Hard metal alloy for cutting tool and cutting tool using the alloy

A cemented carbide with optimized Co, Ni, Ti, Zr, Nb, Ta, and W composition and controlled particle sizes and interfacial lengths addresses the durability issues of cutting tools, providing enhanced resistance to plastic deformation and chipping when cutting alloy steel.

JP2024142103AActive Publication Date: 2024-10-10MITSUBISHI MATERIALS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023054102
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing cutting tools face challenges in achieving both high plastic deformation resistance and chipping resistance, particularly when cutting alloy steel, which affects their durability and performance.

Method used

A cemented carbide composition with specific ranges for Co, Ni, Ti, Zr, Nb, Ta, and W contents, along with controlled average particle sizes and interfacial lengths, forms a hard phase and binder phase with improved resistance to plastic deformation and chipping.

Benefits of technology

The cemented carbide exhibits excellent plastic deformation resistance and chipping resistance, enhancing the durability of cutting tools, especially when cutting alloy steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142103000001_ABST
    Figure 2024142103000001_ABST
Patent Text Reader

Abstract

To provide a hard metal alloy having anti-plastic deformation property and defect resistance in alloy steel cutting.SOLUTION: A hard metal alloy for a cutting tool contains hard phases having an average particle diameter of 0.5 to 4.0 μm and γ phases having an average particle diameter of 2.0 to 3.0 μm, wherein when atomic number ratios Ti, Zr, Nb, Ta and W contained in each of the γ phases are represented by a, b, c, d and e, average values aavg, bavg, cavg, davg, and eavg are 20.0≤aavg≤30.0, 20.0≤bavg≤30.0, 10.0≤cavg≤20.0, 20.0≤davg≤30.0, and 5.0≤e≤15.0, an average value of standard deviation of each of a, b, c, d and e is 10.0 to 15.0, a ratio of an interface length of an interface between the hard phase and a binding phase in the total interface length of the hard phase, and a ratio of an interface length of an interface between the γ phase and the binding phase in the total interface length of the γ phase are 0.45 to 0.55, and a ratio of an interface length of an interface between the γ phase and the γ phase in the total interface length of the γ phase is 0.25 to 0.30.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cemented carbide (WC-based sintered alloy) and a cutting tool using said alloy. [Background technology]

[0002] Cemented carbide has excellent mechanical strength, thermal fatigue resistance, and the like, and is therefore used in tools that are subjected to large impact forces and thermal cycles, such as cutting tools, drilling tools, and metal forming tools.

[0003] On the other hand, the conditions under which tools are used are becoming more and more efficient, and tools are required to have even greater durability. For this reason, proposals have been made to improve the aforementioned characteristics of the cemented carbide used in tools.

[0004] For example, Patent Document 1 describes a cemented carbide which contains at least 0.4 to 0.8 mass% chromium in the binder phase in terms of chromium carbide, and when pulverized, the pulverized powder passed through a #20 mesh is dissolved in dilute hydrochloric acid (HCl:H2O = 1:1) at 50°C for 24 hours and filtered, and the filtrate contains 2 to 6 mass% chromium relative to the total metal amount in the filtrate, and the chromium concentration in the binder phase gradually increases toward the interface with the tungsten carbide particles. It is said that when this cemented carbide is applied to a drill, it enables machining with high hole position accuracy in repeated machining even with an extremely small drill diameter and high-speed cutting. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4351453 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above circumstances and proposals, and aims to provide a cemented carbide which becomes a cutting tool having a cutting edge with excellent resistance to plastic deformation and chipping resistance, even when used in cutting alloy steel. [Means for solving the problem]

