Thermosetting resin composition and color filter

A thermosetting resin composition with a specific polyfunctional epoxy resin and thermal acid generator addresses pigment elution and residual ion issues in color filters, enhancing NMP resistance and storage stability.

JP2024142412AActive Publication Date: 2024-10-11NOF CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023054547
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Conventional color filter protective films fail to adequately suppress pigment elution due to solvent penetration at high temperatures and residual metal ion contamination, leading to display defects and insufficient storage stability.

Method used

A thermosetting resin composition comprising a specific polyfunctional epoxy resin, polyhydric carboxylic acid hemiacetal ester, and thermal acid generator, with a defined functional group equivalent ratio, is used to form a cured film with enhanced NMP resistance and residual metal ionicity, ensuring improved storage stability.

Benefits of technology

The composition forms a protective film with excellent NMP resistance and residual metal ionicity, preventing pigment elution and maintaining stability over extended periods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142412000001
    Figure 2024142412000001
  • Figure 2024142412000002
    Figure 2024142412000002
  • Figure 2024142412000003
    Figure 2024142412000003
Patent Text Reader

Abstract

To provide a thermosetting resin composition which enables formation of a cured film with excellent NMP resistance and residual metal ionic property, and has good storage stability, and a color filter using a protective film composed of the cured product.SOLUTION: A thermosetting resin composition contains component (A): a polyfunctional epoxy resin having two or more epoxy groups in one molecule, component (B): polyvalent carboxylic acid hemiacetal ester represented by formula (1) or formula (2), and component (C): a heat acid generator, wherein the component (C) is 0.05 to 10 pts.mass with respect to 100 pts.mass of the total of the component (A) and the component (B), and the functional group equivalent ratio of the carboxyl groups of the component (B) to the epoxy groups of the component (A) is within a range of 0.25 to 0.95.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermosetting resin composition and a color filter having a protective film formed by curing the thermosetting resin composition. [Background technology]

[0002] Recently, the demands for the display performance of liquid crystal displays have become stricter, and the demands for reliability such as display performance such as brightness, color purity, and contrast as well as the phenomenon called image sticking, in which the image of the display element is fixed, and display unevenness are increasing. According to Patent Document 1, the occurrence of the image sticking is influenced by the fact that Na ions and K ions contained in a developer such as potassium hydroxide or sodium carbonate remain on the surface of the protective film during the photospacer formation process. For this reason, the protective film is required to have a performance (hereinafter, residual metal ion property) that can suppress the remaining of Na ions and K ions even when it comes into contact with a developer such as potassium hydroxide or sodium carbonate. Patent Document 1 proposes a composition that combines an epoxy group or oxetanyl group-containing polymer, a polyvalent carboxylic acid hemiacetal ester, a specific epoxy compound, and a bifunctional bisphenol A type epoxy resin as a resin composition for a color filter protective film having excellent residual metal ion property.

[0003] Furthermore, if the coating liquid for forming the protective film undergoes a change in viscosity (particularly an increase in viscosity), it becomes difficult to apply the coating film with a uniform thickness, so the coating liquid for the protective film is required to have sufficient storage stability. Normally, the coating liquid for the protective film is stored refrigerated (at about 5°C), and considering in-house inventory storage and customer production adjustments, it is preferable that the coating liquid has excellent storage stability for 180 days or more when stored refrigerated (at about 5°C). Patent Document 2 proposes a composition that combines an epoxy-containing polymer and a polyvalent carboxylic acid hemiacetal ester as a resin composition for a color filter protective film having excellent storage stability. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2022-112451 A [Patent Document 2] JP 2001-350010 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, in order to expand the color gamut that can be displayed on a liquid crystal display device, the pigments contained in the colored layer have been made finer and the pigment concentration has been increased. However, this has caused a problem that the pigments pass through the protective film and dissolve into the liquid crystal layer, causing display defects. It is believed that the dissolution of the pigment components occurs through the solvent of the alignment film (N-methyl-2-pyrrolidone, hereinafter referred to as NMP) that penetrates into the protective film in the alignment film formation process, which is a process following the protective film. In this process, the protective film may be exposed to a high temperature of about 180°C in a state where the protective film and NMP are in contact with each other, so the protective film is required to have the ability to suppress the penetration of NMP even at high temperatures (hereinafter referred to as NMP resistance). Note that, while it was considered sufficient for conventional color filter protective films to suppress the penetration of solvents at about 25 to 40°C, in order to suppress the dissolution of the above-mentioned pigment components, it is necessary to suppress the penetration of solvents at temperatures significantly higher than conventional ones. According to the study by the present inventors, the compositions described in Patent Documents 1 and 2 did not sufficiently achieve both NMP resistance and residual metal ion properties.

