Silicon carbide semiconductor device and manufacturing method thereof

The silicon carbide semiconductor device employs a 3C-SiC source contact and 4H-SiC base contact structure to address leakage defects, achieving low resistance ohmic contact and reduced defects through a trench gate configuration.

JP2024141950APending Publication Date: 2024-10-10FUJI ELECTRIC CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023053842
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Trench gate type silicon carbide semiconductor devices face issues with leakage defects due to damage in the source region caused by ion implantation, which inverts the conductivity type and forms a silicide layer, leading to poor ohmic contact and increased resistance.

Method used

The device design includes a 3C-SiC structure for the source contact region and a 4H-SiC structure for the base contact region, with a gate trench and contact trench configuration that avoids the need for a silicide layer, ensuring ohmic contact and reducing leakage defects.

Benefits of technology

This configuration allows for low resistance ohmic contact without a silicide layer, reducing peeling and leakage defects, and minimizing crystal defects at the junctions, thereby enhancing the device's performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141950000001_ABST
    Figure 2024141950000001_ABST
Patent Text Reader

Abstract

To provide a silicon carbide semiconductor device in which a main region can make ohmic contact with a main electrode without a silicide layer therebetween and suppress leakage defects.SOLUTION: A semiconductor device includes a drift layer 2 of a first conductivity type, base regions 6a, 6b of a second conductivity type provided on the upper surface side of the drift layer 2, source contact regions 71a, 71b of the first conductivity type provided on the upper surface side of the base regions 6a, 6b and made of silicon carbide including a 3C structure, a gate electrode 12 provided inside a gate trench 10 via a gate insulating film 11, main electrodes (14, 15, 16) provided inside the contact trenches 8a, 8b and in contact with side surfaces of the source contact regions 71a, 71b, and base contact regions 5a, 5b of the second conductivity type made of silicon carbide having a 4H structure in contact with lower surfaces of the contact trenches 8a, 8b, and the lower surfaces of the contact trenches 8a, 8b are deeper than the lower surfaces of the source contact regions 71a, 71b.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to silicon carbide semiconductor devices and methods of manufacturing the same. [Background technology]

[0002] Patent Document 1 discloses a semiconductor device in which an amorphous layer is formed by ion-implanting phosphorus into a hexagonal single crystal silicon carbide substrate, the amorphous layer is recrystallized into cubic single crystal n-type silicon carbide by heat treatment, and an electrode is formed by vapor-depositing nickel on the upper surface of the n-type silicon carbide.

[0003] Patent Document 2 describes a n-type 4H-SiC + The n-type SiC was formed on the first main surface. - In the epitaxial growth layer, + A type source region, + n-type source region + Type 3C-SiC region and p + and a n-type potential clamping region. + Type 3C-SiC region and p + A semiconductor device is disclosed in which a barrier metal film is formed in contact with a type potential fixing region, and a source wiring electrode is formed on the barrier metal film. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-49198 A [Patent Document 2] International Publication No. 2017 / 042963 Summary of the Invention [Problem to be solved by the invention]

[0005] In a trench-gate silicon carbide semiconductor device, it has been considered to form the source region (main region) from 3C-SiC in order to make ohmic contact with the source electrode (main electrode). In this case, n-type impurity ions are implanted to form n + After forming a p-type source region on the entire surface, a mask is used to implant p-type impurities into the source region, reversing the conductivity type of a portion of the source region to p + From a manufacturing perspective, it is reasonable to form a base contact region on the source region. However, a lot of damage occurs in the part of the source region where the source region is pushed back, which may cause leakage defects.

[0006] In view of the above problems, the present disclosure has an object to provide a silicon carbide semiconductor device and a manufacturing method thereof in which a main region can be in ohmic contact with a main electrode without a silicide layer in a trench-gate type silicon carbide semiconductor device and leakage defects can be suppressed. [Means for solving the problem]

[0007] In order to achieve the above object, one aspect of the present disclosure is a silicon carbide semiconductor device comprising: a drift layer of a first conductivity type made of silicon carbide; a base region of a second conductivity type made of silicon carbide and provided on an upper surface side of the drift layer; a source contact region of the first conductivity type made of silicon carbide including a 3C structure and provided on an upper surface side of the base region; a gate insulating film provided inside a gate trench penetrating the source contact region and the base region; a gate electrode provided inside the gate trench with the gate insulating film interposed therebetween; a main electrode provided inside a contact trench provided away from the gate trench and in contact with at least a side surface of the source contact region; and a base contact region of the second conductivity type made of silicon carbide with a 4H structure and having a higher impurity concentration than the base region, in contact with a lower surface of the contact trench,

[0008] Another aspect of the present disclosure is summarized as a method for manufacturing a silicon carbide semiconductor device, the method including the steps of: forming a base region of a second conductivity type made of silicon carbide on an upper surface side of a drift layer of a first conductivity type made of silicon carbide; forming a source contact region of the first conductivity type made of silicon carbide including a 3C structure on an upper surface side of the base region; forming a gate trench penetrating the source contact region and the base region; forming a gate electrode inside the gate trench via a gate insulating film; forming a contact trench spaced from the gate trench penetrating the source contact region; forming a main electrode inside the contact trench in contact with at least a side surface of the source contact region; and forming a base contact region of the second conductivity type in contact with a lower surface of the contact trench, made of silicon carbide with a 4H structure, and having a higher impurity concentration than the base region, wherein the lower surface of the contact trench is formed deeper than the lower surface of the source contact region. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a trench-gate silicon carbide semiconductor device in which a main region can be in ohmic contact with a main electrode without a silicide layer therebetween and leakage defects can be suppressed, and a manufacturing method thereof. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic cross-sectional view showing an example of a silicon carbide semiconductor device in accordance with a first embodiment. [Diagram 2] 2 is a schematic cross-sectional view showing an enlarged area A of FIG. 1. [Diagram 3] 5A to 5C are schematic cross-sectional views illustrating an example of a method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. [Figure 4] 5 is a schematic cross-sectional view continuing from FIG. 3 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Diagram 5] 5 is a schematic cross-sectional view continuing from FIG. 4 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 6] 6 is a schematic cross-sectional view continuing from FIG. 5 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 7] 7 is a schematic cross-sectional view continuing from FIG. 6 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 8] 8 is a schematic cross-sectional view continuing from FIG. 7 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 9] 9 is a schematic cross-sectional view continuing from FIG. 8 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. [Figure 10] 10 is a schematic cross-sectional view continuing from FIG. 9 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 11] 11 is a schematic cross-sectional view continuing from FIG. 10 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 12] 12 is a schematic cross-sectional view continuing from FIG. 11 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment. FIG. [Figure 13] 10A to 10C are schematic cross-sectional views for illustrating a method for manufacturing a silicon carbide semiconductor device according to a comparative example. [Figure 14] 1 is a schematic cross-sectional view showing an example of a silicon carbide semiconductor device according to a second embodiment. [Figure 15] FIG. 15 is a schematic cross-sectional view showing an enlarged area A of FIG. [Figure 16] 10 is a schematic cross-sectional view illustrating an example of a method for manufacturing a silicon carbide semiconductor device in accordance with a second embodiment. FIG. [Figure 17] 17 is a schematic cross-sectional view continuing from FIG. 16 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the second embodiment. FIG. [Figure 18] 17 for illustrating an example of the method for manufacturing the silicon carbide semiconductor device in accordance with the second embodiment. FIG. [Figure 19] 19 is a schematic cross-sectional view continuing from FIG. 18 for illustrating the example of the method for manufacturing the silicon carbide semiconductor device in accordance with the second embodiment. FIG. [Figure 20] 10 is a schematic cross-sectional view showing an example of a silicon carbide semiconductor device according to a third embodiment. [Figure 21] 10 is a schematic cross-sectional view showing an example of a silicon carbide semiconductor device in accordance with a fourth embodiment. FIG. [Figure 22] 13 is a schematic cross-sectional view showing an example of a silicon carbide semiconductor device in accordance with a fifth embodiment. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the first to fifth embodiments of the present disclosure will be described with reference to the drawings. In the description of the drawings, the same or similar parts are denoted with the same or similar reference numerals, and duplicated explanations will be omitted. However, the drawings are schematic, and the relationship between thickness and planar dimensions, the ratio of thickness of each layer, etc. may differ from the actual ones. In addition, the drawings may include parts with different dimensional relationships and ratios. In addition, the first to fifth embodiments shown below are examples of devices and methods for embodying the technical idea of ​​the present disclosure, and the technical idea of ​​the present disclosure does not specify the materials, shapes, structures, arrangements, etc. of the components as described below.

[0012] In this specification, the source region of a metal-oxide semiconductor field-effect transistor (MOSFET) is "one main region (first main region)" that can be selected as the emitter region of an insulated gate bipolar transistor (IGBT). In addition, in a thyristor such as a MOS-controlled static induction thyristor (SI thyristor), the "one main region" can be selected as the cathode region. The drain region of a MOSFET is the "other main region (second main region)" of the semiconductor device that can be selected as the collector region in an IGBT and as the anode region in a thyristor. In this specification, when the term "main region" is used simply, it means either the first main region or the second main region that is appropriate from the technical common sense of a person skilled in the art.

