Lower roofing material

The roof under-roofing material with a low-density polyethylene film and nonwoven fabric laminated adhesive resin layer addresses the issues of weight, uneven layers, and water ingress, offering lightweight, effective waterproofing and easy installation.

JP2024142212APending Publication Date: 2024-10-10SEIREN CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023054282
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing roof under-roofing materials are heavy, difficult to carry, and result in uneven layers leading to poor exterior appearance due to thickness variations, while also posing risks of adhesive failure and water ingress through nail holes.

Method used

A roof under-roofing material comprising a low-density polyethylene film and nonwoven fabric laminated on both sides of a rubber-based adhesive resin layer, with specific thickness and recess depths to ensure lightweight, effective waterproofing, and easy installation.

Benefits of technology

The material provides excellent nail hole waterproofing, is lightweight, and maintains even layers, ensuring high construction quality without adhesive failure or water ingress, while being easy to handle and install.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142212000001_ABST
    Figure 2024142212000001_ABST
Patent Text Reader

Abstract

To provide a lower roofing material that is thin but still provides excellent nail hole waterproofness, is lightweight and easy to carry, has good workability, and hardly creates a step even when overlapped, so that installation quality of an upper roofing material cannot be degraded.SOLUTION: A lower roofing material according to the present invention is a lower roofing material in which a low-density polyethylene film and non-woven fabric are stacked in order on both sides of an adhesive resin layer, and the adhesive resin layer is a rubber-based composition and has the minimum thickness of 90 μm or more, and the depth of the concave portion of the low-density polyethylene film is 5.0 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a roof underlayment material used under a roofing material such as a tile. [Background technology]

[0002] Conventionally, materials used for roof underlayment include roof underlayment made of asphalt-based and rubber-modified asphalt-based compositions. For example, Patent Document 1 is an example of a method using asphalt-based materials. Asphalt-based materials have a certain degree of fluidity in the range of 0 to 70 degrees Celsius, so they have the effect of filling nail holes made by driving nails, and exhibit waterproofing performance. However, in order to exhibit waterproofing performance, the asphalt needs to flow sufficiently to block the nail holes. To achieve this, a thickness is required to ensure the amount of flow. This makes the material heavy and makes it difficult to carry it around. In addition, when overlaying, the step becomes large depending on the thickness, so the roof overlay material cannot be installed neatly, and there is a risk of degrading the appearance quality.

[0003] Also, a method using rubber-based materials with excellent elasticity is known, for example, Patent Document 2. Rubber-based materials have excellent elasticity, so they have the effect of tightening nail holes and exhibit waterproofing performance. However, sufficient thickness is required to exert their elasticity and tighten nail holes. This makes them heavy and makes it difficult to carry them. In addition, when overlaying, the difference in level becomes large depending on the thickness, so the roofing material cannot be installed neatly, and there is a risk of degrading the appearance quality.

[0004] Although the construction method is different, the applicant has proposed Patent Document 3, which discloses a roof underlayment in which a resin layer made of a rubber-based material with adhesive properties is provided under the roof underlayment and directly attached to the roof board. The adhesive and flexibility of the material allow it to adhere to nails and block nail holes, providing waterproof performance, but since the adhesive layer is provided on the surface, there is a risk that the adhesive layer will stick to the building material or fall off due to mistakes during work. In addition, since a sufficient thickness of the adhesive layer is required to adhere to the sheathing boards, it becomes heavy and difficult to carry, and when layering, steps are created depending on the thickness, so the roof overlay material cannot be installed neatly, and the appearance quality may be reduced. In addition, when using the material, the release paper laminated on the adhesive layer must be peeled off before installation, which generates waste.