[0006] The present invention has been made in view of the above-mentioned conventional techniques, and provides a thermosetting resin composition capable of forming a cured film having excellent NMP resistance and residual metal ions and having good storage stability, and a color filter using a protective film made of the cured product thereof. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted various investigations to solve the above problems, and as a result have found that the above problems can be solved by combining a specific polyfunctional epoxy resin, a specific polyvalent carboxylic acid hemiacetal ester, and a thermal acid generator in a specific ratio range, thereby completing the present invention. That is, the present invention is the following [1] and [2].

[0008] [1] Component (A): a multifunctional epoxy resin having two or more epoxy groups in one molecule; Component (B): a polyvalent carboxylic acid hemiacetal ester represented by the following formula (1) or the following formula (2), Component (C): Contains a thermal acid generator, The amount of the (C) component is 0.05 to 10 parts by mass relative to 100 parts by mass in total of the (A) component and the (B) component, 1. A thermosetting resin composition, wherein the functional group equivalent ratio of the carboxyl group of the component (B) to the epoxy group of the component (A) is in the range of 0.25 to 0.95. [ka] (In the formula, R 1 each independently represents an alkyl group having 1 to 6 carbon atoms.) [ka] (In the formula, R 2 each independently represents an alkyl group having 1 to 6 carbon atoms.)

[0009] [2] A color filter having a protective film formed by curing the thermosetting resin composition according to the above item [1]. Effect of the Invention

[0010] According to the thermosetting resin composition of the present invention, a color filter protective film having excellent NMP resistance and residual metal ions can be formed. The thermosetting resin composition of the present invention also has excellent storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The thermosetting resin composition of the present invention contains the following components (A), (B) and (C):

[0012] <Component (A)> The component (A) is a multifunctional epoxy resin having two or more epoxy groups in one molecule, and is not particularly limited as long as it is a compound having two or more epoxy groups in one molecule, and known materials can be used. Examples of such compounds include epoxy group-containing polymers, bisphenol A type epoxy resins, bisphenol A novolac type epoxy resins, bisphenol F type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol S type epoxy resins, diphenyl ether type epoxy resins, hydroquinone type epoxy resins, naphthalene type epoxy resins, biphenyl type epoxy resins, fluorene type epoxy resins, phenol novolac type epoxy resins, orthocresol novolac type epoxy resins, trishydroxyphenylmethane type epoxy resins, tetraphenylolethane type epoxy resins, dicyclopentadiene phenol type epoxy resins, hydrogenated bisphenol A type epoxy resins, polypropylene glycol type epoxy resins, glycidyl ester type epoxy resins, alicyclic type epoxy resins, and heterocyclic type epoxy resins. These multifunctional epoxy resins may be used alone or in combination of two or more. Among these, it is preferable to use an epoxy group-containing polymer. When an epoxy group-containing polymer is used as a polyfunctional epoxy resin, a sufficient crosslinked structure is obtained, and NMP resistance is improved. In addition, from the viewpoint of storage stability when used in combination with component (C), it is preferable to use an epoxy resin having a glycidyl ether structure.

[0013] (Epoxy group-containing polymer) The epoxy group-containing polymer is a polymer having a structure in which an epoxy group is bonded directly or indirectly via another group to a hydrocarbon chain constituting the polymer main chain. The epoxy group-containing polymer is preferably a copolymer having a structure derived from both components (a1) a monomer having a carbon-carbon unsaturated bond and an epoxy group, and (a2) a monomer having a carbon-carbon unsaturated bond other than (a1).

