Reflective mask blank and reflective mask, and manufacturing methods for reflective mask and semiconductor device

The reflective mask blank design with a lower layer of amorphous or microcrystalline structure and a highly crystalline upper layer addresses adhesion and durability issues in EUV lithography, ensuring precise and durable pattern transfer.

JP2024142177APending Publication Date: 2024-10-10HOYA CORPORATION

Patent Information

Application Number
JP2023054223
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

In EUV lithography, the adhesion between layers of thin films in reflective masks is insufficient, leading to potential separation and defects, especially when high-power exposure light sources are used, which also requires higher durability from these films.

Method used

A reflective mask blank design with a lower layer having an amorphous or microcrystalline structure and an upper layer with higher crystallinity, where the upper layer has a larger crystallite size than the lower layer, and they are made of different materials, enhancing adhesion and durability.

Benefits of technology

Improves adhesion between thin film layers, preventing peeling and maintaining high reflectance, allowing for more precise and durable pattern transfer in EUV lithography, even under high-power exposure conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142177000001_ABST
    Figure 2024142177000001_ABST
Patent Text Reader

Abstract

To provide a mask blank which can enhance adhesion between two layers included in a thin film.SOLUTION: A reflective mask blank comprises: a substrate; a multilayer reflective film provided on the substrate; and a thin film provided on the multilayer reflective film. The thin film includes a lower layer and an upper layer provided on the lower layer. The lower layer is composed of a material including an amorphous structure or a microcrystalline structure. The crystallinity of the upper layer is higher than that of the lower layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective mask used in the manufacture of a semiconductor device, a manufacturing method thereof, and a reflective mask blank used to manufacture a reflective mask. The present invention also relates to a manufacturing method of a semiconductor device using the reflective mask. [Background technology]

[0002] 2. Description of the Related Art In response to the increasing demand for higher density and higher precision in VLSI devices in recent years, extreme ultraviolet (hereinafter referred to as EUV) lithography, which is an exposure technique using EUV light, has been proposed.

[0003] A reflective mask has a multilayer reflective film formed on a substrate to reflect exposure light, and an absorber pattern, which is a patterned absorber film formed on the multilayer reflective film to absorb the exposure light. In EUV lithography using a reflective mask, the light image reflected by the multilayer reflective film of the reflective mask is transferred onto a semiconductor substrate (transfer target) such as a silicon wafer through a reflection optical system. A reflective mask blank is used to manufacture a reflective mask.

[0004] As an example of a reflective mask, Patent Document 1 describes a reflective X-ray mask composed of an X-ray reflective film, and an intermediate layer and an X-ray absorber layer formed in a pattern. In the reflective X-ray mask of Patent Document 1, the etching selectivity between the intermediate layer and the X-ray absorber layer is 5 or more. Patent Document 1 also describes that the intermediate layer is made of a material containing chromium or titanium as a main component.

[0005] As an example of a reflective mask blank, Patent Document 2 describes a mask blank having, on a substrate, a reflective layer that reflects exposure light in a short wavelength range including the extreme ultraviolet region, a buffer layer for protecting the reflective layer when forming a pattern on the absorber layer, and an absorber layer that absorbs the exposure light, in that order. Patent Document 2 also describes that the absorber layer has at least a two-layer structure, with an absorber layer made of an absorber of exposure light in a short wavelength range including the extreme ultraviolet region as a lower layer, and a low-reflection layer made of an absorber of inspection light used to inspect the mask pattern as an upper layer. Patent Document 2 also describes that the upper layer is made of a material containing tantalum (Ta), boron (B), and oxygen (O). Patent Document 2 also describes that the buffer layer is formed of Cr or a substance mainly composed of Cr. Patent Document 2 also describes that the reflectance to the inspection light decreases in the order of the multilayer reflective film surface, the buffer layer surface, and the absorber layer surface, and that the reflectance of the absorber layer surface to the wavelength of light used to inspect the pattern formed on the absorber layer is 20% or less. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 8-213303 [Patent Document 2] Patent No. 4061319 Summary of the Invention [Problem to be solved by the invention]

[0007] The above-mentioned EUV lithography is an exposure technique using extreme ultraviolet light (EUV light). EUV light is light in a wavelength band in the soft X-ray region or the vacuum ultraviolet region, specifically light with a wavelength of about 0.2 to 100 nm. In the case of EUV lithography, EUV light with a wavelength of 13 to 14 nm (for example, a wavelength of 13.5 nm) can be used. In this specification, light includes not only visible light but also electromagnetic waves.

[0008] EUV lithography uses a reflective mask with an absorber pattern. EUV light irradiated onto the reflective mask is absorbed in areas where the absorber pattern exists, and reflected in areas where the absorber pattern does not exist. A multilayer reflective film (including a protective film) is exposed in areas where there is no absorber pattern. The multilayer reflective film exposed on the surface of the reflective mask reflects the EUV light. In EUV lithography, the optical image reflected by the multilayer reflective film (area where there is no absorber pattern) is transferred onto a semiconductor substrate (transfer target) such as a silicon wafer through a reflective optical system.

[0009] The absorber pattern disposed on the multilayer reflective film of the reflective mask is formed by patterning the absorber film of the reflective mask blank. In addition, thin films other than the absorber film, such as a protective film and an etching mask film, may be disposed on the multilayer reflective film. In addition, the absorber film may be composed of multiple different layers (thin films). Therefore, multiple thin films, including at least the multilayer reflective film and the absorber film, are disposed on the substrate of the reflective mask blank.

[0010] When multiple different layers (thin films) are laminated on a substrate, if the adhesion at the interface between adjacent layers is insufficient, one layer may peel off from the other layer during the manufacturing process of the reflective mask blank and / or the manufacturing process of the reflective mask, resulting in defects.

[0011] Furthermore, in the case of EUV lithography using a reflective mask in the semiconductor manufacturing process, a light source (exposure light source) for generating EUV light with a short wavelength of about 13.5 nm is used to transfer a pattern formed on the reflective mask to a transfer target. In recent years, increasing the power of the exposure light source for EUV lithography has been considered. When a high-power exposure light source is used in EUV lithography, thin films such as thin films for pattern formation need to have higher durability. Note that a high-power exposure light source can mean, for example, an exposure light source with a power of 400 W or more.

[0012] Therefore, an object of the present invention is to provide a mask blank capable of improving the adhesion between two layers of a thin film when the thin film contains two layers, and to provide a reflective mask blank having a thin film having higher durability by improving the adhesion between the two layers contained in the thin film.

[0013] Another object of the present invention is to provide a reflective mask manufactured using the reflective mask blank, and a method for manufacturing a semiconductor device using the reflective mask. [Means for solving the problem]

[0014] In order to solve the above problems, the present invention has the following configuration.

[0015] (Configuration 1) Configuration 1 is a reflective mask blank, A substrate; a multilayer reflective film provided on the substrate; a thin film provided on the multilayer reflective film; the thin film includes a lower layer and an upper layer disposed on the lower layer, the underlayer is made of a material having an amorphous structure or a microcrystalline structure, The upper layer has a higher crystallinity than the lower layer.

[0016] (Configuration 2) Configuration 2 is the reflective mask blank of configuration 1, wherein the lower layer and the upper layer are in contact with each other.

[0017] (Configuration 3) Configuration 3 is the reflective mask blank according to configuration 1 or 2, wherein the thin film is an absorber film.

[0018] (Configuration 4) Configuration 4 is the reflective mask blank according to any one of configurations 1 to 3, wherein the difference in crystallite size between the upper layer and the lower layer is 2 nm or more.

[0019] (Configuration 5) Structure 5 is the reflective mask blank of any one of structures 1 to 4, further comprising an etching mask film formed on and in contact with the thin film, the crystallinity of the etching mask film being lower than that of the upper layer.

[0020] (Configuration 6) A sixth aspect of the present invention is a reflective mask blank according to any one of the first to fifth aspects, further comprising a protective film between the multilayer reflective film and the thin film.

[0021] (Configuration 7) A seventh aspect of the present invention is the reflective mask blank according to any one of the first to sixth aspects, wherein the lower layer and the upper layer are made of different materials.

[0022] (Configuration 8) Configuration 8 is the reflective mask blank of any one of configurations 1 to 7, wherein the upper layer contains at least one selected from Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W, and Rh.

[0023] (Configuration 9) A ninth aspect of the present invention is the reflective mask blank of any one of the first to eighth aspects, wherein the crystallite size of the upper layer is greater than 3 nm.

[0024] (Configuration 10) Configuration 10 is a reflective mask, A substrate; a multilayer reflective film provided on the substrate; a thin film having a pattern provided on the multilayer reflective film, the thin film includes a lower layer and an upper layer disposed on the lower layer, the underlayer is made of a material having an amorphous structure or a microcrystalline structure, The upper layer has a higher crystallinity than the lower layer.

[0025] (Configuration 11) Configuration 11 is the reflective mask of configuration 10, wherein the lower layer and the upper layer are in contact with each other.

[0026] (Configuration 12) Configuration 12 is the reflective mask of configurations 10 or 11, wherein the thin film is an absorber film.

[0027] (Configuration 13) Configuration 13 is the reflective mask of any one of configurations 10 to 12, wherein the difference between the crystallite size of the upper layer and the crystallite size of the lower layer is 2 nm or more.

[0028] (Configuration 14) A fourteenth aspect of the present invention is a reflective mask according to any one of the tenth to thirteenth aspects, further comprising a protective film between the multilayer reflective film and the thin film.

[0029] (Configuration 15) Configuration 15 is the reflective mask of any one of configurations 10 to 14, wherein the lower layer and the upper layer are made of different materials.

[0030] (Configuration 16) Structure 16 is the reflective mask of any of Structures 10 to 15, wherein the upper layer includes at least one selected from Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W, and Rh.

[0031] (Configuration 17) Configuration 17 is the reflective mask of any of Configurations 10 to 16, wherein the crystallite size of the upper layer is greater than 3 nm.

[0032] (Configuration 18) Configuration 18 is a method for manufacturing a semiconductor device, characterized in that a reflective mask having a pattern formed on the thin film of the reflective mask blank of any one of Configurations 1 to 9, or a reflective mask of any one of Configurations 10 to 17, is used to transfer the pattern to a transfer target on a semiconductor substrate. Effect of the Invention

[0033] According to the present invention, when the thin film includes two layers, a mask blank capable of improving the adhesion between the two layers of the thin film can be provided. Also, according to the present invention, a reflective mask blank having a thin film having higher durability can be provided, in which the adhesion between the two layers included in the thin film can be improved.