[0005] The applicant also proposed a roof underlayment that does not use asphalt-based or rubber-based materials, as in Patent Document 4. By providing a layer of water-absorbing and swelling resin, the material is thin and lightweight, yet waterproof against nail holes. However, since it does not absorb water and swell instantly, there is a risk that the underlying plywood may become slightly wet if there is heavy rainfall during construction, and further nail hole waterproofing is required. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-36122 A [Patent Document 2] Japanese Patent Application Publication No. 4-238945 [Patent Document 3] Republished Patent No. 2016 / 027799 [Patent Document 4] Republished Patent No. 2012 / 026532 Summary of the Invention [Problem to be solved by the invention]

[0007] To provide an under-roofing material which, although thin, has excellent nail hole waterproofing properties, is lightweight and easy to carry, has good workability, and is unlikely to cause steps even when layered, so that the construction quality of the over-roofing material is not reduced. [Means for solving the problem]

[0008] The roof underlayment of the present invention is a roof underlayment in which a low-density polyethylene film and a nonwoven fabric are laminated in order on both sides of an adhesive resin layer, wherein the adhesive resin layer is a rubber-based composition, has a minimum thickness of 90 μm or more, and the recess depth of the low-density polyethylene film is 5.0 μm or less.

[0009] In addition, the total weight is 400 to 700 g / m 2 and the total thickness is preferably 500 to 800 μm. Effect of the Invention

[0010] To provide an under-roofing material which is thin but has nail hole waterproofing, is lightweight and easy to carry, and hardly causes a step even when layered, so that the quality of construction of the over-roofing material is not deteriorated. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic cross-sectional view showing a roof underlayment as an example of an embodiment of the present invention. FIG. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a roof underlayment which is another example of an embodiment of the present invention. [Diagram 3] FIG. 2 is an enlarged cross-sectional view of a portion of the adhesive resin layer and the low-density polyethylene film. [Figure 4] FIG. 2 is an enlarged cross-sectional view illustrating the depth of a recess in a low-density polyethylene film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The roof underlayment of the present invention will be described below with reference to the drawings. However, the present invention is not intended to be limited to the configuration described below. In the drawings, multiple layers constituting the roof underlayment of the present invention are shown, but the thickness and size of each layer have been appropriately changed for ease of explanation, and do not accurately reflect the size relationship (scale) of the thickness of each layer in the actual roof underlayment.

[0013] As shown in FIG. 1, the roof underlayment material 1 of the present invention has a low-density polyethylene film 4 and a nonwoven fabric 3 laminated in this order on both sides of an adhesive resin layer 5.

[0014] A low-density polyethylene film 4 is laminated on both sides of the adhesive resin layer 5, and the adhesive resin layer 5 can maintain a moderate thickness without penetrating into the unevenness of the nonwoven fabric 3, so that even when nails are hammered in, the change in thickness of the adhesive resin layer 5 can be minimized, and since the adhesive resin layer adheres sufficiently to the nail, even if the adhesive resin layer is thin, it has an effect of preventing water from entering the nail holes, and a lightweight roof underlayment 1 can be obtained.

[0015] The adhesive resin layer 5 is a resin layer having adhesiveness, and its material may be a rubber-based composition, and is preferably a synthetic rubber that is less affected by temperature and is not easily influenced by the polarity of the adherend. Specific examples include butyl rubber, isoprene rubber, styrene butadiene rubber, polyisobutylene rubber, chloroprene rubber, nitrile rubber, and graft rubber. Among them, butyl rubber is preferable because of its excellent waterproofness, weather resistance, heat resistance, chemical resistance, and adhesion to metals. A tackifier is added to at least one synthetic rubber selected from these groups to form an adhesive resin layer having adhesiveness. Also, known antioxidants, ultraviolet absorbers, flame retardants, coloring pigments, etc. can be added.

[0016] The thickness of the adhesive resin layer 5 is preferably 100 to 300 μm, and more preferably 150 to 250 μm in terms of preventing water from entering nail holes and weight. If it is 100 μm or more, sufficient adhesive strength and the effect of preventing water from entering nail holes even after lamination can be obtained. If it is 300 μm or less, workability is improved with ease of work.

