Resin composition and method for forming protective film

A resin composition with specific components addresses corrosion issues in touch panel sensors by providing excellent sweat resistance and adhesion to metal and ITO substrates, enhancing the durability of touch panel protective films.

JP2024142270AInactive Publication Date: 2024-10-10MITSUBISHI PAPER MILLS LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023054400
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing touch panel sensors face issues with corrosion from moisture and salt, leading to increased electrical resistance and wire breakage, and require a protective film that balances sweat resistance and adhesion to metal and ITO substrates.

Method used

A resin composition comprising specific components such as a polymer with acid groups, a photopolymerization initiator, a bifunctional polymerizable compound with hydroxyl groups, and epoxy (meth)acrylate, which forms a protective film that provides excellent sweat resistance and adhesion to metal and ITO substrates.

Benefits of technology

The composition achieves a well-balanced combination of sweat resistance and adhesion, making it suitable for protective films in touch panels, particularly those with metal and ITO substrates, while maintaining durability and functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142270000001
    Figure 2024142270000001
  • Figure 2024142270000002
    Figure 2024142270000002
Patent Text Reader

Abstract

To provide a novel composition.SOLUTION: A composition comprises (A) a polymer with an acid radical, (B) a photopolymerization initiator, (C) a bifunctional polymerizable compound with a hydroxy group, and (D) an epoxy (meth)acrylate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition [for example, a resin composition (photosensitive resin composition) that can be used for a protective film for a touch panel, etc.], and a method for forming a film (for example, an electrode protective film for a touch panel) using the resin composition. [Background technology]

[0002] Touch panel sensors are widely used as an input means for displays in electronic devices such as personal digital assistants (PDAs), notebook PCs, office automation equipment, medical equipment, and car navigation systems.

[0003] Touch panel sensors are classified into optical type, ultrasonic type, resistive film type, surface type electrostatic capacitance type, projected type electrostatic capacitance type, etc. according to the method of position detection, and the resistive film type and projected type electrostatic capacitance type are preferably used in the above-mentioned display applications. The resistive film type touch panel sensor has a structure in which two light-transmitting electrodes having a light-transmitting conductive layer on a support are used, and these light-transmitting electrodes are arranged opposite each other via a dot spacer. By applying a force to one point of the touch panel sensor, the light-transmitting conductive layers come into contact with each other, and the voltage applied to each light-transmitting conductive layer is measured through the other light-transmitting conductive layer, thereby detecting the position where the force is applied. On the other hand, the projected type electrostatic capacitance type touch panel sensor uses one light-transmitting electrode having two layers of light-transmitting conductive layers, or two light-transmitting electrodes having one layer of light-transmitting conductive layer, and detects the change in capacitance between the light-transmitting conductive layers when a finger or the like is brought close, thereby detecting the position where the finger is brought close. The latter is particularly popular in smartphones, tablet PCs, etc., as it has no moving parts and is highly durable, as well as being capable of detecting multiple points simultaneously.

[0004] In a projected capacitive touch panel sensor, a sensor section made up of a plurality of sensors obtained by patterning a light-transmitting conductive layer on a support is arranged, thereby enabling simultaneous detection of multiple points and detection of moving points. In order to take out the change in capacitance detected by this sensor section as an electric signal to the outside, a peripheral wiring section made up of a plurality of peripheral wirings that electrically connects all the sensors of the light-transmitting electrode and a terminal section made up of a plurality of terminals provided to take out the electric signal to the outside is provided. Usually, the light-transmitting conductive layer is located on the display, and the peripheral wiring section and the terminal section are located outside the display, in the so-called frame section. In the prior art, the light-transmitting conductive layer is generally formed of an indium-tin oxide (ITO) conductive film, and the peripheral wiring section and the terminal section are generally formed of metals such as gold, silver, copper, nickel, and aluminum.

[0005] Such touch panel sensors have a problem that if corrosive components such as moisture or salt adhere to the sensor when the fingertip touches the sensor, the optically transparent conductive layer and metal wiring corrode, causing an increase in electrical resistance and disconnection. In order to prevent such corrosion of the optically transparent conductive layer and metal wiring, a projection type touch panel sensor has been disclosed that has a cured photosensitive resin layer as a protective film on the touch panel sensor (e.g., Patent Documents 1 and 2).

[0006] In addition, in the manufacturing process of a touch panel, the touch panel may be curved or may come into contact with a transport roll, resulting in a load being applied. In particular, in a touch panel sensor using a flexible resin film substrate as an electrode substrate for a touch panel, the load on the protective film increases with the curvature of the touch panel sensor, and peeling or cracking may occur. Therefore, a protective film that has high adhesion to an ITO substrate and a metal substrate and can withstand curvature is required. For example, JP 2019-207321 A (Patent Document 3) describes a photosensitive resin composition containing (A) an alkali-soluble polymer having a specific acidic group, (B) a specific photopolymerizable compound, and (C) a photopolymerizable initiator, as a photosensitive resin composition having good adhesion to a conductor substrate and film strength after exposure after development. However, it has been difficult to obtain a protective film that has an excellent balance between the resistance to corrosive components such as moisture and salt, so-called sweat resistance, and adhesion to a metal substrate and an ITO substrate. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2013 / 84883 Brochure [Patent Document 2] JP 2018-77490 A [Patent Document 3] JP 2019-207321 A Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a novel resin composition (photosensitive resin composition) (useful for forming, for example, a protective film, etc.).

[0009] Another object of the present invention is to provide a resin composition that can realize (express) excellent sweat resistance (resistance to corrosive components such as moisture and salt).

[0010] Another object of the present invention is to provide a resin composition that can realize (express) excellent adhesion to a substrate [for example, an inorganic substrate such as a metal (copper, etc.) or a metal oxide (ITO, etc.)].

[0011] Yet another object of the present invention is to provide a resin composition that can achieve a good balance between sweat resistance and adhesion to a substrate (e.g., an inorganic substrate such as a metal (e.g., copper) or a metal oxide (e.g., ITO)). [Means for solving the problem]

[0012] As a result of extensive research, the present inventors have found that a novel composition (photosensitive resin composition) can be obtained by combining specific components, and that such a composition can, in one embodiment, realize (express) excellent sweat resistance and excellent adhesion to a substrate (e.g., a substrate such as copper or ITO), and in another embodiment, can achieve a good balance between such sweat resistance and adhesion to a substrate, and have completed the present invention.

[0013] That is, the present invention relates to the following inventions, etc. [1] A composition comprising (A) a polymer having an acid group, (B) a photopolymerization initiator, (C) a bifunctional polymerizable compound having a hydroxyl group, and (D) an epoxy (meth)acrylate. [2] The composition according to [1], wherein (A) the polymer having an acid group is a polymer having a methacrylate as a polymerization component. [3] The composition according to [1] or [2], wherein the polymerization component of the polymer having an acid group (A) contains 60 mass% or more of methyl methacrylate. [4] The composition according to any one of [1] to [3], wherein (C) the bifunctional polymerizable compound having a hydroxyl group is a (meth)acrylate (compound). [5] (D) The composition according to any one of [1] to [4], wherein the epoxy (meth)acrylate includes an acid-modified epoxy (meth)acrylate. [6] (C) The ratio of the bifunctional polymerizable compound having a hydroxyl group to the polymer having an acid group (A) The composition according to any one of [1] to [5], which is 3 parts by mass or more per 100 parts by mass. [7] The composition according to any one of [1] to [6], wherein the ratio of the (D) epoxy (meth)acrylate is 3 parts by mass or more per 100 parts by mass of the (A) polymer having an acid group. [8] The composition according to any one of [1] to [7], wherein the ratio of the (C) bifunctional polymerizable compound having a hydroxyl group is 0.05 to 20 parts by mass per 1 part by mass of the (D) epoxy (meth)acrylate. [9] A composition comprising (A) a polymer having an acid group, (B) a photopolymerization initiator, (C) a bifunctional polymerizable compound having a hydroxyl group, and (D) an epoxy(meth)acrylate, (A) the polymerization component of the polymer having an acid group contains 60 mass% or more of methyl methacrylate, (C) the bifunctional polymerizable compound having a hydroxyl group includes a di(meth)acrylate of a polyol having three or more hydroxyl groups, (D) the epoxy (meth)acrylate includes an acid-modified epoxy (meth)acrylate; (C) The ratio of the bifunctional polymerizable compound having a hydroxyl group to the polymer having an acid group (A) 5 parts by mass or more per 100 parts by mass, The ratio of the (D) epoxy (meth)acrylate is 5 parts by mass or more based on 100 parts by mass of the (A) polymer having an acid group, A composition, wherein the ratio of (C) the bifunctional polymerizable compound having a hydroxyl group is 0.1 to 10 parts by mass per 1 part by mass of (D) the epoxy (meth)acrylate.

