Tape

The tape with controlled viscosity and internal defects, used in an automatic lamination process, addresses gaps and overlaps in fiber-reinforced composite materials, ensuring gap-free lamination and maintaining mechanical strength.

JP2024141921APending Publication Date: 2024-10-10MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023053801
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for manufacturing fiber-reinforced composite materials in aircraft parts face challenges with gaps and overlaps between tapes, leading to mechanical strength deterioration, despite strict control of tape width.

Method used

A tape composed of thermoplastic resin and fiber base material with controlled viscosity and internal defects, arranged at specific intervals and heated to expand, filling gaps without pressure, using an automatic lamination process.

Benefits of technology

The solution ensures gap-free lamination with maintained mechanical strength, improving the efficiency and quality of molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141921000001_ABST
    Figure 2024141921000001_ABST
Patent Text Reader

Abstract

To provide a tape that can be formed without a gap between the tapes in an automatic laminating apparatus.SOLUTION: A tape contains a thermoplastic resin and a fiber base material, and includes a range in which a viscosity of the thermoplastic resin at a shear rate γ=(125±35)sec-1 measured by a flow tester becomes 1000 Pa s or less at a temperature of a melting point of the thermoplastic resin +20-60°C or a glass transition temperature +120-160°C. An internal defect rate in the tape is 5% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tape, a molded article, and a method for producing a molded article. [Background technology]

[0002] Fiber-reinforced composite materials are used in a wide range of applications, such as aircraft, automobiles, and medical devices, depending on the characteristics of their matrix resins. Thermosetting resins such as epoxy resins and thermoplastic resins such as engineering plastics are used as matrix resins for fiber-reinforced composite materials.

[0003] Regarding thermoplastic resins, engineering plastics such as crystalline nylon 66 (PA66) resin and amorphous polycarbonate (PC) resin have excellent heat resistance and mechanical strength and are widely used as industrial parts. In addition, super engineering plastics such as crystalline polyether ether ketone (PEEK) resin and amorphous polyetherimide (PEI) resin have heat resistance and mechanical strength that exceed those of engineering plastics, so their application to aircraft and other applications as a replacement for metal parts is being considered.

[0004] In light of the above, the application of fiber-reinforced composites to aircraft has been actively studied, and parts made from fiber-reinforced composites with a thermosetting resin matrix in an autoclave have been used. However, autoclave molding has a slow molding cycle, and studies are being conducted to increase the cycle time, such as automatic lamination, in order to reduce molding costs. In addition, in conjunction with the transformation of molding methods, there is also active research being conducted on thermoplastic resins that can be molded by simply changing the state without a curing reaction, with regard to the matrix resin.

[0005] Patent Document 1 proposes a form in which strips (tapes) of unidirectional fibers impregnated with thermosetting resin can be laminated without gaps or overlaps between the tapes. In particular, in the manufacture of aerospace parts, it is necessary to minimize gaps and overlaps between tapes, which have a significant effect on the mechanical properties of the parts, and it is also described that intentional gaps must be imposed because overlaps are more problematic than gaps, and the intentional gaps are reduced by strictly controlling the tape width. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special Publication No. 2013-538264 Summary of the Invention [Problem to be solved by the invention]

[0007] In Patent Document 1, the gap is reduced by strictly controlling the tape width, but no consideration has been given to a method for filling the gap itself. According to the study by the present inventors, it has been found that even if the tape width can be controlled, the mechanical strength may decrease.

[0008] One object of the present invention is to provide a tape that can be molded without gaps between tapes in an automatic lamination device and that can maintain mechanical strength, as well as a molded body using this tape and a method for manufacturing this molded body. [Means for solving the problem]

[0009] Means for Solving the Problems The present inventors have conducted intensive research in view of the above problems and have found that the above problems can be solved by the following invention, thereby completing the present invention.

[0010] The present invention includes the following configurations. [1] The shear rate γ measured by a flow tester containing a thermoplastic resin and a fiber substrate is (125±35) sec -1The viscosity of the thermoplastic resin at a temperature of the melting point of the thermoplastic resin + 20 to 60°C or the glass transition temperature of the thermoplastic resin + 120 to 160°C is 1000 Pa s or less, and the internal defect rate within the tape is 5% or less. [2] The shear rate γ = (125 ± 35) sec, measured using a flow tester, containing a thermoplastic resin and a fiber substrate. -1 a step of arranging at regular intervals a plurality of tapes, the plurality of tapes having a viscosity of 1000 Pa s or less at a temperature of the melting point of the thermoplastic resin + 20 to 60°C or the glass transition temperature of the thermoplastic resin + 120 to 160°C, a step of heating the plurality of tapes, and a step of pressing the tapes with a roller. Effect of the Invention

[0011] According to the present invention, there are provided a tape which can be molded without gaps between tapes in an automatic laminating device, a molded article using this tape, and a method for producing this molded article. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing a schematic diagram of an example of a prepreg manufacturing apparatus. [Diagram 2] FIG. 1 is a diagram illustrating an example of an automatic tape placement device. [Diagram 3] FIG. 4 is a diagram showing an example of a position of a tape on a head. [Figure 4] FIG. 2 is a diagram showing a schematic view of a laminated state before pressing in measuring a tape width change rate. [Diagram 5] FIG. 2 is a diagram showing a schematic diagram of tape spacing when measuring tape spacing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [tape] The tape of the present invention includes a fiber substrate and a thermoplastic resin. In one example, the tape of the present invention is obtained by slitting a prepreg to a predetermined width. The tape can also be obtained by impregnating a fiber bundle of a predetermined width with a matrix resin containing a thermoplastic resin.

[0014] [Tape structure] The width of the tape of the present invention is preferably in the range of 3 mm to 55 mm. The width of the tape is 3 mm or more, which is preferable from the viewpoint of efficiently producing an automatically laminated molded product, since the number of tapes used for producing the molded product can be reduced. The lower limit of the width of the tape is more preferably 4 mm or more, and further preferably 6 mm or more. It is preferable that the tape width is 55 mm or less from the viewpoint of increasing the tape yield, regardless of the planar shape in which the tape is laid. The upper limit of the tape width is more preferably 40 mm or less, and further preferably 30 mm or less.