[0034] According to the present invention, it is also possible to provide a reflective mask manufactured using the reflective mask blank. According to the present invention, it is also possible to provide a method for manufacturing a semiconductor device using the reflective mask. [Brief description of the drawings]

[0035] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a reflective mask blank of the present embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing another example of the reflective mask blank of the present embodiment. [Figure 3A-E] 5A to 5C are schematic cross-sectional views showing an example of a method for manufacturing the reflective mask of the present embodiment. [Figure 4] FIG. 1 is a schematic diagram showing an example of an EUV exposure apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that the following embodiments are intended to specifically explain the present invention, and are not intended to limit the scope of the present invention.

[0037] As shown in FIG. 1, this embodiment is a reflective mask blank 100 having a substrate 1, a multilayer reflective film 2 provided on the substrate 1, and a thin film provided on the multilayer reflective film.

[0038] Fig. 1 is a schematic cross-sectional view showing an example of a reflective mask blank 100 of this embodiment. The reflective mask blank 100 shown in Fig. 1 has a substrate 1, a multilayer reflective film 2 provided on the substrate 1, and a thin film provided on the multilayer reflective film 2. The thin film of the reflective mask blank 100 of this embodiment includes a lower layer and an upper layer provided on the lower layer. In the example shown in Fig. 1, the thin film is an absorber film 4, and the absorber film 4, which is the thin film of this embodiment, has a lower layer 42 and an upper layer 44. In this embodiment, a thin film having a predetermined lower layer and upper layer may be referred to as a "predetermined thin film".

[0039] The predetermined thin film of this embodiment can be any film formed on the multilayer reflective film 2. In the example shown in FIG. 1, a protective film 3, an absorber film 4, and an etching mask film 6 are disposed on the multilayer reflective film 2. The predetermined thin film of this embodiment is preferably at least one selected from the protective film 3, the absorber film 4, and the etching mask film 6. In this case, at least one thin film selected from the protective film 3, the absorber film 4, and the etching mask film 6 can be a predetermined thin film having a lower layer and an upper layer. The lower layer and the upper layer can be a pair of adjacent films as described above. That is, in the reflective mask blank 100 of this embodiment, the lower layer can be the protective film 3, and the upper layer can be the absorber film 4. In this case, the predetermined thin film is the protective film 3 as the lower layer, and the absorber film 4 as the upper layer. Here, when the absorber film 4 is a laminated film including a plurality of layers, the lower layer can be a layer in contact with the protective film 3 among the plurality of layers. In addition, in the reflective mask blank 100 of this embodiment, the lower layer can be the absorber film 4, and the upper layer can be the etching mask film 6. In this case, the predetermined thin film is the lower layer, the absorber film 4, and the upper layer, the etching mask film 6. Here, when the absorber film 4 is a laminated film including a plurality of layers, the upper layer can be a layer in contact with the etching mask film 6 among the plurality of layers.

[0040] Fig. 2 is a schematic cross-sectional view showing another example of the reflective mask blank 100 of this embodiment. The reflective mask blank 100 shown in Fig. 2 does not have an etching mask film 6. Furthermore, in the reflective mask blank 100 of this embodiment, the protective film 3 may or may not be present. The reflective mask blank 100 of this embodiment has at least a multilayer reflective film 2 and an absorber film 4 on a substrate 1. In the example shown in Fig. 2, the predetermined thin film is the absorber film 4, and the absorber film 4, which is the predetermined thin film of this embodiment, has a lower layer 42 and an upper layer 44.

[0041] The absorber film 4 is repeatedly exposed to cleaning liquids in the manufacturing process of a reflective mask blank, the manufacturing process of a reflective mask, and / or the manufacturing process of a semiconductor using a reflective mask. Therefore, in order to reduce peeling of the absorber film 4 in the above-mentioned processes, it is preferable that the absorber film 4 has high adhesion to the film formed above and / or below the absorber film 4. In addition, when the absorber film 4 includes a plurality of layers, it is preferable that the plurality of layers have high adhesion to each other. Therefore, it is preferable that the predetermined thin film of this embodiment includes at least a part of the absorber film 4.

[0042] In the reflective mask blank 100 of this embodiment, the lower layer is made of a material having an amorphous structure or a microcrystalline structure, and the upper layer has a higher crystallinity than the lower layer. The present inventors discovered that when the lower layer and the upper layer, which are two films (layers) arranged in contact with each other, have a predetermined crystallinity, the adhesion between the adjacent lower layer and upper layer can be improved, and a predetermined thin film (upper layer and lower layer) having higher durability can be obtained, and thus arrived at the present invention.

[0043] The crystallinity of the upper and lower layers of a given thin film can be confirmed by X-ray diffraction (XRD). By X-ray diffraction (XRD) of a given thin film or layer, it can be confirmed whether the given thin film or layer has an amorphous structure or a microcrystalline structure. When the given thin film or layer has a crystalline structure or a microcrystalline structure, it can be said that the crystallinity is higher than when it has an amorphous structure. Here, the range of diffraction angle for confirming the crystallinity by X-ray diffraction (XRD) can be 30 degrees or more and 90 degrees or less.

[0044] When no distinguishable sharp peak is observed in the X-ray diffraction profile obtained by the X-ray diffraction (XRD) method of the specified thin film or layer, the specified thin film or layer can be determined to have an amorphous structure. Note that, when the specified thin film or layer has a crystalline structure, a distinguishable sharp peak is observed in the X-ray diffraction profile obtained by the X-ray diffraction (XRD) method of the specified thin film or layer.

[0045] In addition, in this specification, when the maximum peak intensity Imax and the minimum intensity (background intensity) Imin in the above-mentioned X-ray diffraction profile (after fitting described below) are taken as Imax and Imin, respectively, a material is defined as microcrystalline (or amorphous) if the ratio [Imax-Imin] / [Imax+Imin] is 0.15 or less.

[0046] In this specification, the crystallinity of the upper layer is higher than that of the lower layer means that the upper layer has a crystalline structure and the lower layer has an amorphous structure or a microcrystalline structure, or that the upper layer has a microcrystalline structure and the lower layer has an amorphous structure. In this way, when the crystallinity of the upper layer is higher than that of the lower layer, the crystallite size of the upper layer is larger than that of the lower layer.

[0047] Also, the crystallinity can be determined by measuring the crystallite size of a given thin film or layer by X-ray diffraction (XRD). For example, in-plane measurement (2θχ / φ scan) can be used as the X-ray diffraction (XRD) method. A thin film or layer with a larger crystallite size is more crystalline than a thin film or layer with a smaller crystallite size.

[0048] The crystallite size of a given thin film or layer can be determined as follows. That is, first, the profile of the diffraction angle range including the peak in the X-ray diffraction profile obtained by measuring the given thin film or layer by the X-ray diffraction (XRD) method is fitted by the least squares method using the Gaussian function (Equation 1) below to obtain the diffraction angle u and σ. The crystallite size D can be determined from the diffraction angle u and the half-width β calculated from σ by the Scherrer formula (see Equation 2 below). The half-width β can be determined from σ obtained by fitting by the following Equation 3.

number

number

[0049] In formula 2, D is the crystallite size (nm), K is the Scherrer constant 0.9, λ is the wavelength of X-rays (nm), and β is the half-width of the diffraction line (rad). In this specification, λ is the wavelength of X-rays (CuKα1), 0.15405 (nm).

[0050] In addition, when there are multiple peaks observed in a given X-ray diffraction profile, the peak with the highest peak intensity or the peak with the largest peak area (peak with the largest integrated intensity) can be selected, and the crystallite size can be obtained from this peak. When there are multiple peaks with the highest peak intensity and / or the largest peak area, and it is difficult to determine which peak to select, the peak with the smallest half-width can be selected from these multiple peaks.

[0051] The measurement range of the X-ray diffraction profile can be a 2θ range of 30 degrees to 90 degrees (θ range of 15 degrees to 45 degrees).

[0052] Furthermore, when no peak is observed in the X-ray diffraction profile, it can be determined that the measured thin film or layer has an amorphous structure.

[0053] In the reflective mask blank 100 of this embodiment, the difference between the crystallite size of the upper layer and the crystallite size of the lower layer is preferably 2 nm or more, more preferably 5 nm or more. This can improve the adhesion of the upper layer to the lower layer. Furthermore, the crystallite size of the upper layer is preferably larger than 3 nm, more preferably larger than 8 nm. By having the crystallite size of the upper layer larger than a predetermined value, the adhesion of the upper layer to the lower layer can be improved. Furthermore, the crystallite size of the upper layer is preferably 20 nm or less, more preferably 19 nm or less, and even more preferably 18 nm or less. By having the crystallite size of the upper layer be equal to or less than a predetermined value, the surface roughness of a predetermined thin film including the upper layer can be reduced, so that a good thin film surface can be obtained.

[0054] In the specified thin film included in the reflective mask blank 100 of this embodiment, the crystallinity of the upper layer is made high (the crystallite size is made large). Generally, when the crystallinity of a thin film is made high, the surface roughness of the thin film surface increases. On the other hand, in the specified thin film included in the reflective mask blank 100 of this embodiment, the crystallinity of the lower layer is made low by making the lower layer have an amorphous structure or a microcrystalline structure, so that it is possible to prevent the surface roughness of the specified thin film as a whole from becoming too large.

[0055] In the reflective mask blank 100 of this embodiment, the etching rate of the upper layer can be increased by increasing the crystallinity of the upper layer of the predetermined thin film. On the other hand, the lower layer of the predetermined thin film of the reflective mask blank 100 of this embodiment has a relatively low crystallinity, for example, the lower layer has an amorphous structure or a microcrystalline structure, so that the lower layer can have a higher resistance to the etching gas of the upper layer. Therefore, damage to the lower layer during etching of the upper layer can be reduced. This makes it possible to further suppress damage to other thin films or layers (for example, when the predetermined thin film is an absorber film 4, the multilayer reflective film 2 and / or protective film 3, which are other thin films) present further below (towards the substrate) the lower layer of the predetermined thin film, and as a result, the reflectance from the multilayer reflective film 2 can be maintained high.

[0056] Generally, when a thin film is patterned by etching, the larger the crystallite size, the easier it is for the etchant to penetrate into the thin film, and the higher the etching rate. In this embodiment, the crystallinity of the upper layer of a given thin film is high, so that the etching rate of the upper layer can be improved. That is, by making the crystallite size of the upper layer in a given thin film larger than that of the lower layer, the etching rate of the upper layer for etching a region in the given thin film can be made faster than that of the region other than the upper layer. The longer the time required to etch the upper layer, the higher the possibility that films and layers other than the upper layer will be damaged. However, by adopting the above-mentioned configuration, damage to films and layers other than the upper layer, such as the lower layer, can be suppressed.

