Proton conductor, solid electrolyte layer, and solid electrolyte joint having the same

By incorporating specific dopant elements and halogens into the perovskite-structured proton conductor, the proton conductivity is enhanced, addressing the limitations of existing proton conductors and improving performance in medium to low temperature ranges.

JP2024142176APending Publication Date: 2024-10-10MITSUI MINING & SMELTING CO LTD +1

Patent Information

Application Number
JP2023054222
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing proton conductors, such as yttrium-doped barium zirconate, face a decrease in proton conductivity due to factors like precipitation of foreign phases and proton trapping at grain boundaries when dopant concentrations exceed the solid solubility limit, limiting their performance, especially in medium to low temperature ranges.

Method used

Incorporating a dopant element and halogen into a perovskite-structured proton conductor, with specific molar ratios of M, B, and X elements, to create a region with high proton conductivity by replacing part of the B element at the B site in the perovskite structure.

Benefits of technology

The solution achieves significantly higher proton conductivity than conventional methods, maintaining structural stability and reducing grain boundary resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142176000001_ABST
    Figure 2024142176000001_ABST
Patent Text Reader

Abstract

To provide a proton conductor capable of achieving higher proton conductivity than ever before.SOLUTION: A proton conductor according to the present invention includes a composition in which a part of oxygen in a perovskite oxide containing an element capable of becoming a divalent cation at the A site and an element selected from the group consisting of Zr and Ce and an element selected from the group consisting of a trivalent rare earth element and indium at the B site is substituted with a halogen. The molar ratio of M to the sum of B and M (M / (B+M)) satisfies 0.21≤M / (B+M)<0.40. The molar ratio of halogen X to the sum of B and M (X / (B+M)) satisfies 0<X / (B+M)<0.13.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a proton conductor, and also to a solid electrolyte layer and a solid electrolyte assembly including the same. [Background technology]

[0002] The spread of clean energy throughout society is recognized as an important issue in building a sustainable world, and fuel cells are a concrete means of solving this problem. Solid oxide fuel cells (SOFCs), which are made of ceramic materials, can operate at high temperatures and have the highest power generation efficiency of any fuel cell. The solid electrolyte, which is the main component of SOFCs, is made of a material that selectively allows ions to pass through, and oxide ion conductors have traditionally been used. In recent years, it has been reported that the power generation efficiency of SOFCs can be theoretically dramatically improved by using proton conductors instead of oxide ion conductors, and expectations are rising for the realization of proton conducting ceramic fuel cells (PCFCs) that use proton conducting ceramics in the electrolyte layer.

[0003] Various proton conductors with a perovskite structure have been proposed as proton conductive ceramics. Among them, yttrium-doped barium zirconate (hereinafter also referred to as "BZY") is known to have high chemical stability in an atmosphere containing water vapor and carbon dioxide, which is the operating atmosphere of a fuel cell, due to its strong Zr-O bond (see, for example, Patent Document 1).

[0004] In Non-Patent Document 1, a compound having the composition formula BaZr 0.8 Y 0.2 O 3-δThe proton conductivity of samples with an increased concentration of the dopant yttrium has been investigated for a proton conductor represented by the formula: However, although the amount of protons dissolved in solid solution increases by increasing the dopant concentration, it has been reported that the proton mobility decreases due to factors such as precipitation of different phases at the grain boundaries and proton trapping at the dopant sites when the solid solubility limit is exceeded, resulting in a decrease in proton conductivity.

[0005] In Non-Patent Document 2, in order to increase the proton conductivity of BZY, 0.8 Y 0.2 O 3-δ The proton conductor represented by O 2- F the site - However, there is an ever-increasing demand for improved proton conductivity in proton-conducting ceramics, particularly in the low and medium temperature range. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2009-23883 A [Non-patent literature]

[0007] [Non-Patent Document 1] Solid State Ionics 181, 1043-1051, 2010 [Non-Patent Document 2] ChemElectroChem 7, 2242-2247, 2020 Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, an object of the present invention is to provide a proton conductor capable of achieving higher proton conductivity than ever before. [Means for solving the problem]

[0009] As a result of intensive studies to solve the above problems, the inventors of the present invention have found that, in a proton conductor having a perovskite structure, by containing a dopant element capable of improving proton conductivity together with a halogen, there exists a region showing high proton conductivity in a composition in which the M element is dissolved beyond the optimum solid solution amount of the M element that replaces a part of the B element located at the B site, which has been generally adopted heretofore.