[0015] The thickness of the tape of the present invention is preferably in the range of 0.01 to 0.5 mm. A tape thickness of 0.01 mm or more is preferable because it reduces the number of steps required for laminating to a predetermined thickness, making it possible to efficiently manufacture an automatically laminated molded product. The lower limit of the tape thickness is more preferably 0.03 mm or more, and even more preferably 0.05 mm or more. From the viewpoint of increasing the heating efficiency of the tape, it is preferable that the thickness of the tape is 0.5 mm or less. The upper limit of the tape thickness is more preferably 0.4 mm or less, and further preferably 0.3 mm or less. The ratio of width to thickness (width / thickness) of the tape of the present invention is preferably at least 6, more preferably at least 40, and even more preferably at least 50. By being at least the lower limit, a sufficient thickness can be imparted to the molded article even when the width is expanded.

[0016] [Internal defect] Examples of internal defects include voids, cracks, and foreign matter present inside the tape. Internal defects can be measured by image analysis. In image analysis, the tape is embedded in resin and the surface is polished to expose the cross section. Then, a cross-sectional photograph is taken using a microscope or the like, and the resin, reinforcing fibers, and voids are identified by binarizing the photograph using image analysis software. The internal defect rate is calculated from the total area of ​​the photographed area and the void area. If the tape has internal defects, the thermoplastic resin flows into the internal defects during molding, and the surface does not become smooth. From the viewpoint of improving the smoothness of the molded surface, the internal defects of the tape of the present invention are preferably 5% or less. In the case of automatic lamination, since the pressure during molding is low, it is difficult to remove voids during molding, so the internal defects of the tape of the present invention are more preferably 4% or less, and even more preferably 3% or less. The internal defects of the tape may be 0.001% or more.

[0017] [Fiber base material] The fiber substrate contained in the tape of the present invention is preferably a fiber bundle containing a plurality of reinforcing fibers. The number of single fibers in the fiber substrate is preferably 1000 or more, more preferably 3000 or more, from the viewpoint of increasing productivity when automatically laminating the fiber substrate as a tape. From the viewpoint of facilitating impregnation of the thermoplastic resin into the fiber substrate, the number is preferably 100000 or more, more preferably 60000 or less, and even more preferably 50000 or less.

[0018] The fiber diameter of the reinforcing fibers is preferably 1 μm or more, more preferably 3 μm or more, from the viewpoint of increasing the tensile strength and tensile modulus of the molded body, and is preferably 20 μm or less, more preferably 10 μm or less, from the viewpoint of productivity of the fiber base material.

[0019] The reinforcing fiber may be one or more kinds. Examples of the reinforcing fiber include glass fiber, carbon fiber, aramid fiber, polyester fiber, boron fiber, alumina fiber, silicon nitride fiber, and nylon fiber. The carbon fiber also includes graphite fiber. Among these, carbon fiber is preferred because it is lightweight, has high strength, has a high elastic modulus, and is excellent in heat resistance and chemical resistance. Examples of the type of carbon fiber include pitch-based, polyacrylonitrile (PAN)-based, and rayon-based, and any of these types of carbon fiber may be used. From the viewpoint of productivity of carbon fiber, PAN-based carbon fiber is more preferred.

[0020] The fibers contained in the fiber substrate contained in the tape of the present invention are preferably continuous fibers, and the fiber length of the continuous fibers is preferably 50 mm or more. As the fiber substrate using continuous fibers, for example, a sheet form in which the fibers are aligned in one direction, or a woven form (for example, a plain weave, a twill weave, a satin weave, etc.) can be mentioned as a preferable example.

[0021] The ratio of fibers in the tape of the present invention, i.e., the volume fraction (Vf) of fibers relative to the total volume of the tape, is preferably 40% by volume or more, more preferably 45% by volume or more, while it is preferably 80% by volume or less, more preferably 75% by volume or less, even more preferably 70% by volume or less, and particularly preferably 65% ​​by volume or less. If the ratio of fibers is equal to or greater than the lower limit, the strength of the molded article obtained by molding the tape of this embodiment is increased. If the ratio of fibers is equal to or less than the upper limit, it is possible to suppress poor appearance due to insufficient surface resin during molding. The fiber volume content is a value obtained by a measurement method in accordance with ASTM D3171 or JIS K 7075.

[0022] The weight per unit area of ​​the reinforcing fibers in the tape of the present invention, i.e., the fiber weight per unit area (FAW), is set to 10 g / m2 from the viewpoint of efficiently producing an automated laminated molded product. 2 It is preferable that the thickness is 30 g / m or more. 2 More preferably, it is 50 g / m or more. 2From the viewpoint of increasing the heating efficiency of the tape and improving the formability, the fiber weight (FAW) is 500 g / m 2 It is preferable that the thickness is less than 400 g / m 2 More preferably, it is 300 g / m or less. 2 It is even more preferable that:

[0023] [Thermoplastic resin] The thermoplastic resin contained in the tape of the present invention may be either a crystalline resin or an amorphous resin. Examples of the crystalline resin include polyolefin, polyamide, polyester, polyacetal, polyphenylene sulfide, polyaryl ether ketone, and polytetrafluoroethylene. Examples of the amorphous resin include at least one selected from the group consisting of polycarbonate, polymethyl methacrylate, polyvinyl chloride, polystyrene, polyether sulfone, polyether imide, and polyamide imide. Among these, at least one selected from the group consisting of polyaryl ether ketone, polyether imide, and polyamide is more preferred, and polyaryl ether ketone is particularly preferred. Polyaryletherketone is a homopolymer or copolymer containing a monomer unit containing one or more aryl groups, one or more ether groups, and one or more ketone groups. For example, polyetheretherketone, polyetherketoneketone, polyetherketone, polyetherketoneetherketoneketone, polyetheretherketoneketone, polyetherdiphenyletherketone, polyolefin (polyethylene, polypropylene, etc.) resin, modified polyolefin resin, polyester (polyethylene terephthalate, polybutylene terephthalate, etc.) resin, polyphenylene oxide resin, polysulfone resin, ABS resin, etc., and copolymers thereof (for example, polyetherketone-polyetherdiphenyletherketone copolymer and copolymer of acrylonitrile and styrene). Among them, polyetheretherketone is particularly preferred because of its excellent heat resistance, mechanical properties, chemical resistance, etc. The thermoplastic resin may be used alone or in combination of two or more kinds. From the viewpoint of stability in the usage environment, a crystalline thermoplastic resin is preferred.

