a polymerization reaction, thereby obtaining polyamic acid, which is a precursor of the thermoplastic polyimide. In the reaction, the reaction components are dissolved in the organic solvent so that the generated precursor is in the range of 5 to 50% by weight, preferably in the range of 10 to 40% by weight. Examples of organic solvents used in the polymerization reaction include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethylsulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, methylcyclohexane, dioxane, tetrahydrofuran, diglyme, triglyme, methanol, ethanol, benzyl alcohol, and cresol. Two or more of these solvents can be used in combination, and aromatic hydrocarbons such as xylene and toluene can also be used in combination. The amount of such an organic solvent is not particularly limited, but it is preferable to adjust the amount so that the concentration of the polyamic acid solution obtained by the polymerization reaction is about 5 to 50% by weight.

[0063] The synthesized polyamic acid is usually advantageously used as a reaction solvent solution, but it can be concentrated, diluted, or replaced with another organic solvent if necessary. Polyamic acid is generally advantageously used because it has excellent solvent solubility. The viscosity of the polyamic acid solution is preferably within the range of 500 mPa·s to 100,000 mPa·s. If it is outside this range, defects such as uneven thickness and streaks are likely to occur in the film during coating using a coater or the like.

[0064] The method for imidizing the polyamic acid to form a thermoplastic polyimide is not particularly limited, and for example, a heat treatment in which the polyamic acid is heated in the above-mentioned solvent at a temperature in the range of 80 to 400° C. for 1 to 24 hours is preferably used. The temperature may be constant, or the temperature may be changed during the process.

[0065] In the thermoplastic polyimide as component (A), the dielectric properties, thermal expansion coefficient, tensile modulus, glass transition temperature, etc. can be controlled by selecting the types of the tetracarboxylic anhydride component and diamine component, and when two or more types of tetracarboxylic anhydride components or diamine components are used, respectively. In addition, in the thermoplastic polyimide as component (A), when a plurality of polyimide structural units are contained, they may be present as blocks or randomly, but it is preferable that they are present randomly.

[0066] The weight average molecular weight of the thermoplastic polyimide as component (A) is preferably within the range of, for example, 10,000 to 200,000, and within such a range, the weight average molecular weight of the thermoplastic polyimide is easily controlled. In addition, when applied as an adhesive for FPC, for example, the weight average molecular weight of the thermoplastic polyimide is more preferably within the range of 20,000 to 150,000, and further preferably within the range of 40,000 to 150,000. When the weight average molecular weight of the thermoplastic polyimide is less than 20,000, the flow resistance tends to deteriorate. On the other hand, when the weight average molecular weight of the thermoplastic polyimide exceeds 150,000, the viscosity increases excessively and becomes insoluble in a solvent, and defects such as uneven thickness of the adhesive layer and streaks tend to occur during coating work.

[0067] The imide group concentration of the thermoplastic polyimide as component (A) is preferably 22% by weight or less, more preferably 20% by weight or less. Here, the "imide group concentration" means the value obtained by dividing the molecular weight of the imide group (-(CO)2-N-) in the thermoplastic polyimide by the molecular weight of the entire structure of the thermoplastic polyimide. If the imide group concentration exceeds 22% by weight, the molecular weight of the resin itself decreases, and the low moisture absorption property deteriorates due to an increase in polar groups, and Tg and elastic modulus increase.

[0068] The thermoplastic polyimide as component (A) is most preferably a completely imidized structure. However, a part of the thermoplastic polyimide may be an amic acid. The imidization rate can be determined by measuring the infrared absorption spectrum of a thin film of thermoplastic polyimide by a single reflection ATR method using a Fourier transform infrared spectrophotometer (commercially available: FT / IR620 manufactured by JASCO Corporation) at 1015 cm -1 Based on the benzene ring absorber near 1780cm -1 It can be calculated from the absorbance of the C=O stretching derived from the imide group.

[0069] <Crosslink formation> When the thermoplastic polyimide as component (A) has a ketone group, the ketone group can be reacted with the amino group of an amino compound having at least two primary amino groups as functional groups (hereinafter, sometimes referred to as "amino compound for crosslinking") to form a C=N bond, thereby forming a crosslinked structure. The formation of the crosslinked structure can improve the heat resistance of the thermoplastic polyimide forming the adhesive layer. Examples of tetracarboxylic anhydrides suitable for forming a thermoplastic polyimide having a ketone group include 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), and examples of diamine compounds include aromatic diamines such as 4,4'-bis(3-aminophenoxy)benzophenone (BABP) and 1,3-bis[4-(3-aminophenoxy)benzoyl]benzene (BABB).

[0070] For the purpose of forming a crosslinked structure, the resin composition of the present embodiment preferably contains a thermoplastic polyimide as the component (A) containing BTDA residues derived from BTDA in an amount of preferably 50 mol % or more, more preferably 60 mol % or more, based on all tetracarboxylic acid residues, and an amino compound for crosslinking. In the present invention, the term "BTDA residue" refers to a tetravalent group derived from BTDA.

[0071] Examples of the amino compound for forming a crosslink include (I) a dihydrazide compound, (II) an aromatic diamine, and (III) an aliphatic amine. Among these, a dihydrazide compound is preferred. Aliphatic amines other than dihydrazide compounds are likely to form a crosslinked structure even at room temperature, which raises concerns about the storage stability of the varnish, while aromatic diamines require high temperatures to form a crosslinked structure. In this way, when a dihydrazide compound is used, it is possible to achieve both the storage stability of the varnish and a shortened curing time. Examples of the dihydrazide compound include oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid dihydrazide, pimelic acid dihydrazide, suberic acid dihydrazide, azelaic acid dihydrazide, sebacic acid dihydrazide, dodecanedioic acid dihydrazide, maleic acid dihydrazide, fumaric acid dihydrazide, diglyceryl ester dihydrazide, ... Preferred are dihydrazide compounds such as cholic acid dihydrazide, tartaric acid dihydrazide, malic acid dihydrazide, phthalic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, 2,6-naphthoedioic acid dihydrazide, 4,4-bisbenzene dihydrazide, 1,4-naphthoic acid dihydrazide, 2,6-pyridine diacid dihydrazide, itaconic acid dihydrazide, etc. The above dihydrazide compounds may be used alone or in combination of two or more.

[0072] In addition, the above amino compounds, such as (I) dihydrazide compounds, (II) aromatic diamines, and (III) aliphatic amines, can also be used in combination of two or more kinds beyond categories, such as a combination of (I) and (II), a combination of (I) and (III), or a combination of (I), (II) and (III).

[0073] In addition, from the viewpoint of making the network structure formed by the crosslinking by the crosslinking amino compound denser, the crosslinking amino compound used in the present invention preferably has a molecular weight (weight average molecular weight when the crosslinking amino compound is an oligomer) of 5,000 or less, more preferably 90 to 2,000, and even more preferably 100 to 1,500. Among these, crosslinking amino compounds having a molecular weight of 100 to 1,000 are particularly preferred. When the molecular weight of the crosslinking amino compound is less than 90, only one amino group of the crosslinking amino compound forms a C=N bond with a ketone group of the thermoplastic polyimide, and the periphery of the remaining amino group becomes three-dimensionally bulky, so that the remaining amino group tends to have difficulty in forming a C=N bond.