[0010] The present invention has been made based on the above findings, and is a proton conductor having a composition in which a part of oxygen in a perovskite oxide containing an A element at the A site, a B element and an M element at the B site is substituted with an X element, The A element represents at least one element capable of becoming a divalent cation, The B element represents at least one element selected from the group consisting of Zr and Ce, The M element represents at least one element selected from the group consisting of trivalent rare earth elements and indium, The X element represents a halogen, The molar ratio of the M element to the sum of the B element and the M element (M / (B + M)) satisfies 0.21 ≦ M / (B + M) < 0.40, and provides a proton conductor in which the molar ratio of the X element to the sum of the B element and the M element (X / (B + M)) satisfies 0 < X / (B + M) < 0.13.

[0011] Further, the present invention is a solid electrolyte layer including a proton conductor having a composition in which a part of oxygen in a perovskite oxide containing an A element at the A site, a B element and an M element at the B site is substituted with an X element, The A element represents at least one element capable of becoming a divalent cation, The B element represents at least one element selected from the group consisting of Zr and Ce, The M element represents at least one element selected from the group consisting of trivalent rare earth elements and indium, The X element represents a halogen, The molar ratio of the M element to the sum of the B element and the M element (M / (B + M)) satisfies 0.21 ≦ M / (B + M) < 0.40, and provides a solid electrolyte layer including a proton conductor in which the molar ratio of the X element to the sum of the B element and the M element (X / (B + M)) satisfies 0 < X / (B + M) < 0.13.

Advantages of the Invention

[0012] According to the proton conductor of the present invention, it is possible to achieve higher proton conductivity than ever before.

Brief Description of the Drawings

[0013] [Figure 1] FIG. 1(a) and FIG. 1(b) are X-ray diffraction diagrams showing the phase identification results of the proton conductors obtained in the examples and comparative examples. [Diagram 2] FIG. 2 is a scanning electron microscope image showing the observation results of the crystal grains of the proton conductors obtained in the examples and comparative examples. [Diagram 3] FIG. 3 is a chart showing the measurement results of the 19F NMR spectra of the proton conductors obtained in the examples and comparative examples.

Embodiments for Carrying Out the Invention

[0014] Hereinafter, the present invention will be described based on its preferred embodiments. The present invention relates to a proton conductor. The proton conductor of the present invention is composed of a perovskite oxide. A perovskite oxide generally has an element located at the A site and an element located at the B site in the perovskite structure.

[0015] The proton conductor of the present invention contains an A element at the A site in the perovskite structure, and a B element and an M element at the B site. The A element, B element, and M element are different elements from each other.

[0016] The element A is at least one of elements that can become a divalent cation. Examples of such an element A include Group 2 elements Be, Ca, Mg, Sr, and Ba. These elements A may be used alone or in combination of two or more. In particular, using Ba as the element A is preferable because it enhances the proton conductivity of the proton conductor of the present invention.

[0017] The B element is at least one selected from the group consisting of Zr and Ce. These B elements may be used alone or in combination of two or more. In particular, using Zr as the B element is preferable because it improves the proton conductivity of the proton conductor of the present invention and also increases the chemical stability.

[0018] The M element is an element that replaces a part of the B element located at the B site in the perovskite structure. The M element is at least one selected from the group consisting of trivalent rare earth elements and indium. Among the M elements, the rare earth elements include, for example, Sc, Y, and lanthanoid elements. The lanthanoid elements include La, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. These M elements may be used alone or in combination of two or more. From the viewpoint of proton conductivity and proton transport number, the M element is preferably at least one selected from the group consisting of Y, Sc, Yb, Lu, and In, and particularly, when Y is used, the proton conductivity of the proton conductor of the present invention is increased, which is preferable.

[0019] Methods for quantifying the A, B and M elements in the perovskite structure include, for example, wavelength-dispersive or energy-dispersive X-ray fluorescence analysis and ICP emission spectrometry.

[0020] In the proton conductor of the present invention, part of the oxygen element in the perovskite structure is replaced with an X element. The X element is a halogen. Examples of halogens include F, Cl, Br, and I. These halogens may be used alone or in combination of two or more. In particular, it is preferable to use F as the halogen, since it enhances the proton conductivity of the proton conductor of the present invention. This is because F - The ionic radius of the ion is O 2- This is thought to be because the ionic radius of the ion is close to that of the F - The greater electronegativity of ions may lead to increased chemical stability. A part of the oxygen element in the perovskite structure is replaced by the X element, for example, when the X element is F, 19 It can be determined from the chemical shift value of F NMR or the position of the diffraction peak in XRD measurement. 19 The method for determining the F NMR chemical shift values ​​is described in the Examples.

[0021] The X element in the perovskite structure can be quantified by, for example, wavelength-dispersive or energy-dispersive X-ray fluorescence analysis. Alternatively, the X element can be quantified by a fluorine ion electrode method after a sample is fused in an alkali and then separated by steam distillation.