[0014] (a1) The monomer having a carbon-carbon unsaturated bond and an epoxy group may be any known monomer as long as it has a carbon-carbon unsaturated bond and an epoxy group.

[0015] As the (a1) monomer having a carbon-carbon unsaturated bond and an epoxy group, more preferred examples include the monomers represented by the following formulas (3) to (5). [ka] (In the formula, R 3 represents a hydrogen atom or a methyl group, and k represents an integer of 1 to 3.

[0016] [ka] (In the formula, R 4 is a hydrogen atom or a methyl group, R 5 is a -CH2O- group or a -CH2- group, R 6 represents a hydrogen atom or an alkyl group having 1 to 2 carbon atoms, and m represents an integer of 1 to 3.

[0017] [ka] (In the formula, R 7 represents a hydrogen atom or a methyl group, and n represents an integer of 1 to 3.

[0018] Among the above formulas (3) to (5), formula (3) is particularly preferably R 3 is a methyl group, k is 1, and as formula (4), R 4 is a hydrogen atom, R 5is a -CH2O- group, R 6 is a hydrogen atom, m is 1, and as formula (5), R 7 is a methyl group and n is 1.

[0019] The monomer having a carbon-carbon unsaturated bond other than (a2)(a1) may be any compound having a carbon-carbon unsaturated bond and not corresponding to (a1), and any known monomer may be used. Preferred examples of the monomer of component (a2) include monomers represented by the following formulae (6) to (9).

[0020] [ka] (In the formula, R 8 is a hydrogen atom or a methyl group, R 9 represents an alkyl group having 1 to 8 carbon atoms, an aryl group, or an alicyclic hydrocarbon group having 3 to 12 main ring carbon atoms.

[0021] [ka] (In the formula, R 10 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 11 represents an alkyl group, an alkoxy group, a siloxyalkyl group, or an aromatic hydrocarbon group having 1 to 12 carbon atoms.

[0022] [ka] (In the formula, R 12 represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, an alicyclic hydrocarbon group having 3 to 12 carbon atoms, or an aromatic hydrocarbon group.

[0023] [ka] (In the formula, R 13 is a hydrogen atom or a methyl group, R 14 each independently represents a methyl group or an ethyl group, and p represents an integer of 1 to 5.

[0024] Among the above formulas (6) to (9), formula (6) is particularly preferably R 8 is a hydrogen atom or a methyl group, R 9 is a monomer of an alkyl group having 4 carbon atoms or an alicyclic hydrocarbon group having 6 main ring carbon atoms, and as the formula (7), R 10 is a hydrogen atom, R 11 is a monomer having a 6-membered aromatic hydrocarbon group, and as the formula (8), R 12 is a monomer of a six-membered alicyclic hydrocarbon group, and as the formula (9), R 13 and R 14 is a methyl group and p is 3.

[0025] The epoxy group-containing polymer can be obtained by copolymerizing the (a1) component and the (a2) component. The polymerization form may be linear or branched, and may be any of random copolymers, block copolymers, graft copolymers, etc. As each of the (a1) component and the (a2) component, only one type of monomer may be used, or two or more types may be used in combination.

[0026] The polymerization method of the (a1) component and the (a2) component is not particularly limited, and various polymerization methods such as ionic polymerization such as radical polymerization and anionic polymerization can be used. In addition, polymerization methods such as bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization can be used. Furthermore, additives such as catalysts and solvents may be added to the polymerization reaction system as necessary.

[0027] The epoxy equivalent of the component (A) is preferably 100 to 1000 g / mol, more preferably 100 to 600 g / mol, and even more preferably 100 to 300 g / mol. By setting the epoxy equivalent within the above range, a sufficient crosslinked structure is obtained and NMP resistance is improved.

[0028] The weight average molecular weight (Mw) of the component (A) is not particularly limited, but is, for example, 3,000 to 100,000, preferably 4,000 to 80,000, more preferably 5,000 to 50,000, and even more preferably 10,000 to 30,000.