[0074] When crosslinking the ketone group in the thermoplastic polyimide as component (A) with the crosslinking amino compound, the crosslinking amino compound is added to a resin solution containing component (A) to cause a condensation reaction between the ketone group in the thermoplastic polyimide and the primary amino group of the crosslinking amino compound. This condensation reaction hardens the resin solution to become a hardened product. In this case, the amount of the crosslinking amino compound added can be 0.004 mol to 1.5 mol, preferably 0.005 mol to 1.2 mol, more preferably 0.03 mol to 0.9 mol, and most preferably 0.04 mol to 0.6 mol of the primary amino group per 1 mol of the ketone group. When the amount of crosslinking amino compound added is such that the total number of primary amino groups per mole of ketone groups is less than 0.004 moles, crosslinking by the crosslinking amino compound is insufficient, and heat resistance after curing tends to be difficult to exhibit. When the amount of crosslinking amino compound added exceeds 1.5 moles, unreacted crosslinking amino compound acts as a thermoplasticizer, tending to reduce the heat resistance of the adhesive layer.

[0075] The conditions of the condensation reaction for forming crosslinks are not particularly limited as long as the ketone group in the thermoplastic polyimide as component (A) reacts with the primary amino group of the amino compound for forming crosslinks to form an imine bond (C=N bond). The temperature of the heat condensation is preferably within the range of, for example, 120 to 220°C, more preferably within the range of 140 to 200°C, for the purpose of releasing water produced by condensation out of the system, or for the purpose of simplifying the condensation step when the heat condensation reaction is carried out subsequently to the synthesis of the thermoplastic polyimide as component (A). The reaction time is preferably about 30 minutes to 24 hours. The end point of the reaction can be determined by measuring the infrared absorption spectrum using, for example, a Fourier transform infrared spectrophotometer (commercially available product: FT / IR620 manufactured by JASCO Corporation) at 1670 cm. -1 The decrease or disappearance of the absorption peak due to the ketone group in the thermoplastic polyimide resin near 1635 cm -1 This can be confirmed by the appearance of an absorption peak derived from a nearby imine group.

[0076] The thermal condensation of the ketone group of the thermoplastic polyimide as component (A) with the primary amino group of the crosslinking amino compound can be carried out, for example, by the following reaction: (1) A method in which, following the synthesis (imidization) of a thermoplastic polyimide as component (A), an amino compound for crosslinking is added and heated; (2) A method in which an excess amount of an amino compound is charged in advance as a diamine component, and following the synthesis (imidization) of a thermoplastic polyimide as component (A), the remaining amino compound that is not involved in imidization or amidation is used as a crosslinking amino compound and heated together with the thermoplastic polyimide, or (3) The cross-linking can be carried out by a method in which the thermoplastic polyimide composition as component (A) to which the above-mentioned amino compound for cross-linking has been added is processed into a predetermined shape (for example, after being applied to a substrate or formed into a film), and then being heated.

[0077] To impart heat resistance to the thermoplastic polyimide as component (A), the formation of an imine bond has been described as the formation of a crosslinked structure, but the present invention is not limited to this.

[0078] <Thermoplastic polystyrene elastomer> The thermoplastic polystyrene elastomer as component (A) is a copolymer of styrene or its derivative and a conjugated diene compound, including its hydrogenated product. Examples of styrene or its derivative include, but are not limited to, styrene, methylstyrene, butylstyrene, divinylbenzene, vinyltoluene, etc. Examples of conjugated diene compounds include, but are not limited to, butadiene, isoprene, 1,3-pentadiene, etc. In addition, the thermoplastic polystyrene elastomer is preferably hydrogenated, which further improves its thermal stability and makes it less susceptible to deterioration such as decomposition and polymerization, and also enhances its aliphatic properties and improves its compatibility with thermoplastic polyimide.

[0079] The copolymer structure of the thermoplastic polystyrene elastomer as component (A) may be a block structure or a random structure. Preferred examples of the thermoplastic polystyrene elastomer include styrene-butadiene-styrene block copolymer (SBS), styrene-butadiene-butylene-styrene block copolymer (SBBS), styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-ethylene-propylene-styrene block copolymer (SEPS), and styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS), but are not limited thereto.

[0080] The acid value of the thermoplastic polystyrene elastomer as component (A) is 10 mgKOH / g or less, preferably 1 mgKOH / g or less, and more preferably 0 mgKOH / g. By blending a thermoplastic polystyrene elastomer with an acid value of 10 mgKOH / g or less, the dielectric tangent when a resin film is formed can be reduced and good adhesiveness can be maintained. On the other hand, if the acid value exceeds 10 mgKOH / g, the dielectric properties deteriorate due to an increase in polar groups, and the compatibility when used in combination with a thermoplastic polyimide deteriorates, resulting in a decrease in adhesiveness when a resin film is formed. Therefore, the lower the acid value, the better, and one that is not acid-modified (i.e., one with an acid value of 0 mgKOH / g) is most suitable. In the present invention, when used in combination with a thermoplastic polyimide, it is possible to develop excellent adhesiveness, so that a thermoplastic polystyrene elastomer that is not acid-modified (i.e., one with strong aliphatic properties) can also be used.

[0081] The thermoplastic polystyrene elastomer as component (A) preferably has a content ratio of styrene units [-CH2CH(C6H5)-] in the range of 10% by weight to 65% by weight, more preferably in the range of 20% by weight to 65% by weight, and most preferably in the range of 20% by weight to 50% by weight. If the content ratio of styrene units in the thermoplastic polystyrene elastomer is less than 10% by weight, the elastic modulus of the resin decreases and the handling properties as a film deteriorate, while if it is higher than 65% by weight, the resin becomes rigid, making it difficult to use as an adhesive, and the rubber component in the thermoplastic polystyrene elastomer decreases, leading to deterioration of the dielectric properties. In addition, by having the content ratio of styrene units within the above range, the proportion of aromatic rings in the resin film is increased, so that when via holes (through holes) and blind via holes are formed by laser processing in the process of manufacturing a circuit board using the resin film, it is possible to increase the absorbency in the ultraviolet region and further improve the laser processability.

[0082] The weight average molecular weight of the thermoplastic polystyrene elastomer as component (A) is, for example, preferably within the range of 20,000 to 300,000, more preferably within the range of 40,000 to 250,000. If the weight average molecular weight is lower than the above range, the effect of improving the dielectric properties may be reduced, and conversely, if it is higher, the viscosity of the polyimide composition may be high, making it difficult to produce a resin film.

[0083] The thermoplastic polystyrene elastomer as component (A) can be selected from commercially available products. As such commercially available thermoplastic polystyrene elastomers, for example, A1535HU (trade name), G1652MU (trade name), G1726VS (trade name), G1645VS (trade name), FG1901GT (trade name), G1650MU (trade name), G1653VO (trade name), G1654HU (trade name), G1730VO (trade name), MD1653MO (trade name), MD1648VO (trade name), MD6951MO (trade name), etc., manufactured by KRATON, can be preferably used.