[0022] As described above, the proton conductor of the present invention has a perovskite structure. This proton conductor is preferably represented by the composition formula A a (B 1-b M b )O 3-δ X c The details of the elements A, B, M and X in this composition formula are as described above. The elements a, b and c in the composition formula will be described later. δ represents the amount of oxygen deficiency. The value of δ is determined according to the amounts of A element, M element, and X element. The amount of deficiency of anion sites in the perovskite structure is represented by δ-c. In general, δ-c is preferably more than 0.0 and less than 0.3, more preferably more than 0.0 and 0.2 or less, and even more preferably more than 0.0 and 0.1 or less. By setting δ-c to less than 0.3, it is possible to suppress a decrease in the durability of the proton conductor caused by the proton conductor being unable to maintain the perovskite structure.

[0023] The technology of substituting a part of the oxygen element in a proton conductor having a perovskite structure with a halogen is described in the above-mentioned Non-Patent Document 2. As a result of further investigations by the present inventors into the proton conductor described in the same document, it was found that there exists a region showing high proton conductivity in a composition in which the M element is solid-dissolved beyond the optimal solid-solubility amount of the M element substituting a part of the B element located at the B site, which has been generally adopted up to now, by adjusting the amount of halogen substituting a part of the oxygen element in the perovskite structure. In the conventional technology, for example, the technology described in Non-Patent Document 1, when the substitution amount of the M element is increased, the solid-solubility limit is exceeded, and a different phase is precipitated at the crystal grain boundary, which hinders the improvement of proton conductivity. In addition, when the substitution amount of the M element, which is a dopant, is increased, proton trapping by the dopant site may occur, and the proton conductivity may decrease. The reason why proton conductivity increases with increasing substitution amount of M element is thought to be because the valence of B element is tetravalent while the valence of M element is trivalent, and therefore oxygen vacancies occur due to charge compensation caused by substituting B element with M element.

[0024] Specifically, regarding the substitution amount of element X, it is preferable that the value of X / (B + M), which is the molar ratio of element X to the sum of element B and element M, satisfies 0 < X / (B + M) < 0.13, because it can increase the substitution amount of element B with element M, thereby achieving high proton conductivity. However, if the substitution amount of element X is excessive, there is a concern that the amount of anion-site deficiency will decrease and the amount of proton solid solution will decrease. From this point of view, the value of X / (B + M) is more preferably 0.01 ≦ X / (B + M) ≦ 0.09, and even more preferably 0.02 ≦ X / (B + M) ≦ 0.06.

[0025] Regarding the substitution amount of element M, it is preferable that the value of M / (B + M), which is the molar ratio of element M to the sum of element B and element M, satisfies 0.21 ≦ M / (B + M) < 0.40, because it can increase the substitution amount of element B with element M, thereby achieving high proton conductivity. However, if the substitution amount of element B with element M is excessive, there is a concern that proton trapping by the dopant site will occur and the proton conductivity will decrease. From this perspective, the value of M / (B + M) is more preferably 0.23 ≦ M / (B + M) ≦ 0.35, and even more preferably 0.25 ≦ M / (B + M) ≦ 0.30.

[0026] Regarding the difference in the substitution amounts of element M and element X, it is preferable that the value of (M / (B + M)) - (X / (B + M)), which is the difference between the molar ratio of element M to the sum of element B and element M and the molar ratio of element X to the sum of element B and element M, satisfies 0.15 ≦ (M / (B + M)) - (X / (B + M)) ≦ 0.30, because it can increase the substitution amount of element M by a certain amount or more than that of element X, thereby preventing the decrease in the vacancies of the anion site due to charge compensation and improving the proton conductivity. However, if the amount of substitution of the M element is too large compared to the amount of substitution of the X element, there is a concern that the number of vacancies in the anion sites will be too large from the viewpoint of charge compensation, and the proton conductor will not be able to maintain the perovskite structure. From this viewpoint, it is more preferable that the value of (M / (B+M))-(X / (B+M)) is 0.17≦(M / (B+M))-(X / (B+M))≦0.28, and even more preferable that it is 0.20≦(M / (B+M))-(X / (B+M))≦0.25.

[0027] As long as the proton conductor of the present invention has a perovskite structure, some deviation in the composition of each element is permitted. For example, the molar ratio of the sum of the elements B and M to the element A does not need to be strictly 1, and may be, for example, 0.9 to 1.1.

[0028] The proton conductor of the present invention is formed of the above-mentioned composition formula A a (B 1-b M b )O 3-δ X c In the above formula, where the amount of substitution of the X element and the amount of substitution of the M element are represented by the subscripts a, b, and c, it is preferable that a is a number between 0.9 and 1.1 in terms of achieving high proton conductivity. From this viewpoint, a is more preferably between 0.95 and 1.05, and even more preferably between 0.98 and 1.02.