[0029] <(B) component> Component (B) is a vinyl ether-blocked polycarboxylic acid in which the carboxyl group of a polycarboxylic acid represented by the following formula (1) or (2) is rendered latent, i.e., blocked, as a hemiacetal ester with a vinyl ether compound, and can be obtained by the reaction represented by the following general formula (10). [ka] (In the formula, R 1 each independently represents an alkyl group having 1 to 6 carbon atoms.) [ka] (In the formula, R 2 each independently represents an alkyl group having 1 to 6 carbon atoms.) [ka] (In the formula, R 15 is a six-membered aromatic hydrocarbon group, and R 1 , R 2 represents an alkyl group having 1 to 6 carbon atoms, and n represents an integer of 3 or 4.

[0030] As the polycarboxylic acid, trimellitic acid and pyromellitic acid are preferable. Among them, trimellitic acid is particularly preferable from the viewpoint of storage stability. The polycarboxylic acid may be used alone or in combination of two or more kinds.

[0031] The number of carbon atoms excluding the vinyl carbon of the vinyl ether compound (R 1 , R 2The number of carbon atoms in is 1 to 6, preferably 2 to 6. Specific examples of the vinyl ether compound include aliphatic vinyl ether compounds such as methyl vinyl ether, ethyl vinyl ether, i-propyl vinyl ether, n-propyl vinyl ether, n-butyl vinyl ether, i-butyl vinyl ether, t-butyl vinyl ether, and cyclohexyl vinyl ether. Among these, n-propyl vinyl ether and i-propyl vinyl ether are preferred because they are easily available and their curing temperature is suitable for the process of the protective film. The vinyl ether compounds may be used alone or in combination of two or more.

[0032] Component (B) can be obtained by reacting a carboxylic acid with a vinyl ether compound at a temperature ranging from room temperature to 150°C. Since the blocking reaction is an equilibrium reaction, adding a certain excess amount of a vinyl ether compound to the carboxylic acid can promote the reaction and improve the yield. In addition, a catalyst or solvent can be added to the reaction between the carboxylic acid and the vinyl ether compound depending on the purpose. When the acid value of the reaction solution falls to 2.0 mgKOH / g or less due to the progress of the blocking reaction, it is determined that the reaction has progressed sufficiently and the reaction is terminated.

[0033] Examples of the catalyst include tertiary amines, imidazoles, organic phosphorus compounds, quaternary phosphonium salts, diazabicycloalkenes, organic metal compounds, quaternary ammonium salts, boron compounds, and metal halides. The catalysts can be used alone or in combination of two or more.

[0034] Examples of the solvent include aromatic hydrocarbons, ethers, esters, ether esters, ketones, phosphate esters, nitriles, aprotic polar solvents, and propylene glycol alkyl ether acetates. The solvents can be used alone or in combination of two or more.

[0035] The functional group equivalent ratio of the carboxyl group of the (B) component to the epoxy group of the (A) component is 0.25 to 0.95, preferably 0.30 to 0.80, and more preferably 0.40 to 0.65. By setting the blending ratio of the (A) and (B) components within the above range, it becomes possible to achieve both NMP resistance and residual metal ion properties when combined with the (C) component. If the functional group equivalent ratio of the carboxyl group of the (B) component to the epoxy group in the (A) component is less than 0.25, sufficient NMP resistance cannot be obtained, and if it exceeds 0.95, the residual metal ion properties become insufficient.