[0013] In addition, the definitions of directions such as up and down in the following description are merely for the convenience of explanation and do not limit the technical idea of ​​the present disclosure. For example, if an object is rotated 90 degrees and observed, up and down are converted to left and right and read as such, and if it is rotated 180 degrees and observed, up and down are of course read as reversed. In addition, "upper surface" may be read as "front surface" and "lower surface" may be read as "reverse surface."

[0014] In the following description, the first conductivity type is n-type and the second conductivity type is p-type. However, the conductivity types may be selected in the opposite relationship, with the first conductivity type being p-type and the second conductivity type being n-type. The + or - attached to n or p means that the semiconductor region has a relatively high or low impurity concentration, respectively, compared to a semiconductor region without + or -. However, even if the semiconductor regions have the same n and n attached, it does not mean that the impurity concentrations of the respective semiconductor regions are strictly the same.

[0015] Silicon carbide (SiC) crystals also have crystal polymorphism, the main ones being cubic 3C, and hexagonal 4H and 6H. The band gap at room temperature has been reported to be 2.23 eV for SiC with a 3C structure (3C-SiC), 3.26 eV for SiC with a 4H structure (4H-SiC), and 3.02 eV for SiC with a 6H structure (6H-SiC). The following explanation will be given as an example in which 4H-SiC and 3C-SiC are mainly used.

[0016] (First embodiment) <Structure of Silicon Carbide Semiconductor Device> The silicon carbide semiconductor device according to the first embodiment illustrates a case in which an active element includes a trench-gate vertical MOSFET, which is a vertical switching element, as shown in Fig. 1. Note that Fig. 1 illustrates a unit cell including an insulated gate electrode structure (11, 12) embedded in one trench (gate trench) 10, but in reality, a large number of such unit cells are periodically arranged.

[0017] The silicon carbide semiconductor device according to the first embodiment is a first conductivity type (n -The drift layer 2 is formed of an epitaxially grown layer of SiC such as 4H-SiC. The impurity concentration of the drift layer 2 is, for example, 1×10 15 cm -3 That's it, 5 x 10 16 cm -3 The thickness of the drift layer 2 is, for example, about 1 μm or more and 100 μm or less. The impurity concentration and thickness of the drift layer 2 can be appropriately adjusted according to the withstand voltage specifications and the like.

[0018] Base regions 6a, 6b of a second conductivity type (p-type) are provided on the upper surface side of the drift layer 2. The lower surfaces of the base regions 6a, 6b are in contact with the upper surface of the drift layer 2. The base regions 6a, 6b are semiconductor regions made of SiC such as 4H-SiC formed by ion implantation of p-type impurities into the drift layer 2. The base regions 6a, 6b may be epitaxially grown layers made of SiC such as 4H-SiC. The impurity concentration of the base regions 6a, 6b is, for example, 1×10 16 cm -3 That's it, 1×10 18 cm -3 It is about the following.

[0019] A current spreading layer (CSL) of a first conductivity type (n-type) having a higher impurity concentration than the drift layer 2 may be provided between the drift layer 2 and the base regions 6a and 6b. When the current spreading layer is provided, the upper surface of the drift layer 2 may be in contact with the lower surface of the current spreading layer, and the upper surface of the current spreading layer may be in contact with the lower surfaces of the base regions 6a and 6b.

[0020] The upper surface side of the base regions 6a and 6b is provided with a first conductivity type (n + The source regions 7a and 7b are semiconductor regions made of SiC formed by ion-implanting n-type impurities into the drift layer 2, for example.

[0021] The source region 7a is an n-type semiconductor having a 3C structure provided on the upper surface side of the base region 6a. +A source extension region (first region) 71a of the n-type, which is a 4H structure provided on the upper surface side of the source extension region 71a, + The source region 7b includes a n-type source contact region (second region) 72a. The source region 7b includes a 3C structure provided on the upper surface side of the base region 6b. + A source extension region (first region) 71b of a n-type, 4H structure provided on the upper surface side of the source extension region 71b. + The source regions 7a and 7b include a source contact region (second region) 72b. The source regions 7a and 7b will be described in detail later.

[0022] A gate trench 10 is provided penetrating the source regions 7a, 7b and the base regions 6a, 6b from the upper surfaces of the source regions 7a, 7b toward the normal direction (depth direction) of the upper surfaces of the source regions 7a, 7b. The lower surface of the gate trench 10 reaches the drift layer 2. The width of the gate trench 10 is, for example, about 1 μm or less. The source region 7a and the base region 6a are in contact with the left side surface of the gate trench 10. The source region 7b and the base region 6b are in contact with the right side surface of the gate trench 10. The cross section of FIG. 1 illustrates a case where the lower surface and the side surface of the gate trench 10 form a corner, but the lower surface of the gate trench 10 may be a curved surface.

[0023] A gate insulating film 11 is provided along the bottom surface and both side surfaces of the gate trench 10. A gate electrode 12 is embedded inside the gate trench 10 via the gate insulating film 11. The gate insulating film 11 and the gate electrode 12 form a trench-gate type insulated gate electrode structure (11, 12).

[0024] The gate insulating film 11 is a silicon oxide film (SiO 2 film), silicon oxynitride (SiON) film, strontium oxide (SrO) film, silicon nitride (Si 3 N 4 ) film, aluminum oxide (Al 2 O 3 ) film, magnesium oxide (MgO) film, yttrium oxide (Y 2 O 3 ) film, hafnium oxide (HfO2 ) film, zirconium oxide (ZrO 2 ) film, tantalum oxide (Ta 2 O 5 ) film, bismuth oxide (Bi 2 O 3 ) film or a composite film in which a plurality of these films are laminated can be used. As the material for the gate electrode 12, for example, a polysilicon layer doped with a high concentration of p-type impurities or n-type impurities (doped polysilicon layer), or a high melting point metal such as titanium (Ti), tungsten (W), or nickel (Ni) can be used.

[0025] Within the drift layer 2 and below the gate trench 10, a second conductivity type (p + The upper surface of the gate protection region 4b is in contact with the lower surface of the gate trench 10. The upper surface of the gate protection region 4b does not have to be in contact with the lower surface of the gate trench 10. The gate protection region 4b is, for example, a semiconductor region made of SiC such as 4H-SiC formed by ion implantation of p-type impurities into the drift layer 2. The impurity concentration of the gate protection region 4b is, for example, 1×10 17 cm -3 That's it, 1×10 19 cm -3 The gate protection region 4b may be electrically connected to the base region 6a.

[0026] Within the drift layer 2, a second conductivity type (p + The buried regions 4a, 4c are provided at approximately the same depth as the gate protection region 4b. The buried regions 4a, 4c are semiconductor regions made of SiC such as 4H-SiC formed by ion-implanting p-type impurities into the drift layer 2. The impurity concentration of the buried regions 4a, 4c is, for example, 1×10 17 cm -3 That's it, 1×10 19 cm -3 In addition, in the front side or the back side of the paper surface of FIG. 1, the p +A semiconductor region of the type may be selectively provided.

[0027] The upper portion of the drift layer 2 and on the upper surface side of the buried regions 4a and 4c are provided with a second conductivity type (p + The base contact regions 5a and 5b are semiconductor regions made of SiC such as 4H-SiC in which p-type impurities are ion-implanted into the drift layer 2. The impurity concentration of the base contact regions 5a and 5b is, for example, 1×10 18 cm -3 That's it, 1×10 21 cm -3 The lower surfaces of the base contact regions 5a and 5b have a depth approximately equal to that of the lower surfaces of the base regions 6a and 6b, but may be shallower or deeper than the lower surfaces of the base regions 6a and 6b.

[0028] The lower surface of the base contact region 5a is in contact with the upper surface of the buried region 4a. The side surface of the base contact region 5a is in contact with the base region 6a and the source extension region 71a, but is not in contact with the source contact region 72a. The lower surface of the base contact region 5b is in contact with the upper surface of the buried region 4c. The side surface of the base contact region 5b is in contact with the base region 6b and the source extension region 71b, but is not in contact with the source contact region 72b. When the lower surface of the base contact region 5a is shallower than the lower surface of the base region 6a, the lower surface of the base contact region 5a is in contact with the upper surface of the base region 6a, and the upper surface of the buried region 4a is in contact with the lower surface of the base region 6a.

[0029] Although not shown in FIG. 1, a plurality of gate trenches 10 are arranged in the left-right direction of FIG. 1. Between adjacent gate trenches 10, trenches (contact trenches) 8a, 8b different from the gate trenches 10 are provided at a distance from each of the adjacent gate trenches 10. The depths of the contact trenches 8a, 8b are shallower than the depth of the gate trench 10. The lower surface of the contact trench 8a is deeper than the lower surface of the source contact region 72a and shallower than the lower surface of the source extension region 71a. The lower surface of the contact trench 8a is in contact with the upper surface of the base contact region 5a. The side surface of the contact trench 8a is in contact with the side surfaces of the source extension region 71a and the source contact region 72a.

[0030] The bottom surface of the contact trench 8b is deeper than the bottom surface of the source contact region 72b and shallower than the bottom surface of the source extension region 71b. The bottom surface of the contact trench 8b contacts the top surface of the base contact region 5b. The side surfaces of the contact trench 8b contact the side surfaces of the source extension region 71b and the source contact region 72b.