[0017] As shown in FIG. 3, the boundary between the adhesive resin layer 5 and the low-density polyethylene film 4 is affected by the unevenness of the nonwoven fabric 3 and the low-density polyethylene film 4, and has a wavy state with repeated concave and convex portions, but the minimum thickness T of the adhesive resin layer 5 must be 90 μm or more, preferably 100 μm or more, and more preferably 200 μm or more. If it is less than 90 μm, there is a risk that it will not be possible to sufficiently prevent water from entering through the nail holes. The minimum thickness T of the adhesive resin layer 5 can be obtained as follows. Five cross sections of the roof underlayment 1 are observed with an electron microscope (magnification 1000), and the minimum thickness among 10 arbitrary thicknesses of the adhesive resin layer 5 at each observation point is determined as the "minimum thickness", and the average value of the five "minimum thicknesses" is obtained.

[0018] The adhesive strength of the adhesive resin layer 5 is preferably 3.0 N / 10 mm or more, and more preferably 5.0 N / 10 mm or more, since this provides the effect of preventing water from entering the nail holes and makes it easy to adhere strongly to the low-density polyethylene film 4.

[0019] The low-density polyethylene film 4 has convex and concave portions formed therein, and the depth of the concave portion must be 5.0 μm or less. The adhesive resin layer 5 has a sufficient thickness, so that it is easy to obtain a stable nail hole water penetration prevention effect. If it is greater than 5.0 μm, the thickness of the adhesive resin layer 5 is crushed by the convex portions of the low-density polyethylene film 4, and it is difficult to obtain a stable nail hole water penetration prevention. The method of measuring the depth of the concave portion is to observe the cross section of the film with an electron microscope (magnification 1000), measure the height difference between the deepest part of the concave portion and the apex of the adjacent convex portion at 10 points, and obtain the average value. The adjacent convex portion may be on either side of the concave portion to be measured, but all 10 points are convex portions that exist in the same direction. For example, in the case of FIG. 4, the height difference between the concave portion and the apex of the convex portion to the right of the concave portion is measured, and the length indicated by the arrow, for example, L1 and L2, is the measurement portion.

[0020] The depth of the recess is preferably 0.1 to 4.5 μm, more preferably 1.0 to 3.0 μm. If it is 0.1 μm or more, the adhesion between the low-density polyethylene film and the adhesive resin layer is better. If it is 4.5 μm or less, the adhesive resin layer 5 is not crushed and a sufficient thickness can be easily secured.

[0021] The depth of the recess in the low-density polyethylene film 4 before lamination is preferably 10.0 μm or less, so that the adhesive resin layer 5 is not crushed too much even after lamination and integration, and a sufficient thickness is easily obtained.

[0022] The low-density polyethylene film 4 may be embossed in advance, for example, by applying heat and pressure to the film using a metal roll with uneven surfaces, or by applying pressure to the film using a metal roll with uneven surfaces when molding the film, before the film cools and hardens, to emboss the film.

[0023] The low-density polyethylene film 4 may be any film made of low-density polyethylene. 3 It refers to polyethylene having a density of less than 1000 mm. Among them, linear low-density polyethylene is preferred.

[0024] In order to prevent the adhesive resin layer 5 from being torn by the impact of driving a nail into it, it is preferable that the material of the low-density polyethylene film 4 is not destroyed in an Izod impact strength test under the condition of a notch type A of 0.25 mm. Specifically, the density is 0.91 to 0.93 g / m 3 Low density polyethylene and density 0.88~0.93g / m 3 Examples of the linear low density polyethylene include

[0025] The thickness of the low-density polyethylene film 4 is preferably 10 to 100 μm, and more preferably 30 to 80 μm. If the thickness is 10 μm or more, it is preferable because it is easy to obtain strength and is less likely to break during work. If the thickness is 100 μm or less, it is preferable because it is easy to obtain flexibility and is easy to apply according to the roof shape.