[0036] <(C) component> The component (C) is a thermal acid generator, and is not particularly limited as long as it is a compound that generates an acid by heat, and known materials such as sulfonium salt type, ammonium salt type, and iodonium salt type can be used. As for the anion component, known materials such as phosphorus-based, borate-based, and antimony-based materials can be used, but non-antimony materials such as phosphorus-based and borate-based materials are preferable from the viewpoint of hazardousness. Examples of commercially available products of the component (C) include San-Aid SI-80 (Sanshin Chemical Industry Co., Ltd.), SI-100 (Sanshin Chemical Industry Co., Ltd.), SI-110 (Sanshin Chemical Industry Co., Ltd.), SI-150 (Sanshin Chemical Industry Co., Ltd.), SI-B3 (Sanshin Chemical Industry Co., Ltd.), SI-B4 (Sanshin Chemical Industry Co., Ltd.), SI-B5 (Sanshin Chemical Industry Co., Ltd.), TA-100 (Sanshin Chemical Industry Co., Ltd.), TA-100FG (Sanshin Chemical Industry Co., Ltd.), IK-1 (Sanshin Chemical Industry Co., Ltd.), and IK-1FG (Sanshin Chemical Industry Co., Ltd.).

[0037] The amount of component (C) is 0.05 to 10 parts by mass, preferably 0.1 to 7.0 parts by mass, and more preferably 0.15 to 5.0 parts by mass, relative to 100 parts by mass of the total of components (A) and (B). If the amount of component (C) is less than 0.05 parts by mass, sufficient NMP resistance cannot be obtained, and if it exceeds 10 parts by mass, storage stability decreases.

[0038] From the viewpoint of storage stability, it is preferable that the component (C) has an exothermic peak top of 150°C or higher when a mixture of a thermal acid generator and a bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER-828") is subjected to differential scanning calorimetry (heating rate: 10°C / min).

[0039] <Other additives> Additives such as a silane coupling agent, a leveling agent, an antioxidant, a stabilizer, and an organic solvent may be added to the thermosetting resin composition of the present invention as long as they do not impair the effects of the invention.

[0040] <Silane coupling agent> Silane coupling agents are compounds having an alkoxysilyl group (Si-OR) and a reactive group in one molecule. The reactive group is preferably one having an epoxy group. Examples of silane coupling agents having an epoxy group include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. These silane coupling agents can be used alone or in combination of two or more.

[0041] <Leveling agent> The leveling agent is blended for the purpose of improving the appearance of the coating film obtained, and silicone-based, fluorine-based, acrylic-based, etc., which have been generally used in the past in this type of protective film for color filters, can be used without any particular restrictions. Commercially available leveling agents include, for example, Megafac F-410 (DIC Corporation), Megafac F-477 (DIC Corporation), Megafac F-552 (DIC Corporation), Megafac F-553 (DIC Corporation), Megafac F-554 (DIC Corporation), Megafac F-555 (DIC Corporation), Megafac F-556 (DIC Corporation), Megafac F-558 (DIC Corporation), Megafac F-559 (DIC Corporation), Megafac F-561 (DIC Corporation), Megafac F-4430 (Sumitomo 3M Corporation), Megafac F-4432 (DIC Corporation), and Surflon S-611 (AGC Seimi Chemical Corporation). ), S-651 (same company), S-386 (same company), Ftergent 208G (Neos Co., Ltd.), S-602A (same company), S-650A (same company), S-610FM (same company), S-710FM (same company), FTX-218 (same company), BYK-302 (BYK-Chemie Japan Co., Ltd.), BYK-307 (same company), BYK-337 (same company), Polyflow KL-400HF (Kyoeisha Chemical Co., Ltd.), KL-700 (same company), LE-604 (same company), etc. can be used.

[0042] <Antioxidants> As the antioxidant, hindered phenol-based antioxidants such as IRGANOX 1010 (BASF), IRGANOX 1035 (same), IRGANOX 1076 (same), IRGANOX 1135 (same), and IRGANOX 1726 (same), can be used.

[0043] <Stabilizer> The stabilizer refers to the excess vinyl ether, which is added for the purpose of improving the yield of the carboxylic acid hemiacetal ester. Specific examples thereof include the vinyl ethers described in the above "<Component (B)>".

[0044] <Organic solvent> The organic solvent is added for the purpose of adjusting the viscosity of the thermosetting resin composition, etc. Specific examples of the organic solvent include esters such as amyl acetate, ether esters such as ethyl ethoxypropionate and 3-methoxy-3-methyl-1-butyl acetate, ketones such as methyl ethyl ketone and cyclohexanone, and glycol derivatives such as propylene glycol monomethyl ether acetate, propylene glycol diacetate, and diethylene glycol ethyl methyl ether.