[10] The composition according to any one of [1] to [9], which is for use in a protective film for a touch panel.

[11] A laminate comprising a support (a resin film such as PET) and a resin layer laminated on the support, the resin layer being composed of a composition according to any one of [1] to

[10] .

[12] The laminate according to

[11] , further comprising a cover film on the resin layer.

[13] A substrate comprising a substrate and a protective film (protective layer, resin layer) formed on the substrate, the protective film being formed from the composition (cured product (light) of the composition) according to any one of [1] to [9].

[14] The protective substrate according to

[13] , wherein the substrate is an electrode substrate having a metal layer containing at least one metal selected from copper and ITO.

[15] The protective substrate according to

[13] or

[14] , which is a member of a touch panel (or a touch panel).

[16] A method for forming a protective film [protective film having openings (openings corresponding to the non-exposed parts)] on the substrate by laminating (attaching) a resin layer made of the composition according to any one of [1] to [9] on the substrate, exposing the resin layer (imagewise exposing), and removing the non-exposed parts with an alkaline developer.

[17] The method according to

[16] , wherein the substrate is an electrode substrate having a metal layer containing at least one selected from copper and ITO, and a protective film is formed on at least the metal layer (at least a part of the metal layer). Effect of the Invention

[0014] According to one aspect of the present invention, a novel resin composition (photosensitive resin composition) can be provided. Such a composition can be used, for example, to form a protective film (for example, a protective film for a touch panel).

[0015] In another embodiment of the present invention, a resin composition capable of realizing (expressing) excellent sweat resistance (resistance to corrosive components such as moisture and salt) can be provided.

[0016] In another embodiment of the present invention, a resin composition capable of realizing (expressing) excellent adhesion to a substrate (for example, an inorganic substrate such as a metal (copper, etc.) or a metal oxide (ITO, etc.)) can be provided.

[0017] In yet another aspect of the present invention, a resin composition can be provided that can achieve a good balance between sweat resistance and adhesion to a substrate (e.g., an inorganic substrate such as a metal (e.g., copper) or a metal oxide (e.g., ITO)).

[0018] Such a composition is particularly suitable for applications requiring sweat resistance and adhesion (particularly a balance between these), such as protective films for touch panels (eg, electrodes for touch panels) (protective films for touch panels). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will be described in detail below. <Composition> The composition (resin composition) of the present invention contains specific components.

[0020] [(A) Polymer having an acid group (component (A))] The composition of the present invention contains (A) a polymer having an acid group.

[0021] In the polymer having an acid group, examples of the acid group include a carboxy group, a sulfonic acid group (sulfuric acid group, sulfo group), a phosphoric acid group, and an acid anhydride group, and the like, and the carboxy group and the acid anhydride group (particularly, the carboxy group) are preferred. Therefore, the polymer having an acid group may have at least one selected from at least a carboxy group and an acid anhydride group (particularly, at least a carboxy group).

[0022] In the polymer having an acid group, the form in which the acid group is contained is not particularly limited. For example, an acid group may be introduced into a polymer (such as the polymer described above) (for example, a polymer having a functional group A is reacted with a compound having an acid group and a functional group B capable of reacting with and bonding to the functional group A), a compound having an acid group (monomer, etc.) may be introduced as a polymerization component (raw material for the polymer), or a combination of these may be introduced.

[0023] Typically, the polymer having an acid group may have a compound having an acid group as a polymerization component.

[0024] The polymer having an acid group may be any of a thermoplastic resin, a curable resin (such as a thermosetting resin, a photocurable resin, or a cured product thereof), and the like.

[0025] Specific examples of the polymer having an acid group (base polymer of the polymer having an acid group) include organic polymer compounds (polymers) such as (meth)acrylic resins, styrene resins, epoxy resins, amide resins, amide epoxy resins, alkyd resins, and phenolic resins.

[0026] The polymer having an acid group may be used alone or in combination of two or more kinds.

[0027] Among them, it is preferable to use a (meth)acrylic resin from the viewpoint of solubility in an alkaline developer, etc. Therefore, the polymer having an acid group may contain at least a (meth)acrylic resin.

[0028] Examples of (meth)acrylic resins include those having (meth)acrylate ((meth)acrylic acid ester) as a polymerization component, and in particular, those having (meth)acrylate and a monomer having an acid group (e.g., ethylenically unsaturated carboxylic acid) as a polymerization component (copolymerized) [(meth)acrylic polymer]. In addition, the polymer may have other monomers (e.g., other monomers having copolymerizable ethylenically unsaturated groups) as a polymerization component (copolymerized).

[0029] Examples of the (meth)acrylate include aliphatic (meth)acrylates [e.g., alkyl (meth)acrylates, cycloalkyl (meth)acrylates], aromatic (meth)acrylates [e.g., aryl (meth)acrylates, aralkyl (meth)acrylates], and the like.

[0030] The (meth)acrylate [e.g., alkyl (meth)acrylate, etc.] may have a substituent (including those having a substituent). Examples of the substituent include a hydroxy group, a mercapto group, an amino group (including substituted amino groups such as an alkylamino group), an epoxy group, and a halogen atom (e.g., a fluorine atom, a chlorine atom, etc.). The (meth)acrylate may have one or more substituents.

[0031] Representative (meth)acrylates include, for example, alkyl (meth)acrylates [e.g., methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, etc. 1-30 Alkyl (meth)acrylate (e.g., C 1-20 alkyl(meth)acrylates)], cycloalkyl(meth)acrylates [e.g., cyclohexyl(meth)acrylate, etc. 4-10Cycloalkyl (meth)acrylates], aryl (meth)acrylates [e.g., phenyl (meth)acrylate, etc.], aralkyl (meth)acrylates [e.g., benzyl (meth)acrylate, etc.], hydroxy group-containing (meth)acrylates [e.g., hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate], cyclic ether group-containing (meth)acrylates [e.g., glycidyl (meth)acrylate, tetrahydrofuran, etc.], n-butyl (meth)acrylate, etc.], amino group (including substituted amino group)-containing (meth)acrylate [for example, N-substituted amino alkyl (meth)acrylate such as 2-(dimethylamino)ethyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, etc.], halogen atom-containing (meth)acrylate [for example, halo alkyl (meth)acrylate such as 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, etc.], etc. Among them, aliphatic (meth)acrylates such as methyl (meth)acrylate, n-butyl (meth)acrylate, etc. [for example, alkyl (meth)acrylates], etc. are preferred, and it is particularly preferred that the (meth)acrylate contains methyl (meth)acrylate and butyl (meth)acrylate.

[0032] The polymerization component may contain a single (meth)acrylate or a combination of two or more (meth)acrylates.

[0033] Typically, the (meth)acrylic resin [(meth)acrylic polymer] preferably contains at least methacrylate (e.g., an aliphatic methacrylate such as an alkyl methacrylate) as a polymerization component, and more preferably contains alkyl methacrylate [particularly, methyl methacrylate (methyl methacrylate)] as a polymerization component.