[0026] In the present invention, nonwoven fabric 3 is laminated on the outside of each low-density polyethylene film 4, so that waterproofing, strength, and prevention of water seepage through nail holes can be achieved without the adhesive resin adhering to other building materials.

[0027] The material of the nonwoven fabric 3 is preferably composed of polyester, polyamide, or polyolefin filament fibers. In particular, polyester fibers are preferably used in terms of strength and durability. In addition, the types of fibers include spunbond, chemical bond, thermal bond, spunlace, and needle punch. In particular, spunbond is preferable in terms of strength and post-processing.

[0028] The weight of the nonwoven fabric 3 is 30 to 150 g / m 2 is preferable, and more preferably 50 to 100 g / m 2 The weight of the nonwoven fabric 3 is 30 g / m 2 If the weight is 150g / m or more, it is preferable in terms of the ease of obtaining strength. 2 If the thickness is less than this, flexibility is easily obtained, and it is preferable in that construction can be easily performed according to the roof shape.

[0029] Furthermore, it is preferable that an anti-slip resin layer 2 is laminated on the outside of the nonwoven fabric 3, because this allows safe operation. Examples of the anti-slip resin layer 2 include polyolefin resins, polyester resins, acrylic resins, urethane resins, polyvinyl alcohol resins, and epoxy resins. These resins may be used alone or in combination. Among these, polyolefin resins, acrylic resins, and urethane resins are preferred in terms of productivity, processability, and strength.

[0030] To enhance the anti-slip effect, additives can be added to the anti-slip resin layer 2, such as inorganic powders, mineral powders, and thermally expandable microcapsules containing inert gases that can form fine irregularities, as well as fine powdered rubber and urethane beads that improve friction resistance. These additives can be used alone or in combination.

[0031] It is also preferable to add a water repellent to the anti-slip resin layer 2. By adding a water repellent, the effect of preventing water from seeping into the nail holes is improved.

[0032] As shown in Fig. 2, it is more preferable to add a film 6 to the outside of the nonwoven fabric 3 on the side that will be the building material during construction, since even if water seeps into the nail holes, the nonwoven fabric will retain the water and prevent it from spreading. Examples of materials for the film 6 include polyolefin resins, polyester resins, polyamide resins, and polyurethane resins. Among these, polyethylene resins are preferable in terms of toughness, flexibility, productivity, processability, and economy, and low-density polyethylene resins are more preferable.

[0033] A method for producing the roof underlayment material 1 of the present invention will be described.

[0034] In the manufacturing method of this embodiment, a method of first laminating a nonwoven fabric 3 and a low-density polyethylene film 4 is exemplified. Examples of the lamination method include a dry lamination method, a wet lamination method, a T-die lamination method, and a hot melt lamination method, and the T-die lamination method, which can perform film formation and lamination simultaneously, is preferable.

[0035] Next, the film sides of the laminated nonwoven fabric 3 and low-density polyethylene film 4 are laminated together with an adhesive resin layer 5. For forming the adhesive resin layer 5, a calendar method in which the resin is passed between heated rolls to gradually roll and form into a sheet is preferred, because this allows forming and laminating of the resin layer to be performed simultaneously.

[0036] After lamination by the calendar method, the outer nonwoven fabric 3 is coated to form an anti-slip resin layer 2. The coating method is not particularly limited, but may be a method of solidifying the resin by heat treatment using a gravure roll method or the like.

[0037] The order of lamination may be changed as appropriate without interfering with the concept of the present invention. If necessary, a metal film layer such as aluminum may be further laminated to improve the heat shielding effect and durability, or an inorganic fiber layer such as a woven or nonwoven fabric containing glass fiber may be laminated to improve strength.

[0038] The peel adhesion strength between the adhesive resin layer 5 of the roof underlayment 1 and the low-density polyethylene film 4 is preferably 0.25 kN / m or more. If it is less than 0.25 kN / m, there is a risk of peeling during work depending on the conditions, and there is a risk that the waterproofing of the nail holes will not be achieved. The peel adhesion strength is measured in accordance with JIS K6854-3 Adhesives - Test method for peel adhesion strength - Part 3: T-type peel.