[0029] From the viewpoint of achieving high proton conductivity, b is preferably a number of 0.21 or more and less than 0.40.From this viewpoint, b is more preferably 0.23 or more and 0.35 or less, and even more preferably 0.25 or more and 0.30 or less.

[0030] Furthermore, from the viewpoint of achieving high proton conductivity, c is preferably a number greater than 0 and less than 0.13. From this viewpoint, c is more preferably 0.01 or more and 0.09 or less, and even more preferably 0.02 or more and 0.06 or less.

[0031] In the proton conductor of the present invention, from the viewpoint of achieving even higher proton conductivity, it is preferable that the A element located at the A site in the perovskite structure is Ba, the B element and the M element located at the B site are Zr and Y, respectively, and the X element substituted for the oxygen element is F. From the same viewpoint as above, the proton conductor of the present invention has the composition formula Ba a (Zr 1-b Y b )O 3-δ F c (wherein a, b, c and δ are as defined above).

[0032] The proton conductor of the present invention may contain elements capable of improving various properties of the proton conductor, in addition to the above-mentioned elements A, B, M, and X, and oxygen. Examples of such elements include Ni, which is an element contained in a sintering aid used in producing the proton conductor.

[0033] The proton conductor of the present invention can be suitably produced, for example, by a solid-phase sintering method, in which the powders of the source compounds of the elements A, B, M, and X are mixed and the resulting mixed powder is fired in an oxygen-containing atmosphere to obtain the desired proton conductor.

[0034] The source compound for the element A may be, for example, a salt or an oxide containing the element A. As the source compound for the element A, it is particularly preferable to use a carbonate containing the element A, for example, barium carbonate. The B element source compound can be, for example, an oxide or a salt containing the element B. As the B element source compound, it is particularly preferable to use an oxide of the element B, for example, zirconium oxide. As the M element source compound, for example, an oxide or salt containing the M element can be used. As the M element source compound, it is particularly preferable to use an oxide of the M element, for example, yttrium oxide. The X element source compound can be, for example, a halide of the A element, the B element, or the M element. It is particularly preferable to use, as the X element source compound, a halide of the A element, for example, barium fluoride.

[0035] The A element source compound, B element source compound, M element source compound, and X element source compound are mixed so that the molar ratio of A element, B element, M element, and X element will be the composition of the intended proton conductor.

[0036] The sintering of the molded body containing the A element source compound, the B element source compound, the M element source compound, and the X element source compound is preferably carried out at, for example, 1000° C. to 1800° C. in terms of reliably producing the intended proton conductor. From this viewpoint, the sintering temperature is more preferably 1100° C. to 1700° C., and even more preferably 1200° C. to 1600° C. From the viewpoint of reliably producing the desired proton conductor, the firing time is preferably from 1 hour to 48 hours, more preferably from 2 hours to 36 hours, and even more preferably from 5 hours to 24 hours. The firing atmosphere is preferably an oxygen-containing atmosphere such as air.

[0037] The proton conductor thus obtained is suitably used as a proton-conductive solid electrolyte layer. In order to produce the solid electrolyte layer, the following operations are preferably carried out. First, the proton conductor is pulverized in a pulverizer to obtain a powder having a predetermined particle size. A small amount of an organic solvent is added to this powder to form a paste. This paste is molded to obtain a molded body of a predetermined shape. This molded body is fired to obtain a solid electrolyte layer. In order to smoothly proceed with sintering, a sintering aid may be added to the powder. An example of the sintering aid is nickel oxide. Therefore, the solid electrolyte layer contains the proton conductor and also contains elements derived from the sintering aid. In this case, the elements derived from the sintering aid, such as Ni, are not present in the perovskite structure but are present exclusively at the crystal grain boundaries of the perovskite oxide. From the viewpoint of easily ensuring high resistance to water and carbon dioxide and proton conductivity, it is preferable that the content of elements derived from the sintering aid is small. For example, it is preferable that 90 mass % or more of the solid electrolyte layer is the perovskite oxide represented by the above composition.

[0038] The thickness of the solid electrolyte layer is, for example, preferably 1 μm to 50 μm, more preferably 3 μm to 20 μm, in which case the resistance of the solid electrolyte layer can be kept low.

[0039] The solid electrolyte layer can be used as a solid electrolyte junction by disposing electrodes (anode and cathode) on each surface of the solid electrolyte layer. The solid electrolyte layer is sandwiched between the cathode and the anode, and one main surface of the solid electrolyte layer is in contact with the anode and the other main surface is in contact with the cathode.