[0045] (Formation of protective film for color filters) The color filter of the present invention has a layer of a cured product obtained by curing the above-mentioned thermosetting resin composition as a protective film. The thermosetting resin composition is applied so as to cover the colored layer and the black matrix arranged on the substrate. The application method is not particularly limited, and known application methods such as an inkjet method, a spin coating method, and a die coating method can be used.

[0046] The resulting coating film is dried, and if necessary, pre-heated (hereinafter referred to as "pre-baking"), and then subjected to main curing heating (hereinafter referred to as "post-baking") to form a layer of a resin cured product. In this case, preferred pre-baking conditions include 40 to 140°C and 0 to 1 hour, and preferred post-baking conditions include 150 to 280°C and 0.2 to 2 hours. The heating method is not particularly limited, and for example, a curing device such as a closed curing oven or a tunnel oven capable of continuous curing can be used. The heating source is not particularly limited, and can be hot air circulation, infrared heating, high-frequency heating, or the like. EXAMPLES

[0047] The present invention will be specifically described below with reference to examples and comparative examples. <Polymerization Example 1: Synthesis of epoxy group-containing polymer (A-1)> A four-neck flask equipped with a thermometer, a reflux condenser, a stirrer, and a dropping funnel was charged with 76.0 parts by mass of propylene glycol monomethyl ether acetate (PGMEA) as a solvent, and heated with stirring to 88° C. Next, at a temperature of 88° C., 56.9 parts by mass of glycidyl methacrylate (GMA) as component (a1), 43.1 parts by mass of cyclohexyl methacrylate (CHMA) as component (a2), 8.0 parts by mass of a peroxide-based polymerization initiator "Perhexyl O (PHO)" manufactured by NOF Corporation as a polymerization initiator, and 16.0 parts by mass of PGMEA were mixed in advance and dropped at a constant speed from the dropping funnel over a period of 2 hours (dropping component). Thereafter, the temperature was maintained at 88° C. for 5 hours to obtain a 50% PGMEA solution of an epoxy group-containing polymer (A-1) having a weight average molecular weight (Mw) of 12,700 and an epoxy equivalent of 250 g / mol (as active ingredient).

[0048] <Weight average molecular weight (Mw)> The weight average molecular weight (Mw) was determined in terms of polystyrene using a gel permeation chromatography apparatus HLC-8320GPC manufactured by Tosoh Corporation, a column TSKgel HZM-M manufactured by Tosoh Corporation, THF as an eluent, and an RI detector.

[0049] <Polymerization Examples 2 to 5: Synthesis of epoxy group-containing polymers (A-2 to A-5)> The raw materials shown in Table 1 were mixed under the conditions shown in Table 1, and polymers A-2 to A-5 were obtained in the same manner as in Polymerization Example 1. The charged amount, weight average molecular weight, and epoxy equivalent of each raw material are shown in Table 1.

[0050] [Table 1]

[0051] The abbreviations in Table 1 are as follows. Component (a1) GMA: glycidyl methacrylate (a2) Component CHMA: Cyclohexyl methacrylate MPS: methacryloxypropyltrimethoxysilane CHMI: Cyclohexylmaleimide BMA: Butyl methacrylate (Polymerization initiator) PHO: t-Hexylperoxy-2-ethylhexanoate (peroxide polymerization initiator manufactured by NOF Corp., product name: Perhexyl O) (solvent) PGMEA: Propylene glycol monomethyl ether acetate

[0052] <Synthesis Example 1: Synthesis of component (B) (B-1)> In a four-neck flask equipped with a thermometer, a reflux condenser, and a stirrer, 26.8 parts by mass of propylene glycol monomethyl ether acetate (PGMEA) as a solvent, 26.9 parts by mass of trimellitic acid (TMA) as a polycarboxylic acid, and 46.3 parts by mass of n-propyl vinyl ether (NPVE) as a vinyl ether were charged, and the mixture was heated with stirring to 80 ° C. Then, the mixture was stirred while maintaining the temperature, and after confirming that the acid value of the mixture reached 2.0 mg KOH / g or less, the reaction was terminated, and a 60% PGMEA solution of polycarboxylic acid hemiacetal ester (B-1) with an acid value of 0.6 mg KOH / g and a carboxyl group equivalent of 156 g / mol (active ingredient equivalent) was obtained.

