Application method of metal paste and manufacturing method of bonded body

By stopping metal paste discharge before the nozzle's terminal end and advancing it to the end while stopped, the method addresses the issue of paste rising, ensuring stable application and preventing short circuits during bonding processes.

JP2024142569APending Publication Date: 2024-10-11MITSUBISHI MATERIALS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023054754
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The application of sintered metal paste during bonding processes can result in the formation of voids and electrical short circuits due to the metal paste rising at the terminal end, especially when using a discharge nozzle in the advancing direction.

Method used

A method where the metal paste application is stopped before the terminal end of the nozzle's travel direction and the nozzle is advanced to the end while stopped, with the stopping position within a specific range from the terminal end, to prevent excess paste and ensure stable application.

Benefits of technology

This method effectively suppresses the rise of metal paste at the terminal end, ensuring stable application and preventing electrical short circuits, thereby facilitating a reliable bonding process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142569000001_ABST
    Figure 2024142569000001_ABST
Patent Text Reader

Abstract

To provide an application method of a metal paste with which, even if a metal paste is applied by discharging the metal paste while moving a discharge nozzle in a direction of travel, a rise of the metal paste at an end portion of the discharge nozzle in the direction of travel in a paste application scheduled area can be suppressed so that the metal paste can be stably applied.SOLUTION: There is provided an application method of a metal paste 23 in which the metal paste 23 is applied by discharging the metal paste 23 while a discharge nozzle 30 is travelled in a direction of travel. In the application method, the discharge of the metal paste 23 is stopped before an end portion E of the discharge nozzle 30 in the direction of travel in a paste application scheduled area, and also the discharge nozzle 30 is traveled at least to the end portion E while the discharge of the metal paste 23 is stopped.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for applying a metal paste used when joining components together, and a method for producing a joined body in which components are joined via a sintered body of the metal paste. [Background technology]

[0002] For example, electronic devices such as LEDs and power modules have a structure in which a semiconductor element is bonded onto a circuit layer made of a metal material. Here, when electronic components such as semiconductor elements are bonded to circuit layers, a method using a solder material is widely used, as shown in, for example, Patent Document 1. Recently, from the viewpoint of environmental protection, lead-free solders such as Sn-Ag, Sn-In, or Sn-Ag-Cu solders have become mainstream.

[0003] However, as described in Patent Document 1, when an electronic component such as a semiconductor element and a circuit layer are joined via a solder material, there is a risk that a part of the solder will melt when used in a high-temperature environment, resulting in a decrease in the reliability of the joint between the electronic component such as a semiconductor element and the circuit layer. In particular, the heat resistance of semiconductor elements themselves has improved in recent years, and semiconductor devices are sometimes used in high-temperature environments such as the engine compartment of an automobile. In addition, large currents are loaded onto the semiconductor elements, and the amount of heat generated by the semiconductor elements themselves is increasing. For this reason, it has been difficult to deal with this problem using the conventional structure in which the elements are joined with solder material.

[0004] Therefore, as an alternative to solder materials, for example, Patent Documents 2 and 3 propose sintered metal pastes containing metal powder and a solvent. By disposing these metal pastes between the circuit layer and the semiconductor element and firing the metal paste, the circuit layer and the semiconductor element are joined via a joining layer made of a sintered body. The joining layer made of a sintered body of the metal paste has excellent heat resistance and can be used stably even in high-temperature environments and large-current applications. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-172378 A [Patent Document 2] JP 2008-161907 A [Patent Document 3] JP 2011-094223 A Summary of the Invention [Problem to be solved by the invention]

[0006] Incidentally, as shown in Patent Document 1, when solder paste is used, even if the solder paste is applied in dots to the joining surfaces, it becomes liquid at the time of joining, so that joining can be achieved over the entire joining surfaces. On the other hand, as shown in Patent Documents 2 and 3, when a sintered metal paste is used, no liquid phase is generated during bonding, so spot application results in the formation of voids at the bonding interface. For this reason, when a sintered metal paste is used, it is necessary to apply the metal paste to the entire bonding surface. Therefore, when applying a sintered type metal paste, a method is used in which the metal paste is discharged while moving a discharge nozzle in the direction of travel.