[0057] From the diffraction angle of the X-ray diffraction profile of the predetermined layer obtained by the above-mentioned X-ray diffraction (XRD) method, the plane spacing of the predetermined lattice plane can be obtained by Bragg's law. The lattice plane can be one having Miller indices corresponding to the peak with the highest peak intensity or the peak with the largest peak area (peak with the largest integrated intensity) within the diffraction angle range of 30 degrees to 90 degrees in the X-ray diffraction profile. When there are multiple peaks with the highest peak intensity and / or the largest peak area and it is difficult to distinguish the peak to be selected, the peak with the smallest half-width among these multiple peaks can be selected. The lattice plane spacing d of the upper layer obtained by the XRD method is preferably 0.27 nm or less, more preferably 0.25 nm or less, and even more preferably 0.23 nm or less. This makes it possible to suppress the intrusion of oxygen with a kinetic molecular diameter of 0.346 nm and hydrogen with a kinetic molecular diameter of 0.289 nm into the predetermined thin film. As a result, damage and / or deterioration of the predetermined thin film can be suppressed.

[0058] In the reflective mask blank of this embodiment, the lower layer and the upper layer of the predetermined thin film are preferably made of different materials. By making the lower layer and the upper layer of the predetermined thin film of different materials, it becomes easy to control the lower layer and the upper layer to have a predetermined crystallinity. In addition, the selectivity to the etching gas when etching the lower layer and the upper layer can be made appropriate.

[0059] In the reflective mask blank of this embodiment, the lower layer and the upper layer are preferably in contact with each other. By having the lower layer and the upper layer in contact with each other, the adhesion between the adjacent lower layer and upper layer can be improved, and a predetermined thin film (upper layer and lower layer) having higher durability can be obtained.

[0060] 1 and 2 may further include other thin films such as a back surface conductive film 5. Moreover, as shown in FIG. 3A, the reflective mask blank 100 of this embodiment may further include a resist film 11.

[0061] In this specification, "film B is disposed (formed) on film A (or substrate)" means that film B is disposed (formed) in contact with the surface of film A (or substrate), and also includes the case of having another film C between film A (or substrate) and film B. In addition, in this specification, for example, "film B is disposed in contact with the surface of film A (or substrate)" means that film A (or substrate) and film B are disposed so as to be in direct contact with each other without another film being interposed between film A (or substrate) and film B. In addition, in this specification, "on" does not necessarily mean the upper side in the vertical direction. "on" merely indicates the relative positional relationship of a film, a substrate, etc. In this embodiment, when two films, film A and film B, exist in the reflective mask blank 100, if film A is disposed at a position farther from the substrate than film B, it is said that "film A is disposed (disposed) on film B". Since the upper layer of the reflective mask blank 100 of this embodiment is provided on the lower layer, the upper layer is disposed at a position farther from the substrate than the lower layer.

[0062] In the reflective mask blank 100 of this embodiment, the predetermined thin film is preferably an absorber film 4. In the case of the absorber film 4, multiple layers may be formed to improve performance. Therefore, there is a risk that defects due to film peeling may occur due to a decrease in adhesion between the multiple layers included in the absorber film 4. The reflective mask blank 100 of this embodiment can improve the adhesion between the multiple layers included in the absorber film 4, and can manufacture a reflective mask having an absorber film 4 that is less likely to cause defects and has higher durability.

[0063] The above explanation uses a reflective mask blank 100 for manufacturing a reflective mask as an example, but the specified thin films (lower and upper layers) of this embodiment can also be applied to mask blanks other than reflective mask blanks (e.g., binary mask blanks and phase-shift mask blanks, etc.).

[0064] <Reflective mask blank 100> The reflective mask blank 100 of this embodiment will be specifically described. Hereinafter, a case will be described in which the predetermined thin film is an absorber film 4, and the absorber film 4, which is the predetermined thin film of this embodiment, has a lower layer 42 and an upper layer 44.

[0065] <<Substrate 1>> To prevent distortion of the transferred pattern due to heat during exposure to EUV light, the substrate 1 is preferably one having a low thermal expansion coefficient within the range of 0±5 ppb / ° C. Materials having a low thermal expansion coefficient within this range include, for example, SiO2-TiO2 glass, multi-component glass ceramics, etc.

[0066] The main surface (first main surface) of the substrate 1 on which a transfer pattern (absorber pattern 4a described later) is formed is preferably processed to increase its flatness. By increasing the flatness of the main surface of the substrate 1, the positional accuracy and transfer accuracy of the pattern can be increased. For example, in the case of EUV exposure, in a 132 mm×132 mm area of ​​the main surface of the substrate 1 on which a transfer pattern is formed, the flatness is preferably 0.1 μm or less, more preferably 0.05 μm or less, and particularly preferably 0.03 μm or less. In addition, the second main surface (rear surface) on the opposite side to the side on which the transfer pattern is formed is a surface fixed to the exposure device by an electrostatic chuck. In a 142 mm×142 mm area of ​​the rear surface, the flatness is 0.1 μm or less, more preferably 0.05 μm or less, and particularly preferably 0.03 μm or less. In this specification, the flatness is a value that indicates the warpage (deformation amount) of the surface indicated by TIR (Total Indicated Reading). The flatness (TIR) ​​is the absolute value of the difference in height between the highest point on the surface of substrate 1 above the focal plane, which is determined by the least squares method using the surface of substrate 1 as the reference plane, and the lowest point on the surface of substrate 1 below this focal plane.

[0067] In the case of EUV exposure, the surface roughness of the main surface of the substrate 1 on which the transfer pattern is formed is preferably 0.1 nm or less in terms of root mean square roughness (Rq). The surface roughness can be measured by an atomic force microscope.

[0068] The substrate 1 preferably has high rigidity to prevent deformation due to film stress of the thin films (such as the multilayer reflective film 2) formed thereon, and in particular, preferably has a high Young's modulus of 65 GPa or more.

[0069] <<Multilayer reflective film 2>>

[0070] The reflective mask blank 100 of the embodiment includes a multilayer reflective film 2. The multilayer reflective film 2 provides the reflective mask 200 with a function of reflecting EUV light. The multilayer reflective film 2 is a multilayer film in which layers containing substances with different refractive indices as main components are periodically laminated.

[0071] Generally, the multilayer reflective film 2 is a multilayer film in which thin films (high refractive index layers) of a light element or its compound, which is a high refractive index material, and thin films (low refractive index layers) of a heavy element or its compound, which is a low refractive index material, are alternately stacked for about 30 to 60 periods.

[0072] The multilayer film used as the multilayer reflective film 2 can be a structure in which a high refractive index layer / low refractive index layer stack structure in which a high refractive index layer and a low refractive index layer are stacked in this order from the substrate 1 side is stacked multiple times. The multilayer film can also be a structure in which a low refractive index layer / high refractive index layer stack structure in which a low refractive index layer and a high refractive index layer are stacked in this order from the substrate 1 side is stacked multiple times. Note that the top layer of the multilayer reflective film 2, that is, the surface layer of the multilayer reflective film 2 opposite to the substrate 1 side, is preferably a high refractive index layer. In the above-mentioned multilayer film, when a high refractive index layer / low refractive index layer stack structure in which a high refractive index layer and a low refractive index layer are stacked in this order from the substrate 1 side is stacked multiple times, the top layer is a low refractive index layer. In this case, if the low refractive index layer constitutes the top surface of the multilayer reflective film 2, it is easily oxidized, so there is a possibility that the reflectance of the reflective mask 200 will decrease. Therefore, it is preferable to form a high refractive index layer on the topmost low refractive index layer to form the multilayer reflective film 2. On the other hand, in the above-mentioned multilayer film, when a low refractive index layer / high refractive index layer laminate structure in which a low refractive index layer and a high refractive index layer are laminated in this order from the substrate 1 side is one period, the uppermost layer becomes the high refractive index layer. Therefore, in this case, there is no need to form an additional high refractive index layer.

[0073] As the high refractive index layer, a layer containing silicon (Si) can be used. As the material containing Si, in addition to simple Si, a Si compound containing boron (B), carbon (C), nitrogen (N), oxygen (O) and / or hydrogen (H) can be used. By using a high refractive index layer containing Si, a reflective mask 200 having excellent reflectance to EUV light can be obtained. As the low refractive index layer, a simple metal selected from molybdenum (Mo), ruthenium (Ru), rhodium (Rh) and platinum (Pt), or an alloy thereof can be used. In addition, boron (B), carbon (C), nitrogen (N), oxygen (O) and / or hydrogen (H) may be added to these simple metals or alloys. In the reflective mask blank 100 of this embodiment, it is preferable that the low refractive index layer is a molybdenum (Mo) layer and the high refractive index layer is a silicon (Si) layer. For example, as the multilayer reflective film 2 for reflecting EUV light having a wavelength of 13 nm to 14 nm (for example, a wavelength of 13.5 nm), a Mo / Si periodic laminate film in which Mo layers and Si layers are alternately laminated for about 30 to 60 periods can be preferably used. In addition, in the reflective mask blank 100 of this embodiment, the low refractive index layer may be a ruthenium (Ru) layer, and the high refractive index layer may be a silicon (Si) layer. For example, as the multilayer reflective film 2 for reflecting EUV light having a wavelength of 13 nm to 14 nm (for example, a wavelength of 13.5 nm), a Ru / Si periodic laminate film in which Ru layers and Si layers are alternately laminated for about 30 to 40 periods can be preferably used.

[0074] The reflectance of the multilayer reflective film 2 can be 65% or more, and the upper limit can be 73%. The reflectance in this specification means a value when the angle of incidence of the EUV light to the multilayer reflective film 2 (including the protective film 3) is the same as the angle of incidence of the EUV light to the irradiation target used in exposure when transferring a pattern using the reflective mask 200 or a reflective mask 200 manufactured from the reflective mask blank 100. When transferring a pattern, the EUV light from the EUV light source is irradiated onto the reflective mask 200 via an illumination optical system at an angle inclined, for example, from 6 degrees to 8 degrees with respect to a plane perpendicular to the main surface of the reflective mask 200. The angle of incidence of the EUV light to the multilayer reflective film 2 is not particularly limited, but can be, for example, 6 degrees.

[0075] The thickness and period of each of the constituent layers of the multilayer reflective film 2 can be appropriately selected depending on the exposure wavelength. Specifically, the thickness and period of each of the constituent layers of the multilayer reflective film 2 can be selected so as to satisfy the law of Bragg reflection. In the multilayer reflective film 2, there are multiple high refractive index layers and multiple low refractive index layers, but the thicknesses of the high refractive index layers and the low refractive index layers do not necessarily have to be the same.

[0076] The method of forming the multilayer reflective film 2 is known in the art. The multilayer reflective film 2 can be formed by depositing each layer by, for example, ion beam sputtering. In the case of the Mo / Si periodic multilayer film described above, for example, a Si film with a thickness of about 4 nm is first deposited on the substrate 1 by using a Si target by ion beam sputtering or magnetron sputtering, and then a Mo film with a thickness of about 3 nm is deposited by using a Mo target. This constitutes one period, and 30 to 60 periods are laminated to form the multilayer reflective film 2 (the outermost layer is a Si film). Note that, although the number of steps increases in the case of 60 periods compared to 30 periods, the reflectance for EUV light can be increased.

