Thermoplastic elastomer expanded particle, producing method thereof, and thermoplastic elastomer expanded molding, producing method thereof
By setting the extruder cylinder temperature below the melting end temperature and controlling the extrusion process, the method produces foamed thermoplastic elastomer particles with low open cell ratio, improving moldability and cushioning performance of the molded products.
Patent Information
- Application Number
- JP2023054716
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
The manufacturing method for foamed thermoplastic elastomer particles results in a high open cell ratio, affecting moldability and cushioning performance of the resulting foamed molded products.
The method involves melting and kneading a resin composition containing a thermoplastic elastomer with a blowing agent in an extruder, setting the cylinder temperature below the melting end temperature of the elastomer, and cutting the extruded melt-kneaded product to produce expanded thermoplastic elastomer particles with a low open cell ratio.
This approach enables the production of foamed thermoplastic elastomer particles with a low open cell ratio, enhancing moldability and improving cushioning performance, shape flexibility, lightness, compressive strength, and heat insulation properties of the resulting molded articles.
Smart Images

Figure 2024142550000001 
Figure 2024142550000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermoplastic elastomer expanded particle, a method for producing the same, and a thermoplastic elastomer expanded molded article using the expanded particle, and a method for producing the same. [Background technology]
[0002] Expanded molded articles obtained by molding expanded beads that use a thermoplastic elastomer as a base resin have excellent cushioning properties and shape recovery properties after deformation, and are therefore used in components for sporting goods, bedding, automobiles, etc.
[0003] As a method for producing thermoplastic elastomer expanded beads that can provide expanded molded articles for such applications, an extrusion foaming method in which foaming is carried out using an extruder is known from the viewpoint of streamlining the entire process (see Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2016-521796 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the production method described in Patent Document 1 results in a high open cell rate in the resulting expanded beads, which causes problems in the moldability of the extruded expanded beads when producing a foamed molded article and in the cushioning performance of the resulting foamed molded article.
[0006] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide thermoplastic elastomer expanded beads having a low open cell ratio, a method for producing the same, and a thermoplastic elastomer foamed molded article using the expanded beads, and a method for producing the same. [Means for solving the problem]
[0007] The present inventors have discovered that the above problems can be solved by setting the cylinder temperature of an extruder to a specific temperature or lower relative to the melting end temperature of a thermoplastic elastomer and melt-kneading a resin composition containing the elastomer, and have completed the present invention.
[0008] Aspects of the present disclosure relate to the following thermoplastic elastomer expanded beads and a method for producing the same, as well as a thermoplastic elastomer foamed molded article using the expanded beads and a method for producing the same.
[0009] [1] Melting and kneading a resin composition containing a thermoplastic elastomer together with a foaming agent in an extruder; and cutting the resulting blowing agent-containing molten kneaded product while extruding it through a die. The production method, wherein the cylinder temperature of the extruder in the melt-kneading step is (Tem-5)°C or lower, where Tem is the melting end temperature obtained from a DSC curve of the thermoplastic elastomer. [2] The manufacturing method described in [1], wherein the thermoplastic elastomer is a polyester-based thermoplastic elastomer. [3] The method according to [1] or [2], wherein the polyester-based thermoplastic elastomer is a polyetherester-based thermoplastic elastomer. [4] The method according to any one of [1] to [3], wherein the foaming agent is one or more selected from the group consisting of nitrogen, carbon dioxide gas, and air. [5] A method for producing a thermoplastic elastomer foamed molded product, comprising molding a thermoplastic elastomer foamed bead produced by the method according to any one of [1] to [4].
[0010] [6] A thermoplastic elastomer foamed particle containing a resin composition including a thermoplastic elastomer, When the melting end temperature obtained from the DSC curve of the thermoplastic elastomer is expressed as Tem, the Tem of the thermoplastic elastomer is 170° C. or more and 250° C. or less, Expanded particles having an open cell rate of 30% or less. [7] The expanded particles described in [6], having a bulk density of 80 g / L or more and 300 g / L or less. [8] The expanded beads according to [6] or [7], wherein the thermoplastic elastomer is a polyester-based thermoplastic elastomer. [9] The expanded beads according to [8], wherein the polyester-based thermoplastic elastomer is a polyetherester-based thermoplastic elastomer.