[0007] However, when applying a sintered metal paste, the metal paste may be applied so as to rise in the height direction at the end of the nozzle in the direction of travel in the paste application area by discharging the metal paste while moving the nozzle in the direction of travel. Therefore, for example, when a circuit layer and a semiconductor element are bonded, the sintered body of the metal paste may be formed to wrap around to the opposite side of the bonding surface of the semiconductor element, which may cause an electrical short circuit with other members.

[0008] This invention has been made in consideration of the above-mentioned circumstances, and aims to provide a method for applying metal paste, which can suppress the rising of metal paste at the end of the ejection nozzle in the moving direction in the paste application area, even when the metal paste is applied by ejecting the metal paste while moving the ejection nozzle in the moving direction, and can provide a method for manufacturing a joint body, which can stably apply metal paste. [Means for solving the problem]

[0009] In order to solve the above problems, a metal paste application method of aspect 1 of the present invention is a metal paste application method in which metal paste is applied by discharging metal paste while advancing an ejection nozzle in a traveling direction, characterized in that the ejection of the metal paste is stopped before a terminal end of the ejection nozzle in the traveling direction in an area to be paste-applied, and the ejection nozzle is advanced at least to the terminal end while the ejection of the metal paste is stopped.

[0010] According to the metal paste application method of the first aspect of the present invention, the discharge of the metal paste is stopped before the terminal end of the paste application area in the advancing direction of the discharge nozzle, so that no excess metal paste is present near the terminal end E of the paste application area. In addition, since the discharge nozzle is advanced to at least the terminal end while the discharge of the metal paste is stopped, the excess metal paste connected to the discharge nozzle is pulled in the direction of the terminal end E, so that the metal paste can be applied up to the terminal end of the paste application area. Therefore, it is possible to suppress rising of the metal paste at the end portion of the region to be coated with the paste.

[0011] The metal paste application method of aspect 2 of the present invention is characterized in that, in the metal paste application method of aspect 1 of the present invention, the position at which the ejection of the metal paste is stopped is within a range of 0.5 mm to 2.0 mm from the end of the ejection nozzle in the direction of travel in the paste application area. According to the metal paste application method of aspect 2 of the present invention, the range is set to be 0.5 mm or more and 2.0 mm or less from the end of the paste application area in the direction of travel of the discharge nozzle, so that it is possible to further suppress the rise of the metal paste at the end of the paste application area and to apply the metal paste up to the end E of the paste application area.

[0012] The manufacturing method of a joined body of aspect 3 of the present invention is a manufacturing method of a joined body in which a first member and a second member are joined via a sintered body of a metal paste, and includes a paste application step of applying the metal paste to one or both of the joining surface of the first member and the joining surface of the second member, a lamination step of laminating the first member and the second member via the metal paste, and a firing step of firing the metal paste to join the first member and the second member via the sintered body of the metal paste, characterized in that the paste application step is performed using the metal paste application method of aspect 1 or aspect 2 of the present invention.

[0013] According to the method for producing a joint body of the third aspect of the present invention, the method for applying a metal paste of the first or second aspect of the present invention includes the paste application step of applying the metal paste to one or both of the joining surfaces of the first and second members, so that it is possible to suppress the metal paste from rising at the end of the region to be applied with the paste and to suppress the metal paste from wrapping around to the side opposite the joining surface of the first or second member. Also, the metal paste can be applied up to the end of the region to be applied with the paste. Therefore, a bonded body can be manufactured in which the first member and the second member are favorably bonded via the sintered body of the metal paste. Effect of the Invention

[0014] According to the present invention, even when metal paste is applied by discharging the metal paste while moving the discharge nozzle in the traveling direction, it is possible to suppress the rising of the metal paste at the terminal end of the discharge nozzle in the traveling direction in the area intended for paste application, and to provide a method for applying metal paste and a method for manufacturing a joint body, which are capable of stably applying the metal paste. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is an explanatory diagram of a bonded body (semiconductor device) according to one embodiment of the present invention. [Diagram 2] 1 is an explanatory diagram of a method for applying a metal paste according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a flow diagram showing a method for producing a bonded body according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, a method for applying a metal paste and a method for manufacturing a bonded body according to an embodiment of the present invention will be described with reference to the accompanying drawings. The method for producing a bonded body according to the present embodiment is for producing a bonded body 10 in which a first member 11 and a second member 12 are bonded together via a bonding layer 13, as shown in FIG. In the metal paste application method of this embodiment, a metal paste for forming a bonding layer 13 is applied to one or both of the bonding surface of the first member 11 and the bonding surface of the second member 12 .