[0034] When methacrylate is used as a polymerization component, the proportion of the methacrylate [e.g., alkyl methacrylate (methyl methacrylate, etc.)] relative to the total polymerization components may be selected from a range of about 1 mass % or more (e.g., 5 mass % or more), and may be about 10 mass % or more (e.g., 20 mass % or more), preferably 30 mass % or more (e.g., 40 mass % or more), and more preferably 50 mass % or more (e.g., 55 mass % or more). From the viewpoint of exceptionally excellent sweat resistance, adhesion, etc., it is preferably 60 mass % or more (e.g., 65 mass % or more, 70 mass % or more).

[0035] When methacrylate is used as a polymerization component, the upper limit of the proportion of methacrylate [e.g., alkyl methacrylate (methyl methacrylate, etc.)] to all polymerization components can be appropriately selected depending on the types of other polymerization components, and is not particularly limited, but may be, for example, 99 mass% or less (e.g., 98 mass% or less), preferably 97 mass% or less (e.g., 95 mass% or less), and more preferably 93 mass% or less (e.g., 90 mass% or less).

[0036] In addition, these ranges (lower limit and upper limit) may be appropriately combined to select a range (for example, 1 to 99 mass %, 50 to 95 mass %, etc.; the same applies to the following range descriptions).

[0037] Furthermore, when methacrylate is used as a polymerization component, the proportion of the methacrylate [e.g., alkyl methacrylate (methyl methacrylate, etc.)] relative to the total (meth)acrylate may be selected from a range of about 1 mass% or more (e.g., 5 mass% or more), and may be 10 mass% or more (e.g., 20 mass% or more), preferably 30 mass% or more (e.g., 40 mass% or more), more preferably 50 mass% or more (e.g., 55 mass% or more), and particularly preferably 60 mass% or more (e.g., 65 mass% or more, 70 mass% or more), etc.

[0038] When methacrylate is used as a polymerization component, the upper limit of the proportion of methacrylate [e.g., alkyl methacrylate (methyl methacrylate, etc.)] to all (meth)acrylates can be appropriately selected depending on the types of other polymerization components, and is not particularly limited. For example, it may be 100 mass% or less than 100 mass% (e.g., 99 mass% or less, 98 mass% or less, 97 mass% or less, 95 mass% or less, 93 mass% or less, 90 mass% or less), etc.

[0039] Examples of monomers having an acid group (e.g., ethylenically unsaturated carboxylic acid) include unsaturated monocarboxylic acids (e.g., acrylic acid, methacrylic acid, crotonic acid, etc.), unsaturated polycarboxylic acids (e.g., unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, etc.), acid anhydrides (e.g., unsaturated polycarboxylic anhydrides such as maleic anhydride), partial esters of unsaturated polycarboxylic acids (e.g., half esters of unsaturated dicarboxylic acids), etc.

[0040] The polymerization components may contain a single monomer having an acid group, or a combination of two or more kinds of monomers having an acid group.

[0041] When a monomer having an acid group is used as a polymerization component, the ratio of the monomer having an acid group to all the polymerization components varies depending on the type of acid group, and may be selected from a range of about 0.1 mass% or more (e.g., 0.3 mass% or more), for example, 0.5 mass% or more (e.g., 1 mass% or more), preferably 2 mass% or more (e.g., 3 mass% or more), more preferably 5 mass% or more (e.g., 8 mass% or more), and may also be 10 mass% or more (e.g., 12 mass% or more), etc.

[0042] When a monomer having an acid group is used as a polymerization component, the upper limit of the proportion of the monomer having an acid group relative to all the polymerization components may be, for example, 70 mass % or less (e.g., 60 mass % or less), preferably 50 mass % or less (e.g., 40 mass % or less), and more preferably 30 mass % or less (e.g., 25 mass % or less), although it depends on the type of acid group and the like.

[0043] When the polymerization components contain a monomer having a methacrylate and an acid group, the ratio of the monomer having an acid group to the total of the methacrylate and the monomer having an acid group varies depending on the type of acid group, and may be selected from a range of, for example, about 0.1 mass% or more (e.g., 0.3 mass% or more), 0.5 mass% or more (e.g., 1 mass% or more), preferably 2 mass% or more (e.g., 3 mass% or more), more preferably 5 mass% or more (e.g., 8 mass% or more), and may also be 10 mass% or more (e.g., 12 mass% or more), etc.

[0044] When the polymerization components contain a monomer having a methacrylate and an acid group, the upper limit of the proportion of the monomer having an acid group relative to the total of the methacrylate and the monomer having an acid group varies depending on the type of the acid group, and may be, for example, 70 mass% or less (e.g., 60 mass% or less), preferably 50 mass% or less (e.g., 40 mass% or less), and more preferably 30 mass% or less (e.g., 25 mass% or less).

[0045] As described above, the (meth)acrylic resin [(meth)acrylic polymer] may further contain another monomer [a monomer other than a (meth)acrylate and a monomer having an acid group (e.g., a monomer having an ethylenically unsaturated group)] as a polymerization component.

[0046] Examples of other monomers include, but are not limited to, styrene-based monomers (e.g., styrene, α-methylstyrene, p-methylstyrene, p-ethylstyrene, p-methoxystyrene, p-ethoxystyrene, p-chlorostyrene, p-bromostyrene, vinyltoluene, etc.), nitrile-based monomers [e.g., (meth)acrylonitrile], amide-based monomers [e.g., (meth)acrylamide, diacetone acrylamide], vinyl ester-based monomers (e.g., vinyl acetate), vinyl ether-based monomers (e.g., vinyl-n-butyl ether), olefin-based monomers (e.g., ethylene, propylene), halogen-based monomers (e.g., vinyl chloride, vinyl fluoride, vinylidene chloride, vinylidene fluoride, etc.), and the like.

[0047] The polymerization components may contain other monomers either alone or in combination of two or more.

[0048] When the polymerization components contain other monomers, the ratio of the other monomers to the total polymerization components can be selected from a range of, for example, about 50% by mass or less (e.g., 40% by mass or less), and may be 30% by mass or less (e.g., 20% by mass or less, 15% by mass or less, 10% by mass or less, 8% by mass or less, 5% by mass or less, 3% by mass or less), etc.

[0049] The polymer having an acid group may have a polymerizable group [radical polymerizable group, for example, (meth)acryloyl group]. In such a polymer having a polymerizable group (polymer having an acid group), the form of the polymerizable group is not particularly limited, and for example, the polymerizable group may be introduced into a polymer (for example, the above-mentioned polymer) (for example, the polymer having a functional group A may be introduced by reacting with a compound having a functional group B and a polymerizable group that can react with the functional group A and bond).

[0050] Specific examples of polymers having a polymerizable group (and an acid group) include those obtained by reacting (adding) a functional group (e.g., a carboxy group, a hydroxyl group, etc.) possessed by a polymer having an acid group with a polymerizable compound having a functional group (e.g., an isocyanate group) capable of reacting with the functional group to form a bond (e.g., glycidyl (meth)acrylate, 2-methacryloyloxyethyl isocyanate, etc.).

[0051] Such polymers can also be obtained as commercial products, such as Z200M, Z230AA, Z250, Z251, Z254F, Z300, and Z320 (Cyclomer (registered trademark) P, manufactured by Daicel-Allnex Co., Ltd.), CCR-1291H, CCR-1235, ZAR-1035, ZAR-2000, ZFR-1401H, ZFR-1491H, ZCR-1569H, ZCR-1601H, ZCR-1797H, ZCR-1798H, UXE-3000, and UXE-3024 (KAYARAD, manufactured by Nippon Kayaku Co., Ltd.), MAP-4050, MAP-7000, and RA-4101 (ART CURE (registered trademark), manufactured by Negami Chemical Industries Co., Ltd.), and the like.

[0052] The acid value of the polymer having an acid group may be selected, for example, from a range of about 1 mgKOH / g or more (e.g., 5 mgKOH / g or more), and may be about 10 mgKOH / g or more (e.g., 15 mgKOH / g or more), preferably 20 mgKOH / g or more (e.g., 25 mgKOH / g or more), more preferably 30 mgKOH / g or more (e.g., 35 mgKOH / g or more, 40 mgKOH / g or more, 45 mgKOH / g or more), or about 50 mgKOH / g or more (e.g., 55 mgKOH / g or more, 60 mgKOH / g or more, 65 mgKOH / g or more, 70 mgKOH / g or more, 75 mgKOH / g or more).