[0007] The cemented carbide for cutting tools according to an embodiment of the present invention is Co, Ni: 7.0 to 9.0 mass% in total, Ti, Zr, Nb, and Ta, total 4.0 to 12.0 mass%; Contains 5.7 to 6.4 mass% C, The balance is W and inevitable impurities. The hard phase is mainly composed of W carbides, the binder phase is mainly composed of Co and Ni, and the gamma phase is mainly composed of Ti, Zr, Nb, Ta and W carbides. The hard phase has an average grain size of 0.5 to 4.0 μm, and the gamma phase has an average grain size of 2.0 to 3.0 μm; When the atomic ratios of Ti, Zr, Nb, Ta and W contained in the γ phase are a, b, c, d and e (a+b+c+d+e=100.0), the average value a avg , b avg , c avg , d avg , e avg (However, avg +b avg +c avg +d avg +e avg =100.0) is 20.0≦a avg ≦30.0, 20.0≦b avg ≦30.0, 10.0≦c avg ≦20.0, 20.0≦d avg ≦30.0, 5.0≦e avg ≦15.0, The average values ​​of σa, σb, σc, σd, and σe, which are standard deviations of a, b, c, d, and e, respectively, are 10.0 to 15.0; a ratio of an interface length between the hard phase and the binder phase to a total interface length of the hard phase, and a ratio of an interface length between the gamma phase and the binder phase to a total interface length of the gamma phase are both 0.45 to 0.55; The ratio of the interface length between the γ phases to the total interface length of the γ phases is 0.25 to 0.30.

[0008] The cemented carbide according to the above embodiment may satisfy the following (1).

[0009] (1) The Cr content is 0.5 mass% or less.

[0010] A cutting tool according to an embodiment of the present invention uses the above-mentioned cemented carbide for cutting tools. Effect of the Invention

[0011] When the above-mentioned cemented carbide for cutting tools is used as a cutting tool, even when the cutting tool is used for cutting alloy steel, the cutting edge has excellent resistance to plastic deformation and chipping. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic diagram showing an example of the structure of the cemented carbide for tools according to the embodiment of the present invention. [Diagram 2] 1 is a schematic diagram showing an example of the amount of plastic deformation on the flank of a cutting edge, in which the upper figure (the rake face) is a plan view and the lower figure (the flank) is a side view. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present inventors have conducted extensive research in order to obtain a cemented carbide for cutting tools that can achieve the above-mentioned object. As a result, they have found that the average grain size of the hard phase and the γ phase are within a predetermined range, and the composition of the γ phase is a predetermined one, i.e., the average atomic ratio of the metal components contained in the γ phase is within a substantially equal predetermined range, Furthermore, the average value of the standard deviation of each metal component between the γ phases is set within a predetermined range, In addition, by setting the ratio of the interface length of the interface between the hard phase and the binder phase to the total interface length of the hard phase, the ratio of the interface length of the interface between the γ phase and the binder phase to the total interface length of the γ phase, and the ratio of the interface length of the interface between the γ phase and the γ phase to the total interface length of the γ phase within a predetermined range, It has been found that the above object can be achieved.

[0014] Hereinafter, a cemented carbide for cutting tools and a cutting tool using the alloy according to an embodiment of the present invention will be described.

[0015] In this specification and claims, when a numerical range is expressed as "M to N" (M and N are both numerical values), this is equivalent to "greater than or equal to M, less than or equal to N," and the range includes the numerical values ​​of the upper limit (N) and the lower limit (M). When a unit is stated only for the upper limit value (N), the unit of the lower limit value (M) is the same as that of the upper limit value (N).

[0016] 1. Composition and structure of cemented carbide for cutting tools The composition of the cemented carbide for cutting tools according to this embodiment and the details of the structure shown typically in FIG. 1 are as follows.

[0017] (1) Co and Ni It is preferable that one or both of Co and Ni are contained, and the total content of at least one of Co and Ni is preferably 7.0 to 9.0 mass %. The reason is that when used as a cutting tool, if the content is less than 7.0% by mass, the chipping resistance is insufficient, whereas if the content exceeds 9.0% by mass, the plastic deformation resistance decreases.

[0018] Here, Co and Ni are mainly present in the binder phase (which has crystal grains with an fcc structure, and is indicated by reference numeral 1 in FIG. 1) and are the main components of the binder phase, i.e., the main components of the binder phase, with the total of Co and Ni accounting for 50 atomic % or more of all components constituting the binder phase.