[0017] 1, the bonded body 10 in this embodiment is formed by bonding a first member 11 and a second member 12 via a bonding layer 13 made of a silver sintered body. In this embodiment, the bonded body 10 is a semiconductor device in which a circuit layer (first member 11) of an insulating circuit board and a semiconductor element (second member 12) are bonded via the bonding layer 13.

[0018] As shown in the flow diagram of Figure 2, the manufacturing method of the joint body 10 in this embodiment includes a paste application process S01 in which a metal paste is applied to one or both of the joint surfaces of the first member 11 and the second member 12, a lamination process S02 in which the first member 11 and the second member 12 are laminated via the applied metal paste, and a firing process S03 in which the metal paste is fired to join the first member 11 and the second member 12 via a joint layer 13 made of a sintered body of the metal paste.

[0019] (Paste application process S01) In this embodiment, the above-mentioned paste application step S01 is performed by the metal paste application method of this embodiment. The metal paste application method of this embodiment will be described below. In the metal paste application method of this embodiment, as shown in Fig. 3, the metal paste 23 is applied to the joining surface of the first member 11 by discharging the metal paste 23 while moving the discharge nozzle 30 in the traveling direction. Note that the applied thickness of the metal paste 23 is preferably within a range of 20 µm to 200 µm.

[0020] As shown in Figure 3(a), the discharge of the metal paste 23 is stopped just before the terminal end E of the discharge nozzle 30 in the direction of travel in the area to be paste-applied, and the discharge nozzle 30 is caused to advance at least to the terminal end E of the area to be paste-applied while the discharge of the metal paste 23 is stopped. In addition, the direction of movement of the discharge nozzle 30 after the discharge of the metal paste 23 from the discharge nozzle 30 has stopped is not particularly limited as long as it moves to the end point E of the discharge nozzle 30 in the traveling direction, and it may be moved parallel to the coating surface (joining surface), close to the coating surface (joining surface), or away from the coating surface (joining surface).

[0021] It is preferable that the position P at which the ejection of the metal paste 23 is stopped before the end E of the ejection nozzle 30 in the direction of travel in the paste application area is within a range of 0.5 mm to 2.0 mm from the end E of the ejection nozzle 30 in the direction of travel in the paste application area. The position P where the discharge of the metal paste 23 stops is preferably 0.8 mm or more, and more preferably 1.0 mm or more, from the end E of the discharge nozzle 30 in the direction of travel in the region to be applied with the paste.

[0022] The metal paste 23 of the present embodiment contains metal powder and a binder. Here, the binder contains one or more of a solvent, a dispersant, a plasticizer, and a resin. In this embodiment, the metal paste 23 preferably has a viscosity in the range of 30 Pa·s to 250 Pa·s. By setting the viscosity to 30 Pa·s or more, the paste can be made to retain its shape and can be prevented from separating. On the other hand, by setting the viscosity to 250 Pa·s or less, the paste can be discharged well from the discharge nozzle. Moreover, the metal paste 23 in this embodiment preferably has a TI value in the range of 0.4 to 0.9.

[0023] Examples of the metal powder contained in the metal paste 23 include silver powder and copper powder, which have excellent electrical conductivity and sinterability. The silver powder may be made of pure silver or a silver alloy. The copper powder may be made of pure copper or a copper alloy. The metal powder preferably has an average particle size (D50) within the range of 10 nm to 500 nm. The particle size of the metal powder can be obtained, for example, by measuring the projected area of ​​the metal powder using a SEM (scanning electron microscope), calculating the equivalent circle diameter from the projected area obtained, and converting the calculated particle size into a volume-based particle size.