[0053] The acid value (upper limit of the acid value) of the polymer having an acid group is not limited, but may be selected from a range of, for example, about 1000 mgKOH / g or less (e.g., 800 mgKOH / g or less), and from the viewpoint of sweat resistance and the like, may be about 500 mgKOH / g or less (e.g., 400 mgKOH / g or less), preferably 300 mgKOH / g or less (e.g., 250 mgKOH / g or less), and more preferably 200 mgKOH / g or less (e.g., 180 mgKOH / g or less).

[0054] Specific examples of the acid value of the polymer having an acid group include 10 to 500 mgKOH / g, preferably 30 to 300 mgKOH / g, and more preferably 50 to 200 mgKOH / g.

[0055] The acid value can affect not only the alkali development speed, the exposure sensitivity, and the softness of the photosensitive resin layer, but also the adhesion to the substrate and sweat resistance, and a suitable range may be appropriately selected from the ranges described above.

[0056] The acid value can be measured, for example, in accordance with JIS K2501:2003.

[0057] The hydroxyl value of the polymer having an acid group may be 0 mgKOH / g (or the detection limit) or a finite value. The hydroxyl value of a specific polymer having an acid group may be, for example, about 100 mgKOH / g or less (e.g., 80 mgKOH / g or less, 50 mgKOH / g or less, 40 mgKOH / g or less, 30 mgKOH / g or less, 20 mgKOH / g or less, 10 mgKOH / g or less).

[0058] The hydroxyl value can be measured, for example, in accordance with JIS K0070 1992.

[0059] The mass average molecular weight of the polymer having an acid group is not particularly limited, and may be selected from the range of, for example, about 2000 or more (e.g., 3000 to 500,000) from the viewpoints of efficient alkaline development, ease of film formation, softness of the film (photosensitive resin layer), etc., and may be about 3000 or more (e.g., 4000 to 200,000), preferably 5000 or more (e.g., 5000 to 150,000), and more preferably 8000 or more (e.g., 10,000 to 100,000) from the viewpoints of moldability, alkaline solubility, etc.

[0060] The weight average molecular weight may be measured, for example, using GPC in terms of polystyrene, and specifically, may be measured by the method described later.

[0061] [(B) Photopolymerization initiator (component (B))] The composition of the present invention preferably contains a polymerization initiator (particularly a photopolymerization initiator).

[0062] Examples of the polymerization initiator (photopolymerization initiator) include oxime esters such as 1,2-octanedione, 1-[4-(phenylthio)phenyl-,2-(o-benzoyloxime)] (1-[4-(phenylthio)phenyl-1,2-octanedione 2-(o-benzoyloxime)), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-ethanone 1-(o-acetyloxime); benzophenone, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone (Michler's ketone), N,N,N',N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl] aromatic ketones such as 2-morpholino-propanone-1; 2-ethylanthraquinone, phenanthrenequinone, 2-tert-butylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 2-methylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone quinones such as 2-methyl-1,4-naphthoquinone, and 2,3-dimethylanthraquinone; benzoin ether compounds such as benzoin methyl ether, benzoin ethyl ether, and benzoin phenyl ether; benzoin compounds such as benzoin, methylbenzoin, and ethylbenzoin; benzil derivatives such as benzil dimethyl ketal; 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer; acridine derivatives such as 9-phenylacridine and 1,7-bis(9,9′-acridinyl)heptane;Examples of such compounds include acylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide; N-phenylglycine, N-phenylglycine derivatives; and coumarin compounds.

[0063] The photopolymerization initiators can be used alone or in combination of two or more kinds.

[0064] [(C) Bifunctional polymerizable compound having a hydroxyl group (component (C))] The composition of the present invention contains a difunctional polymerizable compound having a hydroxyl group.

[0065] In such a compound, the number of hydroxyl groups may be one or more, for example, 1 to 4, preferably 1 to 3, and more preferably 1 to 2 (for example, 1).

[0066] The polymerizable compound usually has a polymerizable group, such as an ethylenically unsaturated bond-containing group, such as a (meth)acryloyl group or an alkenyl group (e.g., a vinyl group).

[0067] The polymerizable compounds may have the same or different polymerizable groups.

[0068] Representative examples of bifunctional polymerizable compounds having hydroxyl groups include di(meth)acrylates of polyols having three or more hydroxy groups, and dialkenyl ethers of polyols having three or more hydroxy groups.

[0069] Examples of polyols having three or more hydroxyl groups include triols [e.g., alkane polyols such as glycerin, trimethylolpropane, and trimethylolethane (e.g., C 3-10 Alkane polyols, preferably C 3-6alkane polyols)], polyols having 4 or more (e.g., 4 to 6) hydroxyl groups {e.g., tetraols [e.g., alkane tetraols such as pentaerythritol (e.g., C 4-12 alkanetetraols; dimers of triols (such as alkanetriols) such as diglycerin, etc.}.

[0070] Specific examples of bifunctional polymerizable compounds having a hydroxyl group include (meth)acrylates, for example, (meth)acrylates (compounds) such as alkanetriol di(meth)acrylates [for example, 2-hydroxy-1,3-dimethacryloxypropane, 2-hydroxy-1,3-diacryloxypropane, 1-hydroxy-2,3-diacryloxypropane, 1-hydroxy-2,3-diacryloxypropane, 2-hydroxy-3-methacryloxypropyl acrylate, 1-hydroxy-3-methacryloxypropyl acrylate].

[0071] The bifunctional polymerizable compounds having a hydroxyl group may be used alone or in combination of two or more kinds.

[0072] The hydroxyl value of the bifunctional polymerizable compound having a hydroxyl group is not particularly limited, and may be, for example, about 30 mgKOH / g or more (e.g., 50 mgKOH / g or more, 100 mgKOH / g or more, 150 mgKOH / g or more, 200 mgKOH / g or more, 220 mgKOH / g or more) or about 400 mgKOH / g or less (e.g., 380 mgKOH / g or less, 350 mgKOH / g or less, 320 mgKOH / g or less, 300 mgKOH / g or less, 280 mgKOH / g or less).

[0073] The hydroxyl value of a bifunctional polymerizable compound having a hydroxyl group can be measured in accordance with JIS K0070 1992, for example.

[0074] [(D) Epoxy (meth)acrylate (component (D))] The composition of the present invention preferably comprises an epoxy (meth)acrylate.

[0075] The epoxy (meth)acrylate may be monofunctional, but typically is also multifunctional.

[0076] Examples of epoxy (meth)acrylates include epoxy (meth)acrylates {e.g., reaction products of epoxy compounds and unsaturated carboxylic acids [e.g., (meth)acrylic acid]}, modified products of epoxy (meth)acrylates [e.g., acid-modified epoxy (meth)acrylates], etc. The acid-modified epoxy (meth)acrylates may not be those that fall under the above-mentioned polymers having an acid group.

[0077] Examples of epoxy compounds include aromatic (having an aromatic skeleton) epoxy compounds (or epoxy resins, such as phenol novolac type, cresol novolac type, bisphenol A type, bisphenol F type, trisphenol type, tetraphenol type, phenol-xylylene type, and glycidyl ether type epoxy resins), and halogenated epoxy resins (halides of the aromatic epoxy compounds exemplified above).

[0078] The epoxy compounds may be used alone or in combination of two or more kinds.

[0079] Examples of the acid-modified epoxy (meth)acrylate (acid-modified unsaturated epoxy ester resin) include acid (e.g., acid anhydride, phosphoric acid, etc.) modified products of epoxy (meth)acrylate {e.g., a reaction product of an epoxy compound (e.g., the above-mentioned epoxy compound) with an unsaturated carboxylic acid [e.g., (meth)acrylic acid]} [e.g., carboxylic acid-modified (acid anhydride-modified) epoxy (meth)acrylate, phosphoric acid-modified epoxy (meth)acrylate, etc.].