[0019] The binder phase may contain W and C, which are components of the hard phase, one or more of Ti, Zr, Nb, Ta, and W, which are contained in the γ phase, Cr, which controls the growth of the hard phase, and unavoidable impurities. When these elements are present in the binder phase, they are presumed to be in a solid solution state in the binder phase. The method for identifying the bonded phase will be described later.

[0020] (2) Ti, Zr, Nb, Ta The total content of Ti, Zr, Nb and Ta is preferably 4.0 to 12.0 mass %. The reason is that when used as a cutting tool, if the content is less than 4.0% by mass, the plastic deformation resistance is insufficient, whereas if the content exceeds 12.0% by mass, the chipping resistance decreases.

[0021] Ti, Zr, Nb, Ta, and W, which will be described later, are contained in the γ phase. Here, when the atomic ratios of Ti, Zr, Nb, Ta, and W contained in the γ phase are a, b, c, d, and e (a+b+c+d+e=100.0), their average value a avg , b avg , c avg , d avg , e avg (However, avg +b avg +c avg +d avg +e avg =100.0) is 20.0≦a avg ≦30.0, 20.0≦b avg ≦30.0, 10.0≦c avg ≦20.0, 20.0≦d avg ≦30.0, 5.0≦e avg It is preferred that it is ≦15.0.

[0022] If the standard deviations of a, b, c, d, and e are σa, σb, σc, σd, and σe, respectively, their average values ​​are preferably 10.0 to 15.0, because if they are less than 10.0, the plastic deformation resistance is insufficient, whereas if they exceed 15.0, the chipping resistance is reduced.

[0023] In other words, it is preferable that the atomic ratio of the metal components contained in the γ phase is approximately equal within a predetermined range, because this provides excellent resistance to plastic deformation and chipping when used as a cutting tool.

[0024] (3) γ phase Ti, Zr, Nb, and Ta are contained as carbides (not limited to stoichiometric composition) in the gamma phase, that is, as the main components. The term "main components" means that the carbides of these components account for 50 atomic % or more of all the components constituting the gamma phase. In addition to these carbides, the gamma phase may contain WC contained in the hard phase, Co and Ni contained in the binder phase, and unavoidable impurities. In FIG. 1, the gamma phase is indicated by the symbol 3, and some of the gamma phases have gamma phases with different compositions and crystal orientations. In FIG. 1, the symbol 4 indicates the interface between the gamma phases, which will be described later.

[0025] The average grain size of the γ phase is preferably 2.0 to 3.0 μm. The reason is that when used as a cutting tool, if it is less than 2.0 μm, the chipping resistance is insufficient, and if it exceeds 3.0 μm, the plastic deformation resistance is insufficient. Here, the average grain size of the γ phase refers to the circle equivalent diameter, that is, the diameter of a circle having an area equal to that of the γ phase, and the measurement method thereof will be described later.

[0026] (4) C C is contained to form carbides and is mainly contained in the hard phase and γ phase. The C content is preferably 5.7 to 6.4 mass%, and within this content range, a sufficient amount of carbides can be formed in the hard phase and γ phase.

[0027] (5)Cr Cr is an optional component and may be contained in an amount of less than 0.5 mass %, that is, the inclusion of Cr is not essential. Cr dissolves in the binder phase, inhibits the growth of W carbide contained in the hard phase, refines the W carbide, gives the cemented carbide a fine and uniform grain structure, increases toughness, and improves plastic deformation resistance. This function is impaired when the Cr content exceeds 0.5 mass%, causing composite carbides of Cr and W to precipitate in the binder phase, reducing toughness and potentially becoming the starting point for chipping.

[0028] (6) W W is the main component of the hard phase, that is, the main component, and W carbides (mostly WC, but not limited to the stoichiometric composition) account for 50 atomic % or more of all the components that make up the hard phase (indicated by reference symbol 2 in FIG. 1). The hard phase may contain components of the binder phase, components of the γ phase, Cr, and unavoidable impurities that are inevitably mixed in during the manufacturing process. In addition, the crystal structure of the hard phase is an hcp structure, which is different from the crystal structure of the γ phase, which is an fcc structure. The method for identifying the hard phase will be described later.