[0077] <<Protective film 3>> The reflective mask blank 100 of this embodiment preferably includes a protective film 3 between the multilayer reflective film 2 and an absorber film 4 described later. The protective film 3 is disposed in contact with the surface of the multilayer reflective film 2 opposite to the substrate 1. When the reflective mask blank 100 includes the protective film 3, the reflected light of the multilayer reflective film 2 refers to light that is incident on the multilayer reflective film 2 through the protective film 3 and is reflected through the protective film 3. That is, when the reflective mask blank 100 includes the protective film 3, the reflected light from the surface of the protective film 3 in a state in which the protective film 3 is formed on the multilayer reflective film 2 on the substrate 1 may be measured as the reflected light of the multilayer reflective film 2.

[0078] In the reflective mask blank 100 of this embodiment, the protective film 3 is formed between the multilayer reflective film 2 and the absorber film 4, thereby making it possible to suppress damage to the surface of the multilayer reflective film 2 when manufacturing a reflective mask 200 (EUV mask) using the reflective mask blank 100. Therefore, the resulting reflective mask 200 has good reflectance characteristics for EUV light.

[0079] The protective film 3 preferably contains at least one selected from ruthenium (Ru), rhodium (Rh) and iridium (Ir). The protective film 3 more preferably contains at least one selected from ruthenium (Ru) and rhodium (Rh). The protective film 3 may further contain an additive element in addition to the above-mentioned elements. The additive element contained in the protective film 3 is preferably one or more elements selected from Tl, Hf, Ti, Zr, Mn, In, Ga, Cd, Bi, Ta, Pb, Ag, Al, V, Nb, Sn, Zn, Hg, Cr, Fe, Sb, W, Mo and Cu.

[0080] The content of Ru used in the protective film 3 is 50 atomic % or more and less than 100 atomic %, preferably 80 atomic % or more and less than 100 atomic %, and more preferably 95 atomic % or more and less than 100 atomic %. The content of Rh is 10 atomic % or more and less than 70 atomic %, preferably 20 atomic % or more and less than 60 atomic %, and more preferably 30 atomic % or more and less than 50 atomic %. In this case, the protective film 3 can have a sufficient reflectance of EUV light, while also having mask cleaning resistance, an etching stopper function when the absorber film 4 is etched, and a function of preventing deterioration of the multilayer reflective film 2 over time.

[0081] Moreover, the protective film 3 may have a laminated structure of two or more layers.

[0082] In the reflective mask blank 100 of the present embodiment, an underlayer may be formed between the substrate 10 and the multilayer reflective film 2. The underlayer can be formed for the purposes of improving the smoothness of the main surface of the substrate 10, reducing defects, enhancing the reflectance of the multilayer reflective film 2, and correcting stress in the multilayer reflective film 2.

[0083] <<Backside conductive film 5>> The reflective mask blank 100 of this embodiment may have a back surface conductive film 5 for electrostatic chuck. The back surface conductive film 5 may be formed on the second main surface (back surface) of the substrate 1. The second main surface is the main surface opposite to the surface on which the multilayer reflective film 2 is formed. When an intermediate layer such as a hydrogen penetration suppression film is formed on the second main surface of the substrate 1, the back surface conductive film 5 may be formed on the intermediate layer. The sheet resistance required for the back surface conductive film 5 for electrostatic chuck is usually 100Ω / □ (Ω / square) or less. The method for forming the back surface conductive film 5 is, for example, a magnetron sputtering method or an ion beam sputtering method using a target of a metal such as chromium or tantalum, or an alloy thereof. The chromium (Cr)-containing material of the back surface conductive film 5 is preferably a Cr compound containing at least one selected from boron, nitrogen, oxygen, and carbon in Cr. Examples of Cr compounds include CrN, CrON, CrCN, CrCON, CrBN, CrBON, CrBCN, and CrBOCN. The tantalum (Ta)-containing material of the back surface conductive film 5 is preferably Ta, an alloy containing Ta, or a Ta compound containing at least one of boron, nitrogen, oxygen, and carbon in any of these. Examples of Ta compounds include TaB, TaN, TaO, TaON, TaCON, TaBN, TaBO, TaBON, TaBCON, TaHf, TaHfO, TaHfN, TaHfON, TaHfCON, TaSi, TaSiO, TaSiN, TaSiON, and TaSiCON. The thickness of the back surface conductive film 5 is not particularly limited as long as it satisfies the function for electrostatic chuck, but is usually 10 nm to 200 nm. In addition, the back surface conductive film 5 also serves to adjust the stress on the second main surface side of the mask blank 100. That is, the back surface conductive film 5 is adjusted to obtain a flat reflective mask blank 100 by balancing the stress from various films formed on the first main surface side.

[0084] It is to be noted that the reflective mask blank 100 does not necessarily need to include a rear surface conductive film 5. For example, a rear surface conductive film 5 can be formed, if necessary, on a reflective mask blank 100 on which an absorber film 4 described below has been formed.

[0085] <<Absorber film 4>> 1 and 2, the absorber film 4 of the reflective mask blank 100 of this embodiment is disposed on the above-mentioned multilayer reflective film 2. When the reflective mask blank 100 includes a protective film 3, the absorber film 4 is disposed on the protective film 3. The absorber film 4 can be disposed in contact with the surface of the protective film 3. When the reflective mask blank 100 does not include a protective film 3, the absorber film 4 can be disposed in contact with the surface of the multilayer reflective film 2.

[0086] The basic function of the absorber film 4 is to absorb EUV light. The absorber film 4 may be an absorber film 4 for absorbing EUV light, or an absorber film 4 having a phase shift function that also takes into account the phase difference of EUV light. The absorber film 4 having a phase shift function absorbs EUV light and reflects a part of it to shift the phase. That is, in the reflective mask 200 in which the absorber film 4 having a phase shift function is patterned, the absorber film 4 absorbs EUV light to reduce the light and reflects a part of the light at a level that does not adversely affect pattern transfer in the part where the absorber film 4 is formed. In addition, in the region (field portion) in which the absorber film 4 is not formed, the EUV light is reflected from the multilayer reflective film 2 (through the protective film 3 if the protective film 3 exists). Therefore, a desired phase difference is generated between the reflected light from the absorber film 4 having a phase shift function and the reflected light from the field portion. The absorber film 4 having a phase shift function is formed so that the phase difference between the reflected light from the absorber film 4 and the reflected light from the multilayer reflective film 2 is 100 degrees to 310 degrees. The phase difference is preferably 150 degrees or more, more preferably 180 degrees or more, and even more preferably 200 degrees or more. The phase difference is preferably 300 degrees or less, more preferably 280 degrees or less, and even more preferably 250 degrees or less. The light with the inverted phase difference interferes with each other at the pattern edge portion, thereby improving the image contrast of the projected optical image. With the improvement in the image contrast, the resolution increases, and various latitudes related to exposure such as exposure dose latitude and focus latitude can be increased.

[0087] In the reflective mask blank 100 of the present embodiment, the predetermined thin film is preferably an absorber film 4 .

[0088] As shown in Figures 1 and 2, the absorber film 4 (predetermined thin film) of the reflective mask blank 100 of this embodiment can include a lower layer 42 and an upper layer 44. The lower layer 42 is disposed between the upper layer 44 and the multilayer reflective film 2 (or between the upper layer 44 and the protective film 3 if the protective film 3 is present). The absorber film 4 can include films other than the lower layer 42 and the upper layer 44. Since the reflective mask blank 100 of this embodiment has the absorber film 4, which is a predetermined thin film, the adhesion between the two layers (the lower layer 42 and the upper layer 44) included in the absorber film 4 can be improved.

[0089] In the reflective mask blank 100 of the present embodiment, the lower layer 42 and the upper layer 44 are preferably in contact with each other. By having the lower layer 42 and the upper layer 44 in contact with each other, it is possible to reliably improve the adhesion between the lower layer 42 and the upper layer 44.

[0090] The lower layer 42 of the absorber film 4 can be a buffer layer. The buffer layer of the absorber film 4 is a layer disposed in contact with the protective film 3, and is a layer for suppressing adverse effects on the protective film 3 when the absorber film 4 is etched to form the absorber pattern 4a. Specifically, a material that can be etched using an etching gas that does not damage the protective film 3 can be used as the material of the lower layer 42. In this case, when etching the upper layer 44, there is a risk of damage to the protective film 3, but an etching gas that has a high etching rate for the upper layer 44 can be used. Therefore, by including the lower layer 42, which is a buffer layer, and the upper layer 44 in the absorber film 4, the etching time of the absorber film 4 can be shortened, and adverse effects on the protective film 3 can be suppressed when the absorber film 4 is etched to form the absorber pattern 4a.

[0091] Specifically, when the protective film 3 is made of a material containing ruthenium (Ru) and the absorber film 4 is also made of a material containing ruthenium (Ru) (e.g., PtRu), both the protective film 3 and the absorber film 4 are etched with a fluorine-based etching gas. In this case, when the absorber film 4 is etched to form the absorber pattern 4a, there is a possibility that the protective film 3 may be adversely affected. Therefore, by forming the absorber film 4 such that the absorber film 4 includes an upper layer 44 and a lower layer 42, and the lower layer 42 functions as a buffer layer, the adverse effect on the protective film 3 can be suppressed. In this case, the material of the buffer layer, which is the lower layer 42, can be a material that has etching resistance against a fluorine-based etching gas. For example, the material of the buffer layer, which is the lower layer 42, can be a material that can be etched using a chlorine-based etching gas.

[0092] The lower layer 42 of the reflective mask blank 100 of this embodiment is made of a material containing an amorphous structure or a microcrystalline structure. Moreover, the upper layer 44 of the reflective mask blank 100 of this embodiment has a higher crystallinity than the lower layer 42.

[0093] When the predetermined thin film of the reflective mask blank 100 of this embodiment is an absorber film 4, the lower layer 42 of the absorber film 4 is made of a material having an amorphous structure or a microcrystalline structure. In addition, the crystallinity of the upper layer 44 of the absorber film 4 is higher than that of the lower layer 42. The lower layer 42 and the upper layer 44 arranged in contact with each other have a predetermined crystallinity, so that the adhesion between the adjacent lower layer 42 and upper layer 44 can be improved. In addition, by using the reflective mask blank 100 of this embodiment having a predetermined absorber film 4, an absorber pattern 4a having higher durability can be obtained.