[0024] [Physical properties of thermoplastic resin] From the viewpoint of heat resistance, in the case of a crystalline resin, the melting point is preferably 260° C. or higher, and in the case of an amorphous resin, the glass transition temperature is preferably 200° C. or higher. The melting point is a value obtained from the peak top of the crystal melting peak when a temperature rise measurement is performed using a differential scanning calorimeter (DSC). The glass transition temperature is a value obtained by a measurement method in accordance with ASTM D7028.

[0025] Thermoplastic resins are measured by a flow tester at a shear rate of γ = (125 ± 35) sec -1 When the viscosity is measured at 20 to 60°C above the melting point of the thermoplastic resin or 120 to 160°C above the glass transition temperature, the tape can be expanded during molding, and therefore the viscosity range includes a viscosity of 1000 Pa·s or less. The viscosity is preferably 900 Pa·s or less, more preferably 800 Pa·s or less, and even more preferably 700 Pa·s or less. By being equal to or less than the upper limit, the tape can be expanded during molding. The viscosity is usually 10 Pa·s or more, preferably 50 Pa·s or more, more preferably 100 Pa·s or more, and even more preferably 150 Pa·s or more.

[0026] The content of the thermoplastic resin in the tape of the present invention is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more of the total mass of the tape, because this easily ensures sufficient adhesion between the fiber substrate and the thermoplastic resin. The content of the thermoplastic resin in the tape is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 45% by mass or less of the total mass of the tape, because this easily improves the mechanical properties of the molded product.

[0027] [Other ingredients] In the matrix resin containing a thermoplastic resin as the matrix resin, various additives can be blended as other components as necessary, such as antioxidants, heat stabilizers, light stabilizers, plasticizers, lubricants, spreading agents, antistatic agents, flame retardants, fillers, matting agents, processing aids, impact resistance aids, antibacterial agents, antifungal agents, foaming agents, release agents, colorants, ultraviolet absorbers, and thermoplastic polymers. Examples of the antioxidant include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. Examples of the heat stabilizer include a hindered phenol-based heat stabilizer, a sulfur-based heat stabilizer, and a hydrazine-based heat stabilizer. Examples of the plasticizer include phthalates, phosphates, fatty acid esters, aliphatic dibasic acid esters, oxybenzoates, epoxy compounds, and polyesters. Examples of the lubricant include fatty acid esters, fatty acids, metal soaps, fatty acid amides, higher alcohols, and paraffins. Examples of the antistatic agent include cationic antistatic agents, anionic antistatic agents, nonionic antistatic agents, and amphoteric antistatic agents. These additives may be used alone or in combination of two or more kinds.

[0028] When the matrix resin contains these other components, from the viewpoint of durability such as thermal stability, the content of the other components is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the matrix resin (thermoplastic resin), while being preferably 10 parts by mass or less, more preferably 5.0 parts by mass or less.

[0029] [Tape manufacturing method] The tape of the present invention can be obtained by a method of directly obtaining a tape by impregnating a fiber substrate with a resin, or by producing a sheet-like prepreg and then slitting it. The prepreg can be produced by the following method.

[0030] [Prepreg manufacturing method] The method for producing the prepreg is not particularly limited, and the prepreg can be produced by a known method. For example, the prepreg can be produced by impregnating a fiber base material with the above-mentioned thermoplastic resin. Examples of the method for impregnating the thermoplastic resin include a method in which the thermoplastic resin is processed into a film having a thickness of about 10 to 100 μm, or into fibers having a fiber diameter of about 5 to 50 μm, or into powder having an average particle diameter of about 10 to 100 μm, and then adhered to the fiber substrate. Among the above-mentioned impregnation methods, the method of laminating a thermoplastic resin film on a fiber substrate and then heating the same to impregnate the fiber substrate is preferred from the viewpoint of reducing the amount of internal defects.

[0031] When the prepreg contains an additive, the thermoplastic resin and the additive are mixed to prepare a thermoplastic resin composition, and the fiber base material may be impregnated with this thermoplastic resin composition. When the prepreg contains other fibers, a fiber base material containing carbon fibers and other fibers may be impregnated with the thermoplastic resin composition.

[0032] Hereinafter, one embodiment of a method for producing a prepreg will be described. In the manufacturing method of the prepreg of this embodiment, a resin film made of the above-mentioned thermoplastic resin is laminated on a fiber substrate and heated and pressurized to impregnate the fiber substrate with the resin contained in the resin film, thereby manufacturing the prepreg. Specifically, a manufacturing apparatus 10 shown in FIG. 1 is used, and a fiber substrate 11 is unwound from a roll 18. Separately, a resin film 12 unwound from a plurality of rolls 18 is laminated on the upper and lower surfaces of the fiber substrate 11 via a pressure roller 19 to form a laminate, and after preheating with a heater 13, a release film 14 is placed on the upper and lower surfaces of the laminate. Next, the fiber substrate 11 is impregnated with the matrix resin in the laminate by pressing with a hot plate press 15 heated to a melting point (or flow start temperature) or higher in the range of 300 to 450 ° C. and pressing with a cooling press 16 cooled to a solidification temperature or lower. Thereafter, the release film 14 is removed to obtain a prepreg 17.