[0031] An interlayer insulating film 13 is provided on the upper surface side of the gate electrode 12. The interlayer insulating film 13 may be, for example, a silicon oxide film doped with boron (B) and phosphorus (P) (BPSG film), a silicon oxide film doped with phosphorus (P) (PSG film), a non-doped silicon oxide film that does not contain phosphorus (P) or boron (B) and is called "NSG", a silicon oxide film doped with boron (B) (BSG film), a silicon nitride film (Si 3 N 4 The interlayer insulating film 13 is formed of a single layer film such as a SiO 2 film or a laminated film thereof. The interlayer insulating film 13 is provided with contact holes 13a and 13b so as to expose parts of the upper surfaces of the source contact regions 72a and 72b and the contact trenches 8a and 8b.

[0032] First main electrodes (source electrodes) (14, 15, 16) are provided so as to fill the contact trenches 8a, 8b exposed in the contact holes 13a, 13b of the interlayer insulating film 13 and to cover the upper surface of the interlayer insulating film 13 and parts of the upper surfaces of the source contact regions 72a, 72b exposed in the contact holes 13a, 13b. The source electrodes (14, 15, 16) include a barrier metal layer 14, a source wiring layer 15, and a silicide layer 16.

[0033] The silicide layer 16 is selectively provided on the upper surfaces of the base contact regions 5a, 5b exposed at the lower surfaces of the contact trenches 8a, 8b, and is in ohmic contact with the upper surfaces of the base contact regions 5a, 5b with low resistance. The silicide layer 16 is made of nickel silicide (NiSi x The source electrodes (14, 15, 16) may be composed of only the barrier metal layer 14 and the source wiring layer 15 without including the silicide layer 16. In that case, the upper surfaces of the base contact regions 5a, 5b may be in contact with the barrier metal layer 14.

[0034] The barrier metal layer 14 is provided to cover the interlayer insulating film 13, the side surfaces of the contact holes 13a and 13b of the interlayer insulating film 13, the source extension regions 71a and 71b and the source contact regions 72a and 72b exposed on the side surfaces of the contact trenches 8a and 8b, and the silicide layer 16 exposed on the lower surfaces of the contact trenches 8a and 8b. The barrier metal layer 14 is in direct contact with the source extension regions 71a and 71b and the source contact regions 72a and 72b. The barrier metal layer 14 is in ohmic contact with the source contact regions 72a and 72b including the 3C structure with low resistance, but is not in ohmic contact with the source extension regions 71a and 71b including the 4H structure. The barrier metal layer 14 is made of a metal such as titanium nitride (TiN), titanium (Ti), or a TiN / Ti laminated structure with Ti as the lower layer.

[0035] The source wiring layer 15 is provided so as to cover the barrier metal layer 14. The source wiring layer 15 is electrically connected to the source contact regions 72a, 72b and the base contact regions 5a, 5b. The source wiring layer 15 is made of a metal or an alloy such as aluminum (Al), aluminum-silicon (Al-Si), aluminum-copper (Al-Cu), copper (Cu), etc. The source wiring layer 15 is provided separately from a gate wiring layer (not shown) electrically connected to the gate electrode 12.

[0036] The lower surface side of the drift layer 2 is provided with a first conductivity type (n + The drain region 1 is formed of a semiconductor substrate (SiC substrate) made of SiC such as 4H-SiC. The impurity concentration of the drain region 1 is, for example, 1×10 18 cm -3 That's it, 3 x 10 20 cm -3 The thickness of the drain region 1 is, for example, about 30 μm or more and 500 μm or less. Note that, between the drift layer 2 and the drain region 1, a dislocation conversion layer or a recombination promotion layer, which is an n-type buffer layer having a higher impurity concentration than the drift layer 2 and a lower impurity concentration than the drain region 1, may be provided.

[0037] A second main electrode (drain electrode) 17 is provided on the lower surface side of the drain region 1. The drain electrode 17 may be, for example, a single layer film made of gold (Au) or a metal film laminated in the order of titanium (Ti), nickel (Ni) and Au from the drain region 1 side, and further a metal film of molybdenum (Mo), tungsten (W) or the like may be laminated on the bottom layer. Nickel silicide (NiSi x A drain contact layer such as a SiO 2 film may be provided.

[0038] The gate trench 10 shown in Fig. 1 has a planar pattern extending in a stripe shape in the horizontal direction from the front side to the back side of the paper surface of Fig. 1. The gate trench 10 is not particularly limited to a planar pattern extending in a stripe shape, and may have, for example, a dot-like or lattice-like planar pattern. The source extension regions 71a, 71b, the source contact regions 72a, 72b, and the base contact regions 5a, 5b have planar patterns extending in a stripe shape parallel to the gate trench 10.

[0039] Figure 2 is a schematic cross-sectional view enlarging a dashed line region A of the silicon carbide semiconductor device according to the first embodiment shown in Figure 1. With reference to Figure 2, configurations of source extension region 71a and source contact region 72a, and the positional relationship between source extension region 71a, source contact region 72a, base contact region 5a, and insulated gate electrode structure (11, 12) will be described.

[0040] The depth d1 of the source extension region 71a from the top surface of the source contact region 72a is, for example, about 150 nm or more and 450 nm or less. The width w1 of the source extension region 71a is, for example, about 400 nm or more and 1000 nm or less. The right side surface of the source extension region 71a directly contacts the gate insulating film 11 and faces the gate electrode 12 via the gate insulating film 11. The left side surface of the source extension region 71a contacts the base contact region 5a, the side surface of the contact trench 8a, the silicide layer 16, and the barrier metal layer 14. The depth d3 of the contact trench 8a from the top surface of the source contact region 72a is, for example, about 40 nm or more and 450 nm or less.

[0041] The source extension region 71a has fewer crystal defects than the source contact region 72a and does not inherit the crystal defects of the source contact region 72a. The source extension region 71a is made of 4H-SiC. That is, the source extension region 71a is mainly made of 4H-SiC (4H structure) and contains almost no 3C-SiC. The proportion of 4H-SiC contained in the source extension region 71a is, for example, about 90% or more and 100% or less. In addition to 4H-SiC, the source extension region 71a may contain small amounts of amorphous structure, 3C-SiC, etc. The impurity concentration of the source extension region 71a is, for example, 1×10 16 cm -3 That's it, 1×10 20 cm -3 The source extension region 71a contains, for example, nitrogen (N) or phosphorus (P) as an n-type impurity. The source extension region 71a may contain arsenic (As) as an n-type impurity.

[0042] The depth d2 from the upper surface to the lower surface of the source contact region 72a (the thickness of the source contact region 72a) is, for example, about 30 nm or more and 100 nm or less. The width w1 of the source contact region 72a is approximately the same as the width w1 of the source extension region 71a and is, for example, about 400 nm or more and 1000 nm or less.

[0043] The right side surface of the source contact region 72a is in direct contact with the gate insulating film 11 and faces the interlayer insulating film 13 via the gate insulating film 11, but does not face the gate electrode 12. The left side surface of the source contact region 72a is in contact with the side surface of the contact trench 8a and the barrier metal layer 14. A part of the upper surface of the source contact region 72a continuing from the left side surface is exposed in the contact hole 13a of the interlayer insulating film 13 and is in contact with the barrier metal layer 14.

[0044] The source contact region 72a is a region including 3C-SiC (3C structure). The ratio of 3C-SiC included in the source contact region 72a is higher than the ratio of 3C-SiC included in the source extension region 71a, and is, for example, about 10% or more and 100% or less. The source contact region 72a may be a mixed crystal of 3C-SiC and 4H-SiC. The source contact region 72a may include an amorphous structure, 4H-SiC, etc., in addition to 3C-SiC. Since 3C-SiC has a narrower band gap than 4H-SiC, the source contact region 72a including 3C-SiC can make ohmic contact with the barrier metal layer 14 of the source electrode (14, 15, 16) with low resistance without the silicide layer 16. To achieve good ohmic contact, the ratio of 3C-SiC included in the source contact region 72a is preferably 10% or more.

[0045] The impurity concentration of the source contact region 72a is higher than or substantially the same as the impurity concentration of the source extension region 71a. The impurity concentration of the source contact region 72a is, for example, 1×10 20 cm -3 That's it, 1×10 22 cm -3 or less. The source contact region 72a contains, for example, phosphorus (P) or arsenic (As) as an n-type impurity. The source contact region 72a may contain, for example, nitrogen (N) as an n-type impurity. The source contact region 72a may contain, for example, a plurality of types of P, As, and N as an n-type impurity. The source contact region 72a may contain an inert element such as argon (Ar) or helium (He).

[0046] The crystal structures of the source extension region 71a and the source contact region 72a can be made different by changing the element to be ion-implanted, the temperature during ion implantation, the dose (impurity concentration), the activation temperature, etc., for each of the source extension region 71a and the source contact region 72a. The source contact region 72a containing 3C-SiC can be formed, for example, by ion-implanting a high concentration (high dose) of n-type impurities or inert elements into 4H-SiC at room temperature, thereby breaking down the 4H-SiC and forming an amorphous structure by utilizing the damage caused by the ion implantation. Thereafter, activation annealing is performed, and the amorphous structure is recrystallized to become 3C-SiC, thereby forming the source contact region 72a containing 3C-SiC.

[0047] On the other hand, a method for forming source extension region 71a of 4H-SiC is to perform ion implantation of n-type impurities into 4H-SiC at room temperature or a high temperature (e.g., about 200°C or higher and 600°C or lower) at a concentration (dose) that does not destroy the structure of the 4H-SiC, thereby forming source extension region 71a while maintaining the 4H-SiC.