[0094] In the reflective mask blank 100 of this embodiment, the crystallite size of the upper layer 44 of the absorber film 4 is preferably larger than 3 nm, and more preferably larger than 8 nm. When the crystallite size of the upper layer 44 of the absorber film 4 is larger than a predetermined value, the adhesion to the lower layer 42 of the absorber film 4 can be improved. In addition, the crystallite size of the upper layer 44 of the absorber film 4 is preferably 20 nm or less, more preferably 19 nm or less, and further preferably 18 nm or less. When the crystallite size of the upper layer 44 of the absorber film 4 is a predetermined value or less, the surface roughness of the absorber film 4 including the upper layer 44 can be made good.

[0095] By increasing the crystallite size of the upper layer 44 of the absorber film 4, the etching rate of the upper layer 44 can be increased. On the other hand, in the reflective mask blank 100 of this embodiment, the lower layer 42 of the absorber film 4 has a relatively low crystallinity, for example, the lower layer 42 has an amorphous structure or a microcrystalline structure. Therefore, the lower layer 42 can have higher resistance to the etching gas of the upper layer 44, and damage to the lower layer 42 during etching of the upper layer 44 can be reduced. Therefore, damage to other films (for example, the multilayer reflective film 2 and / or the protective film 3) present further below the lower layer 42 of the absorber film 4 (toward the substrate 1) can be further suppressed, and as a result, the reflectance from the multilayer reflective film 2 can be maintained high.

[0096] The lattice spacing of a given lattice plane can be obtained from the diffraction angles of X-rays from the upper layer 44 and the lower layer 42 of the absorber film 4 obtained by the above-mentioned X-ray diffraction (XRD) method. As described above, the lattice plane can be one having Miller indices corresponding to the peak with the highest peak intensity or the peak with the largest peak area (peak with the largest integrated intensity) within the diffraction angle range of 30 degrees to 90 degrees in the X-ray diffraction profile. When there are multiple peaks with the highest peak intensity and / or the largest peak area and it is difficult to distinguish the peak to be selected, the peak with the smallest half-width among these multiple peaks can be selected. The lattice spacing d of the upper layer 44 of the absorber film 4 obtained by the XRD method is preferably 0.27 nm or less, more preferably 0.25 nm or less, and even more preferably 0.23 nm or less. This makes it possible to suppress the intrusion of oxygen with a kinetic molecular diameter of 0.346 nm and hydrogen with a kinetic molecular diameter of 0.289 nm into the absorber film 4. As a result, damage and / or deterioration of the absorber film 4 can be suppressed.

[0097] According to the findings of the present inventors, the correlation between high crystallinity and high film density is considered to be low.The correlation between crystallite size and film density is also considered to be low.Therefore, when crystallinity is high or crystallite size is large, it is not necessarily said that film density is high.

[0098] In the reflective mask blank 100 of this embodiment, the lower layer 42 and the upper layer 44 of the absorber film 4 are preferably made of different materials. By making the lower layer 42 and the upper layer 44 of the absorber film 4 from different materials, it becomes easy to control the lower layer 42 and the upper layer 44 to have a predetermined crystallinity. In addition, by making the lower layer 42 and the upper layer 44 of the absorber film 4 from different materials, the selectivity to the etching gas when etching the lower layer 42 and the upper layer 44 can be made appropriate.

[0099] The lower layer 42 of the absorber film 4 is preferably made of a material that can protect the multilayer reflective film 2 and / or the protective film 3 when the upper layer 44 of the absorber film 4 is etched.

[0100] The lower layer 42 of the absorber film 4 is not particularly limited as long as it is amorphous or microcrystalline and has a crystallite size smaller than that of the upper layer 44. For example, the material of the lower layer 42 of the absorber film 4 may include a material containing at least one selected from Ta, Cr, Ru, Rh, Mo, Nb, Ti, Zr, Y, Si, Pd, Ag, Ir, W, Co, Mn, Sn, V, Ni, Fe, Hf, Cu, Te, Zn, Mg, Ge, and Al. The material of the lower layer 42 of the absorber film 4 may further include at least one selected from O, N, C, and B. Specific examples of the lower layer 42 of the absorber film 4 include a Cr-based material, a Ta-based material, a Ru-based material, a RuCr material, and a RuTa material, and may further include at least one selected from O, N, C, and B in addition to these materials.

[0101] The material of the upper layer 44 of the absorber film 4 is not particularly limited as long as the upper layer 44 can have a higher crystallinity than the lower layer 42. Examples of the material of the upper layer 44 of the absorber film 4 include materials containing at least one selected from Ru, Ta, Cr, Rh, Mo, Nb, Ti, Zr, Y, Si, Pd, Ag, Pt, Au, Ir, W, Co, Mn, Sn, V, Ni, Fe, Hf, Cu, Te, Zn, Mg, Ge, Al, Au, Re, Os, and Rn. The material of the upper layer 44 of the absorber film 4 can further contain at least one selected from N, O, C, B, and H.

[0102] In order to obtain an absorber film 4 having a high extinction coefficient for EUV light, the upper layer 44 of the absorber film 4 preferably contains at least one selected from Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W, and Rh. The upper layer 44 of the absorber film 4 may further contain at least one selected from N, O, C, B, and H. In particular, a material containing Pt and / or Rr is useful for obtaining a phase shift film (absorber film 4) having a high extinction coefficient for EUV light and a low refractive index.

[0103] When the upper layer 44 of the absorber film 4 is made of a material containing Pt and Ru, the material of the lower layer 42 and / or the etching mask film 6 is preferably a Cr-based material or a Ta-based material. The material of the lower layer 42 and / or the etching mask film 6 is preferably a material further containing at least one selected from O, N, C, and B in addition to the above materials.

[0104] When the absorber film 4 is a phase shift film formed on the multilayer reflective film 2, the phase difference between the reflected light from the multilayer reflective film 2 and the reflected light from a predetermined thin film with respect to the EUV light may be 100 degrees or more, preferably 150 degrees or more, more preferably 180 degrees or more, and even more preferably 200 degrees or more. The phase difference between the reflected light from the multilayer reflective film 2 and the reflected light from a predetermined thin film with respect to the EUV light is preferably 300 degrees or less, more preferably 280 degrees or less, and even more preferably 250 degrees or less. When irradiated with EUV light, the reflectance (relative reflectance) from the absorber film 4 relative to the reflectance from the multilayer reflective film 2 is preferably higher than 3%, and more preferably 4% or more. The relative reflectance is preferably 30% or less, more preferably 20% or less, and even more preferably 10% or less.

[0105] Here, the relative reflectance from the absorber film 4 refers to the reflectance of light reflected from the surface of the absorber film 4 relative to the reflectance of light reflected from the multilayer reflective film 2 (including the protective film 3) when irradiated with EUV light. In other words, the relative reflectance (%) of the absorber film 4 is a value obtained by dividing the reflectance of the absorber film 4 by the reflectance of the multilayer reflective film 2 (including the protective film 3) and multiplying the value by 100.

[0106] The thickness of the lower layer 42 of the absorber film 4 is preferably 2 nm or more in order to function as a buffer layer. Also, the thickness of the lower layer 42 is preferably 55 nm or less, and more preferably 25 nm or less, in order to reduce the so-called shadowing effect.

[0107] The thickness of the upper layer 44 of the absorber film 4 is preferably 5 nm or more in order to function as the absorber film 4. Moreover, the thickness of the upper layer 44 is preferably 60 nm or less in order to reduce the so-called shadowing effect, more preferably 50 nm or less, and even more preferably 40 nm or less.

[0108] The absorber film 4 including the lower layer 42 and the upper layer 44 can be formed by magnetron sputtering such as DC sputtering and RF sputtering. Specifically, the lower layer 42 can be formed by using sputtering and a sputtering gas containing the elements contained in the lower layer 42. The same applies to the upper layer 44. For example, the absorber film 4 of a tantalum compound or the like can be formed by a reactive sputtering method using a target containing tantalum and boron, and argon gas to which oxygen or nitrogen has been added.

[0109] The sputtering gas used to form the lower layer 42 and the upper layer 44 preferably contains a rare gas. The rare gas may be one selected from Xe gas, Ar gas, and Kr gas, or a mixed gas of two or more rare gases selected from these rare gases.

[0110] <<Etching mask film 6>> 1, the reflective mask blank 100 of this embodiment can have an etching mask film 6 on an absorber film 4. As a material for the etching mask film 6, it is preferable to use a material having a high etching selectivity of the absorber film 4 to the etching mask film 6 (etching rate of the absorber film 4 / etching rate of the etching mask film 6). The etching selectivity of the absorber film 4 to the etching mask film 6 is preferably 1.5 or more, and more preferably 3 or more.

[0111] The reflective mask blank 100 of this embodiment preferably has an etching mask film 6 on the absorber film 4 .

[0112] In the reflective mask blank 100 of this embodiment, when the absorber film 4 is a predetermined thin film, it is preferable to have an etching mask film 6 formed on the predetermined thin film (absorber film 4) in contact with the predetermined thin film (absorber film 4). In addition, it is preferable that the crystallinity of the absorber film 4 is higher than that of the etching mask film 6. Specifically, it is preferable that the crystallite size of the absorber film 4 is larger than that of the etching mask film 6 by 2 nm or more. When the absorber film 4 includes a plurality of layers, it is preferable that the crystallinity of the upper layer is higher than that of the etching mask film 6. By using the reflective mask blank 100 having such an etching mask film 6, it is possible to suppress peeling off of the etching mask film 6 at an inappropriate timing in the process of manufacturing the reflective mask 200.

[0113] It is preferable to use chromium or a chromium compound as the material of the etching mask film 6. Examples of chromium compounds include materials containing Cr and at least one element selected from N, O, C, and H. It is more preferable that the etching mask film 6 contains CrN, CrO, CrC, CrON, CrOC, CrCN, and / or CrOCN, and is further preferably a CrO-based film containing chromium and oxygen (a CrO film, a CrON film, a CrOC film, or a CrOCN film).

[0114] Tantalum or a tantalum compound is preferably used as the material of the etching mask film 6. Examples of tantalum compounds include a material containing Ta and at least one element selected from N, O, B, and H. More preferably, the etching mask film 6 contains TaN, TaO, TaON, TaBN, TaBO, or TaBON.

[0115] Silicon or a silicon compound is preferably used as the material of the etching mask film 6. Examples of silicon compounds include materials containing Si and at least one element selected from N, O, C, and H, as well as metal silicon (metal silicide) and metal silicon compounds (metal silicide compounds) containing metal in silicon and silicon compounds. Examples of metal silicon compounds include materials containing metal, Si, and at least one element selected from N, O, C, and H.

[0116] The thickness of the etching mask film 6 is preferably 3 nm or more in order to form a pattern with high accuracy in the absorber film 4. Moreover, the thickness of the etching mask film 6 is preferably 15 nm or less in order to make the thickness of the resist film 11 thin.