[0084] By using a thermoplastic polyimide and a thermoplastic polystyrene elastomer in combination as the thermoplastic resin of component (A), the effect of improving heat resistance, the effect of reducing the dielectric tangent, and the effect of improving adhesion can be obtained when the resin film is formed. When a thermoplastic polyimide and a thermoplastic polystyrene elastomer are used in combination, the amount of the thermoplastic polystyrene elastomer relative to 100 parts by weight of the thermoplastic polyimide is preferably in the range of 20 parts by weight to 150 parts by weight, more preferably in the range of 30 parts by weight to 120 parts by weight, and most preferably in the range of 40 parts by weight to 100 parts by weight. If the content of the thermoplastic polystyrene elastomer relative to 100 parts by weight of the thermoplastic polyimide is less than 20 parts by weight, the effect of reducing the dielectric tangent may not be fully exhibited. On the other hand, if the weight ratio of the thermoplastic polystyrene elastomer exceeds 150 parts by weight, the heat resistance, adhesiveness, and flame retardancy of the resin film formed are reduced, and the compatibility between the thermoplastic polyimide and the thermoplastic polystyrene elastomer is deteriorated, the viscosity increases, and there is a concern that the handling property is deteriorated.

[0085] [Component (B); Phosphine compound] The resin composition of the present embodiment contains a phosphine compound as component (B). The phosphine compound as component (B) functions as a flame retardant and also has the effect of lowering the dielectric tangent of the resin film. Therefore, by combining the phosphine compound as component (B) with the thermoplastic resin as component (A), it is possible to impart excellent flame retardancy while improving the dielectric properties of the resin film.

[0086] The phosphine compound of component (B) is preferably one represented by the following general formula:

[0087] [ka]

[0088] In formula (1), X represents a divalent group selected from a phenylene group, a xylylene group, a biphenylene group, a naphthylene group, a methylene group, and an ethylene group, and Ar1 to Ar4 are the same or different and each represents an aryl group.

[0089] The phosphine compound represented by the general formula (1) has a chemical structure in which two phosphine oxide groups are linked by a divalent linking group X. In the general formula (1), the linking group represented by the group X is particularly preferably a xylylene group from the viewpoints of heat resistance and ease of preparation. Specific examples of the aryl group represented by the groups Ar1 to Ar4 in the general formula (1) include a phenyl group, a tolyl group, and a xylyl group. Among these, a phenyl group that contributes greatly to hydrophobicity and flame retardancy is particularly preferred. In other words, the phosphine compound represented by the general formula (1) is particularly preferably one having four phenyl groups. The phosphine compound represented by the general formula (1) is not limited to a single compound, and may be a mixture.

[0090] The phosphine compound of general formula (1) has a low polar group concentration due to its chemical structure containing a large amount of aromatic rings in the molecule, and can improve the dielectric properties of the resin film. In particular, the phosphine compound of general formula (1) has low hygroscopicity and water absorption, so it is less susceptible to the effects of environmental humidity and can stabilize the dielectric properties of the resin film.

[0091] The phosphine compound represented by the general formula (1) preferably has a phosphorus concentration in the molecule within the range of, for example, 10 to 20% by weight. In general, the higher the phosphorus concentration of a flame retardant, the greater the flame retardant effect. However, the phosphine compound represented by the general formula (1) has aryl groups as the groups Ar1 to Ar4, and therefore the presence of multiple aromatic rings shortens the time until char formation, thereby exhibiting sufficient flame retardancy while keeping the phosphorus concentration in the molecule relatively low.

[0092] In addition, the phosphine compound of component (B) has a high melting point of 250°C or more because it contains a large amount of aromatic rings in the molecule. Therefore, it is possible to suppress the occurrence of bleed-out due to heat treatment such as thermal compression bonding and solder mounting in the manufacturing process of FPC. In addition, since the phosphine compound of component (B) is solid at room temperature, it can be dispersed in the varnish when the resin composition is in the state of a liquid composition (varnish) containing a solvent. By maintaining a stable dispersion state in the resin composition, it becomes a uniform dispersion state in the resin film, and the effect of reducing the dielectric tangent and the effect of imparting flame retardancy can be fully exhibited. From this viewpoint, the average particle size of component (B) is preferably, for example, within the range of 0.1 to 10 μm, and more preferably within the range of 0.5 to 5 μm. If the average particle size is less than 0.1 μm, dispersibility tends to deteriorate, and if it exceeds 10 μm, it may cause poor appearance when made into a film, defects when drilling, etc. The average particle size is an average particle size measured by a laser diffraction method, and can be measured, for example, by using a laser diffraction type particle size distribution measuring device (manufactured by Shimadzu Corporation, product name: SALD-2000).

[0093] As the phosphine compound of component (B), commercially available products are available, such as paraxylylenebisdiphenylphosphine oxide (manufactured by UFC, trade name: Mosaflam386, melting point 330° C.), paraphenylenebisdiphenylphosphine oxide (manufactured by Katayama Chemical Industry Co., Ltd., trade name: BPE-3, melting point 300° C.), etc. These may be used in combination of two or more kinds.

[0094] [Optional ingredients] The resin composition of the present embodiment may contain a solvent such as an organic solvent. Examples of the organic solvent include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethylsulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, dioxane, tetrahydrofuran, diglyme, triglyme, and cresol. Two or more of these solvents may be used in combination, and aromatic hydrocarbons such as xylene and toluene may also be used in combination. The content of the organic solvent is not particularly limited, but it is preferable to adjust the amount of use so that the solid content concentration is about 5 to 30% by weight. The solid content in the resin composition means the total of the components excluding the solvent. In addition to the optional components of the amino compound for crosslinking and the solvent, the resin composition of the present embodiment may further contain, as necessary, other optional components such as inorganic fillers, plasticizers, other resin components such as epoxy resins, fluororesins, and olefin resins, curing accelerators, coupling agents, organic fillers, pigments, and flame retardants other than component (B). However, some plasticizers contain many polar groups, which may promote the diffusion of copper from the copper wiring, so it is preferable to avoid using plasticizers as much as possible.

[0095] [Blending ratio] The weight ratio (B / A) of component (B) to component (A) in the resin composition of the present embodiment is preferably within the range of 0.1 to 1, more preferably within the range of 0.2 to 0.8. If the weight ratio (B / A) is less than 0.1, the effect of lowering the dielectric tangent and the flame retardant effect cannot be sufficiently imparted, and the improvement of the dielectric properties and the improvement of the flame retardancy of the resin film may be insufficient. On the other hand, if the weight ratio (B / A) exceeds 1, it may be difficult to form the resin film, and the toughness of the obtained resin film may decrease, resulting in embrittlement. By setting the blending amount of component (B) within the above range, the dielectric properties of the resin film can be improved.

[0096] Furthermore, in order to fully exert the effects of the invention, the resin composition of the present embodiment preferably contains component (A) and component (B) in a total amount of 50% by weight or more, more preferably in the range of 70 to 100% by weight, and most preferably in the range of 80 to 100% by weight, based on the total solid content.

[0097] (viscosity) When the resin composition contains a solvent, the viscosity is preferably within the range of, for example, 500 mPa·s to 100,000 mPa·s in order to uniformly disperse component (B). If the viscosity is outside this range, defects such as uneven thickness and streaks are likely to occur in the resin film during coating, and the uniform dispersion of component (B) cannot be maintained in the resin film, so that the effect of lowering the dielectric tangent and the effect of imparting flame retardancy by component (B) may not be fully exhibited.

[0098] [Preparation of resin composition] In preparing the resin composition, for example, component (B) may be directly mixed into a resin solution of component (A) prepared using any solvent. Alternatively, in consideration of the dispersibility of component (B), component (B) may be mixed in advance into a reaction solvent into which a portion of the raw materials for component (A) has been added, and then the remaining raw materials may be added under stirring to allow polymerization to proceed. In either method, the entire amount of component (B) may be added at once, or it may be added little by little in several separate portions. The raw materials may also be added all at once, or they may be mixed little by little in several separate portions.