[0053] <Acid value> The acid value was measured according to JIS K0070-1992 "Testing methods for acid value, saponification value, ester value, iodine value, hydroxyl value and unsaponifiable matter of chemical products."

[0054] <Synthesis Examples 2 to 3: Synthesis of polycarboxylic acid hemiacetal esters (B-2 to B-3)> The raw materials shown in Table 2 were mixed under the conditions shown in Table 2, and reaction products B-2 to B-3 were obtained in the same manner as in Synthesis Example 1. The amount of each raw material charged, the acid value, and the carboxyl group equivalent are shown in Table 2.

[0055] [Table 2]

[0056] The abbreviations in Table 2 are as follows. (Polycarboxylic Acid) TMA: Trimellitic acid PMA: Pyromellitic acid (Vinyl ether) NPVE: n-propyl vinyl ether IPVE: i-Propyl vinyl ether (solvent) PGMEA: Propylene glycol monomethyl ether acetate

[0057] <Comparative Synthesis Example 1: Synthesis of thermal latent catalyst (CAT-1)> In a four-neck flask equipped with a thermometer, reflux condenser, stirrer, and dropping funnel, 100.0 parts by mass of zinc 2-ethylhexyl acid was charged and stirred at room temperature. Then, 41.1 parts by mass of triethanolamine was dropped at a constant rate from the dropping funnel over 30 minutes. After dropping, the mixture was reacted for 1 hour to obtain a thermally latent catalyst (CAT-1).

[0058] <Examples 1 to 23 and Comparative Examples 1 to 7> Each component shown in Tables 3 to 5 was dissolved and mixed in the amount shown in Tables 3 to 5 to prepare coating solutions of thermosetting resin compositions for color filter protective films of Examples 1 to 23 and Comparative Examples 1 to 7. In Tables 3 to 5, the numerical values ​​showing the content of each component are parts by mass. The abbreviations in Tables 3 to 5 are as follows.

[0059] <Component (A)> EP157: Bisphenol A novolac type epoxy compound (manufactured by Mitsubishi Chemical Corporation, product name: "jER157S70", epoxy equivalent 210g / eq, glycidyl ether type) VG3101L: Glycidyl ether type epoxy compound (manufactured by Printec Co., Ltd., product name: "Techmore VG3101L", epoxy equivalent 210g / eq), glycidyl ether type CEL2021P: 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (manufactured by Daicel Corporation, product name: "Celloxide 2021P", epoxy equivalent 130g / eq), alicyclic epoxy type EP828: Bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "jER-828", epoxy equivalent 190g / eq, glycidyl ether type) <(C) component> C-1: San-Aid SI-110 (manufactured by Sanshin Chemical Industry Co., Ltd., exothermic peak top 160°C) C-2: San-Aid SI-B5 (manufactured by Sanshin Chemical Industry Co., Ltd., exothermic peak top 210°C) C-3: San-Aid SI-B3 (manufactured by Sanshin Chemical Industry Co., Ltd., exothermic peak top 140°C) <Leveling agent> F-477: Fluorine-based leveling agent (manufactured by DIC Corporation, trade name: "Megafac F-477") <Stabilizer> NPVE: n-Propyl vinyl ether IPVE: i-Propyl vinyl ether <Catalyst> ZrOct: Zirconium octylate <Solvent> PGMEA: Propylene glycol monomethyl ether acetate

[0060] The coating liquids of the thermosetting resin compositions of Examples 1 to 23 and Comparative Examples 1 to 7 were each filtered through a membrane filter (material: PE, pore size: 0.2 μm), and then further filtered through a hollow filter (material: PP, pore size: 0.02 μm). The obtained coating liquid of the thermosetting resin composition for the color filter protective film was spin-coated onto a substrate using a spin coater (model 1H-DX-2, manufactured by Mikasa Co., Ltd.). After coating, the substrate was pre-baked in a clean oven at 90°C for 2 minutes, and then post-baked in a clean oven at 230°C for 30 minutes to obtain a cured film with a predetermined film thickness. For the thermosetting resin composition or the obtained cured film, the following evaluations of "NMP resistance", "residual metal ion property", and "storage stability" were performed. The evaluation results are shown in Tables 3 to 5.