[0080] The acid-modified epoxy (meth)acrylate can be produced, for example, by reacting an epoxy compound with an unsaturated carboxylic acid, such as (meth)acrylic acid, to obtain an unsaturated epoxy ester resin, and then further reacting the obtained unsaturated epoxy ester resin with an acid component (e.g., acid anhydride, phosphoric acid).

[0081] Examples of acid anhydrides that can be used include maleic anhydride, succinic anhydride, itaconic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, endomethylenetetrahydrophthalic anhydride, methylendomethylenetetrahydrophthalic anhydride, chlorendic anhydride, methyltetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic anhydride.

[0082] In the acid-modified product, the acids (acid anhydrides, phosphoric acid, etc.) may be used alone or in combination of two or more kinds.

[0083] The acid value of the acid-modified epoxy (meth)acrylate may be selected from a range of, for example, about 1 mgKOH / g or more (e.g., 3 mgKOH / g or more), and may be about 5 mgKOH / g or more (e.g., 10 mgKOH / g or more), preferably 15 mgKOH / g or more (e.g., 20 mgKOH / g or more), more preferably 25 mgKOH / g or more (e.g., 30 mgKOH / g or more, 35 mgKOH / g or more), or may be about 40 mgKOH / g or more (e.g., 45 mgKOH / g or more, 50 mgKOH / g or more).

[0084] The acid value (upper limit of the acid value) of the acid-modified epoxy (meth)acrylate is not limited, but may be selected from a range of, for example, about 500 mgKOH / g or less (e.g., 300 mgKOH / g or less), and may be about 250 mgKOH / g or less (e.g., 200 mgKOH / g or less), preferably 180 mgKOH / g or less (e.g., 160 mgKOH / g or less), and more preferably about 150 mgKOH / g or less (e.g., 120 mgKOH / g or less).

[0085] Specific examples of the acid value of the acid-modified epoxy (meth)acrylate include 10 to 300 mgKOH / g, preferably 20 to 250 mgKOH / g, and more preferably 30 to 200 mgKOH / g (eg, 40 to 120 mgKOH / g).

[0086] The acid value can affect not only the alkali development speed, the exposure sensitivity, and the softness of the photosensitive resin layer, but also the adhesion to the substrate and sweat resistance, and a suitable range may be appropriately selected from the ranges described above.

[0087] The acid value can be measured, for example, in accordance with JIS K2501:2003.

[0088] Representative examples of epoxy (meth)acrylates include bisphenol skeleton-containing epoxy (meth)acrylates [for example, unsaturated epoxy ester resins obtained by using bisphenol A type epoxy resin as the epoxy compound and (meth)acrylic acid as the unsaturated carboxylic acid] and acid-modified products thereof [acid-modified unsaturated epoxy ester resins].

[0089] From the viewpoint of adhesion and the like, preferred epoxy (meth)acrylates include acid-modified epoxy (meth)acrylates [for example, carboxylic acid (acid anhydride)-modified epoxy (meth)acrylates such as carboxylic acid-modified bisphenol-type epoxy (meth)acrylates].

[0090] Therefore, the epoxy (meth)acrylate may contain at least an acid-modified epoxy (meth)acrylate.

[0091] The mass average molecular weight of the epoxy (meth)acrylate is not particularly limited, but from the viewpoints of efficient alkaline development, ease of film formation, softness of the film (photosensitive resin layer), and the like, it may be, for example, about 1,000 to 50,000 (e.g., 1,500 to 30,000), preferably about 2,000 to 25,000, and more preferably about 3,000 to 20,000.

[0092] The weight average molecular weight may be measured, for example, using GPC in terms of polystyrene, and specifically, may be measured by the method described later.

[0093] The composition of the present invention may contain a solvent.

[0094] The solvent is not particularly limited, but examples thereof include organic solvents [ketones such as acetone, methyl ethyl ketone (2-butanone), cyclohexanone, etc.; acetate esters such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, carbitol acetate, etc.; carbitols such as cellosolve and butyl carbitol; aromatic hydrocarbons such as toluene and xylene; amide solvents such as dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc.], non-organic solvents (for example, water), etc. Usually, the solvent may contain at least an organic solvent. The solvents may be used alone or in combination of two or more kinds.

[0095] The composition of the present invention may contain components (other components) other than the above components (A) to (D) and the solvent (solvent) as necessary. Examples of such components include thermal polymerization inhibitors, plasticizers, colorants (dyes, pigments), color reducing agents, thermal color development inhibitors, fillers, defoamers, flame retardants, adhesion imparting agents, leveling agents, peeling promoters, antioxidants, water repellents, oil repellents, etc. The other components may be used alone or in combination of two or more.

[0096] In the composition [or resin layer (photosensitive resin layer) or film (protective film, protective layer), the same applies hereinafter], the proportion of component (A) may be selected from a range of, for example, about 20% by mass or more (e.g., 25% by mass or more) relative to the total amount of components (A), (B), (C), and (D). From the viewpoint of sweat resistance and appropriate adhesion [e.g., ease of lamination (application) of films], it may be about 30% by mass or more (e.g., 35 to 95% by mass), preferably 40% by mass or more (e.g., 40 to 90% by mass), more preferably 45% by mass or more (e.g., 45 to 85% by mass), or may be about 50% by mass or more (e.g., 50 to 80% by mass, 50 to 75% by mass, 50 to 70% by mass, 50 to 65% by mass, 54 to 66% by mass, 55 to 70% by mass).

[0097] In the composition, the proportion of component (B) may be selected from the range of, for example, about 0.01 mass % or more (e.g., 0.03 mass % or more) relative to the total amount of components (A), (B), (C), and (D). From the viewpoint of photopolymerizability, visibility of the resin layer, and the like, it may be about 0.05 mass % or more (e.g., 0.05 to 10 mass %), preferably 0.07 mass % or more (e.g., 0.08 to 7 mass %), and more preferably about 0.1 mass % or more (e.g., 0.1 to 5 mass %, 0.1 to 3 mass %, 0.2 mass % or more).

[0098] In the composition, the proportion of component (C) may be selected from the range of, for example, about 0.5% by mass or more (e.g., 1% by mass or more) relative to the total amount of components (A), (B), (C), and (D). From the viewpoint of sweat resistance, adhesion, and the like, it may be about 2% by mass or more (e.g., 2 to 80% by mass, 2 to 45% by mass, 2 to 25% by mass), preferably 3% by mass or more (e.g., 4 to 50% by mass), more preferably 5% by mass or more (e.g., 7 to 40% by mass, 5 to 25% by mass, 5 to 20% by mass), or about 10% by mass or more (e.g., 10 to 40% by mass, 10 to 35% by mass, 10 to 30% by mass, 12 to 25% by mass, 15 to 50% by mass, 15 to 40% by mass, 15 to 35% by mass).

[0099] In the composition, the proportion of component (C) may be selected from the range of, for example, about 0.1 part by mass or more (e.g., 0.3 part by mass or more) relative to 100 parts by mass of component (A). From the viewpoint of sweat resistance, adhesion, and the like, it may be about 0.5 parts by mass or more (e.g., 0.5 to 200 parts by mass), preferably 1 part by mass or more (e.g., 2 to 150 parts by mass), and more preferably 3 parts by mass or more (e.g., 4 to 100 parts by mass), or about 5 parts by mass or more (e.g., 8 parts by mass or more, 10 parts by mass or more, 12 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 5 to 80 parts by mass, 10 to 70 parts by mass, 15 to 60 parts by mass, 20 to 50 parts by mass, 25 to 45 parts by mass, 5 to 50 parts by mass, 10 to 55 parts by mass).