[10] A thermoplastic elastomer foamed molded article obtained by molding the thermoplastic elastomer foamed beads according to any one of [6] to [9]. Effect of the Invention
[0011] According to the present invention, it is possible to provide thermoplastic elastomer expanded beads having a low open cell ratio and a method for producing the same, as well as a thermoplastic elastomer foamed molded article using the expanded beads and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Method for producing thermoplastic elastomer expanded beads> The method for producing the thermoplastic elastomer expanded beads of the present embodiment includes melt-kneading a resin composition containing a thermoplastic elastomer together with a foaming agent in an extruder; The resulting blowing agent-containing molten kneaded product is extruded through a die while being cut. The cylinder temperature of the extruder in the melt-kneading step is (Tem-5)°C or lower, where Tem is the melting end temperature determined from the DSC curve of the thermoplastic elastomer.
[0013] According to the production method of this embodiment, it is possible to produce expanded thermoplastic elastomer beads having a low open cell ratio.
[0014] <Resin composition> The resin composition contains a thermoplastic elastomer described below as a base resin, and preferably contains the thermoplastic elastomer as a main component. In the present embodiment, in an embodiment containing the thermoplastic elastomer as a main component, the resin composition preferably contains 80% by weight or more of the thermoplastic elastomer, more preferably 90% by weight or more, and even more preferably 95% by weight or more of the thermoplastic elastomer, based on the total amount of the resin composition.
[0015] (Thermoplastic elastomer) Thermoplastic elastomers basically contain hard segments and soft segments. Examples of thermoplastic elastomers include polyamide-based thermoplastic elastomers, polyester-based thermoplastic elastomers, polyolefin-based thermoplastic elastomers, polystyrene-based thermoplastic elastomers, and polyurethane-based thermoplastic elastomers. Among these, polyester-based thermoplastic elastomers are preferred from the viewpoint of obtaining expanded particles with a low open cell ratio.
[0016] The polyester-based thermoplastic elastomer is not particularly limited, and for example, at least one selected from the group consisting of polyetherester-based thermoplastic elastomers in which the soft segment is polyether and polyesterester-based thermoplastic elastomers in which the soft segment is polyester is used. Among these, polyetherester-based thermoplastic elastomers are preferred from the viewpoint of obtaining expanded beads with a low open cell ratio.
[0017] (Physical properties of thermoplastic elastomers) The melting point of the thermoplastic elastomer is not particularly limited, and is preferably from 120° C. to 250° C., and more preferably from 140° C. to 230° C. In this specification, the melting point is determined from the peak of a DSC curve. In this specification, the melting temperature of a thermoplastic elastomer means the temperature range from the melting initiation temperature, which is the temperature at which melting begins in the DSC curve, to the melting end temperature, which is the temperature at which melting ends in the DSC curve. The melting initiation temperature of the thermoplastic elastomer is not particularly limited, but is preferably 100°C or higher and 210°C or lower. The melting end temperature of the thermoplastic elastomer is not particularly limited, but is preferably 170°C or higher and 250°C or lower, and more preferably 180°C or higher and 240°C or lower. The MVR of the thermoplastic elastomer is not particularly limited, and is not more than 2 cm 3 / 10 minutes or more 60cm 3 / 10 minutes or less is preferable, 2 cm 3 / 50cm for more than 10 minutes 3 In this specification, the MVR is a value determined by measurement at a temperature of 230° C. in accordance with ISO 1133.
[0018] (Other ingredients) The resin composition may contain components other than the thermoplastic elastomer (hereinafter, also referred to as "other components") as long as the effects of the present invention are not impaired. Examples of the other components include bubble nucleating agents, (a) stabilizers such as antioxidants, metal deactivators, phosphorus-based processing stabilizers, ultraviolet absorbers, ultraviolet stabilizers, fluorescent brighteners, metal soaps, and antacid adsorbents, and / or (b) additives such as crosslinking agents, chain transfer agents, lubricants, plasticizers, fillers, reinforcing agents, flame retardants, colorants, and antistatic agents. These other components may be used alone or in combination of two or more.