[0039] The total thickness of the roof underlayment 1 is preferably 500 to 800 μm, and more preferably 500 to 700 μm in terms of preventing water ingress through nail holes and weight. If it is 500 μm or more, it is possible to obtain sufficient effects in terms of preventing water ingress through nail holes and strength even after layering. Also, if it is 800 μm or less, it is difficult for steps to be created even when layering, improving workability.

[0040] The total weight of the roof underlayment 1 is 400-700g / m 2 It is preferable that the thickness is in the range of 400 g / m 2 If it is more than 700g / m, it is easy to waterproof the nail holes and maintain the strength. 2 If it is below this, it will be lightweight and not heavy, making it easy to carry. EXAMPLES

[0041] The roof underlayment material of the present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these. The physical properties in the examples and comparative examples were measured and evaluated by the following methods.

[0042] <Adhesive strength of adhesive resin layer> According to JIS Z0237 Adhesive strength 10.4.1 Method 1: 180° peel adhesive strength against test plate, adhesive strength was measured using a test piece made of a 50μm thick polyethylene terephthalate film with an adhesive resin layer formed on it. Note that the test plate used was a SUS304 steel plate with a BA surface finish, and the measurement conditions were a test piece width of 10mm, temperature of 23℃, and humidity of 50%.

[0043] <Minimum thickness of adhesive resin layer> Five cross sections of the roof underlayment were observed using an electron microscope (magnification 1000), and the thickness of the adhesive resin layer was measured at 10 random locations at each observation location. The smallest thickness among these measurements was determined as the "minimum thickness," and the average value of the five "minimum thicknesses" was calculated.

[0044] <Film impact test> The film was evaluated according to JIS K7110 3.2 Izod impact strength of notched test piece, and only the presence or absence of breakage was confirmed. The measurement conditions were test piece length 80 mm, width 10 mm, thickness 4 mm, notch type A 0.25 mm, temperature 23°C, humidity 50%, hammer capacity 1.0 J, and impact speed 3.5 m / s.

[0045] <Depth of recess on film surface> The cross section of the roof underlayment film was observed under an electron microscope (magnification 1000), and the height difference between the deepest point of the depression and the apex of the adjacent depression was measured at 10 points and the average value was calculated.

[0046] <Peel adhesive strength> According to JIS K6854-3 Adhesives - Peel adhesion strength test method - Part 3: T-type peeling, the adhesive resin layer and low-density polyethylene film were bonded together in a T-shape to measure the average peel strength between the adhesive resin layer and the low-density polyethylene film at five points and calculate the average value. The measurement conditions were a width of 25 mm, a temperature of 23°C, and a humidity of 50%.

[0047] <Nail hole waterproofness> In accordance with the 7.8 nail hole waterproofing standard of the Asphalt Waterproofing Subcommittee of the Japan Waterproofing Materials Association, "Modified Asphalt Roofing Underlayment Material," tests were performed with a water head of 150 mm height and ring nails (roof nail 32KL32TZ, manufactured by KM Corporation) and the number of wet spots on the plywood surface was counted. If 7 or more of the 10 test pieces were not wet, the evaluation was rated as ◯, and if there were less than 7, it was rated as ×.

[0048] <Thickness> The thickness of each layer was measured using a thickness measuring instrument G-6 manufactured by Ozaki Manufacturing Co., Ltd. (measurement terminal anvil Φ5 flat, measuring force 1.8 N or less).