[0040] The solid electrolyte joint can be formed, for example, by firing a coating of a paste containing a proton conductor, a binder, a sintering aid, and a dispersion medium. The coating can be formed, for example, by applying an electrolyte paste to the main surface of an anode or a cathode. Prior to firing, a binder removal process may be performed to remove the binder by heating. The firing may be a combination of a pre-firing process performed at a relatively low temperature and a main firing process performed at a higher temperature than the pre-firing process.

[0041] Examples of binders include polymer binders such as cellulose derivatives (such as cellulose ethers) such as ethyl cellulose, vinyl acetate resins (including saponified vinyl acetate resins such as polyvinyl alcohol), and acrylic resins; and / or waxes such as paraffin wax.

[0042] The temperature of the pre-firing is preferably, for example, not lower than 800° C. and lower than 1200° C. The temperature of the main firing is preferably, for example, 1200° C. to 1800° C. The pre-firing and main firing may each be performed in an air atmosphere, or in an oxygen-containing atmosphere containing more oxygen than the air.

[0043] The solid electrolyte junction is useful as various electrochemical devices. Specifically, the solid electrolyte junction can be applied to cells of fuel cells equipped with the solid electrolyte junction, steam electrolysis cells, and the like.

[0044] The cathode in an electrochemical device equipped with a solid electrolyte junction preferably has a porous structure. When the electrochemical device is a fuel cell, as the cathode material, for example, a compound containing lanthanum and having a perovskite structure is preferable. Among these compounds, those containing strontium are more preferable. Specifically, lanthanum strontium cobalt ferrite (LSCF, La 1-x1 Sr x1 Fe 1-y1 Co y1 O 3-δ1 (0 < x1 < 1, 0 < y1 < 1, δ1 is the oxygen deficiency amount)), lanthanum strontium manganite (LSM, La 1-x2 Sr x2 MnO 3-δ1 (0 < x2 < 1, δ1 is the oxygen deficiency amount)), lanthanum strontium cobaltite (LSC, La 1-x3 Sr x3 CoO 3-δ1 (0 < x3 ≤ 1, δ1 is the oxygen deficiency amount)), etc. can be mentioned. From the viewpoint of promoting the reaction between protons and oxide ions, the cathode may contain a catalyst such as Pt. When containing a catalyst, the cathode can be formed by mixing the catalyst and the above material and sintering. When the electrochemical device is a steam electrolysis cell, as the cathode material, a composite of Ni and yttrium-stabilized zirconia or the like can be used.

[0045] The thickness of the cathode is not particularly limited, but can be appropriately determined from, for example, 5 μm to 2 mm and may be about 10 μm to 100 μm.

[0046] On one hand, the anode in a solid electrolyte bonded electrochemical device preferably has a porous structure. As the anode material, known materials used as anodes in electrochemical devices such as fuel cells and steam electrolysis cells can be used without particular limitation. When the electrochemical device is a fuel cell, specific examples of the anode material include composite oxides of nickel oxide, which is a catalyst component, and a proton conductor (e.g., yttrium oxide, BZY, etc.). When the electrochemical device is a steam electrolysis cell, a conductive oxide stable in an oxidizing atmosphere, such as lanthanum manganate added with strontium, can be used as the anode material.

[0047] The thickness of the anode can be appropriately determined, for example, from 5 μm to 2 mm, and may be 10 μm to 100 μm.