[0048] As a method for measuring (observing) the crystal structure of the source extension region 71a and the source contact region 72a, for example, a field emission scanning electron microscope (FE-SEM) and electron backscatter diffraction (EBSD) can be used to measure the area ratio of the crystal structure of the surface. As an example, samples were fabricated by changing the temperature during ion implantation between 500°C and room temperature (25°C) under the same conditions of the ion implantation element, dose (impurity concentration), and activation temperature, and the samples were observed by FE-SEM and EBSD. As a result, the ratio of 4H-SiC on the surface of the 500°C sample was 100%. On the other hand, the ratio of 4H-SiC on the surface of the room temperature sample was 86% and the ratio of 3C-SiC was 14%.

[0049] The method for forming the base contact region 5a of 4H-SiC is the same as the method for forming the source extension region 71a of 4H-SiC. The method for forming the base contact region 5a of 4H-SiC is to perform ion implantation of p-type impurities into 4H-SiC at room temperature or high temperature (e.g., 200° C. or higher and 600° C. or lower) at a concentration (dose) that does not destroy the structure of 4H-SiC, thereby forming the base contact region 5a while maintaining the 4H-SiC. The base contact region 5a contains, for example, aluminum (Al) or boron (B) as the p-type impurity.

[0050] 2, the upper surface of the gate electrode 12 at the end where it contacts the gate insulating film 11 is located deeper than the lower surface of the source contact region 72a at the gate insulating film 11 and shallower than the lower surface of the source extension region 71a at the gate insulating film 11. The upper surface of the gate electrode 12 at the position where it contacts the gate insulating film 11 may be the uppermost surface of the gate electrode 12. For example, if the upper surface of the gate electrode 12 as a whole is a curved surface that is convex downward, the upper surface of the center part of the gate electrode 12 may be located deeper than the upper surfaces of the ends of the gate electrode 12.

[0051] The gate electrode 12 and the source extension region 71a face each other via the gate insulating film 11. The gate electrode 12 and the source contact region 72a do not face each other via the gate insulating film 11. A depression amount d0 of the gate electrode 12 from an upper surface of the source contact region 72a is, for example, about 100 nm or more and 300 nm or less. The depression amount d0 of the gate electrode 12 and the position of the upper surface of the gate electrode 12 at the position where the gate electrode 12 contacts the gate insulating film 11 can be controlled by, for example, adjusting the etching conditions of the gate electrode 12.

[0052] The upper surface of the end portion of the gate electrode 12 that contacts the gate insulating film 11 may be shallower than the lower surface of the source contact region 72a that contacts the gate insulating film 11.

[0053] The source extension region 71b and the source contact region 72b of the source region 7b shown in Fig. 1 have the same configuration as the source extension region 71a and the source contact region 72a of the source region 7a, respectively, and therefore a duplicated description will be omitted. Also, the positional relationship between the source extension region 71b, the source contact region 72b, the base contact region 5b, and the insulated gate electrode structure (11, 12) is the same as the positional relationship between the source extension region 71a, the source contact region 72a, the base contact region 5a, and the insulated gate electrode structure (11, 12) of the source region 7a shown in Fig. 2, and therefore a duplicated description will be omitted.

[0054] During operation of the silicon carbide semiconductor device according to the first embodiment, when the source electrodes (14, 15, 16) are at earth potential, a positive voltage is applied to the drain electrode 17, and a positive voltage equal to or greater than a threshold is applied to the gate electrode 12, an inversion layer (channel) is formed on the side surface of the gate trench 10 in the base regions 6a, 6b, resulting in an ON state. In the ON state, a current flows from the drain electrode 17 to the source electrode (14, 15, 16) via the drain region 1, the drift layer 2, the inversion layer in the base regions 6a, 6b, and the source regions 7a, 7b. On the other hand, when the voltage applied to the gate electrode 12 is less than the threshold, an inversion layer is not formed in the base regions 6a, 6b, resulting in an OFF state, and no current flows from the drain electrode 17 to the source electrode (14, 15, 16).

[0055] According to the silicon carbide semiconductor device of the first embodiment, the source contact regions 72a, 72b including 3C-SiC of the source regions 7a, 7b can make ohmic contact with the source electrodes (14, 15, 16) with low resistance without the silicide layer 16. Therefore, the silicide layer 16 is not required on the contact junction surfaces of the source contact regions 72a, 72b, and peeling of the silicide layer 16 on the contact junction surfaces of the source contact regions 72a, 72b can be suppressed. Furthermore, the side surfaces and parts of the upper surfaces of the source contact regions 72a, 72b make ohmic contact with the source electrodes (14, 15, 16), and therefore the contact resistance can be reduced.

[0056] Furthermore, in the silicon carbide semiconductor device according to the first embodiment, the lower surfaces of the contact trenches 8a, 8b are made deeper than the lower surfaces of the source contact regions 72a, 72b, so that the source contact regions 72a, 72b containing 3C-SiC are not in contact with the base contact regions 5a, 5b made of 4H-SiC. Therefore, compared to a case in which the source contact regions 72a, 72b and the base contact regions 5a, 5b are in contact with each other without providing the contact trenches 8a, 8b, there is no damage due to ion implantation for forming the source extension regions 71a, 71b in the base contact regions 5a, 5b, and leakage defects can be suppressed.

[0057] Furthermore, in the silicon carbide semiconductor device of the first embodiment, the pn junction formed by the 4H—SiC source extension regions 71a, 71b and the 4H—SiC base contact regions 5a, 5b is made of 4H—SiC, and therefore leakage current at the pn junction can be prevented compared to a case in which the pn junction is formed by source contact regions 72a, 72b containing 3C—SiC, which has many remaining crystal defects, and base contact regions 5a, 5b of 4H—SiC.

[0058] Furthermore, in the silicon carbide semiconductor device according to the first embodiment, the upper surface of the gate electrode 12 is made deeper than the lower surface of the source contact region 72a and shallower than the lower surface of the source extension region 71a. As a result, the source extension region 71a, which has relatively few crystal defects and little surface irregularity, of the source region 7a faces the gate electrode 12 via the gate insulating film 11, while the source contact region 72a, which has relatively many crystal defects and much surface irregularity, of the source region 7a, does not face the gate electrode 12 via the gate insulating film 11. This makes it possible to suppress the generation of leakage current between the source region 7a and the gate electrode 12.

[0059] <Method for manufacturing silicon carbide semiconductor device> Next, an example of a method for manufacturing the silicon carbide semiconductor device according to the first embodiment will be described. Note that the method for manufacturing the silicon carbide semiconductor device described below is just one example, and it goes without saying that various other manufacturing methods, including modifications thereof, can be implemented within the spirit and scope of the claims.

[0060] First, n-type impurities such as nitrogen (N) are added. + A semiconductor substrate (SiC substrate) 1 (see FIG. 3) made of SiC such as 4H-SiC is prepared. The top surface of the SiC substrate 1 has an off angle of, for example, 3 degrees to 8 degrees from the {0001} plane. Next, as shown in FIG. 3, n-type impurities such as N are added to the top surface of the SiC substrate 1 to form an n-type substrate with a lower impurity concentration than the SiC substrate 1. - A drift layer 2 made of SiC such as 4H-SiC of the type is epitaxially grown.

[0061] Next, an oxide film is deposited on the upper surface of the drift layer 2 by chemical vapor deposition (CVD) technology or the like. A photoresist film is applied to the upper surface of the oxide film, and the oxide film is patterned by photolithography technology, dry etching technology or the like. Using the patterned oxide film as an ion implantation mask, p-type impurities such as aluminum (Al) are selectively ion-implanted. Note that a photoresist film may be used as the ion implantation mask instead of the oxide film. Thereafter, the oxide film used as the ion implantation mask is removed. As a result, p-type impurities are formed inside the drift layer 2, as shown in FIG. 4. + The buried regions 4a, 4c and p + A gate protection region 4b of the mold is selectively formed.

[0062] In addition, the drift layer 2 shown in FIG. 3 is epitaxially grown up to the middle (lower) portion, and p + The buried regions 4a, 4c and p + Alternatively, the structure shown in FIG. 4 may be obtained by forming the gate protection region 4b of the transistor and epitaxially growing the remaining portion (upper portion) of the drift layer 2.

[0063] Next, to form the base region 6, p-type impurities such as aluminum (Al) are ion-implanted into the entire surface at an acceleration voltage lower than that used for the ion implantation when forming the buried regions 4a, 4c and the gate protection region 4b. Also, to form the source extension region 71, n-type impurities such as nitrogen (N) are ion-implanted into the entire surface at an acceleration voltage lower than that used for the ion implantation when forming the base region 6. As a result, as shown in FIG. 5, a p-type base region 6 made of 4H-SiC is formed on the upper surface side of the buried regions 4a, 4c and the gate protection region 4b. Also, an n-type impurity such as nitrogen (N) is ion-implanted into the entire surface at an acceleration voltage lower than that used for the ion implantation when forming the base region 6. As shown in FIG. + A source extension region 71 of the mold is formed.