[0019] (bubble nucleating agent) Examples of the bubble nucleating agent include a mixture of sodium bicarbonate and citric acid, monosodium citrate, talc, calcium carbonate, etc. The bubble nucleating agent may be used alone or in combination of two or more.
[0020] The total content of other components in the resin composition is not particularly limited. For example, the total content of other components in the resin composition is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less, relative to 100 parts by weight of the resin composition.
[0021] <Foaming agent> The foaming agent used in the manufacturing method of the present embodiment is not particularly limited as long as it is a foaming agent generally used in extrusion foaming. Examples of the foaming agent include (a) (a-1) aliphatic hydrocarbons such as propane, normal butane, isobutane, normal pentane, isopentane, and hexane; (a-2) alicyclic hydrocarbons such as cyclopentane and cyclobutane; (a-3) ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether; (a-4) alcohols such as methanol and ethanol; (a-5) inorganic gases such as air, nitrogen, and carbon dioxide gas, and (b) chemical foaming agents including thermal decomposition type foaming agents such as sodium bicarbonate, azodicarbonamide, and dinitrosopentamethylenetetramine. Among these, from the viewpoint of environmental load, it is more preferable to use one or more selected from the group consisting of nitrogen, carbon dioxide gas, air, and thermal decomposition type foaming agents that generate at least one of them.
[0022] The amount of the foaming agent used is preferably 0.5 to 15 parts by weight, and more preferably 0.5 to 10 parts by weight, based on 100.0 parts by weight of the above-mentioned resin composition.
[0023] <Melt-kneading process> Examples of extruders used for melt-kneading include single-screw extruders and twin-screw extruders. Among these, twin-screw extruders are preferred because of their excellent melt-kneading properties.
[0024] From the viewpoint of sufficiently melt-kneading the resin composition and the foaming agent and obtaining thermoplastic elastomer expanded particles having a low open cell ratio, the cylinder temperature of the extruder is, when the melting end temperature obtained from the DSC curve of the thermoplastic elastomer described above is expressed as Tem, not more than (Tem-5)° C., preferably not more than (Tem-10)° C., and more preferably not more than (Tem-15)° C. The cylinder temperature is preferably not less than (Tem-40)° C., and more preferably not less than (Tem-30)° C.
[0025] <Step of cutting the molten mixture while extruding it through the die> In this embodiment, the foaming agent-containing melt-kneaded product obtained in the above-mentioned melt-kneading step is cut while being extruded from a die. The die temperature is not particularly limited, but from the viewpoint of obtaining thermoplastic elastomer expanded particles with a low open cell ratio, it is preferably 120°C or more and 240°C or less, more preferably 125°C or more and 220°C or less, and even more preferably 130°C or more and 210°C or less. In this specification, the die temperature means the die set temperature. The molten kneaded material is extruded through holes provided in the die into a region where the pressure is lower than the internal pressure of the extruder (hereinafter, also referred to as "low pressure region"). The molten kneaded material may be extruded into a gas phase or into a liquid phase. The pressure of the low pressure region is not particularly limited, but is preferably 5 MPa or less, and more preferably 1 MPa or less. The extruded molten kneaded material immediately starts to foam, and when foaming is completed, a thermoplastic elastomer extruded foam is obtained.
[0026] In this embodiment, the extruded molten kneaded material is cut into particles to obtain thermoplastic elastomer expanded particles. In the cutting step, the molten kneaded material (extruded foam) may be cut during foaming, or the molten kneaded material (extruded foam) after foaming may be cut into small pieces. The method for cutting the extruded molten kneaded material is not particularly limited. For example, the molten kneaded material may be cut along the extrusion direction with a cutter or the like provided next to the die.
[0027] The low pressure region may be either a gas phase or a liquid phase, but is preferably a gas phase, since expanded beads having a relatively high expansion ratio can be obtained. Water or the like may be sprayed onto the expanded beads cut in the gas phase to cool the surface.