[0117] <Reflection mask 200> This embodiment is a reflective mask 200 provided with an absorber pattern 4a obtained by patterning the absorber film 4 of the reflective mask blank 100 described above.

[0118] As shown in FIG. 3E, the reflective mask 200 of this embodiment has an absorber pattern 4a formed by patterning an absorber film 4 on the multilayer reflective film 2 or on the protective film 3 of the above-mentioned reflective mask blank 100.

[0119] The absorber pattern 4a corresponds to the "thin film having a pattern" in this embodiment. The absorber pattern 4a, which is a predetermined thin film having a pattern, includes the lower layer 42 and the upper layer 44 provided on the lower layer 42, as described above. Therefore, the reflective mask 200 of this embodiment includes the lower layer 42 and the upper layer 44 having a pattern (shown as the lower layer pattern 42a and the upper layer pattern 44a, respectively, in FIG. 3E). In the reflective mask 200 of this embodiment, the lower layer pattern 42a is made of a material having an amorphous structure or a microcrystalline structure, and the crystallinity of the upper layer pattern 44a is higher than that of the lower layer pattern 42a. Therefore, the adhesion between the two layers (the lower layer pattern 42a and the upper layer pattern 44a) of the reflective mask 200 of this embodiment can be improved. In addition, the predetermined thin film (the lower layer pattern 42a and the upper layer pattern 44a) of the reflective mask 200 of this embodiment can have higher durability.

[0120] 3A to 3E are schematic cross-sectional views showing an example of a method for manufacturing the reflective mask 200. The reflective mask blank 100 of the present embodiment described above can be used to manufacture the reflective mask 200 of the present embodiment. An example of the method for manufacturing the reflective mask 200 will be described below.

[0121] First, a reflective mask blank 100 is prepared, which includes a substrate 1, a multilayer reflective film 2, an absorber film 4 having an upper layer 44 and a lower layer 42, and an etching mask film 6. The reflective mask blank 100 may have a protective film 3. Next, a resist film 11 is formed on the etching mask film 6 to obtain a reflective mask blank 100 with the resist film 11 (FIG. 3A). A pattern is written on the resist film 11 by an electron beam lithography device, and a developing and rinsing process is further performed to form a resist pattern 11a (FIG. 3B).

[0122] Next, the etching mask film 6 is dry-etched using the resist pattern 11a as a mask. As a result, the portion of the etching mask film 6 that is not covered by the resist pattern 11a is etched, and the etching mask pattern 6a is formed (FIG. 3C). The resist pattern 11a is removed by a resist stripper.

[0123] Next, the absorber film 4 is dry-etched using the etching mask pattern 6a as a mask. As a result, the portions of the absorber film 4 (upper layer 44 and lower layer 42) that are not covered by the etching mask pattern 6a are etched, and the absorber pattern 4a is formed (FIG. 3D). At this time, the upper layer 44 and the lower layer 42 can be etched using different etching gases. For example, when etching the lower layer 42, etching can be performed using an etching gas that does not damage the protective film 3. Also, when etching the upper layer 44, since the lower layer 42 covers the protective film 3, the protective film 3 is not damaged. In order to further reduce the possibility of the protective film 3 being damaged, an etching gas that has a high etching rate for the upper layer 44 can be used.

[0124] As the etching gas for the absorber film 4 (upper layer 44 and lower layer 42), for example, a fluorine-based gas and / or a chlorine-based gas can be used. As the fluorine-based gas, CF4, CHF3, C2F6, C3F6, C4F6, C4F8, CH2F2, CH3F, C3F8, SF6, F2, etc. can be used. As the chlorine-based gas, Cl2, SiCl4, CHCl3, CCl4, BCl3, etc. can be used. In addition, a mixed gas containing a fluorine-based gas and / or a chlorine-based gas and O2 at a predetermined ratio can be used. These etching gases may further contain an inert gas such as He and / or Ar, as necessary.

[0125] When the upper layer 44 and the lower layer 42 are etched with different etching gases, it is preferable to use the above-mentioned fluorine-based gas as the etching gas for etching the upper layer 44. In this case, it is preferable to use the above-mentioned chlorine-based gas as the etching gas for etching the lower layer 42. Depending on the material of the protective film 3, the above-mentioned chlorine-based gas may be used for etching the upper layer 44, and the above-mentioned fluorine-based gas may be used for etching the lower layer 42.

[0126] Next, after the absorber pattern 4a is formed, the etching mask pattern 6a is removed by dry etching. After removing the etching mask pattern 6a, a wet cleaning process using an acidic or alkaline aqueous solution is performed, thereby obtaining the reflective mask 200 of this embodiment (FIG. 3E).

[0127] The reflective mask 200 thus obtained has a structure in which a multilayer reflective film 2, a protective film 3, and an absorber pattern 4a are laminated on a substrate 1.

[0128] The region (reflective region) where the multilayer reflective film 2 covered by the protective film 3 is exposed has the function of reflecting EUV light. The region where the multilayer reflective film 2 and the protective film 3 are covered by the absorber pattern 4a has the function of absorbing EUV light. The reflective mask 200 of this embodiment can improve the adhesion between the upper layer pattern 44a and the lower layer pattern 42a included in the absorber pattern 4a, so that the film peeling of the reflective mask 200 can be suppressed. In addition, the reflective mask 200 of this embodiment can have higher durability. By using the reflective mask 200 of this embodiment, a reflective region that maintains a high reflectance to EUV light can be obtained, so that a finer pattern can be transferred to a transfer target in EUV lithography.

[0129] <Method of Manufacturing Semiconductor Device> The method for manufacturing a semiconductor device according to this embodiment includes a step of performing a lithography process using an EUV exposure tool 50 by using a reflective mask 200 having a pattern formed on the above-mentioned predetermined thin film (absorber film 4) to transfer the thin film pattern (absorber pattern 4a) to a transfer target on a semiconductor substrate, thereby forming a transfer pattern. Fig. 4 is a schematic diagram showing an example of the EUV exposure tool 50.

[0130] A transfer pattern can be formed on a semiconductor substrate 60 (transfer recipient) by lithography using the reflective mask 200 of this embodiment. This transfer pattern has a shape transferred from the pattern of the reflective mask 200. By forming a transfer pattern on the semiconductor substrate 60 by the reflective mask 200, a semiconductor device can be manufactured.

[0131] In the reflective mask 200 of this embodiment, the adhesion between the upper layer pattern 44a and the lower layer pattern 42a included in the absorber pattern 4a can be improved, so that peeling of the reflective mask 200 can be suppressed. In addition, the reflective mask 200 having higher durability can be obtained. Therefore, by using the reflective mask 200 of this embodiment, a reflective region that maintains a high reflectance to EUV light can be obtained, so that the reflective mask 200 having a high reflectance to EUV light can be obtained. Therefore, by using the reflective mask 200 of this embodiment, a semiconductor device can be made high-density and high-precision.

[0132] A method of transferring a pattern to a semiconductor substrate 60 with a resist by using EUV light will be described with reference to FIG.

[0133] 4 shows a schematic configuration of an EUV exposure tool 50 which is a tool for transferring a transfer pattern onto a resist film 11 formed on a semiconductor substrate 60. In the EUV exposure tool 50, an EUV light generation unit 51, an irradiation optical system 56, a reticle stage 58, a projection optical system 57, and a wafer stage 59 are precisely arranged along the optical path axis of the EUV light. The container of the EUV exposure tool 50 is filled with hydrogen gas.

[0134] The EUV light generation unit 51 has a laser light source 52, a tin droplet generation unit 53, a capture unit 54, and a collector 55. When the high-power carbon dioxide laser from the laser light source 52 is irradiated onto the tin droplets released from the tin droplet generation unit 53, the tin in the droplet state is converted into plasma and EUV light is generated. The generated EUV light is collected by the collector 55 and passes through the irradiation optical system 56 to be incident on the reflective mask 200 set on the reticle stage 58. The EUV light generation unit 51 generates EUV light with a wavelength of, for example, 13.53 nm.

[0135] The EUV light reflected by the reflective mask 200 is reduced by the projection optical system 57 to a pattern image light, usually about 1 / 4, and projected onto the semiconductor substrate 60 (transferred substrate). As a result, a given circuit pattern is transferred to the resist film on the semiconductor substrate 60. A resist pattern can be formed on the semiconductor substrate 60 by developing the exposed resist film. An integrated circuit pattern can be formed on the semiconductor substrate 60 by etching the semiconductor substrate 60 using the resist pattern as a mask. A semiconductor device is manufactured through these steps and other necessary steps. EXAMPLES

[0136] Examples will now be described, but the present invention is not limited to these examples.

[0137] In Examples 1 to 11 and Comparative Examples 1 and 2, a reflective mask blank 100 was produced in which a multilayer reflective film 2, a protective film 3, an absorber film 4 and an etching mask film 6 were formed on a first main surface of a substrate 1. Then, using the reflective mask blanks 100 of Examples 1 to 11 and Comparative Examples 1 and 2, the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 were produced. Note that for each of Examples 1 to 11 and Comparative Examples 1 and 2, a plurality of reflective mask blanks 100 and a plurality of reflective masks 200 were produced. Measurement values ​​such as crystallite size described later are average values ​​of a plurality of samples (specifically, five samples) of each Example and Comparative Example.

[0138] (Reflective mask blank 100) Table 1 shows the composition of the upper layer 44 of the absorber film 4 of the reflective mask blank 100 of the examples and comparative examples, the sputtering gas used in film formation by the sputtering method, the film thickness and the crystalline state. Table 2 shows the composition of the lower layer 42 of the absorber film 4 of the reflective mask blank 100 of the examples and comparative examples, the sputtering gas used in film formation by the sputtering method, the film thickness and the crystalline state. In the crystalline state shown in Tables 1 and 2, C means a crystalline structure, MC means a microcrystalline structure, and A means an amorphous structure. The absorber films 4 of the examples and comparative examples are all phase shift films having a phase shift function. The reflective mask blanks 100 of the examples and comparative examples were produced as follows.

[0139] A SiO2-TiO2-based glass substrate 1, which is a low-thermal expansion glass substrate 1 having a size of 6025 (approximately 152 mm × 152 mm × 6.35 mm) with both the first and second main surfaces polished, was prepared as the substrate 1. In order to obtain a flat and smooth main surface, polishing was performed by a rough polishing process, a precision polishing process, a localized polishing process, and a touch polishing process.