[0100] In the composition, the proportion of component (D) may be selected from the range of, for example, about 0.5% by mass or more (e.g., 1% by mass or more) relative to the total amount of components (A), (B), (C), and (D). From the viewpoint of sweat resistance, adhesion, and the like, it may be about 2% by mass or more (e.g., 2 to 80% by mass, 2 to 45% by mass, 2 to 25% by mass), preferably 3% by mass or more (e.g., 4 to 50% by mass), and more preferably 5% by mass or more (e.g., 7 to 40% by mass, 5 to 25% by mass), or about 10% by mass or more (e.g., 10 to 40% by mass, 10 to 35% by mass, 10 to 30% by mass, 12 to 25% by mass, 15 to 50% by mass, 15 to 40% by mass, 15 to 35% by mass, 20% by mass or more, 20 to 35% by mass, 24 to 31% by mass).

[0101] In the composition, the proportion of component (D) may be selected from a range of, for example, about 0.1 part by mass or more (e.g., 0.3 part by mass or more) relative to 100 parts by mass of component (A). From the viewpoint of sweat resistance, adhesion, and the like, it may be about 0.5 parts by mass or more (e.g., 0.5 to 200 parts by mass), preferably 1 part by mass or more (e.g., 2 to 150 parts by mass), and more preferably 3 parts by mass or more (e.g., 4 to 100 parts by mass), or about 5 parts by mass or more (e.g., 8 parts by mass or more, 10 parts by mass or more, 12 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, 5 to 80 parts by mass, 10 to 70 parts by mass, 15 to 60 parts by mass, 20 to 50 parts by mass, 25 to 45 parts by mass, 5 to 50 parts by mass, 10 to 55 parts by mass).

[0102] In the composition, the proportion of component (C) may be selected from a range of, for example, about 0.01 part by mass or more (e.g., 0.02 part by mass or more) relative to 1 part by mass of component (D). From the viewpoint of sweat resistance, adhesion, and the like, it may be about 0.03 part by mass or more (e.g., 0.03 to 30 parts by mass), preferably 0.05 part by mass or more (e.g., 0.05 to 20 parts by mass), and more preferably 0.1 part by mass or more (e.g., 0.1 to 10 parts by mass), or may be about 0.2 parts by mass or more (e.g., 0.3 parts by mass or more, 0.5 parts by mass or more, 0.7 parts by mass or more, 0.2 to 10 parts by mass, 0.2 to 5 parts by mass, 0.2 to 3 parts by mass, 0.2 to 2 parts by mass, 0.3 to 10 parts by mass, 0.5 to 5 parts by mass, or 0.7 to 3 parts by mass).

[0103] In the composition, the ratio of the total amount of component (C) and component (D) may be selected from the range of, for example, about 0.2 parts by mass or more (e.g., 0.5 parts by mass or more) relative to 100 parts by mass of component (A). From the viewpoint of sweat resistance, adhesion, and the like, it is about 1 part by mass or more (e.g., 1 to 500 parts by mass), preferably 2 parts by mass or more (e.g., 3 to 300 parts by mass), and more preferably 5 parts by mass or more (e.g., 8 to 200 parts by mass). or may be about 10 parts by mass or more (for example, 15 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, 50 parts by mass or more, 60 parts by mass or more, 70 parts by mass or more, 10 to 150 parts by mass, 20 to 150 parts by mass, 30 to 120 parts by mass, 40 to 100 parts by mass, 50 to 90 parts by mass, 50 to 80 parts by mass, 10 to 100 parts by mass, 20 to 120 parts by mass).

[0104] When the composition contains other components, the proportion of the other components relative to the total amount of components (A), (B), (C), (D) and other components may be, for example, 30 mass% or less (e.g., 25 mass% or less, 20 mass% or less, 15 mass% or less, 10 mass% or less, 5 mass% or less, etc.) or 0.01 mass% or more (e.g., 0.05 mass% or more, 0.1 mass% or more, 0.5 mass% or more, 1 mass% or more), etc.

[0105] In addition, when the composition contains a solvent, the proportion of the solvent and components other than the solvent [solid contents, for example, components (A), (B), (C), and (D) (and further other components as necessary)] can be appropriately selected, and may be, for example, about 1 mass % or more (e.g., 3 to 90 mass %), preferably 5 mass % or more (e.g., 8 to 80 mass %), more preferably about 10 mass % or more (e.g., 15 to 70 mass %), or may be about 20 mass % or more (e.g., 20 to 80 mass %, 25 to 70 mass %, 30 to 65 mass %).

[0106] <Uses of the composition> The application form of the composition of the present invention can be appropriately selected depending on various applications, and for example, the composition may be used to form a resin layer (photosensitive resin layer, film).

[0107] The resin layer may be formed alone, or may be formed on a support (substrate, support) (or may be formed to form a laminate).

[0108] A representative laminate includes a laminate including a support (a film-like substrate) and a resin layer (a resin layer formed from the composition) laminated on the support.

[0109] The support (support material) can be selected depending on the application of the resin layer, and examples thereof include resins (e.g., polyethylene terephthalate, polycarbonate, etc.), metals, etc. The shape of the support can also be selected depending on the application of the resin layer, and examples thereof include a film (sheet) shape.

[0110] A typical support is a resin film.

[0111] The support may be transparent (transparent film, etc.), depending on the use of the resin layer, etc. Such a transparent support may have a total light transmittance of, for example, 50% or more, 60% or more, etc., and a haze of 10% or less, etc.

[0112] The thickness of the support (for example, a film) may vary depending on the application, and may be, for example, 1 to 300 μm (eg, 2 to 200 μm), preferably 3 to 100 μm, and more preferably 5 to 50 μm.

[0113] Such a laminate may further include another layer. Such another layer may be located on the same side or the opposite side of the resin layer as the support (for example, on the resin layer), and may be selected according to the intended use of the laminate, and may be a functional layer, a protective layer (a cover layer, a layer for protecting the resin layer, a cover film), a layer combining these [for example, a functional layer, a resin layer, and a protective layer (cover layer) are provided in this order on the support], or a layer having both purposes (such as a functional layer having a protective or covering function).

[0114] The cover layer (or cover film) may be peelable (peelable from the resin layer) (has releasability) and may have been subjected to a release treatment (for example, coating with a release agent such as silicone).

[0115] Specific examples of the cover layer (cover film) include resin films that may have been release-treated [e.g., olefin-based resin films (e.g., polyethylene films, polypropylene films), resin films coated with a release agent such as silicone (polyethylene terephthalate films, etc.)].

[0116] The thickness of the resin layer can be selected depending on the application of the resin layer, etc., and may be selected, for example, from a range of about 1 μm or more (e.g., 1 to 300 μm). From the viewpoints of resolution, sweat resistance, adhesion, etc., it may be preferably about 2 μm or more (e.g., 2 to 200 μm), more preferably about 3 μm or more (e.g., 4 to 100 μm), or may be 50 μm or less (e.g., 40 μm or less, 30 μm or less, 20 μm or less, 15 μm or less, 2 to 20 μm, 4 to 15 μm).

[0117] Representative examples of the laminate include a laminate film [dry film resist (DFR)] in which a resin layer is laminated on a support (carrier film), and a laminate film in which a support, a resin layer, and a cover film are laminated in this order.

[0118] The resin layer (laminate) is not particularly limited as long as it can be formed from the composition, but typically, it can be formed by coating (applying) the composition on a support. The coating (application) method can be selected according to the shape of the support and the thickness of the resin layer, and is not particularly limited, and a conventional coating method can be used. If necessary, drying treatment, heating treatment, etc. may be performed after application.

[0119] The resin layer is formed from the composition of the present invention and is suitable for use as, for example, a protective film (particularly, a protective film for a touch panel).

[0120] Such a resin layer (protective film) and the like will be described in detail below.

[0121] [Protective film, etc.] The protective film (protective layer, resin layer) is formed from the above-mentioned composition.

[0122] Although various substrates can be used as the target of the protective film (protection target), the protective film is particularly suitable for protecting electrode substrates (such as electrode substrates for touch panels).

[0123] Therefore, the present invention also includes a substrate (protective substrate) that includes a substrate and a protective film (protective layer, resin layer) formed on the substrate.