[0033] When the prepreg 17 is manufactured using the manufacturing apparatus 10, the resin films 12 laminated on the upper and lower surfaces of the fiber base material 11 may be of the same type or different types. The thermoplastic resin described above can be used for the resin film 12. The fiber base material described above can be used for the fiber base material 11.

[0034] In the manufacturing apparatus 10, the resin film 12 is laminated on the top and bottom surfaces of the fiber base material 11, but the fiber base material 11 and the resin film 12 may be interchanged. That is, the fiber base material 11 may be laminated on the top and bottom surfaces of the resin film 12 to form a laminate, and the matrix resin in the laminate may be impregnated into the fiber base material 11 by heating and pressurizing, to produce a prepreg.

[0035] Examples of the form of prepreg obtained in this manner include unidirectional prepreg (UD prepreg) in which a sheet-like fiber base material with fibers aligned in one direction is impregnated with a matrix resin, and cross prepreg in which a fiber fabric is impregnated with a matrix resin. The thickness of one prepreg sheet can be 0.04 to 0.7 mm or 0.04 to 0.4 mm.

[0036] [Molded body] The molded product can be obtained by molding the above-mentioned tape. For example, two or more of the above-mentioned tapes are arranged in parallel, and the resin contained in the tape dissolves and expands the width of the tape, forming a single integrated product. The molded article may be a laminate obtained by laminating only one or more of the tapes of the above-mentioned embodiment. The molded article may be a laminate obtained by laminating a combination of the tape of the above-mentioned embodiment and a tape other than the above-mentioned embodiment, a laminate obtained by laminating a combination of a prepreg and a sheet in which a plurality of tapes are integrated, or a laminate obtained by laminating a combination of a sheet in which a plurality of tapes are integrated, a tape, and a prepreg.

[0037] The stacking configuration of the tapes in the laminate is not particularly limited. The number of tapes stacked in the laminate can be appropriately set depending on the thickness of the tape and the thickness required for the molded article. When the tape is a UD tape, the fiber direction of the carbon fiber of each UD tape to be laminated can be appropriately set according to the physical properties required for the molded product. The fiber direction of the carbon fiber of each UD tape may be the same direction. For example, when isotropy is required for the physical properties of the molded product, it is preferable to laminate the UD tapes so that the fiber directions of the carbon fibers in a plan view of each UD tape to be laminated are a combination of 0° and 90°, a combination of 0°, 45°, 90°, and -45°, or a combination of 0°, 60°, and -60°, and are laminated symmetrically in the thickness direction of the laminate.

[0038] [Method of manufacturing molded body] The molded article can be obtained by molding the tape of the present invention. The method for forming the tape is not particularly limited, but examples include methods in which one sheet of the tape of the above-mentioned embodiment or a stack of multiple sheets is formed by a mold press method, an autoclave method, a hot / cold press method, etc., or an automatic lamination method. In particular, the tape of this embodiment is particularly effective when used in automatic lamination.

[0039] [Automatic stacking method] In one example of the automatic lamination method, a tape is continuously placed on a molding surface using an automatic lamination device, and the placed tape is continuously pressed to obtain a molded body. The tape may be made deformable by heating it before it is placed on the molding surface, or may be made deformable by heating it after it is placed on the molding surface. The tape placed on the molding surface may be made deformable by heating the molding surface. A plurality of tapes may be placed on the molding surface at the same time. A plurality of tapes may be discharged from the same head of the automatic lamination device, or a plurality of tapes may be discharged from each of the plurality of heads. A plurality of tapes may be arranged in parallel and placed on the molding surface, or a plurality of tapes may be stacked and placed on the molding surface.

[0040] Specifically, the shear rate γ measured by a flow tester is γ=(125±35) sec ―1 The method includes a step of arranging at intervals a plurality of tapes, the viscosity of which is 1000 Pa s or less at a temperature of the melting point of the thermoplastic resin + 20 to 60°C or the glass transition temperature + 120 to 160°C of the thermoplastic resin; a step of heating the plurality of tapes; and a step of pressing the tapes with a roller, wherein the tapes are expanded in width during the heating step or the pressing step to fill in the gaps between adjacent tapes.

[0041] In the placing step, the tape unwound from the bobbin is placed on the molding surface via the head. The ends of the placed tapes are spaced apart. In the placing step, the tapes may be placed on the molding surface at the same time, or a tape may be placed on the molding surface and then another tape may be placed on the molding surface at a distance. In the automatic lamination shown in FIG. 5, the distance (D) between the width direction end of the reference tape (R) and the width direction end of the adjacent tape (O) on the tape (R) side is preferably 0.5 mm or less, more preferably 0.4 mm or less, and even more preferably 0.2 mm or less, from the viewpoint of obtaining a molded body of uniform thickness without a recess. The distance (D) is preferably 0.01 mm or more, more preferably 0.05 mm or more, and even more preferably 0.1 mm or more, from the viewpoint of obtaining a molded body of uniform thickness without a protrusion.

[0042] In the above process, the tape surface temperature observed by thermography is adjusted to be the melting point of the thermoplastic resin contained in the tape +20 to 60°C or the glass transition temperature +120 to 160°C. The heated tape surface temperature is preferably the melting point of the thermoplastic resin contained in the tape +20°C or more or the glass transition temperature +120°C or more, more preferably the melting point +30°C or more or the glass transition temperature +130°C or more, and even more preferably the melting point +35°C or more or the glass transition temperature +135°C or more. The heated tape surface temperature is preferably the melting point +60°C or less or the glass transition temperature +160°C or less, more preferably the melting point +50°C or less or the glass transition temperature +150°C or less, and even more preferably the melting point +45°C or less or the glass transition temperature +145°C or less, since deterioration of the resin contained in the tape due to excessive heating can be suppressed.