[0099] The resin composition of the present embodiment, when used to form an adhesive layer, has excellent flexibility and thermoplasticity, and has favorable properties for use, for example, as an adhesive for coverlay films that protect wiring parts of FPCs and rigid-flex circuit boards, adhesive layers in multilayer circuit boards, bonding sheets, and the like.

[0100] [Resin film] The resin film of the present embodiment is a resin film containing component (A) and component (B). Specifically, it is a resin film containing a thermoplastic resin of component (A) as a resin component, and is obtained by forming the above-mentioned resin composition into a film.

[0101] For the same reasons as those explained for the resin composition above, the weight ratio (B / A) of component (B) to component (A) of the resin film of this embodiment is preferably within the range of 0.1 to 1, and more preferably within the range of 0.2 to 0.8. In addition, in the resin film of this embodiment, the total amount of component (A) and component (B) relative to the entire resin film is preferably 50% by weight or more, more preferably in the range of 70 to 100% by weight, and most preferably in the range of 80 to 100% by weight.

[0102] The resin film of the present embodiment is not particularly limited as long as it is a film (sheet) including a thermoplastic polyimide layer containing component (A) and component (B), and may be in a state of being laminated to a substrate such as a resin sheet, for example, a copper foil, a glass plate, a polyimide-based film, a polyamide-based film, or a polyester-based film.

[0103] <Dielectric properties> (Dielectric constant) In order to ensure impedance matching when used in a circuit board such as an FPC and to reduce loss of an electric signal, the resin film of the present embodiment has a relative dielectric constant (ε1) at 20 GHz measured by a split post dielectric resonator (SPDR) when left for 24 hours under conditions of a temperature of 24 to 26° C. and a humidity of 45 to 55% RH (humidity controlled conditions) and a relative dielectric constant (ε2) at 20 GHz measured under the same conditions when left for 48 hours under conditions of a temperature of 24 to 26° C. and immersed in pure water (water absorption conditions), both of which are preferably 3.0 or less, more preferably 2.8 or less. If the relative dielectric constant (ε1) and the relative dielectric constant (ε2) exceed 3.0, inconveniences such as loss of electric signals are likely to occur on the transmission path of high-frequency signals when used in a circuit board such as an FPC.

[0104] (Dielectric tangent) In order to reduce loss of electrical signals when the resin film of the present embodiment is used in a circuit board such as an FPC, the dielectric loss tangent (Tan δ1) at 20 GHz measured by a split post dielectric resonator (SPDR) when left for 24 hours under constant temperature and humidity conditions of a temperature of 24 to 26° C. and a humidity of 45 to 55% RH (humidity controlled conditions) is preferably 0.0015 or less, more preferably 0.0012 or less, in order to reduce loss of electrical signals when the resin film is used in a circuit board such as an FPC. If the dielectric loss tangent under humidity controlled conditions exceeds 0.0015, problems such as loss of electrical signals are likely to occur in the transmission of high frequency signals in the 1 GHz to 60 GHz band when the resin film is used in a circuit board such as an FPC.

[0105] Furthermore, when the resin film of the present embodiment is left for 48 hours under conditions of immersion in pure water at a temperature of 24 to 26° C. (water absorption conditions), the dielectric loss tangent (Tan δ2) at 20 GHz measured by a split post dielectric resonator (SPDR) is preferably 0.0030 or less, more preferably 0.0025 or less. If the dielectric loss tangent under water absorption conditions exceeds 0.0030, the film becomes susceptible to the influence of environmental humidity when used in a circuit board such as an FPC, and inconveniences such as electrical signal loss are likely to occur in the transmission of high-frequency signals in the 1 GHz to 60 GHz band, for example.

[0106] (moisture absorption dependence) In addition, the difference (Tan δ2-Tan δ1) between the dielectric tangent (Tan δ1) at the time of humidity control and the dielectric tangent (Tan δ2) at the time of water absorption is preferably less than 0.0020, more preferably 0.0015 or less. If the difference (Tan δ2-Tan δ1) is 0.0020 or more, for example, when used in a circuit board such as an FPC, the dielectric tangent increases when wet, which tends to cause inconveniences such as loss of electrical signals on the transmission path of high-frequency signals.

[0107] (glass transition temperature) The resin film of the present embodiment preferably has a glass transition temperature (Tg) of 180° C. or less, and more preferably in the range of 30° C. to 150° C. If the resin film has a Tg of 180° C. or less, thermocompression bonding at a low temperature is possible, and the internal stress generated during lamination can be alleviated, and dimensional change after circuit processing can be suppressed. If the resin film has a Tg of more than 180° C., the bonding temperature becomes high, and there is a risk of impairing dimensional stability after circuit processing.

[0108] (Flame retardant) The resin film of the present embodiment exhibits excellent flame retardancy. That is, the resin film of the present embodiment, in a multilayer film state, passes the VTM-0 criterion measured by the method shown in the Examples below in accordance with the UL94 thin material vertical flame test, and preferably has an average burning time of less than 8 seconds, more preferably less than 5 seconds.

[0109] (Thickness) The thickness of the resin film of the present embodiment is not particularly limited, but is preferably in the range of 5 μm to 150 μm, and more preferably in the range of 8 μm to 125 μm. If the thickness of the resin film is less than 5 μm, there is a risk of problems such as wrinkles occurring during transportation in the production of the resin film, while if the thickness of the resin film exceeds 150 μm, there is a risk of a decrease in productivity of the resin film.

[0110] The resin film of the present embodiment can be preferably used as a circuit board material, for example, as a coverlay film for a circuit board, a bonding sheet, an adhesive layer for a metal-clad laminate, etc. Preferred application examples of the resin film of the present embodiment will be described below.

[0111] [Laminate] The laminate according to one embodiment of the present invention has a substrate and an adhesive layer laminated on at least one surface of the substrate, the adhesive layer being made of the above-mentioned resin film. The laminate may also include any layer other than the above. Examples of the substrate in the laminate include substrates made of inorganic materials such as copper foil and glass plate, and substrates made of resin materials such as polyimide film, polyamide film, and polyester film. Preferred embodiments of the laminate include a coverlay film and a resin-coated copper foil.

[0112] [Coverlay film] The coverlay film, which is one embodiment of the laminate, has a coverlay film material layer as a substrate and an adhesive layer laminated on one side of the coverlay film material layer, the adhesive layer being made of the above-mentioned resin film. Note that the coverlay film may include any layer other than those described above.

[0113] The material of the coverlay film material layer is not particularly limited, but for example, polyimide-based films such as polyimide, polyetherimide, polyamideimide, polyamide-based films, polyester-based films, etc. can be used. Among these, it is preferable to use polyimide-based films with excellent heat resistance. In addition, the coverlay film material can contain a black pigment in order to effectively exhibit light-shielding properties, concealing properties, design properties, etc., and can also contain optional components such as matte pigments that suppress the gloss of the surface within a range that does not impair the effect of improving the dielectric properties.

[0114] The thickness of the coverlay film material layer is not particularly limited, but is preferably within the range of, for example, 5 μm or more and 100 μm or less. The thickness of the adhesive layer is not particularly limited, but is preferably within the range of, for example, 10 μm to 75 μm.