[0029] (7) Hard phase The average grain size of the hard phase is preferably 0.5 to 4.0 μm, because when used as a cutting tool, if the average grain size is less than 0.5 μm, the chipping resistance is insufficient, whereas if it exceeds 4.0 μm, the plastic deformation resistance is reduced. Here, the average grain size of the hard phase refers to the equivalent circle diameter, that is, the diameter of a circle having the same area as the hard phase, as in the case of the γ phase, and the method of measurement will be described later.

[0030] (8) Inevitable impurities As described above, the hard phase, γ phase, and binder phase may contain impurities that are inevitably (unintentionally) mixed in during the manufacturing process, and the amount of such impurities is preferably 0.3% by mass or less, with the total amount of the cemented carbide being 100% by mass.

[0031] (9) Ratio of interface length of each phase The total interface length of a phase refers to the length of the interface between the phase and another phase. The ratio of the interface length of the "interface between the hard phase and the binder phase" (hard phase / binder phase) to the total interface length of the hard phase, and The ratio of the interface length between the γ phase and the binder phase (γ phase / binder phase) to the total interface length of the γ phase are both between 0.45 and 0.55, The ratio of the interface length between the γ phase and the γ phase (γ phase / γ phase) to the total interface length of the γ phase is 0.25 to 0.30. It is preferable that: If these ratios are satisfied, the fracture resistance and plastic deformation resistance are further improved when used as a cutting tool.

[0032] 2.Measurement method The composition of the entire cemented carbide for cutting tools, the average atomic ratio of Ti, Zr, Nb, Ta and W contained in the γ phase, the average grain size of the hard phase and the γ phase, and the interface length are measured as follows.

[0033] (1) Overall composition of cemented carbide for cutting tools The surface or cross section of the cemented carbide for cutting tools is mirror-finished using, for example, a focused ion beam device (FIB device), a cross-section polisher device (CP device), or the like. Then, this mirror-finished surface is observed in multiple fields (e.g., 4000x magnification, 5 fields) using a field emission scanning electron microscope (SEM) (each field is, for example, a square measuring 25 μm (vertical) × 25 μm (horizontal)). Area analysis is then performed using an electron probe microanalyzer (EPMA) to measure the composition for each field. Here, the beam diameter of the EPMA can be, for example, 1 μm. The alloy compositions obtained in each field are then averaged to determine the composition of the entire alloy.

[0034] (2) Average atomic ratio of Ti, Zr, Nb, Ta, and W in the gamma phase First, the hard phase, γ phase and binder phase are identified by the following measurements. 1) For the mirror-finished surface on which the composition of the entire cemented carbide for cutting tools is to be measured, a rectangular observation field of view of, for example, 24 μm (vertical) × 72 μm (horizontal) is set as one field of view on the mirror-finished surface, and the EBSD pattern and EDS data are simultaneously captured using a field emission scanning electron microscope (SEM) equipped with an energy dispersive X-ray spectrometer (EDS) and an electron backscattered diffraction device (EBSD measurement device (e.g., OIM Data Collection manufactured by EDAX / TSL (now AMETEK))) at an acceleration voltage of 15 kV and a measurement point interval of 50 nm.

[0035] Examples of software used for analyzing EBSD patterns include TSL OIM Data Collection version 6 and TSL OIM Analysis version 7.

[0036] 2) Phases that are determined to have an hcp crystal structure from the EBSD pattern analysis are defined as hard phases. The average of the EDS count values ​​of Co and Ni detected from all measurement points identified as fcc phases is calculated, and measurement points identified as fcc phases with EDS count values ​​of Co and Ni higher than the average value are defined as binder phases, and the remaining measurement points that are not defined as binder phases are defined as γ phases.