[0043] In the pressing step, the tape is pressed to widen it, and the gap between adjacent tapes is filled. The pressing pressure can be, for example, 0.1 to 1.0 MPa for the first layer, and is adjusted to the extent that the release film serving as the base and the tape are bonded. For the second layer and subsequent layers, the pressing pressure can be 0.1 to 0.8 MPa, and is adjusted to the extent that the material of the lower layer and the tape are bonded. In addition, from the viewpoint of ensuring the time for widening the tape, the time for pressing the tape is preferably 0.1 seconds or more, more preferably 0.5 seconds or more, and even more preferably 1 second or more. In order to prevent the fibers from flowing too much, the time for pressing the tape is preferably 10 seconds or less, more preferably 5 seconds or less, and even more preferably 3 seconds or less.

[0044] The temperature when applying pressure is preferably 50° C. or less, more preferably 40° C. or less, and even more preferably 30° C. or less, in order to prevent excessive flow of the resin contained in the tape. The temperature of the pressing body for pressing the tape can be 0° C. or more.

[0045] When multiple tapes are laminated at the same time, gaps are likely to occur between the tapes, so it is preferable to adjust the temperature and pressure so that the tape itself can expand by heating and pressurizing to fill the gaps.

[0046] The temperature of the molding surface is preferably at least 200°C lower than the surface temperature of the tape, more preferably at least 150°C lower than the surface temperature of the tape, and even more preferably at least 100°C lower than the surface temperature of the tape, since this facilitates close contact between the molding surface and the tape. The temperature of the molding surface is preferably at most 60°C lower than the surface temperature of the tape, more preferably at most 80°C lower than the surface temperature of the tape, and even more preferably at most 90°C lower than the surface temperature of the tape, since this prevents excessive flow of the resin contained in the tape. The temperature of the molding surface is preferably equal to or higher than the glass transition point of the thermoplastic resin contained in the tape, since this facilitates adhesion between the molding surface and the tape, and is preferably equal to or lower than the melting point of the thermoplastic resin or equal to or lower than the glass transition point + 120°C, since this prevents excessive flow of the resin contained in the tape.

[0047] [Automatic stacking device] The automatic lamination device is an automatic lamination device that automatically laminates tapes to manufacture molded bodies, and is equipped with a means (A) for unwinding tapes from multiple bobbins, a means (B) for arranging multiple tapes, a means (C) for heating the tapes, and a means (D) for applying pressure to the arranged tapes. 2, the automatic lamination device 27 includes a creel 21 to which one or more bobbins 20 around which tape 22 is wound can be attached, and a head 25 that places the tape 22 unwound from the bobbin 20 on a molding surface. The molding surface may be a base plate 26, a mold placed on the base plate 26, or a tape that has already been placed.

[0048] An embodiment of the automatic lamination device will be described below with reference to the drawings.

[0049] (Means (A)) The means (A) is a means for unwinding the tape 22 from the bobbin 20 . The tape 22 is paid out from the bobbin 20, and the paid out tape 22 is guided to the head 25. The creel 21 to which the bobbin 20 is attached may be a single weight or multiple weights. In particular, when multiple weights are used, multiple tapes 22 can be stacked at the same time, which provides excellent molding efficiency. There is no particular limitation on the method of unwinding the tape 22, but there are various methods, such as a method of unwinding the tape 22 mechanically by rotating the bobbin 21, or an automatic method of unwinding the tape 22 by tension from the head 25. The tape 22 may be unwound from the bobbin 20 by a unwind roll.

[0050] (Means (B)) Means (B) is a means for placing the tape 22 on the base plate 26, which is performed by the head 25. An example of the head 25 is a method as shown in FIG. 3. A plurality of tapes 22 are fed from the bobbin 20 and taken into the head 25 in a line. The taken-in plurality of tapes 22 are arranged at regular intervals inside the head 25. The arranged tapes 22 are discharged from the head 25 and placed on the base plate 26. The tape arrangement positions, the intervals between the tapes, the number of layers, and the layering speed can be arbitrarily adjusted by a program. When multiple tapes are layered at the same time, partitions can be provided between the tapes to prevent the tapes from adhering to each other before being placed on the forming surface. Immediately after the tapes are placed on the forming surface, gaps often remain between the tapes.

[0051] (Means (C)) The means (C) is a means for heating the tape. When the tape 22 is discharged from the head 25, the tape 22 is heated by a heating means 23 provided in the head 25. The heated tape 22 is compressed and cooled by a roller 24 provided in the head 25. The heating means 23 is generally a laser, and temperature control is performed by simultaneously monitoring the laser output and temperature by thermography. The temperature monitoring means is preferably provided in the head 25. It may also be provided on a roller described below, independent of the head 25, so that the tape 22 is heated after it is placed thereon. When the roller is provided with a heating means, it is preferable that the roller is provided with at least two rollers, a heating roller and a cooling roller. Heating means using a heating roller includes heating by vibration of the roller.

[0052] (Means (D)) The means (D) is a means for applying pressure to the disposed tape. The pressure applying means typified by the roller 24 can be a mechanism such as a flat plate-shaped pressure device other than a roller, and the tape is cooled by the pressure applying means and solidified at the same time as a pressure of up to about 1 MPa is applied. The pressure applying roller 24 may be provided after the heating means 23, or may be integrated with the heating means 23. EXAMPLES

[0053] The present invention will be specifically described below with reference to examples, but the present invention is not limited by the following description as long as it does not deviate from the gist of the invention. The values ​​of various production conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​between the examples.

[0054] <Example 1> A thermoplastic resin film to be used for the tape was obtained by extruding polyether ether ketone resin (Polypla-Evonik Co., Ltd., VESTAKEP3300G, melting point: 340°C) into a film shape. The thickness of the film was 0.023 mm. Next, the thermoplastic resin film prepared above was laminated on a carbon fiber sheet in which PAN-based carbon fibers (Mitsubishi Chemical Co., Ltd. product "MR50R", 570 tex, 12,000 strands) were oriented in one direction, and the film was heat-melted and impregnated into the carbon fiber sheet to produce a tape. 1m 2 The weight of carbon fiber per unit (FAW) is 190g / m 2 It was.