[0048] Regarding the above-described embodiments, the present invention further discloses the following proton conductors, solid electrolyte layers, fuel cell cells, and steam electrolysis cells. [1] A proton conductor having a composition in which a part of oxygen in a perovskite oxide containing an A element at the A site, a B element and an M element at the B site is substituted with an X element, The A element represents at least one element that can be a divalent cation, The B element represents at least one element selected from the group consisting of Zr and Ce, The M element represents at least one element selected from the group consisting of trivalent rare earth elements and indium, The X element represents a halogen, The molar ratio of the M element to the sum of the B element and the M element (M / (B + M)) satisfies 0.21 ≦ M / (B + M) < 0.40, A proton conductor in which the molar ratio of the X element to the sum of the B element and the M element (X / (B + M)) satisfies 0 < X / (B + M) < 0.13. 〔2〕The proton conductor according to 〔1〕, wherein the difference between the molar ratio of the M element to the sum of the B element and the M element and the molar ratio of the X element to the sum of the B element and the M element satisfies 0.15 ≦ (M / (B + M)) - (X / (B + M)) ≦ 0.30. 〔3〕The proton conductor according to 〔1〕 or 〔2〕, wherein the A element is a Group 2 element and the M element is a rare earth element. 〔4〕The A element is barium, the B element is zirconium, the M element is yttrium, and the X element is fluorine. The proton conductor according to any one of 〔1〕 to 〔3〕. 〔5〕A solid electrolyte layer comprising a proton conductor having a composition in which a part of oxygen in a perovskite oxide containing the A element at the A site, the B element and the M element at the B site is substituted with the X element, wherein the A element represents at least one element that can be a divalent cation, the B element represents at least one element selected from the group consisting of Zr and Ce, the M element represents at least one element selected from the group consisting of trivalent rare earth elements and indium, the X element represents a halogen, the molar ratio of the M element to the sum of the B element and the M element (M / (B + M)) satisfies 0.21 ≦ M / (B + M) < 0.40, and the molar ratio of the X element to the sum of the B element and the M element (X / (B + M)) satisfies 0 < X / (B + M) < 0.13. A solid electrolyte layer comprising a proton conductor. 〔6〕A solid electrolyte layer comprising a proton conductor represented by the composition formula A a (B 1-b M b )O 3-δ X c . In the formula, the A element represents at least one element that can be a divalent cation, the B element represents at least one element selected from the group consisting of Zr and Ce, the M element represents at least one element selected from the group consisting of trivalent rare earth elements and indium, X represents a halogen; δ represents the amount of oxygen deficiency, a is a number between 0.9 and 1.1, b represents a number between 0.21 and 0.40, c represents a number greater than 0 and less than 0.13. [7] A solid electrolyte junction comprising the solid electrolyte layer according to [5] or [6] and an electrode disposed on each surface of the solid electrolyte layer. [8] A fuel cell comprising the solid electrolyte assembly according to [7]. [9] A steam electrolysis cell comprising the solid electrolyte junction according to [7]. EXAMPLES

[0049] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".

[0050] Example 1 Barium carbonate, zirconium oxide, yttrium oxide, and barium fluoride were weighed out in amounts such that the molar ratio of Ba, Zr, Y, and F was the composition shown in Table 1 below, and mixed in a ball mill for 48 hours. The mixed powder was fired in a Tammann tube of a Tammann tube type atmospheric electric furnace at 1300°C for 10 hours in air generated by an air compressor to obtain a synthetic powder made of a proton conductor. XRD confirmed that this synthetic powder had a perovskite structure. The obtained synthetic powder was mixed again in a ball mill for 50 hours. 1 mol% of NiO was added to this synthetic powder, mixed in a ball mill for 10 hours, and then pressed to obtain a molded body of a specified shape. This molded body was heat-treated in the Tammann tube of a Tammann tube-type atmospheric electric furnace at 1500°C for 24 hours in air generated by an air compressor to obtain a pellet-shaped high-density solid electrolyte. Both sides of this solid electrolyte were polished uniformly.

[0051] [Example 2 and Comparative Examples 1, 2, 3 and 4] Barium carbonate, zirconium oxide, yttrium oxide, and barium fluoride were weighed out in amounts such that the molar ratio of Ba, Zr, Y, and F was the composition shown in Table 1 below, and a sintered body made of a proton conductor was obtained. A solid electrolyte was obtained in the same manner as in Example 1 except for this.

[0052] 〔evaluation〕 The solid electrolytes obtained in the examples and comparative examples were subjected to composition analysis by the following method. Furthermore, phase identification was performed by the following method. Furthermore, electrical conductivity was measured by the following method. Furthermore, crystal grains were observed by the following method. Furthermore, NMR spectrum measurement was performed by the following method. The results are shown in Tables 1 and 2. The phase identification results are shown in Figure 1. The crystal grain observation results are shown in Figure 2. The NMR spectrum measurement results are shown in Figure 3.

[0053] [Composition analysis] Quantitative analysis of Ba, Zr, and Y was performed by inductively coupled plasma (ICP) atomic emission spectrometry. Quantitative analysis of F was performed by fluoride ion electrode method after vapor distillation separation of the sample after alkali fusion.

[0054] [Method of identifying phase] The phase of the powder was identified using powder X-ray diffraction (XRD) (Rigaku's RINT-TTR3 X-ray diffraction device). The powder was ground in a zirconia mortar, and the resulting powder sample was filled into a dedicated glass holder and measured. CuKα radiation was used as the radiation source, with a tube voltage of 50 kV and a tube current of 300 mA. The goniometer scanning method was the 2θ / θ method.