[0037] 3) Here, when the measurement results of adjacent EBSD measurement points are the same phase, the area between those measurement points (middle) is considered to be the interface of the phase only when the difference in orientation obtained from both measurement points is 5 degrees or more. Note that interfaces may exist not only on the outer periphery of a phase but also on the inner periphery, and the interface length is the sum of the lengths of both the outer and inner interfaces.

[0038] 4) For the gamma phases thus determined, EPMA analysis (beam diameter can be 1 μm, for example) is performed on four different gamma phases per observation field to determine the atomic ratio of Ti, Zr, Nb, Ta, and W contained in each gamma phase, and the measured values ​​of at least 20 values ​​obtained in five observation fields are averaged, and a avg , b avg , c avg , d avg and e avgWhen the number of γ phases in one observation field is less than 4, increase the number of observation fields so that the total number of γ phases measured is at least 20, and a avg , b avg , c avg , d avg and e avg Request.

[0039] (3) Average grain size of the hard phase and γ phase While measuring and analyzing the EBSD patterns mentioned above, the average grain size is measured for the phases identified as hard phases and γ phases. The average grain size of each phase is determined by calculating the area of ​​at least 300 particles for each phase, calculating the diameter of the circle equal to that area, and averaging them. Examples of software used to measure the average grain size and the interface length described later include TSL OIM Data Collection version 6 and TSL OIM Analysis version 7.

[0040] (4)Interface length While measuring and analyzing the EBSD patterns described above, in the same field of view as that for determining the average grain size, the total interface length of the hard phase and the γ phase, as well as the interface lengths of hard phase / hard phase, hard phase / binder phase, hard phase / γ phase, binder phase / binder phase, binder phase / γ phase, and γ phase / γ phase are determined. In measuring these interface lengths, the number of observation fields is set so that the total number of hard phases, γ phases, and binder phases in the total field of view is 300 or more. Then, based on the measured values ​​obtained in multiple measurement fields, the ratio of the interface length between the hard phase and the binder phase to the total interface length of the hard phase, the ratio of the interface length between the gamma phase and the binder phase to the total interface length of the gamma phase, and the ratio of the interface length between the gamma phase and the gamma phase to the total interface length of the gamma phase are calculated. EXAMPLES

[0041] The use of the cemented carbide for tools of the present invention as a cutting tool (insert for turning) will be specifically described with reference to examples, but the present invention is not limited to these examples.

[0042] First, WC powder, Co powder, Ni powder, Cr3C2 powder, TiC powder, ZrC powder, NbC powder and TaC powder having particle sizes in the range of 1.5 to 6.0 μm were prepared as powders for sintering.

[0043] Next, these powders were mixed to obtain the composition shown in Table 1 to prepare powder for sintering. The powder was wet mixed in a ball mill for 72 hours, dried, and then pressed at a pressure of 100 MPa to prepare a powder compact.

[0044] Next, these powder compacts were subjected to a liquid phase sintering (main sintering) process in which they were held at a predetermined temperature for a predetermined time. In this embodiment, the main sintering was performed under the conditions shown in Table 2, that is, in a vacuum atmosphere of 0.1 Pa or less, by heating to a holding temperature range of 1440°C and holding at that holding temperature for 2 hours, or by heating to a holding temperature range of 1470°C and holding at that holding temperature for 1 hour. Thereafter, the inside of the furnace was maintained in a vacuum atmosphere of 0.1 Pa or less, and the material was cooled to 1200°C at 1 to 5°C / min, and held at 1200°C for 10 to 20 hours under the vacuum atmosphere of 0.1 Pa or less (cooling rate and holding time are shown in Table 2). Then, cemented carbide 1 to 10 shown in Table 3 (hereinafter referred to as Examples 1 to 10) were produced.

[0045] For comparison, comparative cemented carbide alloys 1' to 9' (hereinafter referred to as Comparative Examples 1' to 9') were produced. The manufacturing process is one in which the alloy composition is outside the above-mentioned range in the manufacturing processes of Examples 1 to 10, the cooling rate after main sintering exceeds 5°C / min, and / or the holding time at 1200°C is less than 10 hours.