[0064] In order to cause less damage during ion implantation of the source extension region 71 compared to ion implantation for forming the source contact region 72 described later, phosphorus (P) (atomic number 15) having a relatively small atomic number is preferable as the n-type impurity, and nitrogen (N) (atomic number 7) having a relatively small atomic number is more preferable. Note that, in addition to P or N, arsenic (As) (atomic number 33) having a relatively large atomic number may also be implanted. The temperature during ion implantation is set to be higher than that for ion implantation of the source contact regions 72a and 72b described later, for example, at a temperature of 200° C. or higher and 600° C. or lower. The dose during ion implantation is set so that the impurity concentration of the source extension region 71 is, for example, 1×10 16 cm -3 That's it, 1×10 20 cm -3 The dose during ion implantation is set to about 2×10 15 cm -2 It is set to less than this.

[0065] 6, in order to form the source contact region 72, n-type impurities such as nitrogen (N) are ion-implanted into the entire surface at an acceleration voltage lower than that of the ion implantation used to form the source extension region 71. As a result, n + A source contact region 72 of the type is selectively formed.

[0066] During ion implantation of the source contact region 72, the structure of 4H-SiC on the upper surface side of the source extension region 71 is broken to form an amorphous structure. In FIG. 6, N is exemplified as an n-type impurity, but in order to cause higher damage than the ion implantation of the source extension region 71 described above, phosphorus (P) having a relatively larger number of atoms is preferable as the n-type impurity, and arsenic (As) having a relatively larger number of atoms is more preferable. In the ion implantation of the source contact region 72, the same impurity as that in the ion implantation of the source extension region 71 described above may be implanted, or a different impurity may be implanted. The temperature during ion implantation is set lower than the temperature during ion implantation of the source extension region 71 described above, for example, at 20° C. or higher and 150° C. or lower. The dose during ion implantation is set so that the impurity concentration of the source contact region 72 is, for example, 1×10 20 cm -3 That's it, 1×10 22 cm -3 The dose of ions to be implanted into the source extension region 71 is set to, for example, 2×10 15 cm -2 It is set to the above level.

[0067] When ion implanting the source contact region 72, an inert element such as argon (Ar) or helium (He) may be ion implanted instead of the n-type impurity. The total dose of the inert element ion implantation, including the dose of the ion implantation of the source extension region 71 described above, is, for example, 2×10 15 cm -2 or more. When an inert element is ion-implanted, the ion-implantation of n-type impurities is performed only when forming the source extension region 71, so that the impurity concentrations of the source extension region 71 and the source contact region 72 are approximately the same. After the ion-implantation for forming the source contact region 72, the oxide film 20 used as the ion-implantation mask is removed.

[0068] Next, an oxide film 21 (see FIG. 7) is deposited on the upper surface of the base region 6 by CVD or the like. A photoresist film is applied to the upper surface of the oxide film 21, and the oxide film 21 is patterned by photolithography, dry etching, or the like. Using the patterned oxide film 21 as an etching mask, a part of the source contact region 72 and the source extension region 71 located above the buried regions 4a and 4c is selectively removed by dry etching such as reactive ion etching (RIE) as shown in FIG. 7. As a result, contact trenches 8a and 8b are formed. The lower surfaces of the contact trenches 8a and 8b are dug deeper than the lower surface of the source contact region 72. The source extension region 71 is exposed at the lower surfaces of the contact trenches 8a and 8b. The source extension region 71 and the source contact region 72 are exposed at the side surfaces of the contact trenches 8a and 8b. The lower surfaces of the contact trenches 8a and 8b may be dug deeper than the lower surface of the source extension region 71.

[0069] Next, the oxide film 21 used as the etching mask is used as an ion implantation mask to selectively implant p-type impurities such as aluminum (Al) or boron (B) ions, thereby inverting (reversing) the conductivity type of a portion of the source extension region 71 from n-type to p-type, as shown in FIG. 8. As a result, p-type 4H-SiC is formed on the upper surface side of the buried regions 4a and 4c. + The base contact regions 5a, 5b are selectively formed. The sides of the base contact regions 5a, 5b are not in contact with the source contact region 72, but are in contact with the source extension region 71 and the base region 6. Note that a photoresist film may be used as a mask for both etching and ion implantation instead of the oxide film 21. Thereafter, the oxide film 21 used as the mask for both is removed.

[0070] The order of the ion implantation for forming the buried regions 4a, 4c and the gate protection region 4b, the ion implantation for forming the base region 6, the ion implantation for forming the source extension region 71, the ion implantation for forming the source contact region 72, and the ion implantation for forming the base contact regions 5a, 5b is not limited to this, and the order may be reversed.

[0071] 7 and 8 may be reversed. That is, ion implantation for forming the base contact regions 5a and 5b shown in Fig. 8 is performed before the dry etching shown in Fig. 7 (similar to the structure shown in Fig. 13 described later). Then, the dry etching shown in Fig. 7 may be performed to obtain the structure shown in Fig. 8.

[0072] Next, activation annealing (heat treatment) is performed at a temperature of, for example, about 1600° C. or higher and 1900° C. or lower using an annealing furnace or the like to simultaneously activate the p-type impurities or n-type impurities ion-implanted into the buried regions 4a, 4c, the gate protection region 4b, the source extension region 71, the source contact region 72, the base contact regions 5a, 5b, etc. At this time, the amorphous structure of the source contact region 72 is recrystallized to become 3C-SiC, and the source contact region 72 containing 3C-SiC is formed.

[0073] Although the case where one activation anneal is performed after all the ion implantation steps is exemplified here, activation anneal may be performed multiple times individually after each ion implantation step. Also, before activation anneal, a cap film made of carbon (C) may be formed, activation anneal is performed in a state where the substrate is covered with the cap film, and the cap film may be removed after activation anneal.

[0074] Next, an oxide film 22 (see FIG. 9) is deposited on the upper surfaces of the source contact region 72 and the base contact regions 5a, 5b by CVD or the like. A photoresist film is applied to the upper surface of the oxide film 22, and the oxide film 22 is patterned by photolithography, dry etching, or the like. Using the patterned oxide film 22 as an etching mask, a dry etching technique such as RIE is used to selectively remove parts of the source contact region 72, the source extension region 71, the base region 6, and the gate protection region 4b in the depth direction from the upper surface of the source contact region 72, as shown in FIG. 9, to dig a gate trench 10.

[0075] The gate trench 10 divides the source extension region 71 into two source extension regions 71a and 71b, the source contact region 72 into two source contact regions 72a and 72b, and the base region 6 into two base regions 6a and 6b. The source extension region 71a and the source contact region 72a form the source region 7a, and the source extension region 71b and the source contact region 72b form the source region 7b. Thereafter, the oxide film 22 used as the etching mask is removed. Note that instead of the oxide film 22, a photoresist film may be used as the etching mask.

[0076] Next, a gate insulating film 11 (see FIG. 10) is formed on the lower and side surfaces of the gate trench 10 and on the upper surfaces of the source contact regions 72a, 72b and the base contact regions 5a, 5b by CVD technology, high temperature oxidation (HTO) method, thermal oxidation method, etc. When forming the gate insulating film 11, a heat treatment (PDA: Post Deposition Annealing) is performed at, for example, about 900° C. or more and 1350° C. or less.

[0077] Next, a polysilicon layer (doped polysilicon layer) doped with a high concentration of impurities such as phosphorus (P) or boron (B) is deposited by CVD technology or the like so as to fill the inside of the gate trench 10. After that, a part of the polysilicon layer and a part of the gate insulating film 11 are selectively removed by photolithography technology and dry etching. As a result, as shown in FIG. 10, an insulated gate electrode structure (11, 12) consisting of the gate insulating film 11 and the gate electrode 12 is formed. At this time, the amount of depression of the gate electrode 12 may be adjusted so that the upper surface of the gate electrode 12 at the position where it contacts the gate insulating film 11 is deeper than the lower surfaces of the source contact regions 72a, 72b and shallower than the lower surfaces of the source extension regions 71a, 71b.

[0078] Next, an interlayer insulating film 13 (see FIG. 11) is deposited on the upper surface of the insulated gate electrode structure (11, 12) by CVD technology or the like. A portion of the interlayer insulating film 13 is selectively removed by photolithography technology, dry etching technology or the like, and contact holes 13a, 13b that expose portions of the upper surfaces of the source contact regions 72a, 72b and the contact trenches 8a, 8b are opened in the interlayer insulating film 13, as shown in FIG. 11. Thereafter, a heat treatment (reflow) may be performed to planarize the interlayer insulating film 13.

[0079] Next, a silicide layer 16 (see FIG. 12) is formed by a sputtering technique or a vapor deposition method and a heat treatment, and a part of the silicide layer 16 is selectively removed by a photolithography technique and an etching technique. As a result, the silicide layer 16 is selectively formed on the upper surfaces of the base contact regions 5a, 5b exposed on the lower surfaces of the contact trenches 8a, 8b. The silicide layer 16 makes ohmic contact with the base contact regions 5a, 5b with low resistance.

[0080] 12, a barrier metal layer 14 and a source wiring layer 15 are sequentially formed by sputtering or deposition so as to fill the contact trenches 8a and 8b and cover the upper surfaces of the source contact regions 72a and 72b and the interlayer insulating film 13. As a result, a source electrode (14, 15, 16) consisting of the barrier metal layer 14, the source wiring layer 15, and the silicide layer 16 is formed. The barrier metal layer 14 makes low-resistance ohmic contact with parts of the upper surfaces and the side surfaces of the source contact regions 72a and 72b.