[0115] The coverlay film of the present embodiment can be produced by the method exemplified below. First, as a first method, a varnish-like resin composition containing a solvent is applied to one side of a film material layer for a coverlay, and then the composition is dried at a temperature of, for example, 80 to 180°C to form an adhesive layer, thereby forming a coverlay film having a film material layer for a coverlay and an adhesive layer.

[0116] As a second method, a varnish-like resin composition containing a solvent is applied onto any substrate, dried at a temperature of, for example, 80 to 180°C, and then peeled off to form an adhesive film for the adhesive layer. This adhesive film is then thermocompressed to a film material layer for the coverlay at a temperature of, for example, 60 to 220°C to form a coverlay film.

[0117] [Copper foil with resin] The resin-coated copper foil, which is another embodiment of the laminate, is obtained by laminating an adhesive layer on at least one side of a copper foil as a base material, and the adhesive layer is made of the above-mentioned resin film. Note that the resin-coated copper foil of this embodiment may include any layer other than the above.

[0118] The thickness of the adhesive layer in the resin-coated copper foil is preferably within the range of 2 to 150 μm, and more preferably within the range of 2 to 125 μm. If the thickness of the adhesive layer is less than the lower limit, problems such as insufficient adhesion may occur. On the other hand, if the thickness of the adhesive layer exceeds the upper limit, problems such as reduced dimensional stability may occur. In addition, from the viewpoint of lowering the dielectric constant and the dielectric loss tangent, the thickness of the adhesive layer is preferably 3 μm or more.

[0119] The material of the copper foil in the resin-coated copper foil is preferably one mainly composed of copper or a copper alloy. The thickness of the copper foil is preferably 35 μm or less, more preferably in the range of 5 to 25 μm. From the viewpoint of production stability and handling, the lower limit of the thickness of the copper foil is preferably 5 μm. The copper foil may be a rolled copper foil or an electrolytic copper foil. In addition, a commercially available copper foil can be used as the copper foil.

[0120] The resin-attached copper foil may be prepared, for example, by forming a seed layer by sputtering a metal on a resin film, and then forming a copper layer by, for example, copper plating, or by laminating a resin film and a copper foil by a method such as thermocompression bonding. Furthermore, the resin-attached copper foil may be prepared by casting a coating solution of a resin composition to form an adhesive layer on the copper foil, drying the coating film, and then carrying out a required heat treatment.

[0121] [Metal-clad laminate] (First aspect) The metal-clad laminate according to one embodiment of the present invention includes an insulating resin layer and a metal layer laminated on at least one surface of the insulating resin layer, at least one of the insulating resin layers being made of the above-mentioned resin film. Note that the metal-clad laminate according to this embodiment may include any layer other than those described above.

[0122] (Second aspect) The metal-clad laminate according to another embodiment of the present invention is a so-called three-layer metal-clad laminate, which includes, for example, an insulating resin layer, an adhesive layer laminated on at least one side of the insulating resin layer, and a metal layer laminated on the insulating resin layer via the adhesive layer, and the adhesive layer is made of the above-mentioned resin film. The three-layer metal-clad laminate may include any layer other than the above. The three-layer metal-clad laminate may have an adhesive layer on one or both sides of the insulating resin layer, and the metal layer may be provided on one or both sides of the insulating resin layer via the adhesive layer. In other words, the three-layer metal-clad laminate may be a single-sided metal-clad laminate or a double-sided metal-clad laminate. A single-sided or double-sided FPC can be manufactured by processing the wiring circuit by etching the metal layer of the three-layer metal-clad laminate.

[0123] The insulating resin layer in the three-layer metal-clad laminate is not particularly limited as long as it is made of a resin having electrical insulation properties, and examples thereof include polyimide, epoxy resin, phenolic resin, polyethylene, polypropylene, polytetrafluoroethylene, silicone, ETFE, etc., but is preferably made of polyimide. The polyimide layer constituting the insulating resin layer may be a single layer or multiple layers, but preferably includes a non-thermoplastic polyimide layer.

[0124] The thickness of the insulating resin layer in the three-layer metal-clad laminate is, for example, preferably in the range of 1 to 125 μm, more preferably in the range of 5 to 100 μm. If the thickness of the insulating resin layer is less than the lower limit, problems such as insufficient electrical insulation may occur. On the other hand, if the thickness of the insulating resin layer exceeds the upper limit, problems such as the metal-clad laminate being more likely to warp may occur.

[0125] The thickness of the adhesive layer in the three-layer metal-clad laminate is preferably, for example, within the range of 0.1 to 125 μm, and more preferably within the range of 0.3 to 100 μm. In the three-layer metal-clad laminate of the present embodiment, if the thickness of the adhesive layer is less than the above lower limit, problems such as insufficient adhesion may occur. On the other hand, if the thickness of the adhesive layer exceeds the above upper limit, problems such as reduced dimensional stability may occur. In addition, from the viewpoint of reducing the dielectric constant and dielectric loss tangent of the entire insulating layer, which is a laminate of an insulating resin layer and an adhesive layer, the thickness of the adhesive layer is preferably 3 μm or more.

[0126] The ratio of the thickness of the insulating resin layer to the thickness of the adhesive layer (thickness of the insulating resin layer / thickness of the adhesive layer) is preferably within a range of, for example, 0.03 to 3.0, and more preferably within a range of 0.05 to 2.0. By setting such a ratio, it is possible to suppress warping of the three-layer metal-clad laminate. Furthermore, the insulating resin layer may contain a filler as necessary. Examples of the filler include silicon dioxide, aluminum oxide, magnesium oxide, beryllium oxide, boron nitride, aluminum nitride, silicon nitride, aluminum fluoride, calcium fluoride, and metal salts of organic phosphinic acid. These can be used alone or in combination of two or more.

[0127] (Third aspect) A metal-clad laminate according to yet another embodiment of the present invention is, for example, as shown in Fig. 1, a laminated type metal-clad laminate 100 formed by laminating at least two single-sided metal-clad laminates via an adhesive layer 10. The laminated type metal-clad laminate 100 comprises a first single-sided metal-clad laminate 21, a second single-sided metal-clad laminate 22, and an adhesive layer 10 laminated between the first single-sided metal-clad laminate 21 and the second single-sided metal-clad laminate 22, and the adhesive layer 10 is made of the above-mentioned resin film. Here, the first single-sided metal-clad laminate 21 has a first metal layer M1 and a first insulating resin layer 31 laminated on at least one side of the first metal layer M1. The second single-sided metal-clad laminate 22 has a second metal layer M2 and a second insulating resin layer 32 laminated on at least one side of the second metal layer M2. The adhesive layer 10 is disposed so as to abut against the first insulating resin layer 31 and the second insulating resin layer 32. The laminated metal-clad laminate 100 may include any layer other than those described above.

[0128] The first insulating resin layer 31 and the second insulating resin layer 32 in the laminated metal-clad laminate 100 may have the same configuration as the insulating resin layers in the three-layer metal-clad laminate of the second embodiment. The laminated metal-clad laminate 100 is prepared by preparing a first single-sided metal-clad laminate 21 and a second single-sided metal-clad laminate 22, i) a method of placing a resin film between the first insulating resin layer 31 and the second insulating resin layer 32 and laminating them together; or, ii) A method of applying a resin composition onto the first insulating resin layer 31 or the second insulating resin layer 32 and performing a heat treatment to form the adhesive layer 10; It can be produced by such methods.