[0024] Examples of the solvent include alcohol-based solvents, glycol-based solvents, acetate-based solvents, hydrocarbon-based solvents, and mixtures thereof. Examples of alcohol-based solvents include α-terpineol, isopropyl alcohol, ethyl hexanediol, and mixtures thereof. Examples of glycol-based solvents include ethylene glycol, diethylene glycol, polyethylene glycol, and mixtures thereof. Examples of acetate-based solvents include butyl carbitol acetate. Examples of hydrocarbon-based solvents include decane, dodecane, tetradecane, and mixtures thereof.

[0025] The content of the solvent is preferably within the range of 0% by mass to 30% by mass, with the entire metal paste being taken as 100% by mass. Even if the content of the solvent is 0% by mass, if a dispersant or the like is contained as part of the binder, there is no problem because the dispersant or the like functions as a solvent. If the content of the solvent exceeds 30% by mass, the viscosity becomes too low, and the shape retention during application may be easily deteriorated. The content of the solvent is more preferably within the range of 0% by mass to 10% by mass.

[0026] Examples of the resin contained in the metal paste 23 include an epoxy resin, a silicone resin, an acrylic resin, and a mixture thereof. Epoxy resins include bisphenol A type epoxy resins, novolac type epoxy resins, cyclic aliphatic type epoxy resins, and mixtures thereof. Silicone resins include methyl silicone resins, epoxy modified silicone resins, polyester modified silicone resins, and mixtures thereof. Acrylic resins include acrylate monomer resins.

[0027] The content of the resin is preferably within the range of 0% by mass to 3% by mass, with the entire metal paste being taken as 100% by mass. If the content of the resin exceeds 3 mass %, sintering of the silver powder is hindered, and the mechanical strength of the bonding layer may decrease. The content of the resin is more preferably in the range of 0% by mass to 2.5% by mass, and even more preferably in the range of 0% by mass to 2.0% by mass.

[0028] Aliphatic amines can be used as dispersants contained in the metal paste. Aliphatic amines have amine groups that have high affinity with silver, so they are easily attached to the surface of silver particle aggregates, and the aliphatic groups suppress further aggregation of the silver particle aggregates, thereby improving the dispersibility of the silver powder in the silver paste. Examples of aliphatic amines include hexylamine, cyclohexylamine, aniline, heptylamine, octylamine, 2-ethylhexylamine, nonylamine, decylamine, dodecylamine, and tetradodecylamine.

[0029] (Lamination process S02) Next, the first member 11 and the second member 12 are laminated via the applied metal paste 23 to form a laminate. Note that the applied metal paste 23 may be dried before the first member 11 and the second member 12 are laminated.

[0030] (Firing process S03) This laminate is heat-treated to sinter the metal paste 13, thereby bonding the first member 11 and the second member 12 via the bonding layer 13 made of a sintered metal body. The heating temperature during the heat treatment is appropriately set depending on the metal paste used, but is preferably within the range of 150° C. or more and 300° C. or less, for example. The holding time at the heating temperature is preferably within the range of 1 minute to 180 minutes. Furthermore, during the heat treatment, the laminate may be pressed in the lamination direction at a pressure of 30 MPa or less. The atmosphere during the heat treatment may be a nitrogen atmosphere, preferably a nitrogen atmosphere with an oxygen concentration of 500 ppm (volume basis) or less, and more preferably a nitrogen atmosphere with an oxygen concentration of 100 ppm (volume basis) or less.

[0031] According to the metal paste application method of the present embodiment configured as described above, the discharge of metal paste 23 is stopped before the end E in the direction of travel of discharge nozzle 30 in the region to be paste-applied, so that the presence of excess metal paste 23 near the end E of the region to be paste-applied is suppressed. In addition, since the discharge nozzle 30 is caused to move at least up to the end E of the region to be paste-applied while the discharge of metal paste 23 is stopped, the metal paste can be applied up to the end E of the region to be paste-applied. Therefore, the metal paste 23 can be prevented from rising at the end portion E of the area to be paste-applied, and the metal paste 23 can be prevented from flowing around to the surface opposite the joining surface of the first component 11 or the surface opposite the joining surface of the first component 11 during stacking and joining.