[0028] In this embodiment, the melt-kneaded product may be cooled before being extruded from the die. Examples of cooling devices used for cooling include a single-screw extruder, a static mixer, and a melt cooler. The temperature of the cooling device is not particularly limited as long as it is a temperature suitable for foaming the obtained melt-kneaded product. For example, the temperature of the cooling device is preferably 120°C or more and 240°C or less, more preferably 125°C or more and 220°C or less, and even more preferably 130°C or more and 210°C or less. In the cooling device, a die for extruding the cooled molten kneaded material is provided at the leading end in the extrusion direction of the molten kneaded material, so that the molten kneaded material can be cut while being extruded from the die in the above-mentioned manner.
[0029] <Thermoplastic elastomer expanded particles> The thermoplastic elastomer expanded particles of the present embodiment contain a resin composition containing a thermoplastic elastomer. When the melting end temperature of the thermoplastic elastomer determined from the DSC curve is denoted as Tem, the Tem of the thermoplastic elastomer is preferably 170° C. or higher and 250° C. or lower, The open cell ratio of the expanded thermoplastic elastomer particles is preferably 30% or less.
[0030] The thermoplastic elastomer expanded beads of this embodiment are obtained by the above-mentioned production method. Therefore, the resin composition and the thermoplastic elastomer are the same as those in the embodiment described in the above section "Production method of thermoplastic elastomer expanded beads".
[0031] <Physical properties of thermoplastic elastomer expanded beads> (Open cell ratio) The open cell ratio of the thermoplastic elastomer expanded beads is preferably as low as possible. The upper limit of the open cell ratio of the expanded beads is preferably 30% or less, more preferably 25% or less, even more preferably 20% or less, even more preferably 15% or less, and particularly preferably 10% or less. The lower limit of the open cell ratio of the expanded beads is not particularly limited, and is, for example, 0.0% or more. According to the above configuration, (a) the expanded beads have an advantage that the cells are hardly broken and shrunk during molding, so that the expanded beads have excellent moldability, and (b) the expanded molded product obtained using the expanded beads exhibits characteristics such as arbitrary shape, cushioning properties, light weight, compressive strength, and heat insulation properties.
[0032] (Bulk density) The bulk density of the thermoplastic elastomer expanded particles is not particularly limited, but is preferably 80 g / L to 300 g / L, more preferably 85 g / L to 250 g / L, even more preferably 90 g / L to 250 g / L, and even more preferably 95 g / L to 230 g / L. The above configuration has the advantage that the thermoplastic elastomer foamed molded product obtained using the expanded particles exhibits characteristics such as shape arbitrariness, cushioning properties, light weight, and heat insulation properties.
[0033] (average cell diameter) The average cell diameter of the thermoplastic elastomer expanded beads is not particularly limited, and is preferably, for example, 300 μm to 1200 μm, more preferably 500 μm to 1100 μm. When the average cell diameter of the expanded beads is 300 μm or more, the shrinkage of the expanded molded article tends to be small, and when it is 1200 μm or less, the molding cycle during in-mold foam molding tends to be shortened.
[0034] <Thermoplastic elastomer foam molded product and its manufacturing method> The thermoplastic elastomer foamed molded article of the present embodiment is produced by molding the above-mentioned thermoplastic elastomer foamed beads. The method for producing the foamed molded article includes molding the thermoplastic elastomer foamed beads produced by the above-mentioned method. The method of molding the thermoplastic elastomer expanded beads is not particularly limited, and for example, a method of molding the thermoplastic elastomer expanded beads in a mold is preferred. Specifically, the expanded beads can be obtained by filling a mold that can be closed but not sealed, and heating with steam or the like to mold the expanded beads. As a method for producing the expanded molded product, for example, (a) a method in which the expanded beads are pressurized with an inorganic gas to impregnate the particles with the inorganic gas and impart a predetermined particle internal pressure, and then the expanded beads are filled into a mold and heat-fused with steam or the like (for example, JP-B-51-22951), (b) a method in which the expanded beads are compressed with gas pressure, filled into a mold, and heat-fused with steam or the like by utilizing the recovery force of the beads (for example, JP-B-53-33996), (c) a method in which the expanded beads are filled into a mold with an expanded gap, the mold is closed to a predetermined gap, the filled expanded beads are compressed, and then heat-fused with steam or the like can be used. In this embodiment, when a foamed molded article is produced by the above method (c), the pressure range of steam or the like required to obtain a good foamed molded article is wide. That is, the molding range of the foamed beads is wide.