[0046] That is, the sintering powders having the composition shown in Table 1 were wet mixed in a ball mill for 72 hours, dried, and then pressed under a pressure of 100 MPa to produce a powder compact. The compact was then sintered under the conditions shown in Table 2, i.e., in a vacuum atmosphere of 0.1 Pa or less, by heating to a holding temperature range of 1440°C and holding at that temperature for 2 hours, or by heating to a holding temperature range of 1470°C and holding at that temperature for 1 hour. Thereafter, the inside of the furnace was kept in a vacuum atmosphere of 0.1 Pa or less, and the compact was cooled to 1200°C at 1 to 10°C / min, and held at 1200°C for 0 to 20 hours to produce Comparative Examples 1' to 9' shown in Table 4.

[0047] The cross sections of the cemented carbide alloys of Examples 1 to 10 and Comparative Examples 1' to 9' were measured as described above, and the measured values ​​shown in Tables 3 and 4, respectively, were obtained. In Tables 3 and 4, the hard phase / binder phase ratio, γ phase / binder phase, and γ phase / γ phase refer to the ratio of the interface length between the hard phase and binder phase to the total interface length of the hard phase, the ratio of the interface length between the γ phase and binder phase to the total interface length of the γ phase, and the ratio of the interface length between the γ phase and γ phase to the total interface length of the γ phase, respectively.

[0048] [Table 1]

[0049] In Table 1, "-" indicates that no compound was added.

[0050] [Table 2]

[0051] [Table 3]

[0052] It was confirmed that the contents of inevitable impurities in both the Examples and Comparative Examples were within the above-mentioned preferable range.

[0053] [Table 4]

[0054] Next, no coating layer was formed on the surfaces of Examples 1 to 5 and Comparative Examples 1' to 5', but a coating layer having an average layer thickness shown in Table 5 was formed by CVD on the surfaces of Examples 6 to 10 and Comparative Examples 6' to 9'.

[0055] Although the coating layer is formed by vapor deposition in a three-layer laminate structure here, the number of layers is not limited to three, and the coating layer may have a one, two, or four or more layer laminate structure. Further, there is no particular limitation on the vapor deposition conditions for the hard coating layer, but the chemical vapor deposition conditions for TiN, TiCN, and Al2O3 in the above-mentioned Examples 6 to 10 and Comparative Examples 6' to 9' were as follows.

[0056] [TiN chemical vapor deposition conditions] Reactive gas (volume %): TiCl42%, N230%, H2 balance Reaction pressure: 7kPa Reaction temperature: 1000℃

[0057] [TiCN chemical vapor deposition conditions] Reactive gas (volume %): TiCl42%, CH3CN 0.7%, N2 10%, H2 balance Reaction pressure: 7 kPa Reaction temperature: 900℃

[0058] [Al2O3 chemical vapor deposition conditions] Reactive gas (volume %): AlCl3 2.2%, CO2 5.5%, HCl 2.2%, H2S 0.2%, H2 remaining Reaction pressure: 7kPa Reaction temperature: 1000℃

[0059] [Table 5]

[0060] Next, cutting test 1 was performed on Examples 1 to 5 and Comparative Examples 1' to 5' in which no coating layer was formed, and cutting test 2 was performed on Examples 6 to 10 and Comparative Examples 6' to 9' in which a coating layer was formed. The amount of plastic deformation on the flank of the cutting edge was measured, and the wear state of the cutting edge was observed.

[0061] Cutting test 1: Dry external turning of alloy steel (JIS SNCM439) round bar (diameter 200 mm) Work material: JIS SNCM439 Cutting speed: 100m / min Cutting depth: 1.0mm Feed: 0.9mm / rev Cutting time: 1 minute

[0062] Cutting test 2: Dry external turning of alloy steel (JIS SNCM439) round bar (diameter 200 mm) Work material: JIS SNCM439 Cutting speed: 150m / min Cutting depth: 1.0mm Feed: 1.2mm / rev Cutting time: 1 minute