[0055] [Measurement of Electrical Conductivity of Solid Electrolyte] Platinum films were formed on both sides of the solid electrolyte by sputtering, and the electrical conductivity of the solid electrolyte was measured by the AC impedance method. The measurement was performed by applying an AC voltage with an amplitude of 10 mV and a frequency range of 500 kHz to 10 Hz. The measurement was performed in a humidified nitrogen atmosphere (water vapor partial pressure: 0.05 atm). The sample was kept at 600°C to be fully hydrated, and then the temperature was lowered at 5°C / min, and after each 50°C decrease, the sample was held for 50 minutes, and then the AC impedance measurement was performed. The total resistance (intragranular resistance + grain boundary resistance) was calculated from the obtained Nyquist Plot to obtain the electrical conductivity. Since it is believed that proton conduction occurs in a humidified nitrogen atmosphere, the electrical conductivity in a humidified nitrogen atmosphere was used as an evaluation index for proton conductivity.

[0056] [Observation of crystal grains] The crystal grains were observed using an FE gun-type scanning electron microscope (JSM-7900F manufactured by JEOL Ltd.) The solid electrolyte was crushed and the microstructure (secondary electron image) of the cross section was observed.

[0057] [NMR measurement] 19 F NMR spectra were measured under the following conditions: Magnetic field: 14.1 T( 1 H 600MHz, 19F 564MHz) Spectrometer: Bruker AVANCE NEO600 Measurement and data processing software: Bruker TopSpin NMR probe: 1.3mm MAS probe Sample rotation speed: 60 kHz Chemical shift and radio frequency intensity standards: Polytetrafluoroethylene powder. Standard for chemical shift values: The maximum point of the peak of polytetrafluoroethylene powder is set to -122.7 ppm. Measurement method: OLDFIELD ECHO method Spectral center (O1 value - SR value (chemical shift value notation)): -122.7 ppm Radio frequency pulse intensity: The intensity shall be set so that the pulse width which maximizes the polytetrafluoroethylene powder peak when the spectrum center is -122.7 ppm is 1.5 μs. Radio frequency pulse width: excitation pulse 1.5μs, echo pulse 3.0μs Interval between excitation pulse and echo pulse: 15.17μs Measurement interval: 1.0 μs (DW=0.5 μs on the above software) Number of measurement points: 12,000 points (TD=24,000 on the above software) Number of spectral points (SI on the above software): 32768 points Repeat wait time (D1 on the above software): 16 seconds Number of integrations (NS on the above software): 64 times

[0058] The "OLDFIELD ECHO method" is described in "Solid-State Spin-Echo Fourier Transform NMR of 1969" by A. K. Kunwar et al., Journal of Magnetic Resonance (1969), Vol. 69 (1986), p. 124. 39 K and 67 This is based on the "Zn Salts at High Field" report.

[0059] [Table 1]

[0060] From the ICP emission spectroscopy and the XRD measurement results described later, it was found that the solid electrolytes of each of the Examples and Comparative Examples had the measured compositions shown in Table 1, and it was also found that there was no significant difference in the Ni element content. As is clear from the results shown in Table 1, it can be seen that the solid electrolytes obtained in Examples 1 and 2 have higher electrical conductivity than the solid electrolyte obtained in the Comparative Example.

[0061] From the X-ray diffraction diagram shown in FIG. 1(a), it was confirmed that the solid electrolyte of each Example exhibited a cubic perovskite structure, similar to each Comparative Example, and the presence of a different phase other than the perovskite structure was not confirmed. 1(b) is an enlarged view of the 2θ range of 52.4° to 53.6°. From Comparative Examples 1, 2 and 3 shown in this figure, it was found that the peak shifts to the lower angle side as the amount of fluorine doped increases. Furthermore, it was confirmed from Examples 1 and 2 and Comparative Example 4 that as the doping amount of yttrium increases in addition to the doping amount of fluorine, the peak shifts significantly to the lower angle side. The above results suggest that yttrium and fluorine are in a solid solution.

[0062] 2, it can be seen that the crystal grains of Examples 1 and 2 and Comparative Examples 2 to 4, in which the doping amounts of yttrium and fluorine are increased, are coarse compared to Comparative Example 1. This suggests that the crystal grain size increases and the grain boundary resistance decreases by increasing the doping amounts of yttrium and fluorine.

[0063] As shown in FIG. 3, the fluorine-doped solids obtained in Examples 1 and 2 and Comparative Examples 2 to 4 19 In the F NMR spectrum, the chemical shift values ​​of two overlapping peaks (P1, P2) were confirmed. In Fig. 3, the baseline was created from Comparative Example 1. The spectra of Examples 1 and 2 and Comparative Examples 2 to 4 were normalized by the sample mass after subtracting the baseline created in Comparative Example 1 from the original spectrum. In addition, the peaks were separated by the pseudo-Voigt function shown in the following formula (1).