[0081] Although the source contact regions 72a, 72b and the base contact regions 5a, 5b are connected to the source electrodes (14, 15, 16) through the contact holes 13a, 13b, the source contact regions 72a, 72b and the base contact regions 5a, 5b may be connected to the source electrodes (14, 15, 16) through individual contact holes.

[0082] Next, as necessary, the SiC substrate 1 is thinned from the lower surface side by grinding, chemical mechanical polishing (CMP), or the like to adjust the thickness to form the drain region 1. Next, a drain electrode 17 (see FIG. 1) made of gold (Au) or the like is formed on the entire lower surface of the drain region 1 by a sputtering method, a vapor deposition method, or the like. In this manner, the silicon carbide semiconductor device shown in FIG. 1 is completed.

[0083] Here, a method for manufacturing a silicon carbide semiconductor device according to a comparative example will be described. In the method for manufacturing a silicon carbide semiconductor device according to the comparative example, the difference between the impurity concentration for satisfying the contact resistance required for source contact regions 72a, 72b and the impurity concentration for satisfying the contact resistance required for base contact regions 5a, 5b is utilized in a rational manner from the viewpoint of manufacturing, and after the procedure for forming source contact region 72, the conductivity type of a part of the n-type region is inverted (returned) to p-type to form base contact regions 5a, 5b.

[0084] Specifically, in the method for manufacturing a silicon carbide semiconductor device according to the comparative example, after the procedure of forming source contact region 72 shown in FIG. 6, oxide film 21 (see FIG. 13) is deposited on the upper surface of source contact region 72, and oxide film 21 is patterned. Next, as shown in FIG. 13, the patterned oxide film 21 is used as an ion implantation mask to selectively implant ions of p-type impurities such as aluminum (Al), thereby inverting (reversing) the conductivity type of part of source extension region 71 and source contact region 72 from n-type to p-type. As a result, p-type impurities are formed on the upper surface sides of buried regions 4a, 4c. + Mold base contact regions 5a, 5b are selectively formed.

[0085] However, in the method for manufacturing a silicon carbide semiconductor device according to the comparative example, leakage defects may occur in the bumped-back portions of source contact region 72, which are regions A1 and A2 shown by dashed lines in Fig. 13. This is presumably because the ion implantation for forming source contact region 72 and the ion implantation for forming base contact regions 5a and 5b cause a lot of damage, turning the upper parts of base contact regions 5a and 5b into 3C-SiC, which becomes the source of leakage.

[0086] In contrast, according to the method for manufacturing the silicon carbide semiconductor device according to the first embodiment, as shown in Fig. 7, the contact trenches 8a, 8b are formed by selectively removing parts of the source extension region 71 and the source contact region 72. Then, as shown in Fig. 8, by ion-implanting p-type impurities into the lower surfaces of the contact trenches 8a, 8b, it is possible to form the base contact regions 5a, 5b by driving back parts of the source extension region 71 without driving back the source contact region 72. Thus, there is no overlapping region between the ion implantation for forming the source contact region 72 and the ion implantation for forming the base contact regions 5a, 5b, and the crystal structure of the base contact regions 5a, 5b is not broken and becomes 4H-SiC, so that leakage defects can be suppressed.

[0087] 8 is performed first, and then the contact trenches 8a, 8b are formed as shown in FIG 7. In this case, the upper portions of the base contact regions 5a, 5b that have been damaged by the ion implantation of the p-type impurities can be removed during the formation of the contact trenches 8a, 8b. Therefore, the crystal structure of the remaining base contact regions 5a, 5b becomes 4H-SiC, and leakage defects can be suppressed.

[0088] Furthermore, according to the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment, the oxide film 21 can be used as a common mask for the etching mask used to form the contact trenches 8a, 8b and for the ion implantation used to form the base contact regions 5a, 5b. This eliminates the need to consider alignment accuracy, and can reliably prevent the formation of an overlapping region between the ion implantation used to form the source contact region 72 and the ion implantation used to form the base contact regions 5a, 5b. Furthermore, compared to the case in which the source contact region 72 and the base contact regions 5a, 5b are formed using separate masks so as not to form an overlapping region between the ion implantation used to form the source contact region 72 and the ion implantation used to form the base contact regions 5a, 5b, an increase in the number of steps and manufacturing costs can be suppressed.

[0089] Second embodiment <Structure of Silicon Carbide Semiconductor Device> The silicon carbide semiconductor device according to the second embodiment differs from the silicon carbide semiconductor device according to the first embodiment shown in Fig. 1 in that the side surfaces of the contact holes 13a, 13b in the interlayer insulating film 13 and the side surfaces of the contact trenches 8a, 8b are provided so as to be continuous with each other, as shown in Fig. 14. The base contact regions 5a, 5b are narrower than the widths of the contact trenches 8a, 8b. Step portions 71x, 71y are provided at the lower portions of the side surfaces of the source extension regions 71a, 71b that contact the contact trenches 8a, 8b.

[0090] FIG. 15 is a schematic cross-sectional view of an enlarged broken-line region A shown in FIG. 14. A step portion 71x is provided at the bottom of the left side surface of the source extension region 71a. The width w2 of the step portion 71x is, for example, about 10 nm or more and 300 nm or less. The side surface of the step portion 71x contacts the base contact region 5a. The upper surface of the step portion 71x contacts the lower surface of the trench contact 8a and the silicide layer 16. By providing the silicide layer 16 not only on the upper surfaces of the base contact regions 5a and 5b but also on the step portion 71x of the source extension region 71a, it is possible to suppress variations in the ohmic contact areas of the base contact regions 5a and 5b.

[0091] The left side surface of the source extension region 71a above the step portion 71x is in contact with the side surface of the trench contact 8a, the silicide layer 16, and the barrier metal layer 14. The left side surface of the source contact region 72a is in contact with the side surface of the trench contact 8a and the barrier metal layer 14. The upper surface of the source contact region 72a is not in contact with the barrier metal layer 14, and is covered with the gate insulating film 11 and the interlayer insulating film 13.

[0092] The source extension region 71b and the source contact region 72b of the source region 7b shown in FIG. 14 have the same configurations as the source extension region 71a and the source contact region 72a of the source region 7a, respectively, and therefore will not be described again.

[0093] 15, the positional relationship between the source extension region 71b and the source contact region 72b of the source region 7b and the base contact region 5b, the gate insulating film 11, and the gate electrode 12 is similar to the positional relationship between the source extension region 71a and the source contact region 72a of the source region 7a and the base contact region 5a, the gate insulating film 11, and the gate electrode 12, and therefore a duplicated description will be omitted. The other configuration of the silicon carbide semiconductor device according to the second embodiment is substantially similar to that of the silicon carbide semiconductor device according to the first embodiment, and therefore a duplicated description will be omitted.

[0094] In the silicon carbide semiconductor device according to the second embodiment, the source contact regions 72a, 72b including 3C-SiC in the source regions 7a, 7b can make ohmic contact with the source electrodes (14, 15, 16) with low resistance without the silicide layer 16. Therefore, the silicide layer 16 is not required on the contact junction surfaces of the source contact regions 72a, 72b, and peeling of the silicide layer 16 on the contact junction surfaces of the source contact regions 72a, 72b can be suppressed. Furthermore, since only the side surfaces of the source contact regions 72a, 72b make ohmic contact with the source electrodes (14, 15, 16), the lateral miniaturization of the unit cell can be facilitated.

[0095] Furthermore, in the silicon carbide semiconductor device according to the second embodiment, the bottom surfaces of the contact trenches 8a, 8b are made deeper than the bottom surfaces of the source contact regions 72a, 72b, so that the source contact regions 72a, 72b containing 3C-SiC are not in contact with the base contact regions 5a, 5b made of 4H-SiC. Therefore, compared to a case in which the source contact regions 72a, 72b and the base contact regions 5a, 5b are in contact with each other without providing the contact trenches 8a, 8b, damage due to ion implantation for forming the source extension regions 71a, 71b in the base contact regions 5a, 5b is not caused, and leakage defects can be suppressed.

[0096] Furthermore, in the silicon carbide semiconductor device of the second embodiment, the pn junction formed by the 4H-SiC source extension regions 71a, 71b and the 4H-SiC base contact regions 5a, 5b is made of 4H-SiC, and therefore leakage current at the pn junction can be prevented compared to a case in which the pn junction is formed by source contact regions 72a, 72b containing 3C-SiC, which has many remaining crystal defects, and base contact regions 5a, 5b of 4H-SiC.

[0097] Furthermore, in the silicon carbide semiconductor device according to the second embodiment, the upper surface of the gate electrode 12 is made deeper than the lower surface of the source contact region 72a and shallower than the lower surface of the source extension region 71a. As a result, the source extension region 71a, which has relatively few crystal defects and little surface irregularity, of the source region 7a faces the gate electrode 12 via the gate insulating film 11, while the source contact region 72a, which has relatively many crystal defects and much surface irregularity, does not face the gate electrode 12 via the gate insulating film 11. This makes it possible to suppress the generation of leakage current between the source region 7a and the gate electrode 12.

[0098] <Method for manufacturing silicon carbide semiconductor device> The method for manufacturing the silicon carbide semiconductor device in accordance with the second embodiment is similar to the method for manufacturing the silicon carbide semiconductor device in accordance with the first embodiment up to the step of forming source contact region 72 shown in FIG.