[0129] [Circuit board] The circuit board according to the present invention is obtained by wiring the metal layer of the metal-clad laminate of the above embodiment. One or more metal layers of the metal-clad laminate are patterned by a conventional method to form a wiring layer (conductor circuit layer), thereby manufacturing a circuit board such as an FPC. The circuit board may include a coverlay film that covers the wiring layer. EXAMPLES

[0130] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following examples, various measurements and evaluations were performed according to the following methods, unless otherwise specified.

[0131] [Viscosity measurement] The viscosity was measured at 25° C. using an E-type viscometer (manufactured by Brookfield, product name: DV-II+Pro). The rotation speed was set so that the torque was 10% to 90%, and the value was read when the viscosity stabilized 2 minutes after the start of the measurement.

[0132] [Measurement of weight average molecular weight (Mw) of thermoplastic resin] The weight average molecular weight was measured by gel permeation chromatography (manufactured by Tosoh Corporation, product name: HLC-8220GPC was used). Polystyrene was used as a standard substance, and tetrahydrofuran (THF) was used as a developing solvent.

[0133] [Measurement of relative permittivity and dielectric loss tangent] The relative dielectric constant and dielectric loss tangent of the resin film at 20 GHz were measured using a vector network analyzer (Agilent, product name: E8363C) and an SPDR resonator. The resin film used in the measurement was left for 24 hours under conditions of temperature: 24 to 26°C and humidity: 45 to 55% RH (humidity-controlled conditions) or left for 48 hours under conditions of temperature: 24 to 26°C and immersed in pure water (water-absorption conditions).

[0134] [Measurement of storage modulus and glass transition temperature (Tg)] The storage modulus was measured by cutting a resin film into a size of 5 mm x 20 mm, and using a dynamic viscoelasticity device (DMA: manufactured by TA Instruments, product name: RSA-G2), heating it stepwise from 30°C to 400°C at a heating rate of 4°C / min and a frequency of 11 Hz. The maximum temperature at which the value of Tan δ during the measurement was maximized was defined as Tg. The storage modulus at 30°C was 1.0×10 8 Pa or more, and the storage modulus at 300°C is 1.0×10 7 Resins with a storage modulus of less than 1.0 x 10 Pa at 30°C are judged to be "thermoplastic" 9 Pa or more, and the storage modulus at 300°C is 5.0×10 7 Polyimides with a thermal expansion coefficient of 100 Pa or more were judged to be "non-thermoplastic".

[0135] [Flame retardancy evaluation] To evaluate flame retardancy, the multilayer film was cut into samples of 200±5mm x 50±1mm, rolled into a cylindrical shape with a diameter of approximately 12.7mm and a length of 200±5mm, and test pieces were prepared and combustion tests were conducted in accordance with the UL94VTM standard. A sample that passed the VTM-0 criteria and had an average burning time of less than 5 seconds was rated as "Excellent." A sample that passed the VTM-0 criteria and had an average burning time of 5 to 10 seconds was rated as "Good." A sample that did not pass the VTM-0 criteria was rated as "Fail."

[0136] [Method for measuring amine value] Approximately 2 g of the dimer diamine composition is weighed into a 200-250 mL Erlenmeyer flask, and phenolphthalein is used as an indicator. A 0.1 mol / L ethanolic potassium hydroxide solution is dropped into the solution until the solution turns light pink, and the solution is dissolved in approximately 100 mL of neutralized butanol. 3-7 drops of phenolphthalein solution are added thereto, and titration is performed with 0.1 mol / L ethanolic potassium hydroxide solution while stirring until the sample solution turns light pink. Five drops of bromophenol blue solution are added thereto, and titration is performed with 0.2 mol / L hydrochloric acid / isopropanol solution while stirring until the sample solution turns yellow. The amine value is calculated according to the following formula (1). Amine value = {(V2 x C2) - (V1 x C1)} x M KOH / m (1) Here, the amine value is expressed as mg-KOH / g, and M KOH is the molecular weight of potassium hydroxide, 56.1. V and C are the volume and concentration of the solution used in the titration, respectively, and the subscripts 1 and 2 represent a 0.1 mol / L ethanolic potassium hydroxide solution and a 0.2 mol / L hydrochloric acid / isopropanol solution, respectively. Furthermore, m is the sample weight in grams.

[0137] [Calculation of GPC and chromatogram area percentage] For GPC, 20 mg of the dimer diamine composition was pretreated with 200 μL of acetic anhydride, 200 μL of pyridine, and 2 mL of THF to prepare a 100 mg solution, which was then diluted with 10 mL of THF (containing 1000 ppm of cyclohexanone) to prepare a sample. The prepared sample was measured using a Tosoh Corporation product name: HLC-8220GPC under the following conditions: column: TSK-gel G2000HXL, G1000HXL, flow rate: 1 mL / min, column (oven) temperature: 40° C., injection volume: 50 μL. Cyclohexanone was used as a standard substance to correct the elution time.

[0138] In this case, the retention times were adjusted so that the peak top of the cyclohexanone main peak was at a retention time of 27 to 31 minutes, and the period from the peak start to the peak end of the cyclohexanone main peak was 2 minutes, and the peak top of the main peak excluding the cyclohexanone peak was at a retention time of 18 to 19 minutes, and the period from the peak start to the peak end of the main peak excluding the cyclohexanone peak was at a retention time of 2 minutes to 4 minutes 30 seconds, (a) Component represented by the main peak; (b) A component represented by a GPC peak detected at a time later than the minimum retention time of the main peak; (c) Components represented by GPC peaks detected at earlier retention times than the minimum value of the main peak on the earlier side; was detected.

[0139] The abbreviations used in the examples represent the following compounds. BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride PMDA: Pyromellitic dianhydride m-TB: 2,2'-dimethyl-4,4'-diaminobiphenyl BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane TPE-R: 1,3-bis(4-aminophenoxy)benzene BTDA: 3,3',4,4'-benzophenonetetracarboxylic dianhydride DDA: aliphatic diamine having 36 carbon atoms (manufactured by Croda Japan Co., Ltd., product name: PRIAMINE 1074, distilled and purified, amine value: 210 mg KOH / g, mixture of dimer diamines having cyclic and chain structures, component (a): 97.9%, component (b): 0.3%, component (c): 1.8%, aromatic ring ratio: 8.2 mol%) The "%" for component (a), component (b), and component (c) refer to the area percentage of the chromatogram in the GPC measurement. The molecular weight of DDA was calculated using the following formula. Molecular weight = 56.1 x 2 x 1000 / amine value] Polystyrene elastomer: KRATON, product name: MD1653MO (hydrogenated polystyrene elastomer, styrene unit content: 30% by weight, Mw: 80,499, no acid value, Tg: 79°C, thermoplastic) NMP: N-methyl-2-pyrrolidone DMAc: N,N-dimethylacetamide N-12: Dodecanedioic acid dihydrazide Mosaflam 386: paraxylylene bisdiphenylphosphine oxide (manufactured by UFC, product name: Mosaflam 386, melting point: 330°C, phosphorus concentration: 12% by weight) OP935: organic phosphinic acid aluminum salt (manufactured by Clariant Japan, product name: Exolit OP935, no melting point, phosphorus concentration: 23% by weight)

[0140] (Synthesis Example 1) <Preparation of Thermoplastic Resin Solution> In a 500 ml separable flask, 21.34 g of BTDA (0.06622 mol), 12.99 g of BPDA (0.04414 mol), 46.7042 g of DDA (0.08741 mol), 8.97104 g of BAPP (0.02185 mol), 126 g of NMP, and 84 g of xylene were charged and mixed well at 40 ° C for 1 hour to prepare a polyamic acid solution. This polyamic acid solution was heated to 190 ° C, heated and stirred for 5 hours, and an amount of xylene was added so that the solid concentration after polymerization was 31%, and polyimide solution 1 (solid content: 31 wt%, weight average molecular weight: 35,886, viscosity: 2,580 mPa s, Tg: 63 ° C) in which imidization was completed was prepared. The polyimide film obtained by applying the polyimide acid solution 1 onto a substrate and drying it to convert it into an imidized film was measured for its storage modulus, which was found to be "thermoplastic."