[0035] Thermoplastic elastomer foam molded articles are used as components for sporting goods, bedding, automobiles, etc. EXAMPLES
[0036] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0037] <Evaluation> For Resins A-1 and A-2 described below, the melting point, melting end temperature, and MVR were measured according to the following methods. For the extruded foamed particles described below, the bulk density, average cell diameter, and open cell ratio were measured according to the following methods.
[0038] (Melting point, melting temperature) The following steps (1) to (3) were carried out using a Seiko Instruments Inc. DSC6200 differential scanning calorimeter. (1) 5 mg to 6 mg of resin was melted by increasing the temperature from 40° C. to 250° C. at a heating rate of 10° C. / min. (2) Thereafter, the molten resin was crystallized by lowering the temperature from 250° C. to 40° C. at a rate of 10° C. / min. (3) After that, the crystallized resin was further heated from 40° C. to 250° C. at a heating rate of 10° C. / min. The temperature of the peak (melting peak) of the DSC curve of the resin obtained during the second heating (i.e., at (3)) was taken as the melting point of the resin, and the temperature from when melting started (melting initiation temperature) to when melting ended (melting end temperature) was taken as the melting temperature.
[0039] (MVR) In accordance with the provisions of Method B described in ISO 1133 (1997), a Melt Indexer S-01 (manufactured by Toyo Seiki Seisakusho) was used, and the amount of resin extruded from the die in a certain time under conditions of 230°C and 2.16 kg was converted into the amount extruded in 10 minutes.
[0040] (Bulk density) The bulk density of the extruded foam particles was calculated by carrying out the following steps (1) to (3) in this order. (1) The extruded foam particles are poured into a measuring cup whose internal volume Vk (L) has been accurately measured in advance, until the measuring cup overflows. (2) The powder surface (top) of the container is scraped off, and the weight Wb (g) of the extruded foam particles in the container is measured. (3) The bulk density of the extruded foam particles was calculated using the following formula: Bulk density (g / L) = weight of foam particles Wb (g) / volume of container Vk (L)
[0041] (average cell diameter) Ten pieces were randomly taken from the extruded foam particles and cut with great care so as not to destroy the cell membrane. The cut surface of each sample was observed with a microscope (Keyence: VHX digital microscope), a line equivalent to a length of 1 mm was drawn on the part excluding the surface layer, the number of cells through which the line passed was counted, and the average cell diameter was then measured according to ASTM D3576.