[0032] In the metal paste application method of this embodiment, if the position at which the ejection of metal paste 23 is stopped is set within a range of 0.5 mm to 2.0 mm from the end E of the ejection nozzle 30 in the direction of travel in the area intended to be applied with the paste, it is possible to further suppress the rising of the metal paste at the end of the area intended to be applied with the paste, and the metal paste can be applied up to the end E of the area intended to be applied with the paste.

[0033] According to the manufacturing method of the joined body of this embodiment, the metal paste application method of this embodiment includes a paste application step S01 in which the metal paste 23 is applied to one or both of the joining surfaces of the first member 11 and the second member 12, so that it is possible to suppress the metal paste 23 from rising up at the end portion E of the paste application area and to suppress the metal paste from wrapping around to the side opposite the joining surface of the first member 11 or the second member 12. In addition, the metal paste can be applied up to the end portion E of the paste application area. Therefore, a bonded body can be manufactured in which the first member 11 and the second member 12 are bonded well via the bonding layer 13 made of a sintered metal.

[0034] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. In this embodiment, the first member is a circuit layer, the second member is a semiconductor element, and the bonded body is an electronic device (semiconductor device), but the present invention is not limited to this and may be a bonded body in which the first member and the second member are bonded via a bonding layer made of a sintered body of the silver paste of the present invention. EXAMPLES

[0035] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.

[0036] First, the metal pastes shown in Table 1 were prepared. Paste A-1 is Example 7 of the present invention in Japanese Patent No. 6930578. Pastes A-2 and A-3 are pastes in which the viscosity is adjusted by changing the solvent ratio of paste A-1. Paste B is paste A-1 in which the silver powder is replaced with copper powder.

[0037] [Table 1]

[0038] The above-mentioned metal paste was filled into a syringe and a coating test was carried out. As a dispensing device, a Musashi Engineering PC-controlled desktop robot with image recognition function, 350PCsmartSMΩX, was used. The opening size of the discharge port of the slit nozzle used was 0.3mm x 10mm. A copper substrate measuring 35 mm×35 mm×2 mm thick was prepared as the coating target.

[0039] The length of the discharge nozzle in the direction of travel of the area to be coated with the paste was 10 mm, and the metal paste was applied under the conditions shown in Tables 2 to 5, with the height of the discharge nozzle from the coating surface, the distance traveled in the direction of travel of the discharge nozzle while the metal paste was being discharged (discharge distance), the distance traveled in the direction of travel of the discharge nozzle after discharging of the metal paste had stopped (empty drag distance), and the distance traveled in the height direction during empty drag. The moving speed of the discharge nozzle in the forward direction was 20 mm / s, and the moving speed of the discharge nozzle in the height direction was 10 mm / s.

[0040] The thickness of the applied metal paste was measured at the center of the area to be applied with the paste and at the end of the area to be applied with the paste, and the difference in thickness between the end and the center was evaluated. The evaluation results are shown in Tables 2 to 5. The coating thickness of the metal paste was determined as the maximum height measured in the "volume and area measurement" mode using a 3D shape measuring device (Keyence VR5200) after setting a reference on the coating surface of the copper substrate.

[0041] [Table 2]

[0042] [Table 3]

[0043] [Table 4]

[0044] [Table 5]

[0045] As shown in Table 2, comparing Invention Examples 1 to 7 and Comparative Example 1, in which paste A-1 was used as the metal paste and the nozzle height was 0.15 mm, in Invention Examples 1 to 7, in which the discharge of the metal paste was stopped just before the end of the area to be applied with the discharge nozzle proceeded to the end of the area to be applied with the paste, the difference in coating thickness between the end and the center in the direction of advancement was smaller than in Comparative Example 1, in which the metal paste was discharged to the end of the area to be applied with the paste, and the rise of the metal paste was suppressed. Note that in Invention Examples 6 and 7, the discharge nozzle was also moved in the height direction after the discharge of the metal paste was stopped, and the rise of the metal paste was also suppressed.