[0141] (Synthesis Example 2) <Preparation of Thermoplastic Resin Solution> Under a nitrogen stream, 34.04 g of BTDA (0.1057 mol), 55.89 g of DDA (0.1046 mol), 126 g of NMP, and 84 g of xylene were charged into a 1000 ml separable flask and mixed thoroughly at 40°C for 1 hour to prepare a polyamic acid solution. This polyamic acid solution was heated to 190°C, heated and stirred for 5 hours, and an amount of xylene was added so that the solid content concentration after polymerization was 31%, to prepare polyimide solution 2 (solid content: 31 wt%, weight average molecular weight: 52,800, viscosity: 4,750 mPa·s, Tg: 46°C) in which imidization was completed. The storage modulus of the polyimide film obtained by applying polyimide acid solution 2 to a substrate and drying it to imidize it was measured, and the result was "thermoplastic".

[0142] (Synthesis Example 3) <Preparation of polyamic acid solution for insulating resin layer> Under a nitrogen stream, 69.56 g of m-TB (0.328 mol), 542.75 g of TPE-R (1.857 mol), and DMAc in an amount that would result in a solids concentration of 12 wt% after polymerization were added to the reaction vessel and stirred at room temperature to dissolve. Next, 194.39 g of PMDA (0.891 mol) and 393.31 g of BPDA (1.337 mol) were added, and the polymerization reaction was continued by stirring at room temperature for 3 hours to prepare polyamic acid solution 1 (viscosity: 2,700 mPa s). The storage modulus of the polyimide film prepared using polyamic acid solution 1 was 4.3 × 10 at 30 °C. 9 Pa, 9.4 × 10 at 300 °C 7 Pa and was "non-thermoplastic."

[0143] (Synthesis Example 4) <Preparation of polyamic acid solution for insulating resin layer> Under a nitrogen stream, 64.20 g of m-TB (0.302 mol), 5.48 g of bisaniline-M (0.016 mol), and DMAc in an amount that would result in a solids concentration of 15% by weight after polymerization were added to the reaction vessel and stirred at room temperature to dissolve. Next, 34.20 g of PMDA (0.157 mol) and 46.13 g of BPDA (0.157 mol) were added, and the polymerization reaction was continued by stirring at room temperature for 3 hours to prepare polyamic acid solution 2 (viscosity: 28,000 mPa s). The storage modulus of the polyimide film prepared using polyamic acid solution 2 was 7.0 × 10 at 30 °C. 9 Pa, 5.4 × 10 at 300 °C 8 Pa and was "non-thermoplastic."

[0144] (Example 1) <Preparation of single-sided metal-clad laminate> On copper foil 1 (electrolytic copper foil, thickness: 12 μm, surface roughness Rz on the resin layer side: 0.6 μm), polyamic acid solution 1 was uniformly applied so that the thickness after curing was about 1.6 μm, and then heated and dried at 120 ° C to remove the solvent. Next, polyamic acid solution 2 was uniformly applied thereon so that the thickness after curing was about 2.4 μm, and heated and dried at 120 ° C to remove the solvent. Furthermore, a stepwise heat treatment was performed from 120 ° C to 360 ° C to complete the imidization, and a single-sided metal-clad laminate 1 was prepared.

[0145] [Example 1] Resin varnish 1 was prepared by mixing 37.5% by weight of polystyrene elastomer, 1.5% by weight of N-12, and 17.4% by weight of Mosaflam386 with polyimide solution 1 (43.6% by weight as solid content), and adding a certain amount of xylene and NMP so that the solid content concentration was 26%. This was applied to the silicone-treated surface of a release substrate (length x width x thickness = 320 mm x 240 mm x 25 μm) so that the thickness after drying was 25 μm, and then heated and dried at 100 ° C for 5 minutes and 120 ° C for 15 minutes, and peeled off from the release substrate to obtain resin film 1. The various evaluation results of resin film 1 are as follows. Thermoplastic, Tg: 65℃, Relative permittivity (ε1) and dielectric loss tangent (Tanδ1) under humidity control at 20GHz: 2.57 and 0.0011, Relative permittivity (ε2) and dielectric loss tangent (Tanδ2) under water absorption: 2.57 and 0.0016, Tanδ2-Tanδ1: 0.0005

[0146] [Examples 2 to 6] Resin varnishes 2 to 6 were prepared in the same manner as in Example 1, except that the raw material compositions shown in Table 1 were used. Resin films 2 to 6 were prepared in the same manner as in Example 1, using resin varnishes 2 to 6 instead of resin varnish 1. All of resin films 2 to 6 were thermoplastic. The results of evaluation of various characteristics are shown in Table 2.

[0147] Comparative Example 1 Resin varnish 7 was prepared by mixing 2.7% by weight of N-12 and 19.5% by weight of OP935 with polyimide solution 2 (77.8% by weight as solid content), and adding a certain amount of xylene and NMP so that the solid content concentration was 26%. This was applied to the silicone-treated surface of a release substrate (length x width x thickness = 320 mm x 240 mm x 25 μm) so that the thickness after drying was 25 μm, and then heated and dried at 100 ° C for 5 minutes and 120 ° C for 15 minutes, and peeled off from the release substrate to obtain resin film 7. The various evaluation results of resin film 7 are as follows. Thermoplastic, Tg: 34°C, Relative permittivity (ε1) and dielectric loss tangent (Tanδ1) under humidity control at 20GHz: 2.65 and 0.0022, Relative permittivity (ε2) and dielectric loss tangent (Tanδ2) under water absorption: 2.65 and 0.0037, Tanδ2-Tanδ1: 0.0015

[0148] Comparative Example 2 Resin varnish 8 was prepared by mixing 34.7% by weight of polystyrene elastomer, 1.4% by weight of N-12, and 23.6% by weight of OP935 with polyimide solution 1 (40.3% by weight as solid content), and adding a certain amount of xylene and NMP so that the solid content concentration was 26%. This was applied to the silicone-treated surface of a release substrate (length x width x thickness = 320 mm x 240 mm x 25 μm) so that the thickness after drying was 25 μm, and then heated and dried at 100 ° C for 5 minutes and 120 ° C for 15 minutes, and peeled off from the release substrate to obtain resin film 8. The results of evaluation of various properties of resin film 8 are as follows. Thermoplastic, Tg: 64℃, Relative permittivity (ε1) and dielectric loss tangent (Tanδ1) under humidity control at 20GHz: 2.52 and 0.0013, Relative permittivity (ε2) and dielectric loss tangent (Tanδ2) under water absorption: 2.49 and 0.0033, Tanδ2-Tanδ1: 0.0020

[0149] [Table 1]

[0150] If the weight ratio of the phosphine compound of component (B) to the thermoplastic resin of component (A) is less than 0.1, it is not possible to impart sufficient low dielectric and flame retardant effects to the polyimide, and if it exceeds 1.0, the amount of the phosphine compound is too large, so that the toughness of the film decreases and it is impossible to form a film.