[0049] [Example 1] First, a nonwoven fabric and a low-density polyethylene film are laminated. A polyester spunbond nonwoven fabric (Toray Industries, Inc., Axstar G2050-1SBKO, basis weight 50 g / m 2 ) on a low-density polyethylene film (Hayashi Ichiji Co., Ltd., a film with embossed leather grain, natural L-LDPE, recess depth 3.2 μm, thickness 50 μm, density 0.91 to 0.93 g / m 3 The laminate (which does not break in an Izod impact test) was laminated with polyethylene pellets (Petrothene 212, manufactured by Tosoh Corporation) via an adhesive layer having a thickness of 20 μm by extrusion lamination to obtain laminate A. Next, a polyester spunbond nonwoven fabric (Toray Industries, Inc., Axstar G2070-1S, basis weight 70 g / m 2 ) was laminated with the same low-density polyethylene film and polyethylene pellets as above by extrusion lamination via an adhesive layer having a thickness of 20 μm, thereby obtaining laminate B.

[0050] Next, the laminate A and the laminate B are laminated with an adhesive resin sandwiched between the film sides of each laminate. The adhesive resin was prepared as follows: 100 parts by weight of butyl rubber (Mooney viscosity ML1+8 (125°C) 32, specific gravity 0.92) was mixed with tackifier (aliphatic hydrocarbon resin, softening point 97°C, weight average molecular weight Mw1310) 30 parts by weight, softener (higher fatty acid ester, melting point 60°C, ash content 0.3% or less, specific gravity 0.92) 10 parts by weight, filler (heavy calcium carbonate, average particle size 3.2μm, apparent density 0.40) 30 parts by weight, vulcanizing agent (phenol-formaldehyde resin, softening point 86°C, ash content 0.1% or less) 2 parts by weight, reinforcing agent (carbon black, average particle size 43nm, ash content 0.2%, bulk density 380kg / m 3 ) were kneaded together to obtain an adhesive resin. The adhesive strength of the adhesive resin was 5.3 N / 10 mm. The obtained adhesive resin was formed into a sheet by a calendar method, and the adhesive resin was sandwiched between the film-side surfaces of the laminate A and the laminate B to obtain a laminate. The thickness of the adhesive resin layer was 200 μm.

[0051] The resin for the anti-slip resin layer was applied to both sides of the laminate, i.e., both nonwoven fabric sides, by gravure coating to a solid content of 5 g / m 2 The resin was applied so that it adhered to the roof, forming an anti-slip resin layer, and a roof underlayment like that shown in Figure 1 was obtained. The resin for the anti-slip resin layer was prepared by adding 3 parts by weight of an isocyanate-based crosslinking agent (NE crosslinking agent, Dainichiseika Chemicals Mfg. Co., Ltd.), 0.3 parts by weight of a crosslinking accelerator (Crisbon Accel T81, DIC Corporation), 22 parts by weight of a thermal blowing agent made of acrylic resin (Matsumoto Microsphere F-36D, Matsumoto Yushi Seiyaku Co., Ltd.), and 1.7 parts by weight of a fluorine-based water repellent (Daikin Corporation, Daifree FB-961) to 100 parts by weight of an acrylic resin (Paraclon W248E, Negami Chemicals Co., Ltd.). The measurement and evaluation results of each physical property are shown in Table 1.

[0052] [Example 2] The low-density polyethylene films of laminate A and laminate B were embossed to form pyramidal depressions on the surface, with the depression depth of 1.9 μm (Hayashi Ichiji Co., Ltd., High-Sided Film Natural L-LDPE, thickness 50 μm, density 0.91 to 0.93 g / m). 3A roof underlayment was obtained by processing in the same manner as in Example 1, except that the embossed surface was made to be the adhesive resin layer laminated on the embossed surface side. The measurement results and evaluation results of each physical property are shown in Table 1.

[0053] [Example 3] The low-density polyethylene films of Laminate A and Laminate B were embossed to form pyramidal depressions on the surface, with the depression depth of 9.4 μm (Hayashi Ichiji Co., Ltd., High-Sided Film Natural L-LDPE, thickness 50 μm, density 0.91 to 0.93 g / m). 3 A roof underlayment was obtained by processing in the same manner as in Example 1, except that the embossed surface was made to be the adhesive resin layer laminated on the embossed surface side. The measurement results and evaluation results of each physical property are shown in Table 1.