[0055] <Measurement of tape width change rate> The method for measuring the tape width change rate will be explained with reference to FIG. The obtained tape 22 was cut into 12 tapes of 6.4 mm x 328 mm so that the orientation direction of the carbon fibers was the longitudinal direction, and the cut tapes were each given sample numbers 1 to 12. Then, only the odd-numbered tapes were divided into three in the longitudinal direction and photographed, and the tape width was calculated using the image analysis software WINROOF. The average of the tape widths obtained from the three photographs was defined as the width of one tape, and the average of the widths of the six tapes was defined as the pre-molding tape width.

[0056] Next, a polyimide film 31 (Kapton 200H 50 μm, manufactured by Toray DuPont Co., Ltd.), a graphite sheet 32 ​​(PF-100 1.0 mm, manufactured by Toyo Tanso Co., Ltd.), a polyimide film 31, 12 tapes 22, a polyimide film 31, a graphite sheet 32, and a polyimide film 31 were placed in this order in the lower die of a titanium die (not shown), and the upper die was closed. The tapes 22 were arranged with sufficient gaps so that the 12 tapes 22 would not overlap each other. Next, the die was preheated for 30 minutes in a heating platen set at 380° C. in a two-stage heating and cooling press (50-ton press, manufactured by Shinto Metal Industries Co., Ltd.) while measuring the die temperature, and then the die was transferred to a cooling platen set at 20° C., and cooling was started by applying a pressure of 1 MPa. After the die temperature reached 100° C., the die was removed from the press machine, and 12 tapes were obtained from the die.

[0057] The odd-numbered tapes removed from the mold were similarly divided into three longitudinal sections and photographed, and the tape width was calculated using WINROOF. The average of the tape widths obtained from the three photographs was taken as the width of one tape, and the average of the widths of the six tapes was taken as the width of the tape after molding.

[0058] The width change rate of each of the six tapes was calculated from the tape width before and after molding using the following formula.

[0059] Width change rate [%] = (Tape width after molding - Tape width before molding) / Tape width before molding x 100

[0060] The width change rates of the six tapes were averaged to calculate the average width change rate of the sample of Example 1. The average width change rate was 10.7%.

[0061] <Measurement of thermoplastic resin viscosity> Using a flow tester (Shimadzu Corporation, CFT-500D), the nozzle was set at φ1×L10mm, preheated for 5 minutes, and the heating plate temperature for tape width change measurement was set at 380℃, with a shear rate of 121sec. ―1 The viscosity was measured at 911 Pa s.

[0062] Table 1 shows the average rate of change in tape width and the thermoplastic resin viscosity and shear rate at the heating platen temperature in measuring the rate of change in tape width.

[0063] <Example 2> The heating plate temperature in the tape width change rate measurement was changed to 400° C., and the tape thickness measurement and internal defect rate measurement described below were performed in the same manner as in Example 1, except that the tape width change rate and viscosity were measured. The results are shown in Table 1.

[0064] <Measurement of tape thickness before and after molding> The thickness of the tape before and after molding was observed as follows. For the tape before molding, a part of the prepared tape sheet was cut out, embedded in resin, and polished until the thickness direction cross section could be observed well. Thereafter, the thickness of the tape before molding was measured using a microscope (Keyence Corporation, VHX-5000). The photographing range was the tape thickness × width 5000 μm. In addition, two places, the longitudinal center (range 155-175 mm from one longitudinal end) and the longitudinal end (range 0-20 mm from one longitudinal end), were cut out from the tape after molding, and each was embedded and polished in the same manner as the tape before molding. After polishing, the thickness of the longitudinal center and end of the tape after molding was measured by observing the thickness direction cross section with a microscope. The photographing range was the tape thickness × width 600 μm. In addition, the maximum thickness in the photographing range was taken as the tape thickness. The results are shown in Table 1.

[0065] <Measurement of internal defect rate of pre-molded and post-molded tapes, and resin content of post-molded tapes> For the images used in the thickness measurement, the image processing software ImageJ was used to calculate the internal defect rate of the tape before and after molding, and the resin content of the tape after molding. A part of the image used in the thickness measurement was cut out as the calculation area, and the area obtained by ImageJ was set to the range of 1,500,000 to 4,000,000. The results are shown in Table 1.

[0066] <Example 3> The tape width change rate and viscosity were measured in the same manner as in Example 1, except that the tape thermoplastic resin was changed to a polyetherimide resin (Ultem CRS5011, manufactured by SABIC Innovative Plastics, glass transition temperature Tg: 228° C.). The results are shown in Table 1.

[0067] <Example 4> The tape width change rate and viscosity were measured in the same manner as in Example 1, except that the thermoplastic resin was changed to a polyetherimide resin (Ultem 1040A, manufactured by SABIC Innovative Plastics, glass transition temperature Tg: 216° C.) and the heating plate temperature in the tape width change rate measurement was changed to 360° C. The results are shown in Table 1.

[0068] <Example 5> The tape width change rate and viscosity were measured in the same manner as in Example 4, except that the heating plate temperature in the tape width change rate measurement was changed to 380° C. The results are shown in Table 1.

[0069] <Example 6> The tape width change rate and viscosity were measured in the same manner as in Example 1, except that the thermoplastic resin was changed to a polyamide resin (TS-590, manufactured by Kuraray Co., Ltd., melting point: 263° C.) and the heating plate temperature in the tape width change rate measurement was changed to 300° C. The results are shown in Table 1.

[0070] <Comparative Example 1> Except for the fact that the thermoplastic resin was not sufficiently impregnated by lowering the process temperature and pressure during tape preparation, the tape width change rate, viscosity, tape thickness, and internal defect rate were measured in the same manner as in Example 2. The results are shown in Table 2.

[0071] <Comparative Example 2> The tape width change rate and viscosity were measured in the same manner as in Example 1, except that the thermoplastic resin was changed to a polyetherimide resin (UltemCRS5001, manufactured by SABIC Innovative Plastics, glass transition temperature Tg: 228° C.) and the heating plate temperature in the tape width change rate measurement was changed to 340° C. The results are shown in Table 2.