[0140] Next, a multilayer reflective film 2 was formed on the main surface (first main surface) of the substrate 1. The multilayer reflective film 2 formed on the substrate 1 was a periodic multilayer reflective film made of molybdenum (Mo) and silicon (Si) in order to make the multilayer reflective film 2 suitable for EUV light with a wavelength of 13.5 nm. The multilayer reflective film 2 was formed by alternately laminating Mo layers and Si layers on the substrate 1 by ion beam sputtering in a krypton (Kr) gas atmosphere using a Mo target and a Si target. First, a Si film was formed with a thickness of 4.2 nm, and then a Mo film was formed with a thickness of 2.8 nm. This constitutes one period, and 40 periods were laminated in the same manner, and finally a Si film was formed with a thickness of 4.0 nm to form the multilayer reflective film 2.

[0141] Next, a protective film 3 made of a RuRhCr film was formed on the multilayer reflective film 2. The protective film 3 was formed to a thickness of 3.5 nm by DC magnetron sputtering using a RuRhCr target (Ru:Rh:Cr=60at%:30at%:10at%) in an Ar gas atmosphere.

[0142] Next, a predetermined absorber film 4 was formed on the protective film 3. The films were formed in the order of the lower layer 42 and the upper layer 44. Only in Comparative Example 1, a top layer was further formed on the upper layer 44.

[0143] As shown in Tables 1 and 2, the absorber membrane 4 of Examples 1 to 11 and Comparative Examples 1 and 2 has a lower layer 42 and an upper layer 44.

[0144] The lower layer 42 of Examples 1 to 11 and Comparative Example 1 was formed as follows. Table 2 shows the composition of the lower layer 42 of Examples 1 to 11 and Comparative Examples 1 and 2.

[0145] A chromium nitride film (CrN film) was deposited to a thickness of 50 nm on the multilayer reflective film 2 as the lower layer 42 in Examples 1 to 11 and Comparative Example 1. This chromium nitride film was formed by DC magnetron sputtering using a Cr target and a gas in which 10% nitrogen was added to Ar as the sputtering gas.

[0146] The lower layer 42 of Comparative Example 2 was formed as follows.

[0147] A RuZr film was formed as the lower layer 42 of Comparative Example 2. The lower layer 42 of Comparative Example 2 was formed under the following conditions. Target: Ru target, Zr target Sputtering gas: Ar gas Output: 150W (Ru target), 50W (Zr target) Film thickness: 5 nm

[0148] Next, the upper layer 44 was formed on the lower layer 42 of Examples 1 to 11 and Comparative Examples 1 and 2. The upper layer 44 was formed as follows. Table 1 shows the composition of the upper layer 44 of Examples 1 to 11 and Comparative Examples 1 and 2.

[0149] The PtRu film in Example 1 was formed by DC magnetron sputtering using a target containing Pt and Ru and xenon (Xe) as a sputtering gas. Table 1 shows the composition and thickness of the obtained PtRu film.

[0150] The PtRu film of Example 2 was formed by DC magnetron sputtering using a target containing Pt and Ru and argon (Ar) as a sputtering gas. Table 1 shows the composition and thickness of the obtained PtRu film.

[0151] The PtRuN film of Example 3 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ru and a sputtering gas containing xenon and nitrogen.

[0152] The PtRuN film of Example 4 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ru and a sputtering gas consisting of argon and nitrogen. Table 1 shows the composition and thickness of the obtained PtRuN film.

[0153] The PtRuO film of Example 5 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ru and a sputtering gas consisting of argon and oxygen. Table 1 shows the composition and thickness of the obtained PtRuO film.

[0154] The PtRuBN film of Example 6 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt, Ru, and B, and a sputtering gas consisting of xenon and nitrogen. Table 1 shows the composition and thickness of the obtained PtRuBN film.

[0155] The PtRuB film of Example 7 was formed by DC magnetron sputtering using a target containing Pt, Ru, and B and xenon (Xe) as a sputtering gas. Table 1 shows the composition and film thickness of the obtained PtRuB film.

[0156] The RuN film of Example 8 was formed by DC magnetron sputtering (reactive sputtering) using a Ru target and a sputtering gas consisting of xenon (Xe) and nitrogen. Table 1 shows the composition and thickness of the obtained RuN film.

[0157] The PtTa film of Example 9 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ta and a sputtering gas consisting of xenon (Xe). Table 1 shows the composition and thickness of the obtained PtTa film.

[0158] The PtRuB film of Example 10 was formed by DC magnetron sputtering using a target containing Pt, Ru, and B and xenon (Xe) as a sputtering gas. Table 1 shows the composition and thickness of the obtained PtRuB film.

[0159] The PtRuO film of Example 11 was formed by DC magnetron sputtering (reactive sputtering) using a target containing Pt and Ru and a sputtering gas consisting of argon and oxygen. Table 1 shows the composition and thickness of the obtained PtRuO film.

[0160] The TaBN film (upper layer 44) and the TaBO film (top layer) of Comparative Example 1 were formed as follows.

[0161] A tantalum boron alloy nitride (TaBN) film was formed to a thickness of 50 nm as an upper layer 44 on the lower layer 42 of Comparative Example 1. This TaBN film was formed by DC magnetron sputtering using a target containing Ta and B, and 10% nitrogen added to Ar. As shown in Table 1, the composition ratio of this TaBN film was Ta 0.8, B 0.1, and N 0.1. The crystal state of the TaBN film was amorphous.

[0162] On the upper layer 44 of Comparative Example 1, a tantalum boron alloy oxide (TaBO) film was formed to a thickness of 12 nm as a top layer. This TaBO film was formed by DC magnetron sputtering using a target containing Ta and B, and adding 30% oxygen to Ar. Between the formation of the upper layer 44 and the formation of the top layer, the DC power was temporarily stopped, and the gas used for film formation was changed. The composition ratio of the TaBO film of the top layer formed here was Ta 0.4, B 0.1, and O 0.5. The crystal state of the TaBO film of the top layer was amorphous.

[0163] The RuN film (upper layer 44) of Comparative Example 2 was formed as follows.

[0164] The RuN film (upper layer 44) of Comparative Example 2 was formed by reactive sputtering using a Ru target and a nitrogen-containing sputtering gas shown in Table 1. Table 1 shows the composition and thickness of the obtained RuN film. The gas pressure during sputtering was 2.0×10 -1 Pa, and the input power density per target area is 1.7 W / cm 2 The deposition rate was 0.017 nm / sec.

[0165] Next, an etching mask film 6 made of CrN was formed on the absorber film 4 of each of Examples 1 to 11 and Comparative Examples 1 and 2. The CrN film, which is the etching mask film 6, was formed by DC magnetron sputtering (reactive sputtering) using a target containing Cr and a sputtering gas in which 10% nitrogen was added to Ar as the sputtering gas. The composition of the CrN film was Cr:N=90at%:10at%, and the film thickness was 16nm.

[0166] In this manner, the reflective mask blanks 100 of Examples 1 to 11 and Comparative Examples 1 and 2 were manufactured.

[0167] (Crystallite size) The lower layer 42 and the upper layer 44 were formed under the same conditions as those of the absorber film 4 (lower layer 42 and upper layer 44) of the reflective mask blank 100 of Examples 1 to 11 and Comparative Examples 1 and 2, and the crystallite size was measured. As the X-ray diffraction (XRD) method of a predetermined layer, an X-ray diffraction profile was obtained using in-plane measurement (2θχ / φ scan). From the diffraction angle u and half-width β of the obtained X-ray diffraction profile, the crystallite size D was obtained by Scherrer's formula (see Formula 2 below). Note that the half-width β was calculated by performing fitting by the least squares method using the above-mentioned Gaussian function (Formula 1) to the region including the peak with the highest peak intensity at diffraction angles of 30 degrees to 90 degrees in the X-ray diffraction profile, and substituting this σ into the above-mentioned formula (3). D = Kλ / β cos(2 / u) (Equation 2)

[0168] In formula 1, D is the crystallite size (nm), K is the Scherrer constant of 0.9, λ is the wavelength of X-ray (CuKα1) of 0.15405 (nm), and β is the half-width of the diffraction line (rad). The diffraction angle u is a value obtained by the fitting.

[0169] The crystallite size of the lower layer 42 determined as described above was less than 1 nm in all of Examples 1 to 11 and Comparative Example 1. The crystallite size of the lower layer 42 in Comparative Example 2 was 7.5 nm.

[0170] The crystallite size of the upper layer 44 obtained as described above was as follows. That is, the crystallite size of the upper layer 44 of Example 1 was 13.2 nm. The crystallite size of the upper layer 44 of Example 2 was 12.0 nm. The crystallite size of the upper layer 44 of Example 3 was 10.6 nm. The crystallite size of the upper layer 44 of Example 4 was 8.2 nm. The crystallite size of the upper layer 44 of Example 5 was 11.8 nm. The crystallite size of the upper layer 44 of Example 6 was 9.3 nm. The crystallite size of the upper layer 44 of Example 7 was 8.4 nm. The crystallite size of the upper layer 44 of Example 8 was 18 nm. The crystallite size of the upper layer 44 of Example 9 was 15.8 nm. The crystallite size of the upper layer 44 of Example 10 was 4.7 nm. The crystallite size of the upper layer 44 of Example 11 was 3.2 nm. The crystallite size of the upper layer 44 of Comparative Example 1 was less than 1 nm. The crystallite size of the upper layer 44 in Comparative Example 2 was 6.5 nm. In Examples 1 to 11, the difference between the crystallite size of the upper layer 44 and the crystallite size of the lower layer 42 was 2 nm or more. On the other hand, the difference between the crystallite size of the upper layer 44 and the crystallite size of the lower layer 42 in Comparative Examples 1 and 2 was 1 nm or less.

[0171] (film density) The upper layer 44 was formed under the same conditions as the upper layer 44 of the absorber film 4 of the reflective mask blank 100 in Examples 1 to 4, and the film density of the upper layer 44 in Examples 1 to 4 was calculated. The film density was obtained by fitting the X-ray reflectivity obtained by X-ray reflectometry (XRR) to the X-ray reflectivity profile calculated from a thin film model. The film densities of Examples 1 to 4 obtained in this manner were as follows. That is, the film density of the upper layer 44 in Example 1 was 16.4 g / cm 3 The film density of the upper layer 44 in Example 2 was 17.2 g / cm 3 The film density of the upper layer 44 in Example 3 was 11.7 g / cm 3 The film density of the upper layer 44 in Example 4 was 17.1 g / cm 3 It was.

[0172] In addition, from the above-mentioned measurement results of crystallite size and film density, it can be understood that the film density is about the same between the upper layer of Example 2 and the upper layer of Example 4, but the crystallite size is significantly different. In addition, when comparing the upper layer of Example 3 with the upper layer of Example 4, the crystallite size of Example 4, which has a higher film density, is smaller. That is, the upper layer of Example 4, which has a higher film density, has a lower crystallinity than the upper layer of Example 3. Therefore, it is considered that the correlation between crystallite size (crystallinity) and film density is low. In addition, the upper layer of Example 3 and the upper layer of Example 4 have the same composition ratio, but the film density and crystallite size are not the same. Therefore, it is considered that the correlation between the composition ratio of the film and the crystallite size (crystallinity) or film density is also low.