[0064]

number

[0065] In formula (1), x is 19 The horizontal axis value (chemical shift value) of the F MAS NMR spectrum is shown. x0 represents the chemical shift value of the peak top, S is the scaling factor for adjusting the peak vertical axis value to the actual measurement, η represents the peak area ratio of the Lorentz function (first term) in the range from -∞ (minus infinity) to +∞ (plus infinity), Δ represents the half-width of the peak, π stands for pi, ln represents the natural logarithm function, exp represents the natural exponential function.

[0066] For peak separation, fitting was performed using the solver function of the calculation software to minimize the mean square deviation of the chemical shift values ​​between the measured spectrum and the calculated spectrum in the range of -150 ppm to 5 ppm, with the variables x0, Δ, η, and S of the pseudo-Voigt functions for the number of peaks.

[0067] The fitting variables for Examples 1 and 2 and Comparative Examples 2 to 4 are shown in Table 2. In this specification, x0 obtained by the above-mentioned peak separation is taken as the chemical shift value of each peak. The "pseudo-Voigt function" is based on "6. Profile Functions and Pattern Decomposition Methods" in "Special Feature: New Developments in Powder Diffraction Methods" Journal of the Crystallographic Society of Japan, 34, 86 (1992).

[0068] [Table 2]

[0069] Table 2 shows the fitting parameters for the peaks P1 and P2 present in Examples 1 and 2 and Comparative Examples 2 to 4. It was found that the peaks were present at approximately -65 to -75 ppm and -80 to -90 ppm, respectively. Therefore, in addition to the composition analysis, 19 The presence of fluorine in the crystals can also be confirmed by F NMR measurement.

Claims

1. A proton conductor having a composition in which part of oxygen in a perovskite oxide containing an A element in an A site and an B element and an M element in a B site is substituted with an X element, The A element represents at least one element capable of becoming a divalent cation, The B element represents at least one element selected from the group consisting of Zr and Ce, M element represents at least one element selected from the group consisting of trivalent rare earth elements and indium, The X element represents a halogen. the molar ratio of the M element to the sum of the B element and the M element (M / (B+M)) satisfies 0.21≦M / (B+M)<0.40; A proton conductor, in which the molar ratio of an X element to the sum of B and M elements (X / (B+M)) satisfies 0<X / (B+M)<0.

13.

2. 2. The proton conductor according to claim 1, wherein a difference between a molar ratio of M element to the sum of B element and M element and a molar ratio of X element to the sum of B element and M element satisfies 0.15≦(M / (B+M))−(X / (B+M))≦0.

30.

3. 3. The proton conductor according to claim 1, wherein the A element is a Group 2 element and the M element is a rare earth element.

4. The A element is barium, The B element is zirconium, The M element is yttrium, 3. The proton conductor according to claim 1, wherein the element X is fluorine.

5. A solid electrolyte layer comprising a proton conductor having a composition in which part of oxygen in a perovskite oxide containing an A element in an A site and an B element and an M element in a B site is substituted with an X element, The A element represents at least one element capable of becoming a divalent cation, The B element represents at least one element selected from the group consisting of Zr and Ce, M element represents at least one element selected from the group consisting of trivalent rare earth elements and indium, The X element represents a halogen. the molar ratio of the M element to the sum of the B element and the M element (M / (B+M)) satisfies 0.21≦M / (B+M)<0.40; A solid electrolyte layer comprising a proton conductor, the molar ratio (X / (B+M)) of an element X to the sum of elements B and M satisfying 0<X / (B+M)<0.

13.

6. Composition formula A a (B 1-b M b ) O 3-δ X c A solid electrolyte layer comprising a proton conductor represented by the formula: In the formula, element A represents at least one element capable of becoming a divalent cation, The B element represents at least one element selected from the group consisting of Zr and Ce, M element represents at least one element selected from the group consisting of trivalent rare earth elements and indium, X represents a halogen; δ represents the amount of oxygen deficiency, a represents a number of 0.9 or more and 1.1 or less, b represents a number equal to or greater than 0.21 and less than 0.40; c represents a number greater than 0 and less than 0.

13.

7. A solid electrolyte assembly comprising the solid electrolyte layer according to claim 6 and electrodes disposed on both sides of the solid electrolyte layer.

8. A fuel cell comprising the solid electrolyte assembly according to claim 7.

9. A steam electrolysis cell comprising the solid electrolyte assembly according to claim 7.

Citation Information

Patent Citations

  • Proton conductor

    JP2009023883A

Cited By

  • Proton-conducting solid electrolyte and method for producing the same

    JP2026130565A

  • Proton conductive solid electrolyte, proton conductive fuel cell, steam electrolysis cell, and method for producing proton conductive solid electrolyte

    WO2026197291A1