[0124] Depending on the type of substrate, such protective substrates can be used as (or can form) various devices or device components (for example, as touch panel components (such as electrodes of a touch panel)).

[0125] As such a substrate, for example, plastic, glass, rubber, ceramics, etc. are preferably used. Such a substrate preferably has a total light transmittance of 60% or more. Among plastics, a resin film having flexibility is preferably used because of its excellent handling properties. Specific examples of resin films used as substrates include polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), acrylic resins, epoxy resins, fluororesins, silicone resins, polycarbonate resins, diacetate resins, triacetate resins, polyarylate resins, polyvinyl chloride, polysulfone resins, polyethersulfone resins, polyimide resins, polyamide resins, polyolefin resins, and cyclic polyolefin resins.

[0126] The thickness of the substrate (for example, a resin film) may be, for example, about 50 to 300 μm. The substrate may be provided with a known layer such as an easy-adhesion layer.

[0127] The substrate (e.g., electrode substrate) may have a metal layer. Such a metal layer may be provided on the substrate (base substrate) as described above, and may form a pattern (e.g., a pattern according to various purposes and applications such as a sensor portion, a wiring portion, a terminal portion, etc.).

[0128] The metal layer (metal forming a pattern) can be selected depending on the application, function, etc., and examples thereof include metals or alloys (gold, silver, copper, nickel, aluminum, etc.), metal oxides (e.g., ITO, etc.), etc. In particular, in touch panels (electrodes of touch panels, light-transmitting conductive layers of touch panels, etc.), etc., the metal layer may contain at least copper, ITO, etc.

[0129] The method for forming the protective film on the substrate is not particularly limited, and the composition may be directly coated on the substrate, or a laminate may be used as described above.

[0130] For example, a laminate having a resin layer formed thereon in advance may be prepared, and the resin layer (resin layer side) of the laminate may be attached to the substrate (for example, at least the electrode (metal layer) in the case of an electrode substrate), thereby laminating the resin layer on the substrate. In addition, when the laminate has a cover film, the resin layer may be laminated on the substrate after peeling off the cover film.

[0131] The laminate can be formed by coating the composition (coating liquid) on a support, drying, etc., as described above. As the support, a transparent film that transmits actinic rays is preferable, as described above. The total light transmittance of the transparent film is preferably 60% or more, and the haze value is preferably 10% or less. The thickness of the support is preferably thin because light refraction is small, and preferably thick because coating stability is excellent, and is preferably 5 to 50 μm, etc. Examples of such films include films of polyethylene terephthalate and polycarbonate. As the cover film, for example, a film of a resin with high releasability is used as long as it can peel off the uncured or cured resin layer (photosensitive resin composition). Examples of the film include a polyethylene film, a polypropylene film, and a polyethylene terephthalate film coated with a release agent such as silicone.

[0132] The thickness of the resin layer (photosensitive resin layer) can be selected from the above-mentioned range, and may be, for example, 2 to 20 μm (eg, 4 to 15 μm).

[0133] A method of attaching a resin layer to a substrate [for example, an electrode substrate (electrode substrate for touch panel)] includes laminating the resin layer by heating the resin layer and pressing it against the substrate [for example, an electrode substrate (electrode substrate for touch panel)] using a laminator or the like. In this case, the heating temperature of the resin layer is preferably 70 to 130°C, and the pressing pressure is preferably 0.1 to 1.0 MPa, but these conditions are not particularly limited. In addition, if the resin layer is heated to 70 to 130°C as described above, it is not necessary to preheat the substrate [for example, an electrode substrate (electrode substrate for touch panel)] in advance, but the substrate can be preheated to further improve adhesion.

[0134] After forming a resin layer on a substrate [for example, an electrode substrate (electrode substrate for touch panel)] in this way, the resin layer is irradiated with light or exposed to light (for example, exposed through a mask material) to form a photocured portion (a cured product of the resin layer, a cured product of the resin layer at a portion irradiated with light or exposed to light) at a predetermined location. As a light source for exposure, a known light source that effectively radiates ultraviolet light, such as a carbon arc lamp, a mercury vapor arc lamp, an ultra-high pressure mercury lamp, a high pressure mercury lamp, a xenon lamp, etc., can be used. The irradiation amount and irradiation time of the light source (ultraviolet light, etc.) can be appropriately set according to the resin layer. Examples of the exposure method (for example, an exposure method through a mask) include a contact exposure method in which a mask pattern is closely attached to the dry film and exposed to light, and a non-contact exposure method in which a mask pattern is not closely attached to the dry film and exposed to light using parallel light.

[0135] The non-exposed areas (areas that have not been exposed (masked areas, etc.)) can be removed, for example, with an alkaline developer.

[0136] Examples of the method for removing the unexposed area with an alkaline developer include a method for removing the unexposed area by developing it using a known method such as spraying, rocking immersion, brushing, scraping, etc. As the alkaline developer, one that is safe, stable, and easy to operate is preferably used, and for example, a dilute solution of sodium carbonate at 20 to 50° C. (e.g., a 0.5 to 2.0 mass % aqueous solution) is used. EXAMPLES

[0137] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0138] (Examples 1 to 6, Comparative Examples 1 to 3) A composition (coating liquid for photosensitive resin layer) was prepared so that the blending ratio of each component was as shown in Table 1. The unit of blending amount of each component in Table 1 is parts by mass. The prepared coating liquid was applied onto a polyethylene terephthalate (PET) film (16 μm thick, total light transmittance 88%, haze value 2%) using a wire bar and dried at 100° C. for 5 minutes, a photosensitive resin layer (dry film thickness: 9 μm) was provided on one side of the PET film, and a polypropylene film (25 μm thick) was laminated as a cover film on the photosensitive resin layer to obtain laminates of Examples 1 to 6 and Comparative Examples 1 to 3 having a photosensitive resin layer and a cover film in this order on the PET film.

[0139] [Table 1]

[0140] In Table 1, the components are as follows:

[0141] <(A) Polymer Having Acid Group> (A-1): 35% by mass solution of copolymer resin obtained by copolymerizing methyl methacrylate / n-butyl acrylate / methacrylic acid in a mass ratio of 71 / 5 / 24, solvent: propylene glycol monomethyl ether, mass average molecular weight Mw 50000, acid value 136 mgKOH / g, hydroxyl value 0 mgKOH / g) (A-2): 35% by mass solution of copolymer resin obtained by copolymerizing methyl methacrylate / methacrylic acid in a mass ratio of 76 / 24, solvent: propylene glycol monomethyl ether, mass average molecular weight Mw 50,000, acid value 136 mgKOH / g, hydroxyl value 0 mgKOH / g) (A-3): 35% by mass solution of copolymer resin obtained by copolymerizing methyl methacrylate / methacrylic acid in a mass ratio of 88 / 12, solvent: propylene glycol monomethyl ether, mass average molecular weight Mw 50,000, acid value 78 mgKOH / g, hydroxyl value 0 mgKOH / g) (A-4): 35% by mass solution of copolymer resin obtained by copolymerizing methyl methacrylate / n-butyl acrylate / methacrylic acid in a mass ratio of 71 / 17 / 12, solvent: propylene glycol monomethyl ether, mass average molecular weight Mw 50000, acid value 78 mgKOH / g, hydroxyl value 0 mgKOH / g) (A-5): 35% by mass solution of copolymer resin obtained by copolymerizing methyl methacrylate / n-butyl acrylate / methacrylic acid in a mass ratio of 55 / 21 / 24, solvent: propylene glycol monomethyl ether, mass average molecular weight Mw 50000, acid value 136 mgKOH / g, hydroxyl value 0 mgKOH / g) (A-6): 35% by mass solution of copolymer resin obtained by copolymerizing methyl methacrylate / n-butyl acrylate / methacrylic acid in a mass ratio of 55 / 33 / 12, solvent: propylene glycol monomethyl ether, mass average molecular weight Mw 50000, acid value 78 mgKOH / g, hydroxyl value 0 mgKOH / g)

[0142] <(B) Photopolymerization initiator> (B-1): 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(o-benzoyloxime)] (Irgacure OXE01, manufactured by BASF Japan Ltd.)