[0061] <NMP resistance> 100 μL of NMP was dropped onto a 10 cm square non-alkali glass substrate (EAGLEXG, manufactured by Corning Inc.) on which a 1.5 μm thick cured film was formed, covered with an 8 cm square cover glass, and then heated at 180°C for 15 minutes. After heating, the cover glass was removed, and the NMP on the surface of the cured film was removed by air blowing. The film thickness of the cured film before and after the test was measured, and the film thickness change rate was calculated. A film thickness change rate of 30% or less before and after the test was considered qualified.

[0062] <Residual metal ion property> A non-alkali glass substrate (EAGLEXG, Corning) with a 1.5 μm thick cured film was irradiated with 3,000 mJ / cm using a UV cleaning device (Model Ai UV-Ozone Cleaning Device, Iwasaki Electric Co., Ltd.). 2 After irradiating the substrate with UV-ozone, it was immersed in 0.05wt% potassium hydroxide developer for 60 seconds. The substrate was then washed with pure water for 10 seconds and thoroughly dried with air blower. The substrate was subjected to a fluorescent X-ray device (model ZSX100e, Rigaku Corporation) to measure the residual potassium content on the cured film surface. Residual potassium content of 0.6% or less was considered to be acceptable.

[0063] <Storage stability> The coating liquid of the thermosetting resin composition was left in a sealed container at 5° C., and the time (days) until the viscosity at a measurement temperature of 25° C. doubled from the viscosity immediately after preparation of the coating liquid was measured. When the time until the viscosity of the coating liquid doubled was 180 days or more, it was judged as ⊚, when it was 90 days or more but less than 180 days, it was judged as ◯, and when it was less than 90 days, it was judged as x.

[0064] [Table 3]

[0065] [Table 4]

[0066] [Table 5]

[0067] From the results of Tables 3 and 4, in Examples 1 to 23, the cured films had good NMP resistance and residual metal ion properties, and the thermosetting resin compositions also had good storage stability in a refrigerator (5°C). On the other hand, from the results of Table 5, in Comparative Examples 1 to 5, component (C) was not used or the amount of component (C) was too small, so the NMP resistance was insufficient. Furthermore, in Comparative Examples 6 and 7, the functional group equivalent ratio of the carboxyl group in component (B) to the epoxy group in component (A) was too large or too small, so the residual metal ion properties or NMP resistance was insufficient.

Claims

1. Component (A): a multifunctional epoxy resin having two or more epoxy groups in one molecule; Component (B): a polyvalent carboxylic acid hemiacetal ester represented by the following formula (1) or the following formula (2), Component (C): Contains a thermal acid generator, The amount of the (C) component is 0.05 to 10 parts by mass relative to 100 parts by mass in total of the (A) component and the (B) component, A thermosetting resin composition, characterized in that the functional group equivalent ratio of the carboxyl group of the component (B) to the epoxy group of the component (A) is in the range of 0.25 to 0.

95. [Formula 1] (In the formula, R 1 each independently represents an alkyl group having 1 to 6 carbon atoms. [Case 2] (In the formula, R 2 each independently represents an alkyl group having 1 to 6 carbon atoms.

2. A color filter comprising a protective film formed by curing the thermosetting resin composition according to claim 1.

Citation Information

Patent Citations

  • Thermosetting resin composition for protecting film of color filter

    JP2006274067A

  • Thermosetting resin composition and color filter including cured film thereof

    JP2019124853A

  • Thermosetting composition

    JP2020037621A

  • Thermosetting composition containing polyhemiacetal ester resin and powdery thermosetting composition

    WO2000040641A1