[0099] Next, in the method for manufacturing a silicon carbide semiconductor device according to the second embodiment, without forming contact trenches 8a, 8b, as shown in Fig. 13, an oxide film 21 is patterned on the upper surface of base region 6, and p-type impurities such as aluminum (Al) are selectively ion-implanted using the patterned oxide film 21 as an ion implantation mask, thereby inverting (reversing) the conductivity type of part of source extension region 71 and source contact region 72 from n-type to p-type. As a result, p-type impurities are formed on the upper surface sides of buried regions 4a, 4c. + The base contact regions 5a and 5b are selectively formed in the regions A1 and A2 shown by the broken lines in FIG.

[0100] Next, an annealing furnace or the like is used to perform activation annealing (heat treatment) at, for example, about 1600°C or higher and 1900°C or lower, thereby simultaneously activating the p-type impurities or n-type impurities ion-implanted into the buried regions 4a, 4c, the gate protection region 4b, the source extension region 71, the source contact region 72, the base contact regions 5a, 5b, etc. At this time, the amorphous structure of the source contact region 72 is recrystallized and becomes 3C-SiC, thereby forming the source contact region 72 containing 3C-SiC. In addition, the part of the source contact region 72 that is implanted above the base contact regions 5a, 5b also becomes 3C-SiC.

[0101] Next, an oxide film 22 (see FIG. 16) is deposited on the upper surfaces of the source contact region 72 and the base contact regions 5a, 5b by CVD or the like. A photoresist film is applied to the upper surface of the oxide film 22, and the oxide film 22 is patterned by photolithography, dry etching, or the like. Using the patterned oxide film 22 as an etching mask, a portion of the source contact region 72, the source extension region 71, the base region 6, and the gate protection region 4b is selectively removed in the depth direction from the upper surface of the source contact region 72 by dry etching such as RIE, as shown in FIG. 16, to dig a gate trench 10. Note that a photoresist film may be used as an etching mask instead of the oxide film 22. Thereafter, the oxide film 22 used as the etching mask is removed.

[0102] Next, a gate insulating film 11 (see FIG. 17) is formed on the lower and side surfaces of the gate trench 10 and on the upper surfaces of the source contact regions 72a, 72b and the base contact regions 5a, 5b by CVD, high temperature oxidation (HTO), thermal oxidation, or the like.

[0103] Next, a polysilicon layer (doped polysilicon layer) doped with a high concentration of impurities such as phosphorus (P) or boron (B) is deposited by CVD technology or the like so as to fill the inside of the gate trench 10 via the gate insulating film 11. After that, a part of the polysilicon layer and a part of the gate insulating film 11 are selectively removed by photolithography technology and dry etching. As a result, an insulated gate electrode structure (11, 12) consisting of the gate insulating film 11 and the gate electrode 12 is formed as shown in FIG.

[0104] Next, an interlayer insulating film 13 (see FIG. 18) is deposited on the upper surfaces of the insulated gate electrode structures (11, 12), the source contact regions 72a, 72b, and the base contact regions 5a, 5b by CVD or the like. Part of the interlayer insulating film 13 is selectively removed by photolithography, dry etching, or the like. As a result, as shown in FIG. 18, contact holes 13a, 13b are opened in the interlayer insulating film 13, exposing parts of the upper surfaces of the source contact regions 72a, 72b and the upper surfaces of the base contact regions 5a, 5b.

[0105] Next, using the interlayer insulating film 13 as an etching mask, the source contact region 72, the source extension region 71, and parts of the base contact regions 5a, 5b located above the buried regions 4a, 4c are selectively removed by dry etching such as RIE, as shown in Fig. 19. As a result, contact trenches 8a, 8b having a width wider than that of the base contact regions 5a, 5b are formed in a self-aligned manner. Also, the 3C-SiC parts on the upper parts of the base contact regions 5a, 5b are removed, and the 4H-SiC parts of the base contact regions 5a, 5b remain.

[0106] The bottom surfaces of the contact trenches 8a, 8b are formed deeper than the bottom surfaces of the source contact regions 72a, 72b. Step portions 71x, 71y are formed in the source extension regions 71a, 71b. The step portions 71x, 71y of the base contact regions 5a, 5b and the source extension regions 71a, 71b are exposed at the bottom surfaces of the contact trenches 8a, 8b. The source extension regions 71a, 71b and the source contact regions 72a, 72b are exposed at the side surfaces of the contact trenches 8a, 8b. After that, a heat treatment (reflow) may be performed to planarize the interlayer insulating film 13.

[0107] Other steps of the method for manufacturing a silicon carbide semiconductor device in accordance with the second embodiment are substantially similar to those of the method for manufacturing a silicon carbide semiconductor device in accordance with the first embodiment, and therefore overlapping descriptions will be omitted.

[0108] According to the method for manufacturing a silicon carbide semiconductor device in accordance with the second embodiment, the source extension region 71 and the source contact region 72 are punched back to form the base contact regions 5a, 5b as shown in Fig. 13, and then the 3C-SiC portions of the source contact regions 72 of the base contact regions 5a, 5b are selectively removed to form the contact trenches 8a, 8b as shown in Fig. 19. Thus, only the 4H-SiC portions remain in the base contact regions 5a, 5b, thereby suppressing leakage defects.

[0109] Furthermore, according to the method for manufacturing the silicon carbide semiconductor device of the second embodiment, the contact trenches 8a, 8b can be formed in a self-aligned manner using the interlayer insulating film 13 as an etching mask. Therefore, it is not necessary to consider the alignment accuracy, and the 3C-SiC portion of the source contact region 72 of the base contact regions 5a, 5b that is struck against the source contact region 72 can be reliably removed. Furthermore, compared to the case where the source contact region 72 and the base contact regions 5a, 5b are formed using separate masks so as not to form an overlapping region between the ion implantation for forming the source contact region 72 and the ion implantation for forming the base contact regions 5a, 5b, an increase in the number of steps and manufacturing costs can be suppressed.

[0110] Third embodiment 20 is a cross section of a silicon carbide semiconductor device according to a third embodiment, and shows a cross section at a position corresponding to the cross section of the silicon carbide semiconductor device according to the first embodiment shown in FIG. 2. As shown in FIG. 20, the silicon carbide semiconductor device according to the third embodiment differs from the silicon carbide semiconductor device according to the first embodiment shown in FIG. 2 in that the lower surface of the contact trench 8a is deeper than the lower surface of the source extension region 71a. The depth d3 of the contact trench 8a from the upper surface of the source contact region 72a is deeper than the depth d1 of the source extension region 71a from the upper surface of the source contact region 72a. A part of the left side surface of the base region 6a contacts the side surface of the contact trench 8a, the silicide layer 16, and the barrier metal layer 14.

[0111] Although not shown in the figure, the bottom surface of the other contact trench 8b (see FIG. 1) is also deeper than the bottom surface of the source extension region 71b (see FIG. 1). Since other configurations of the silicon carbide semiconductor device in accordance with the third embodiment are substantially similar to those of the silicon carbide semiconductor device in accordance with the first embodiment, duplicated descriptions will be omitted.

[0112] According to the silicon carbide semiconductor device of the third embodiment, even if the lower surfaces of the contact trenches 8a, 8b are deeper than the lower surfaces of the source extension regions 71a, 71b, as in the silicon carbide semiconductor device of the first embodiment, the source contact regions 72a, 72b containing 3C-SiC can be in ohmic contact with the source electrode (14, 15, 16) without the silicide layer 16 therebetween, and the base contact regions 5a, 5b of 4H-SiC are not in contact with the source contact regions 72a, 72b containing 3C-SiC, thereby suppressing leakage defects.

[0113] (Fourth embodiment) Fig. 21 is a cross section of a silicon carbide semiconductor device according to a fourth embodiment, and shows a cross section at a position corresponding to the cross section of the silicon carbide semiconductor device according to the second embodiment shown in Fig. 15. As shown in Fig. 21, the silicon carbide semiconductor device according to the fourth embodiment differs from the silicon carbide semiconductor device according to the second embodiment shown in Fig. 15 in that, in the lower part of the contact trench 8a, the silicide layer 16 is selectively provided only on the upper surface of the base contact region 5a, and is not provided on the upper surface of the step portion 71x of the source extension region 71a.

[0114] Although not shown, in the lower part of the other contact trench 8b (see FIG. 14), a silicide layer 16 is selectively provided only on the upper surface of the base contact region 5b, and is not provided on the upper surface of the step portion 71y of the source extension region 71b. Since other configurations of the silicon carbide semiconductor device according to the fourth embodiment are substantially similar to those of the silicon carbide semiconductor device according to the second embodiment, duplicated descriptions will be omitted.

[0115] According to the silicon carbide semiconductor device of the fourth embodiment, as in the silicon carbide semiconductor device of the second embodiment, the source contact regions 72a, 72b containing 3C-SiC can be in ohmic contact with the source electrode (14, 15, 16) without the silicide layer 16 therebetween, and the base contact regions 5a, 5b of 4H-SiC are not in contact with the source contact regions 72a, 72b containing 3C-SiC, thereby suppressing leakage defects.