[0173] (Lattice spacing of upper layer 44) The upper layer 44 was formed under the same conditions as the upper layer 44 of the absorber film 4 of the reflective mask blank 100 m in Examples 1 to 11, and the lattice spacing of the upper layer 44 in Examples 1 to 11 and Comparative Examples 1 and 2 was measured. The upper layer 44 was measured by X-ray diffraction (XRD) method, and the lattice spacing of the lattice planes was obtained by Bragg's law from the diffraction angle of the X-ray diffraction profile from the upper layer 44 obtained by the measurement. The lattice spacing of the upper layer 44 in Examples 1 to 11 was all 0.23 nm or less. As described above, the lattice planes can be used that have Miller indices corresponding to the peak with the largest peak intensity or the peak with the largest peak area within the diffraction angle range of 30 degrees to 90 degrees in the X-ray diffraction profile. In Examples 1 to 11, the lattice spacing was obtained using the peak with the largest peak intensity.

[0174] (Reflective mask 200) Next, reflective masks 200 were manufactured using the reflective mask blanks 100 of Examples 1 to 11 and Comparative Examples 1 and 2. The manufacture of the reflective masks 200 will be described with reference to Fig. 3A to Fig. 3E. Five reflective mask blanks 100 were manufactured for each of the Examples and Comparative Examples.

[0175] First, as shown in FIG. 3A, a resist film 11 was formed on the absorber film 4 of the reflective mask blank 100. A desired pattern such as a circuit pattern was then drawn (exposed) on the resist film 11, and the resist film 11 was then developed and rinsed to form a predetermined resist pattern 11a (FIG. 3B). Next, the etching mask film 6 (CrN film) was dry-etched using the resist pattern 11a as a mask to form an etching mask pattern 6a (FIG. 3C). Next, the resist pattern 11a was peeled off by oxygen ashing. Next, the upper layer 44 of the absorber film 4 was dry-etched using the resist pattern 11a as a mask, and the lower layer 42 was dry-etched to form an absorber pattern 4a (FIG. 6D). Then, the etching mask pattern 6a was removed by dry etching (FIG. 6E).

[0176] Finally, wet cleaning was performed using pure water (DIW), thereby manufacturing the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2.

[0177] (Phase difference of phase shift) The absorber pattern 4a of the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 is a pattern of a phase shift film. Therefore, the phase difference between the reflected light from the multilayer reflective film 2 and the reflected light from the absorber film 4 for EUV light was measured for the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2. The phase difference of the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 is 100 degrees or more and 300 degrees or less, and it can be said that they have an appropriate phase shift function.

[0178] (Reflectance of multilayer reflective film 2) When the multilayer reflective film 2 of the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 was irradiated with EUV light, the reflectance (relative reflectance) from the absorber film 4 relative to the reflectance from the multilayer reflective film 2 was higher than 3% and equal to or lower than 30%. Therefore, it can be said that the relative reflectance of the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 is within an appropriate range.

[0179] (Evaluation of Adhesion) When five reflective mask blanks 100 and reflective masks 200 of Examples 1 to 11 were manufactured as described above, no peeling of the film occurred in any of the samples in the process of the reflective mask blank 100 and the manufacturing process of the reflective mask 200. On the other hand, when five reflective mask blanks 100 and reflective masks 200 of Comparative Examples 1 and 2 were manufactured as described above, defects occurred in some samples in all of the comparative examples due to peeling of the absorber film 4. It was possible to identify that the peeling of the absorber film 4 was caused by peeling at the interface between the upper layer 44 and the lower layer 42. Therefore, it can be said that the upper layer 44 and the lower layer 42 of the absorber film 4 of the reflective mask blanks 100 and the reflective masks 200 of Examples 1 to 11 of this embodiment have high adhesion.

[0180] (Durability evaluation) In Examples 1 to 11 and Comparative Examples 1 and 2, a simulation was performed of an exposure transfer image when a defect-free reflective mask 200 was exposed and transferred to a resist film (transfer target) on a semiconductor device using EUV light. When the exposure transfer image obtained in this simulation was verified, the reflectance and phase shift amount were within the ranges that satisfied the design specifications in all of the Examples and Comparative Examples. Furthermore, the reflective masks 200 of Examples 1 to 11 and Comparative Examples 1 and 2 were exposed to EUV light at a cumulative dose of 20 kJ / cm2. 2 The cumulative irradiation dose was 20 kJ / cm. 2 This corresponds to, for example, using the reflective mask 200 about 50,000 times. A simulation was performed on the reflective mask 200 after the intermittent irradiation, in which the reflective mask 200 was exposed to EUV light and transferred onto a resist film (transfer target) on a semiconductor device. When the exposure transfer image obtained by this simulation was examined, it was found that in Examples 1 to 11, the cumulative dose of exposure was 20 kJ / cm 2 The change in reflectance and the change in phase shift amount before and after irradiation with EUV light of 100 kJ / cm2 were within 0.5%. From the above, it can be seen that the reflective mask 200 manufactured from the reflective mask blank 100 of the example of this embodiment has high durability and can withstand exposure transfer with EUV light with a cumulative irradiation amount of, for example, 20 kJ / cm2. 2On the other hand, in Comparative Example 1, similarly to the Example, the cumulative exposure dose was 20 kJ / cm 2 , and the exposure transfer was performed with high accuracy on the resist film on the semiconductor device. 2 When the exposed transferred image after irradiation with EUV light of 20 kJ / cm2 was checked, it was found that some of the reflective masks 200 had a cumulative irradiation dose of 20 kJ / cm2. 2 The change in reflectance and the change in phase shift before and after irradiation with EUV light were greater than 0.5%.

[0181] (Semiconductor device manufacturing) The reflective mask 200 of Examples 1 to 11 was set on an EUV scanner, and EUV exposure was performed on a wafer having a film to be processed and a resist film formed on a semiconductor substrate 60, which was a transfer object. Then, by developing this exposed resist film, a resist pattern could be formed with high accuracy on the semiconductor substrate 56 having the film to be processed formed thereon.

[0182] [Table 1]

[0183] [Table 2] [Explanation of symbols]

[0184] 1 Board 2 Multilayer reflective film 3 Protective film 4. Absorber membrane 4a Absorber pattern 5 Backside conductive film 6 Etching mask film 6a Etching mask pattern 11 Resist film 11a Resist pattern 42 Lower layer 42a Lower Pattern 44 Upper layer 44a Upper layer pattern 50 EUV exposure equipment 51 EUV light generation section 52 Laser light source 53 Tin droplet generation part 54 Capture unit 55 Collector 56 Irradiation optical system 57 Projection optical system 58 Reticle Stage 59 Wafer Stage 60 Semiconductor Substrate 100 Reflective mask blank 200 Reflective mask

Claims

1. A reflective mask blank, A substrate; a multilayer reflective film provided on the substrate; a thin film provided on the multilayer reflective film; the thin film includes a lower layer and an upper layer disposed on the lower layer, the underlayer is made of a material having an amorphous structure or a microcrystalline structure, A reflective mask blank, characterized in that the upper layer has a higher crystallinity than the lower layer.

2. The reflective mask blank according to claim 1 , wherein the lower layer and the upper layer are in contact with each other.

3. 3. The reflective mask blank according to claim 1, wherein the thin film is an absorber film.

4. 3. The reflective mask blank according to claim 1, wherein a difference in crystallite size between the upper layer and the lower layer is 2 nm or more.

5. 3. The reflective mask blank according to claim 1, further comprising an etching mask film formed on said thin film in contact with said thin film, said etching mask film having a lower crystallinity than said upper layer.

6. 3. The reflective mask blank according to claim 1, further comprising a protective film between the multilayer reflective film and the thin film.

7. 3. The reflective mask blank according to claim 1, wherein the lower layer and the upper layer are made of different materials.

8. 3. The reflective mask blank according to claim 1, wherein the upper layer contains at least one selected from Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W, and Rh.

9. 3. The reflective mask blank according to claim 1, wherein the crystallite size of the upper layer is greater than 3 nm.

10. A reflective mask, A substrate; a multilayer reflective film provided on the substrate; a thin film having a pattern provided on the multilayer reflective film, the thin film includes a lower layer and an upper layer disposed on the lower layer, the underlayer is made of a material having an amorphous structure or a microcrystalline structure, A reflective mask, characterized in that the upper layer has higher crystallinity than the lower layer.

11. 11. The reflective mask according to claim 10, wherein the lower layer and the upper layer are in contact with each other.

12. 12. The reflective mask according to claim 10, wherein the thin film is an absorber film.

13. 12. The reflective mask according to claim 10, wherein a difference in crystallite size between the upper layer and the lower layer is 2 nm or more.

14. 12. The reflective mask according to claim 10, further comprising a protective film between the multilayer reflective film and the thin film.

15. 12. The reflective mask according to claim 10, wherein the lower layer and the upper layer are made of different materials.

16. 12. The reflective mask according to claim 10, wherein the upper layer contains at least one selected from the group consisting of Ag, Au, Pt, Pd, Ir, Re, Os, Ru, Ta, Cr, Ti, Nb, Mo, W and Rh.

17. 12. The reflective mask according to claim 10, wherein the crystallite size of the upper layer is greater than 3 nm.

18. 11. A method for manufacturing a semiconductor device, comprising: transferring a pattern onto a transfer target on a semiconductor substrate using a reflective mask having a pattern formed on the thin film of the reflective mask blank according to claim 1, or the reflective mask according to claim 10.

Citation Information

Patent Citations

  • Reflecting mask blank and reflecting type mask and its manufacturing method

    JP2004039884A

  • Reflective mask blank for EUV lithography

    JP2015008265A

  • Reflection type mask blank, reflection type mask, substrate with conductive film, and method for manufacturing semiconductor device

    JP2021128247A

  • Reflection-type mask blank, reflection-type mask and method for manufacturing same, and method for manufacturing semiconductor device

    WO2020184473A1

  • Reflective x-ray mask and manufacture thereof

    JP1996213303A

Cited By

  • Reflective photomask blank, reflective photomask and its manufacturing method

    CN123113231A

  • Reflective photomask blank, reflective photomask, and method for producing same

    EP4841345A1

  • Reflective photomask blank, method for manufacturing a reflective photomask, and method for manufacturing a reflective photomask blank

    JP7910252B1

  • Reflective mask blank, reflective mask, and method for manufacturing reflective mask

    WO2026105668A1

  • Reflective mask blank, method for producing reflective mask blank, reflective mask, method for producing reflective mask

    WO2026110799A1