[0143] <(C) Photopolymerizable compound> (C-1): 2-hydroxy-1,3-dimethacryloxypropane (hydroxyl value 245 mg KOH / g) (C-2): 2-Hydroxy-3-methacryloxypropyl acrylate (hydroxyl value 261 mg KOH / g) (C-3): 1,9-nonanediol dimethacrylate (hydroxyl value 0 mgKOH / g) (C-4): Pentaerythritol triacrylate (hydroxyl value 188 mg KOH / g)

[0144] <(D) Epoxy (meth)acrylate> (D-1) KAYARAD (registered trademark) UXE-3024 (trade name, manufactured by Nippon Kayaku Co., Ltd., solid content 65 mass%, acid value 60 mg KOH / g, mass average molecular weight 10,000, hydroxyl value 18 mg KOH / g)

[0145] The acid value, hydroxyl value and weight average molecular weight were measured as follows.

[0146] <Acid value> The number of milligrams (mg) of potassium hydroxide required to neutralize the acidic components contained in 1 g of the sample was measured by indicator titration using phenolphthalein in accordance with JIS K0070 1992.

[0147] <Hydroxyl value> Measurements were performed in accordance with JIS K0070 1992. 1 g of sample was weighed out and placed in a round-bottom flask, 5 ml of acetic anhydride-pyridine reagent was added, a ground-plate air condenser was attached, and the flask was heated in an oil bath at 95-100°C for 1 hour. After cooling, 1 ml of water was added from above the air condenser and the flask was shaken to decompose the acetic anhydride. The flask was again heated in the oil bath for 10 minutes. After cooling, the air condenser and the neck of the flask were washed with 5 mL of neutralized ethanol, and titrated with 0.1 mol / L potassium hydroxide-ethanol solution. A blank test was performed in the same manner. The hydroxyl group was calculated using the following formula. Hydroxyl value = (ab) × N × 56.11 / d + c a: Amount of potassium hydroxide-ethanol solution consumed in the blank test (ml) b: Amount of potassium hydroxide-ethanol solution consumed when using the sample (ml) c: acid value d: amount of sample (g) N: Molar concentration of potassium hydroxide-ethanol solution used in titration

[0148] <Mass average molecular weight> The measurement was performed by gel permeation chromatography (GPC) (standard polystyrene equivalent).

[0149] <Preparation of ITO substrate after heat treatment> The cover film of the laminate of the examples and comparative examples was peeled off and the photosensitive resin layer surface exposed was attached to the ITO layer surface of the ITO base material (size 10 cm x 10 cm) in which the ITO layer was laminated on the polycyclic olefin resin base material. Next, the photosensitive resin layer was exposed to ultraviolet light from the PET film side through a photomask having a square pattern of 1 cm on each side. Next, the PET film was peeled off and alkali development was performed with a 1.0 mass % sodium carbonate aqueous solution at 30 ° C. to remove the photosensitive resin layer in the unexposed area. Next, a heat treatment was performed at 150 ° C. for 30 minutes to obtain an ITO base material after heat treatment having a protective film formed of the photosensitive resin layer.

[0150] <Preparation of ITO / copper substrate after heat treatment> The ITO / copper substrate was changed to an ITO / copper substrate (size 10 cm × 10 cm) in which an ITO layer and a copper layer were laminated in this order on a polycyclic olefin resin substrate, and the cover film of the laminate of the examples and comparative examples was peeled off and the exposed photosensitive resin layer surface was attached to the copper layer surface, and in the same manner as above, a heat-treated ITO / copper substrate having a protective film formed of a cured photosensitive resin layer was obtained.

[0151] <Evaluation of Adhesion> The heat-treated ITO substrate and the heat-treated ITO / copper substrate in the area where the protective film was formed were subjected to a cross-cut adhesion test in accordance with JIS K5400-8.5 (JIS D0202) to evaluate the adhesion of the protective film. The number of peeled pieces in each cross-cut was counted and evaluated according to the following evaluation criteria. The results are shown in Table 2. <Adhesion evaluation criteria> A: 0 pieces of grid peeled off. B: The number of peeled grids is greater than 0% and less than 5% of the total. C: The number of peeled grids is more than 5% and 15% or less. D: The number of peeled grids is more than 15% and 35% or less. E: The number of peeled grids exceeds 35% of the total.

[0152] <Sweat resistance evaluation> An artificial sweat solution was prepared by mixing 5 parts by mass of sodium chloride, 5 parts by mass of disodium hydrogen phosphate dodecahydrate, and 2.1 parts by mass of 99% acetic acid with 100 parts by mass of pure water. The artificial sweat solution was then dropped into 20 locations on the protective film of the ITO / copper substrate after the heat treatment described above using a dropper, and dried at room temperature. The dried ITO / copper substrate was then stored for 100 hours in an atmosphere of 60°C and 95% RH, and the discoloration of the copper surface was observed. The results are shown in Table 2. The practical level is B or higher. <Sweat resistance evaluation criteria> A: No discoloration is observed on the copper surface. B: One black discoloration is observed on the copper surface. C: Black discoloration is observed in 2 to 5 places on the copper surface. D: Black discoloration is observed in 6 to 20 places on the copper surface.

[0153] [Table 2]

[0154] The results in Table 2 show that the composition of the present invention can form a film that has an excellent balance of sweat resistance and adhesion to a substrate [e.g., a metal or metal oxide (e.g., a copper substrate and an oxide ITO substrate)], and that such a film is suitable as a protective film for a touch panel, etc. In particular, the compositions of Examples 1 to 4 not only exhibited excellent adhesion to the substrate even after heat treatment, but also exhibited extremely excellent sweat resistance, achieving a good balance between sweat resistance and adhesion. [Industrial Applicability]

[0155] According to the present invention, a novel composition (resin composition) can be provided. Such a composition can be suitably used for applications such as a protective film (e.g., a protective film for a touch panel).

Claims

1. A composition comprising (A) a polymer having an acid group, (B) a photopolymerization initiator, (C) a bifunctional polymerizable compound having a hydroxyl group, and (D) an epoxy (meth)acrylate.

2. A composition comprising: (A) a polymer having an acid group; (B) a photopolymerization initiator; (C) a bifunctional polymerizable compound having a hydroxyl group; and (D) an epoxy (meth)acrylate, (A) the polymerization component of the polymer having an acid group contains 60 mass% or more of methyl methacrylate, (C) the bifunctional polymerizable compound having a hydroxyl group includes a di(meth)acrylate of a polyol having three or more hydroxyl groups, (D) the epoxy (meth)acrylate contains an acid-modified epoxy (meth)acrylate; The ratio of the bifunctional polymerizable compound (C) having a hydroxyl group is 5 parts by weight or more per 100 parts by weight, The ratio of the epoxy (meth)acrylate (D) is 5 parts by mass or more based on 100 parts by mass of the polymer (A) having an acid group, A composition, in which the ratio of the difunctional polymerizable compound having a hydroxyl group (C) is 0.1 to 10 parts by mass per 1 part by mass of the epoxy (meth)acrylate (D).

3. The composition according to claim 1 or 2, which is used for a protective film of a touch panel.

4. 3. A method for forming a protective film on a substrate, comprising laminating a resin layer comprising the composition according to claim 1 or 2 on the substrate, exposing the resin layer to light, and removing the unexposed areas with an alkaline developer.

Citation Information

Patent Citations

  • Photosensitive resin composition, photosensitive resin laminate, production method of resin pattern, production method of cured film and method for manufacturing display device

    JP2018077490A

  • Photosensitive resin composition, transfer film using photosensitive resin composition, production method of resin pattern, and production method of cured film pattern

    JP2019207321A

  • Method for forming protective film on electrode for touch panel, photosensitive resin composition and photosensitive element, and method for manufacturing touch panel

    WO2013084883A1