[0072] <Comparative Example 3> The tape width change rate and viscosity were measured in the same manner as in Comparative Example 2, except that the heating plate temperature in the tape width change rate measurement was changed to 380° C. The results are shown in Table 2.

[0073] <Comparative Example 4> Tape weight is 145g / m 2 Except for the above, the tape width change rate and viscosity were measured in the same manner as in Comparative Example 3. The results are shown in Table 2.

[0074] <Comparative Example 5> The tape width change rate and viscosity were measured in the same manner as in Comparative Example 2, except that the heating plate temperature in the tape width change rate measurement was changed to 400° C. The results are shown in Table 2.

[0075] <Comparative Example 6> The tape width change rate and viscosity were measured in the same manner as in Comparative Example 2, except that the heating plate temperature in the tape width change rate measurement was changed to 400° C. and no pressure was applied during cooling in the tape width change rate measurement. The results are shown in Table 2.

[0076] TIFF2024141921000002.tif24049

[0077] TIFF2024141921000003.tif24151

[0078] It can be seen from Tables 1 and 2 that by controlling the viscosity of the thermoplastic resin within an appropriate range, the tape width change rate can be 10% or more even at a low pressure of 1 MPa. In Comparative Example 6, no pressure is applied during cooling, so the width expands by nearly 5% just due to the weight of the mold during preheating, and tape width change rates of 10% or less are due to the width expanding due to the weight of the mold itself, and it is difficult to imagine that the viscosity of the thermoplastic resin is so high that the width can be expanded suitably by applying pressure.

[0079] Example 2 and Comparative Example 1 are experiments for comparing tapes produced with different internal defect rates. Internal defects are mainly gaps (voids) inside the tape, and Comparative Example 1, which used a tape with many internal defects, had a higher resin area ratio after molding than Example 1. This is thought to be because resin was filled in the positions where voids originally existed, forming resin-located parts. The formation of resin-rich parts causes a decrease in the mechanical properties of the molded body. The thickness after molding was also thinner in Comparative Example 1 than in Example 2, and this is also thought to be due to the resin filling the voids. If the thickness changes significantly before and after molding, accurate design becomes difficult.

[0080] In Comparative Example 5, the viscosity of the thermoplastic resin is 806 Pa s (1000 Pa s or less) at a temperature of the glass transition temperature of the thermoplastic resin + 172°C, and the width change rate of the tape is sufficiently high, but it is suggested that the molding temperature needs to be high in order to increase the width change rate. It is thought that high-temperature molding will cause resin degradation, which will be a factor in reducing the mechanical properties of the molded product.

[0081] [summary] In summary, the present invention may have the following embodiments. [Embodiment 1] Contains thermoplastic resin and fiber substrate, shear rate γ measured by flow tester = 90~160(125±35)sec -1 a viscosity range of the thermoplastic resin at a temperature of 1000 Pa s or less, 900 Pa s or less, 800 Pa s or less, or 700 Pa s or less at a temperature of the melting point of the thermoplastic resin + 20 to 60°C or a glass transition temperature of the thermoplastic resin + 120 to 160°C, and the internal defect rate within the tape is 5% or less, 4% or less, or 3% or less. [Embodiment 2] 2. The tape of claim 1, wherein the thermoplastic resin comprises at least one selected from the group consisting of polyolefins, polyamides, polyesters, polyacetals, polyphenylene sulfides, polyaryletherketones, polytetrafluoroethylenes, polycarbonates, polymethylmethacrylates, polyvinyl chlorides, polystyrenes, polyethersulfones, polyetherimides, and polyamideimides. [Embodiment 3] 3. The tape of claim 1 or 2, wherein the fibrous substrate comprises a unidirectionally aligned sheet. [Embodiment 4] 4. The tape of any one of claims 1 to 3, comprising carbon fibre as the fibre substrate. [Embodiment 5] 5. The tape of any one of the preceding claims, having a width of no more than 55 mm, no more than 40 mm, or no more than 30 mm. [Embodiment 6] 6. The tape of any one of the preceding claims, having a width of 3 mm or more, 4 mm or more, or 5 mm or more. [Embodiment 7] The fiber base material contains reinforcing fibers, and the fiber basis weight of the reinforcing fibers is 500 g / m 2 Below 400g / m 2 Less than or equal to 300g / m 2 7. The tape of any one of claims 1 to 6, wherein: [Embodiment 8] The fiber base material contains reinforcing fibers, and the fiber basis weight of the reinforcing fibers is 10 g / m 2 More than 30g / m 2 or more than 50g / m 2 The tape according to any one of embodiments 1 to 7, wherein [Embodiment 9] 9. The tape of any one of the preceding claims, having a thickness of at least 0.01 mm, at least 0.03 mm, or at least 0.05 mm. [Embodiment 10] 10. The tape of any one of the preceding claims, having a thickness of no more than 0.5 mm, no more than 0.4 mm, or no more than 0.3 mm. [Embodiment 11] 11. The tape of any one of claims 1 to 10, wherein the fiber substrate contains 1000 or more, or 3000 or more single fibers. [Embodiment 12] 12. The tape of any one of claims 1 to 11, wherein the fibrous substrate contains no more than 100,000 single fibers, no more than 60,000 single fibers, or no more than 50,000 single fibers. [Embodiment 13] 13. The tape of any one of the preceding claims, wherein the fibrous substrate comprises reinforcing fibers, the reinforcing fibers having a filament diameter of 1 μm or more, or 3 μm or more. [Embodiment 14] 14. The tape of any one of claims 1 to 13, wherein the fibrous substrate comprises reinforcing fibers, the reinforcing fibers having a filament diameter of 20 μm or less or 10 μm or less. [Embodiment 15] A molded article using the tape according to any one of embodiments 1 to 14. [Embodiment 16] A method for producing a molded article, comprising placing the tape according to any one of embodiments 1 to 15 while heating it. [Embodiment 17] 17. The method for producing a molded article according to claim 16, wherein a plurality of the tapes are arranged side by side. [Embodiment 18] The shear rate γ = (125 ± 35) sec, measured by a flow tester, includes a thermoplastic resin and a fiber substrate. -1 a step of arranging at regular intervals a plurality of tapes, the plurality of tapes having a viscosity of 1000 Pa·s or less, 900 Pa·s or less, 800 Pa·s or less, or 700 Pa·s or less at a temperature of the melting point of the thermoplastic resin + 20 to 60°C or the glass transition temperature of the thermoplastic resin + 120 to 160°C, a step of heating the plurality of tapes, and a step of pressing the tapes with a roller. [Embodiment 19] 19. The method of claim 18, wherein the regular interval is 0.5 mm or less, 0.4 mm or less, or 0.2 mm or less. [Embodiment 20] 20. The method for producing a molded article according to claim 18 or 19, wherein the constant interval is 0.01 mm or more, 0.05 mm or more, or 0.1 mm or more. [Embodiment 21] 21. The method for producing a molded article according to any one of claims 18 to 20, wherein the heating temperature is at least the melting point of the thermoplastic resin + 20°C, at least the melting point + 30°C, at least the melting point + 35°C, or at least the glass transition temperature + 120°C, at least the glass transition temperature + 130°C, or at least the glass transition temperature + 120°C. [Embodiment 22] 22. The method for producing a molded article according to any one of claims 18 to 21, wherein the pressure applied by the rollers is 0.1 MPa or more. [Embodiment 23] 23. The method for producing a molded article according to any one of claims 18 to 22, wherein the pressure applied by the rollers is 1.0 MPa or less. [Industrial Applicability]