[0046] Furthermore, as shown in Table 2, when comparing Example 8 of the present invention and Comparative Example 2 in which Paste A-1 was used as the metal paste and the nozzle height was 0.10 mm, in Example 8 of the present invention in which the ejection of the metal paste was stopped just before the end of the area to be applied with the paste and the ejection nozzle was advanced to the end of the area to be applied with the paste, the difference in coating thickness between the end and the center in the advancing direction was smaller than in Comparative Example 2 in which the metal paste was ejected to the end of the area to be applied with the paste, and the rising of the metal paste was suppressed.

[0047] As shown in Table 3, comparing Examples 11 to 14 of the present invention, in which Paste A-2 was used as the metal paste, with Comparative Example 11, in Examples 11 to 14 of the present invention, in which the ejection of the metal paste was stopped just before the end of the area intended to be applied with the paste and the ejection nozzle was advanced to the end of the area intended to be applied with the paste, the difference in coating thickness between the end and the center in the advancing direction was smaller than in Comparative Example 11, in which the metal paste was ejected to the end of the area intended to be applied with the paste, and the rising of the metal paste was suppressed.

[0048] As shown in Table 4, comparing Examples 21 to 24 of the present invention and Comparative Example 21, in which Paste A-3 was used as the metal paste, in Examples 21 to 24 of the present invention, in which the ejection of the metal paste was stopped just before the end of the area intended to be applied with the paste and the ejection nozzle was advanced to the end of the area intended to be applied with the paste, the difference in coating thickness between the end and the center in the advancing direction was smaller than in Comparative Example 21, in which the metal paste was ejected to the end of the area intended to be applied with the paste, and the rising of the metal paste was suppressed.

[0049] As shown in Table 5, comparing Examples 31 to 34 of the present invention, in which Paste B was used as the metal paste, with Comparative Example 31, in Examples 31 to 34 of the present invention, in which the ejection of the metal paste was stopped just before the end of the area intended to be applied with the paste and the ejection nozzle was advanced to the end of the area intended to be applied with the paste, the difference in coating thickness between the end and the center in the advancing direction was smaller than in Comparative Example 31, in which the metal paste was ejected to the end of the area intended to be applied with the paste, and the rising of the metal paste was suppressed.

[0050] From the above, it was confirmed that according to the present invention, even when metal paste is applied by ejecting the metal paste while moving the ejection nozzle in the direction of travel, it is possible to suppress the rising of the metal paste at the end of the ejection nozzle in the direction of travel in the area intended for paste application, and it is possible to apply metal paste in a stable manner. [Explanation of symbols]

[0051] 10 Junction (semiconductor device) 11 First component (circuit layer) 12 Second component (semiconductor element) 13 Bonding layer 23 Metal Paste 30 Discharge nozzle

Claims

1. A method for applying a metal paste, comprising the steps of: discharging a metal paste while moving a discharge nozzle in a travel direction to apply the metal paste; A method for applying a metal paste, comprising: stopping the discharge of the metal paste just before the end of the discharge nozzle in the direction of travel of the discharge nozzle in an area to be applied with the paste; and advancing the discharge nozzle to at least the end while the discharge of the metal paste is stopped.

2. The method for applying metal paste according to claim 1, characterized in that the position at which the ejection of the metal paste is stopped is within a range of 0.5 mm to 2.0 mm from the end of the ejection nozzle in the direction of travel in the area intended for paste application.

3. A method for producing a joined body in which a first member and a second member are joined via a sintered body of a metal paste, comprising the steps of: a paste application step of applying the metal paste to one or both of a joining surface of the first member and a joining surface of the second member; a lamination step of laminating the first member and the second member via the metal paste; a firing step of firing the metal paste to bond the first member and the second member via a sintered body of the metal paste; having 3. A method for producing a joint body, comprising the step of: applying a metal paste according to claim 1 or 2.

Citation Information

Patent Citations

  • Semiconductor manufacturing device

    JP1995007030A

  • Coating device and method of bonding paste

    JP2001135652A

  • Copper paste for joining, method for manufacturing joined body, and method for manufacturing semiconductor device

    JP2021064612A

  • Power module, substrate therefor and method for manufacturing the both

    JP2004172378A

  • Low-temperature joining material and joining method

    JP2008161907A