[0054] [Example 4] The amount of the tackifier in the adhesive resin was changed to 15 parts by weight, and the mixture was kneaded to obtain an adhesive resin. The adhesive strength of the adhesive resin was 3.7 N / 10 mm. Except for the above, a roof underlayment was obtained by processing in the same manner as in Example 1. The measurement results and evaluation results of each physical property are shown in Table 1.

[0055] [Example 5] The amount of the tackifier in the adhesive resin was changed to 40 parts by weight, and the amount of the softener was changed to 15 parts by weight, and the mixture was kneaded to obtain an adhesive resin. The adhesive strength of the adhesive resin was 8.6 N / 10 mm. Except for the above, a roof underlayment was obtained by processing in the same manner as in Example 1. The measurement results and evaluation results of each physical property are shown in Table 1.

[0056] [Example 6] Except for changing the thickness of the adhesive resin layer to 100 μm, a roof underlayment was obtained by processing in the same manner as in Example 1. The measurement results and evaluation results of each physical property are shown in Table 1.

[0057] [Example 7] After obtaining an integrated laminate in the same manner as in Example 1, a low-density polyethylene film (manufactured by Hayashi Ichiji Co., Ltd., a film with a leather-grain embossed surface, natural L-LDPE, recess depth 4.2 μm, thickness 50 μm, density 0.91 to 0.93 g / m) was applied to the surface of the laminate on the side B. 3 , which does not break in the Izod impact test) was laminated with polyethylene pellets (Petrothene 212, manufactured by Tosoh Corporation) via an adhesive layer of 20 μm thickness using the extrusion lamination method to obtain a roof underlayment as shown in Figure 2. The measurement results and evaluation results of each physical property are shown in Table 1.

[0058] [Comparative Example 1] A roof underlayment was obtained in the same manner as in Example 1, except that an adhesive resin layer was formed directly on the nonwoven fabric surface without laminating a low-density polyethylene film. The measurement results and evaluation results of each physical property are shown in Table 1. The peel adhesion strength was measured using a sample in which the nonwoven fabric and the low-density polyethylene film were bonded in a T-shape.

[0059] [Comparative Example 2] The low-density polyethylene films of laminate A and laminate B were embossed to form pyramidal depressions on the surface, with the depression depth being 16.3 μm (Hayashi Ichiji Co., Ltd., High-Sided Film Natural L-LDPE, thickness 50 μm, density 0.91 to 0.93 g / m). 3 A roof underlayment was obtained by processing in the same manner as in Example 1, except that the embossed surface was made to be the adhesive resin layer laminated on the embossed surface side. The measurement results and evaluation results of each physical property are shown in Table 1.

[0060] [Table 1]

[0061] As shown in Table 1, the roof underlayment according to the embodiment was lightweight and thin, but excellent in nail hole waterproofing and peel adhesive strength. In contrast, the roof underlayment according to the comparative example was evaluated as poor in nail hole waterproofing and peel adhesive strength. [Explanation of symbols]

[0062] 1. Roof underlayment 2 Anti-slip resin layer 3. Nonwoven fabric 4. Low density polyethylene film 5 Adhesive resin layer 6. Film L1, L2 measurement section

Claims

1. A roof underlayment material in which a low-density polyethylene film and a nonwoven fabric are laminated in order on both sides of an adhesive resin layer, The adhesive resin layer is a rubber-based composition and has a minimum thickness of 90 μm or more; The low-density polyethylene film has a recess depth of 5.0 μm or less.

2. Total weight is 400-700g / m 2 The roof underlayment material according to claim 1, wherein the total thickness is 500 to 800 μm.

Citation Information

Patent Citations

  • Waterproof sheet

    JP1992238945A

  • Roof underlayment material

    JP2004036122A