[0042] (Open cell ratio) According to the method described in PROSEDURE C of ASTM D2856-87, the calculation was carried out by carrying out the following steps (1) to (3) in this order. (1) The volume of the extruded foam particles, Vc (cm), was measured using an air-comparison specific gravity meter. 3 ) was measured. (2) Next, the entire amount of the extruded foam particles after measuring Vc was submerged in ethanol contained in a measuring cylinder. (3) After that, the apparent volume Va (cm) of the extruded foam particles was calculated from the amount of rise in the position of the ethanol in the measuring cylinder. 3 ) was sought. (4) The open cell ratio of the extruded foam particles was calculated using the following formula: Open cell rate (%) = ((Va-Vc) x 100) / Va
[0043] [Examples 1 to 4, Comparative Examples 1 to 4] (raw resin) In the examples and comparative examples, the following resins A-1 and A-2 were used as thermoplastic elastomers. Resin A-1: Polyether ester thermoplastic elastomer (DSM, Arnitel (registered trademark) EL430, melting point 163.7°C, melting temperature: 120.0 to 193.0°C, MVR: 33 cm 3 / 10 minutes) Resin A-2: Polyether ester thermoplastic elastomer (DSM, Arnitel (registered trademark) PM381, melting point: 208.4°C, melting temperature: 191.4 to 229.7°C, MVR: 4.7 cm 3 / 10 minutes
[0044] (Production Examples 1 to 4 of Thermoplastic Elastomer Expanded Particles, and Comparative Production Examples 1 to 4) The apparatus used for producing thermoplastic elastomer expanded particles (hereinafter sometimes referred to as "extruded expanded particles") was a twin-screw extruder with a shaft diameter of φ15 mm, a melt cooler, a diverter valve, and a die connected in series. The resins shown in Tables 1 and 2 were fed to the twin-screw extruder at 1.0 kg / h and melted at the cylinder temperatures and screw rotation speeds shown in Tables 1 and 2. Furthermore, carbon dioxide gas, which is a foaming agent, was fed from the pressure-injection section provided midway through the extruder in the amount shown in Tables 1 and 2 per 100 parts by weight of the resin composition using a metering pump, and the resulting composition was further melt-kneaded. The obtained molten mixture was cooled by passing it through a melt cooler connected to the tip of the twin-screw extruder and set to the temperature shown in Tables 1-2. Thereafter, the molten mixture was extruded into the air from a die (φ0.7 mm×2 holes) attached to the tip of the melt cooler to be foamed. The extruded foam was rotated at 1000 rpm with four cutter blades while spraying a mist of 70 mL / min of water and 27 mL / min of air, and cut immediately after extrusion (mist cut method) to obtain foamed particles. The obtained extruded foamed particles were dried in a 75°C drying chamber for 4 hours or more, and left to stand at room temperature for 24 hours or more, and the bulk density, average cell diameter, and open cell ratio were measured. The results are shown in Tables 1-2.
[0045] [Table 1]
[0046] [Table 2]
[0047] From Tables 1 and 2, it can be seen that by setting the cylinder temperature of the extruder to (resin melting end temperature - 5) °C or less and melt-kneading a resin composition containing a thermoplastic elastomer, expanded beads having an open cell ratio of 30% or less can be obtained.
Claims
1. Melting and kneading a resin composition containing a thermoplastic elastomer together with a foaming agent in an extruder; and cutting the resulting blowing agent-containing molten kneaded product while extruding it through a die. The production method, wherein the cylinder temperature of the extruder in the melt-kneading step is (Tem-5)°C or lower, where Tem is the melting end temperature of the thermoplastic elastomer determined from a DSC curve.
2. The method according to claim 1 , wherein the thermoplastic elastomer is a polyester-based thermoplastic elastomer.
3. The method according to claim 2 , wherein the polyester-based thermoplastic elastomer is a polyetherester-based thermoplastic elastomer.
4. The method according to claim 1 or 2, wherein the foaming agent is at least one selected from the group consisting of nitrogen, carbon dioxide gas, and air.
5. A method for producing a thermoplastic elastomer foamed molded article, comprising molding the thermoplastic elastomer foamed beads produced by the method according to claim 1 or 2.
6. A thermoplastic elastomer expanded particle containing a resin composition including a thermoplastic elastomer, When the melting end temperature obtained from the DSC curve of the thermoplastic elastomer is expressed as Tem, the Tem of the thermoplastic elastomer is 170° C. or higher and 250° C. or lower, The expanded particles have an open cell ratio of 30% or less.
7. The expanded beads according to claim 6, having a bulk density of 80 g / L or more and 300 g / L or less.
8. The expanded beads according to claim 6 or 7, wherein the thermoplastic elastomer is a polyester-based thermoplastic elastomer.
9. The expanded bead according to claim 8, wherein the polyester-based thermoplastic elastomer is a polyetherester-based thermoplastic elastomer.
10. A thermoplastic elastomer foamed molded article obtained by molding the thermoplastic elastomer foamed beads according to claim 6 or 7.
Citation Information
Patent Citations
Production of expanded pellets
JP2016521796A