[0151] [Table 2]

[0152] [Example 7] Resin varnish 1 was applied to the insulating resin layer side of single-sided metal-clad laminate 1 so that the thickness after drying was 46 μm, and then the resin varnish was dried by stepwise heat treatment from 80 ° C to 200 ° C to prepare single-sided metal-clad laminate 1 with adhesive layer. Two sheets of this single-sided metal-clad laminate 1 with adhesive layer were prepared, laminated with the adhesive layer side facing each other, and pressed at 180 ° C for 2 hours under a pressure of 3.5 MPa to prepare metal-clad laminate 1. The copper foil layer of metal-clad laminate 1 was etched away using an aqueous ferric chloride solution to obtain multilayer film 1. The evaluation results of the flame retardancy of multilayer film 1 are shown in Table 3.

[0153] [Examples 8 to 12] Multilayer films 2 to 6 were obtained using resin varnishes 2 to 6 in the same manner as in Example 7. The evaluation results of the flame retardancy of each multilayer film are shown in Table 3.

[0154] Comparative Example 3 Resin varnish 7 was applied to the insulating resin layer side of single-sided metal-clad laminate 1 so that the thickness after drying was 46 μm, and then the resin varnish was dried by stepwise heat treatment from 80 ° C to 200 ° C to prepare single-sided metal-clad laminate 7 with adhesive layer. Two sheets of this single-sided metal-clad laminate 7 with adhesive layer were prepared, laminated with the adhesive layer side facing each other, and pressed at 180 ° C for 2 hours under a pressure of 3.5 MPa to prepare metal-clad laminate 7. The copper foil layer of metal-clad laminate 7 was etched and removed using an aqueous ferric chloride solution to obtain multilayer film 7. The evaluation results of the flame retardancy of multilayer film 7 are shown in Table 3.

[0155] Comparative Example 4 A multilayer film 8 was obtained in the same manner as in Comparative Example 3, except that resin varnish 8 was used. The evaluation results of the flame retardancy of multilayer film 8 are shown in Table 3.

[0156] [Table 3]

[0157] In Examples 1 to 6, the deterioration of the dielectric tangent under water absorption conditions is suppressed compared to Comparative Example 2, and it is found that the effect of the low polarity skeleton of the phosphine compound having a phosphine oxide group is expressed. In addition, in Examples 7 to 12, it was possible to obtain a multilayer film having a higher flame retardant effect compared to Comparative Example 3. From the above, it was verified that in this embodiment, it is possible to design and provide a metal-clad laminate that combines low dielectric properties and flame retardancy derived from a low polarity skeleton.

[0158] Although the embodiment of the present invention has been described in detail above for the purpose of illustration, the present invention is not limited to the above embodiment, and various modifications are possible. [Explanation of symbols]

[0159] 10...adhesive layer, 21...first single-sided metal-clad laminate, 22...second single-sided metal-clad laminate, 31...first insulating resin layer, 32...second insulating resin layer, M1...first metal layer, M2...second metal layer, 100...laminated metal-clad laminate

Claims

1. The following components (A) and (B): (A) a thermoplastic resin having an aliphatic chain or an alicyclic skeleton and a glass transition temperature (Tg) of 180° C. or lower; And, (B) a phosphine compound having a melting point of 250° C. or higher and having a phosphine oxide group; A resin composition comprising:

2. The resin composition according to claim 1, wherein a weight ratio (B / A) of the component (B) to the component (A) is within a range of 0.1 to 1.

3. The resin composition according to claim 1, wherein the phosphine compound of the component (B) has two or more phosphine oxide groups.

4. 2. The resin composition according to claim 1, wherein the phosphine compound of component (B) has a linking group in the molecule that links two or more phosphine oxide groups, and the linking group includes at least one selected from the group consisting of a phenylene group, a xylylene group, a biphenylene group, a naphthylene group, a methylene group and an ethylene group.

5. 2. The resin composition according to claim 1, wherein the phosphine compound of the component (B) is represented by the following general formula: [Formula 1] [In formula (1), X represents a divalent group selected from a phenylene group, a xylylene group, a biphenylene group, a naphthylene group, a methylene group, and an ethylene group; 1 ~Ar 4 are the same or different and each represents an aryl group.

6. 2. The resin composition according to claim 1, wherein the component (A) contains a thermoplastic polystyrene elastomer.

7. The resin composition according to claim 6, wherein the thermoplastic polystyrene elastomer has an acid value of 10 mgKOH / g or less.

8. The resin composition according to claim 6, wherein the component (A) further contains a thermoplastic polyimide.

9. 9. The resin composition according to claim 8, wherein the thermoplastic polyimide contains a tetracarboxylic anhydride residue derived from a tetracarboxylic anhydride component and a diamine residue derived from a diamine component, and contains an aliphatic diamine in an amount of 40 mol % or more relative to the diamine component.

10. The resin composition according to claim 9, wherein the aliphatic diamine is a dimer diamine composition mainly composed of a dimer diamine obtained by substituting two terminal carboxylic acid groups of a dimer acid with primary aminomethyl groups or amino groups.

11. The following components (A) and (B): (A) a thermoplastic resin having an aliphatic chain or an alicyclic skeleton and a glass transition temperature (Tg) of 180° C. or lower; And, (B) a phosphine compound having a melting point of 250° C. or higher and having a phosphine oxide group; A resin film containing

12. After 24 hours of constant temperature and humidity conditioning at a temperature of 24 to 26°C and a humidity of 45 to 55% RH, the dielectric loss tangent (Tan δ) at a frequency of 20 GHz measured by a split post dielectric resonator (SPDR) was 1 ) and the dielectric loss tangent (Tan δ) at a frequency of 20 GHz measured by a split post dielectric resonator (SPDR) after 48 hours under pure water immersion conditions at a temperature of 24 to 26 ° C. 2 ) and the difference Tan δ 2 -Tan δ 1 The resin film according to claim 11, wherein the viscosity is less than 0.0020.

13. A laminate comprising a substrate and an adhesive layer laminated on at least one surface of the substrate, the adhesive layer being made of the resin film according to claim 11.

14. A coverlay film having a coverlay film material layer and an adhesive layer laminated on the coverlay film material layer, wherein the adhesive layer is made of the resin film according to claim 11.

15. A resin-coated copper foil comprising an adhesive layer and a copper foil laminated thereon, the adhesive layer being made of the resin film according to claim 11.

16. A metal-clad laminate having an insulating resin layer and a metal layer laminated on at least one surface of the insulating resin layer, wherein at least one layer of the insulating resin layer is made of the resin film described in claim 11.

17. A circuit board obtained by wiring the metal layer of the metal-clad laminate according to claim 16.

Citation Information

Patent Citations

  • Automatic focusing device

    JP1987067509A

  • Polyimide composition, resin film, laminate, cover ray film, copper foil with resin, metal-clad laminate and circuit board

    JP2021070824A

  • Resin composition, method for producing resin composition, prepreg, resin-coated film, resin-coated metal foil, metal-clad laminate, and wiring board