[0116] Furthermore, in the silicon carbide semiconductor device of the fourth embodiment, the silicide layer 16 is selectively provided only on the upper surfaces of the base contact regions 5a, 5b, and is not provided on the upper surfaces of the step portions 71x, 71y of the source extension region 71a, thereby making it possible to suppress peeling of the silicide layer 16 on the upper surfaces of the step portions 71x, 71y.

[0117] Fifth embodiment As shown in FIG. 22, the silicon carbide semiconductor device according to the fifth embodiment has an n-type 4H—SiC +1 in that source extension regions 71a, 71b of the silicon carbide semiconductor device in accordance with the first embodiment are formed thinly. Other configurations of the silicon carbide semiconductor device in accordance with the fifth embodiment are substantially similar to those of the silicon carbide semiconductor device in accordance with the first embodiment, and therefore repeated description will be omitted.

[0118] In the method for manufacturing a silicon carbide semiconductor device in accordance with the fifth embodiment, ion implantation for source extension region 71 is not performed on the upper surface side of base region 6 in the procedure shown in Fig. 5. Instead, in the procedure shown in Fig. 6, n-type impurities such as nitrogen (N) are selectively ion-implanted to form n-type impurities on the upper surface side of base region 6. + In the fifth embodiment, a source contact region 72 of the silicon carbide semiconductor device is selectively formed. In ion implantation, a concentration gradient always occurs on the deeper side, so a low concentration portion naturally occurs in contact with the deep side of the source contact region 72. Since the low concentration portion becomes a 4H—SiC structure after heat treatment, this 4H—SiC portion is used as the source extension region 71. The other steps of the method for manufacturing the silicon carbide semiconductor device according to the fifth embodiment are substantially similar to those of the method for manufacturing the silicon carbide semiconductor device according to the first embodiment, and therefore repeated explanations will be omitted.

[0119] In the silicon carbide semiconductor device according to the fifth embodiment, n + Even when the type source extension regions 71a, 71b are formed thin, as in the silicon carbide semiconductor device of the first embodiment, the source contact regions 72a, 72b containing 3C-SiC can be in ohmic contact with the source electrode (14, 15, 16) without the silicide layer 16 therebetween, and the base contact regions 5a, 5b of 4H-SiC are not in contact with the source contact regions 72a, 72b containing 3C-SiC, thereby suppressing leakage defects.

[0120] (Other embodiments) As described above, the first to fifth embodiments of the present disclosure have been described, but the descriptions and drawings forming a part of this disclosure should not be understood as limiting the present disclosure. Various alternative embodiments, examples, and operating techniques will be apparent to those skilled in the art from this disclosure.

[0121] For example, although a MOSFET is exemplified as the silicon carbide semiconductor device according to the first to fifth embodiments, n + Instead of the drain region of type 1, p + The present invention can also be applied to insulated gate bipolar transistors (IGBTs) that have a collector region of a type other than IGBTs. In addition to IGBTs alone, the present invention can also be applied to reverse conducting IGBTs (RC-IGBTs) and reverse blocking insulated gate bipolar transistors (RB-IGBTs).

[0122] Furthermore, the configurations disclosed in the first to fifth embodiments may be appropriately combined within a range that does not cause a contradiction. For example, in the silicon carbide semiconductor device according to the second embodiment, the lower surfaces of the contact trenches 8a, 8b may be formed deeper than the lower surfaces of the source extension regions 71a, 71b, as in the silicon carbide semiconductor device according to the third embodiment.

[0123] In addition, in the silicon carbide semiconductor device according to the second embodiment, as in the silicon carbide semiconductor device according to the fifth embodiment, n + The source regions 7a and 7b are of the n type. + n + Alternatively, the source contact regions 72a and 72b may be formed only from the source contact regions 72a and 72b.

[0124] Thus, the present disclosure naturally includes various embodiments not described herein. Therefore, the technical scope of the present disclosure is defined only by the invention-specifying matters related to the scope of the claims appropriate from the above description. [Explanation of symbols]

[0125] 1...Drain region (SiC substrate) 2. Drift layer 4a, 4c...Buried area 4b…Gate protection area 5a, 5b...Base contact region 6, 6a, 6b...Base region 7a, 7b…Source region 8a, 8b...Contact trench 10…Gate trench 11...Gate insulating film 12...Gate electrode 13...Interlayer insulating film 13a, 13b...Contact holes 14...Barrier metal layer 15…Source wiring layer 16...Silicide layer 17…Drain electrode 20, 21, 22...Oxide film 71, 71a, 71b...Source extension area 71x, 71y...Step section 72, 72a, 72b...Source contact region

Claims

1. a drift layer of a first conductivity type made of silicon carbide; a second conductivity type base region made of silicon carbide and provided on an upper surface side of the drift layer; a first conductivity type source contact region made of silicon carbide having a 3C structure, the source contact region being provided on an upper surface side of the base region; a gate insulating film provided inside a gate trench penetrating the source contact region and the base region; a gate electrode provided inside the gate trench with the gate insulating film interposed therebetween; a main electrode provided inside a contact trench spaced apart from the gate trench and in contact with at least a side surface of the source contact region; a second conductivity type base contact region in contact with a lower surface of the contact trench, made of silicon carbide having a 4H structure and having a higher impurity concentration than the base region; Equipped with The bottom surface of the contact trench is deeper than the bottom surface of the source contact region. Silicon carbide semiconductor device.

2. The main electrode contacts the top and side surfaces of the source contact region. The silicon carbide semiconductor device according to claim 1 .

3. The main electrode is in contact with a side surface of the source contact region and is not in contact with a top surface of the source contact region. The silicon carbide semiconductor device according to claim 1 .

4. a source extension region of a first conductivity type provided in contact with a lower surface of the source contact region and made of silicon carbide having a 4H structure; The silicon carbide semiconductor device according to claim 1 .

5. a bottom surface of the contact trench is shallower than a bottom surface of the source extension region; The side surface of the contact trench contacts the source extension region. The silicon carbide semiconductor device according to claim 4 .

6. The impurity concentration of the source extension region is lower than the impurity concentration of the source contact region. The silicon carbide semiconductor device according to claim 4 .

7. The impurity concentration of the source extension region is the same as the impurity concentration of the source contact region. The silicon carbide semiconductor device according to claim 4 .

8. The upper surface of the gate electrode is located deeper than the lower surface of the source contact region. The silicon carbide semiconductor device according to claim 1 .

9. The bottom surface of the base contact region is flush with the bottom surface of the base region or is located shallower than the bottom surface of the base region. The silicon carbide semiconductor device according to claim 1 .

10. The main electrode includes a silicide layer in contact with an upper surface of the base contact region. The silicon carbide semiconductor device according to claim 1 .

11. The ratio of the 3C structure contained in the source contact region is 10% or more and 100% or less. The silicon carbide semiconductor device according to claim 1 .

12. The source contact region contains phosphorus or arsenic as an impurity. The silicon carbide semiconductor device according to claim 1 .

13. The impurity concentration of the source contact region is 1×10 20 / cm 3 That's it, 1 x 10 22 / cm 3 is less than or equal to The silicon carbide semiconductor device according to claim 1 .

14. The impurity concentration of the source extension region is 1×10 16 / cm 3 That's it, 1 x 10 20 / cm 3 is less than or equal to The silicon carbide semiconductor device according to claim 4 .

15. The source extension region contains nitrogen or phosphorus as an impurity. The silicon carbide semiconductor device according to claim 4 .

16. The impurity concentration of the base contact region is 1×10 19 / cm 3 That's it, 1 x 10 21 / cm 3 is less than or equal to The silicon carbide semiconductor device according to claim 1 .

17. The base contact region contains aluminum as an impurity. The silicon carbide semiconductor device according to claim 1 .

18. forming a base region of a second conductivity type made of silicon carbide on an upper surface side of a drift layer of a first conductivity type made of silicon carbide; forming a first conductivity type source contact region made of silicon carbide including a 3C structure on an upper surface side of the base region; forming a gate trench through the source contact region and the base region; forming a gate electrode on the inner side of the gate trench via a gate insulating film; forming a contact trench spaced from the gate trench and extending through the source contact region; forming a master electrode inside the contact trench and in contact with at least a side surface of the source contact region; forming a second conductivity type base contact region in contact with a lower surface of the contact trench, made of silicon carbide having a 4H structure and having a higher impurity concentration than the base region; Including, The bottom surface of the contact trench is formed deeper than the bottom surface of the source contact region. A method for manufacturing a silicon carbide semiconductor device.

19. The step of forming the contact trench includes selectively removing a portion of the source contact region using a mask that is also used in the ion implantation for forming the base contact region. The method for manufacturing a silicon carbide semiconductor device according to claim 18.

20. forming an interlayer insulating film on an upper surface of the gate electrode; forming a contact hole in the interlayer insulating film; Further comprising: The step of forming the contact trench includes selectively removing a portion of the source contact region by using the interlayer insulating film in which the contact hole is formed as a mask. The method for manufacturing a silicon carbide semiconductor device according to claim 18.

Citation Information

Patent Citations

  • Semiconductor device and manufacturing method thereof

    JP2009049198A

  • Semiconductor device and method for manufacturing the semiconductor device

    JP2010238738A

  • Semiconductor device and semiconductor device manufacturing method

    JP2013058601A

  • Semiconductor device

    JP2019117859A

  • Trench gate type semiconductor device

    JP2021012995A