[0082] The prepreg and molded article of the present invention can be used for structural parts such as sports goods, automobiles, pressure tanks, aircraft, and tension rods. [Explanation of symbols]

[0083] 10 Manufacturing equipment 11 Carbon fiber substrate 12 Resin film 13. Heater 14 Release film 15 Hot plate press 16 Cooling press 17 Prepreg 18 rolls 19 Pressure Roller 20 Bobbin 21 Creel 22, 32, 42 Tape 23 Heating means 24 Roller 25, 35 head 26, 36, 56 Baseplate 27 Automatic Lamination Device 41 Polyimide film 43 Graphite Sheet 51 Reference Tape (R) 52 Adjacent Tapes (O) 53 Spacing (D)

Claims

1. The shear rate γ measured by a flow tester containing a thermoplastic resin and a fiber substrate is (125±35) sec -1 the viscosity of the thermoplastic resin at a temperature of the melting point of the thermoplastic resin + 20 to 60°C or the glass transition temperature of the thermoplastic resin + 120 to 160°C includes a range of 1000 Pa s or less, and the internal defect rate within the tape is 5% or less.

2. 2. The tape according to claim 1, wherein the thermoplastic resin comprises at least one selected from the group consisting of polyolefin, polyamide, polyester, polyacetal, polyphenylene sulfide, polyaryl ether ketone, polytetrafluoroethylene, polycarbonate, polymethyl methacrylate, polyvinyl chloride, polystyrene, polyethersulfone, polyetherimide and polyamideimide.

3. 3. The tape of claim 1 or 2, comprising a unidirectionally aligned sheet.

4. The tape of claim 1 or 2, wherein the fibrous substrate comprises carbon fiber.

5. 3. The tape of claim 1 or 2, having a width of 55 mm or less.

6. 3. The tape of claim 1 or 2, having a width of 16 mm or more.

7. The fiber substrate contains reinforcing fibers, and the fiber basis weight of the reinforcing fibers is 500 g / m 2 3. The tape of claim 1 or 2, wherein:

8. 3. The tape according to claim 1 or 2, having a thickness of 0.01 mm or more and 0.5 mm or less.

9. 3. The tape according to claim 1 or 2, having a thickness of 0.05 mm or more and 0.19 mm or less.

10. 3. The tape according to claim 1, wherein the number of single fibers in the fiber substrate is 1,000 or more and 100,000 or less.

11. The tape according to claim 1 or 2, wherein the fiber substrate comprises reinforcing fibers, and the reinforcing fibers have a fiber diameter of 1 μm or more and 20 μm or less.

12. A molded article using the tape according to claim 1 or 2.

13. A method for producing a molded article, comprising disposing the tape according to claim 1 or 2 while heating it.

14. The method for producing a molded article according to claim 12, wherein a plurality of the tapes are arranged in a width direction of the tape.

15. A thermoplastic resin and a fiber substrate are included, and the shear rate γ measured by a flow tester is (125±35) sec -1 The method for producing a molded product includes a step of arranging, at intervals, a plurality of tapes, the viscosity of which at a temperature of the thermoplastic resin is 1000 Pa·s or less at a temperature of the melting point of the thermoplastic resin + 20 to 60°C or the glass transition temperature + 120 to 160°C of the thermoplastic resin, a heating step of heating the plurality of tapes, and a pressing step of pressing the tapes with a roller, wherein the tapes are expanded in width in the heating step or the pressing step to fill in the gaps between adjacent tapes.

16. The method for producing a molded article according to claim 15, wherein the interval is 0.5 mm or less.

17. The method for producing a molded article according to claim 15 or 16, wherein the interval is 0.01 mm or more.

18. The method for producing a molded article according to claim 15 or 16, wherein the heating temperature in the heating step is a melting point of the thermoplastic resin plus 20°C or more or a glass transition temperature of the thermoplastic resin plus 120°C or more.

19. The method for producing a molded body according to claim 15 or 16, wherein a pressing pressure in the pressing step is 0.1 MPa or more and 1.0 MPa or less.

Citation Information

Patent Citations

  • Unidirectionally-oriented tape-shaped prepreg, and molded article thereof

    WO2019017057A1

  • Improved composite materials

    JP2013538264A