[0063] After the cutting tests 1 and 2, the amount of plastic deformation on the flank of the cutting edge was measured, and the wear state of the cutting edge was observed. The amount of plastic deformation on the flank of the cutting edge was measured by drawing a line segment (9) on the ridge where the flank of the main cutting edge (6) and the rake face (5) intersect at a position sufficiently away from the cutting edge (7) on the flank of the main cutting edge side of the tool, extending the line segment toward the cutting edge portion, and measuring the maximum distance between the extended line segment and the ridge of the cutting edge portion (perpendicular to the extended line segment), and this was taken as the amount of plastic deformation on the flank of the cutting edge (8). When the amount of plastic deformation on the flank was 0.100 mm or more, the wear state was determined to be cutting edge deformation (see FIG. 2).

[0064] The results of cutting test 1 are shown in Table 6, and the results of cutting test 2 are shown in Table 7. In Tables 6 and 7, "*" indicates that cutting was interrupted every 20 seconds to observe the cutting edge, and it was confirmed that the chipping was caused by plastic deformation. In addition, since the chipping occurred on the cutting edge and it was difficult to distinguish the ridge line, the amount of plastic deformation could not be measured.

[0065] [Table 6]

[0066] [Table 7]

[0067] As is clear from Table 6 showing the results of Cutting Test 1 and Table 7 showing the results of Cutting Test 2, all of the Examples exhibited little plastic deformation on the flank, which affects the tool life, and exhibited excellent toughness and resistance to plastic deformation without uneven wear or chipping. In contrast, all of the Comparative Examples exhibited large plastic deformation of the tool in a given cutting time, making it difficult to perform machining to obtain the required workpiece dimensions. [Explanation of symbols]

[0068] 1 bonded phase 2 Hard phase 3. γ phase 4. γ-γ phase interface 5. Scooping surface 6 Main cutting edge side flank 7 Cutting edge 8. Amount of plastic deformation on the flank of the cutting edge 9 Extended line segments

Claims

1. Co, Ni: 7.0 to 9.0 mass% in total; Ti, Zr, Nb, and Ta in total 4.0 to 12.0 mass%; Contains 5.7 to 6.4 mass% C; The balance is W and inevitable impurities. The hard phase mainly contains W carbides, a binder phase mainly contains Co and Ni, and a gamma phase mainly contains Ti, Zr, Nb, Ta and W carbides, The hard phase has an average grain size of 0.5 to 4.0 μm, and the gamma phase has an average grain size of 2.0 to 3.0 μm; When the atomic ratios of Ti, Zr, Nb, Ta and W contained in each of the γ phases are a, b, c, d and e (where a+b+c+d+e=100.0), the average value a avg , b avg , c avg , d avg , e avg (However, a avg +b avg +c avg +d avg + e avg = 100.0) is 20.0 ≦ a avg ≦30.0, 20.0≦b avg ≦30.0, 10.0≦c avg ≦20.0, 20.0≦d avg ≦e≦30.0, 5.0≦e≦15.0, the average values ​​of σa, σb, σc, σd, and σe, which are standard deviations of a, b, c, d, and e, respectively, are 10.0 to 15.0; a ratio of an interface length between the hard phase and the binder phase to a total interface length of the hard phase, and a ratio of an interface length between the gamma phase and the binder phase to a total interface length of the gamma phase are both 0.45 to 0.55; The ratio of the interface length between the gamma phases to the total interface length of the gamma phases is 0.25 to 0.

30.

1. A cemented carbide for cutting tools, comprising:

2. 2. The cemented carbide for cutting tools according to claim 1, further comprising 0.5 mass % or less of Cr.

3. A cutting tool using the cemented carbide for cutting tools according to claim 1 or 2.

Citation Information

Patent Citations

  • Coated cemented carbide with binder phase enriched surface zone

    JP2006328529A

  • Cemented carbide and cutting tool

    JP2020132971A

  • Cutting tool

    JP2022130147A

  • Hard metal alloy and tool using the hard metal

    JP2022151698A

  • Cemented carbide body containing zirconium and niobium and method of making the same

    US20050120825A1