Polyurethane resin composition for coating elastomer base material, and laminate
A polyurethane resin composition with a polyurethane resin and carbodiimide compound addresses adhesion and solvent resistance issues, offering versatile application to elastomer substrates with improved performance and sustainability.
Patent Information
- Application Number
- JP2023055353
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing polyurethane resin compositions for coating elastomer substrates lack sufficient adhesion and solvent resistance, and require specialized processes like photocuring or dielectric heating, making them less versatile and difficult to apply to complex shapes.
A polyurethane resin composition comprising a polyurethane resin and a carbodiimide compound, with specific elastic modulus and Asker C hardness ranges, applied in an aqueous medium, providing excellent adhesion and solvent resistance to elastomer substrates.
The composition achieves high adhesion and solvent resistance, reducing solvent use and contributing to environmental sustainability, while being applicable to various elastomer shapes without specialized heating processes.
Smart Images

Figure 2024142933000001 
Figure 2024142933000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyurethane resin composition for coating an elastomeric substrate, and to a laminate. [Background technology]
[0002] Since elastomers have poor solvent resistance, their surfaces are provided with a coating film using a coating agent such as solvent-based polyurethane.
[0003] In recent years, coating agents using various types of polyurethane resins for forming such coating films have been developed. Patent Document 1 discloses an aqueous dispersion of a photocurable polyurethane resin having an elongation at break of 10 to 400%. Patent Document 1 also reports that a coating agent using the aqueous dispersion has excellent adhesion to an elastomer substrate.
[0004] Patent Document 2 discloses a water-based paint containing an aqueous dispersion of a polyurethane resin, a carbodiimide compound, an antifriction agent, silicone oil, and a filler. Patent Document 2 reports that a coating obtained by applying the water-based paint and drying it by dielectric heating has excellent adhesion to rubber substrates.
[0005] Patent Document 3 discloses an aqueous dispersion of a polyurethane resin having an alicyclic structure content of 5 to 43% by weight based on the solid content and having an isocyanato group to which a blocking agent is bonded. Patent Document 3 reports that a coating using the aqueous dispersion has excellent adhesion to a rubber substrate.
[0006] Patent Document 4 discloses an aqueous dispersion of a polyurethane resin having a structure derived from a compound having one acidic group and one hydroxyl group in one molecule, and reports that a urethane film using the aqueous dispersion has a low elastic modulus. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2018-076532 A [Patent Document 2] JP 2007-167704 A [Patent Document 3] International Publication No. 2014 / 038565 [Patent Document 4] International Publication No. 2014 / 103689 Summary of the Invention [Problem to be solved by the invention]
[0008] In coating applications, the appropriate material can vary greatly depending on the substrate to be coated, and high adhesion and solvent resistance are required for use in coating applications. In Patent Document 1, a special photocuring process is required for the production of the coating. Therefore, the coating agent in Patent Document 1 is not very versatile. In addition, Patent Document 1 did not consider adhesion to flexible substrates or solvent resistance. In Patent Document 2, special dielectric heating is required, and the electric field inside the heated object must be made uniform, which makes it difficult to apply to rubber substrates with complex shapes. In addition, in Patent Document 2, the composition of the urethane resin dispersion used is not clear. In Patent Document 3, further improvement in the solvent resistance of the coating was sought. In Patent Document 4, further improvements in the adhesion of the urethane film to the substrate and in the solvent resistance were sought.
[0009] An object of the present invention is to solve the above-mentioned problems in the conventional art and to provide a polyurethane resin composition for coating an elastomer substrate, which has excellent adhesion and solvent resistance. [Means for solving the problem]
[0010] The present inventors have conducted various investigations to overcome the problems of the conventional techniques described above, and as a result have found that a polyurethane resin composition for coating an elastomer substrate, which comprises a polyurethane resin (A) and a carbodiimide compound (B), wherein the polyurethane resin (A) has a modulus of elasticity of a film having a thickness of 60 μm and is not more than 100 MPa, and the elastomer substrate has an Asker C hardness of 40 to 80, has excellent adhesion to the elastomer substrate and excellent solvent resistance, thereby completing the present invention.
[0011] Specifically, the present invention relates to the following [1] to
[11] . [1] A polyurethane resin composition for coating an elastomeric substrate, comprising: The polyurethane resin composition contains a polyurethane resin (A) and a carbodiimide compound (B), The elastic modulus of a film of the polyurethane resin (A) having a thickness of 60 μm is more than 0 MPa and not more than 100 MPa, The Asker C hardness of the elastomer base material is 40 to 80. A polyurethane resin composition for coating an elastomeric substrate. [2] The polyurethane resin composition according to [1], wherein the polyurethane resin (A) has a structure derived from the acidic group-free polyol (Aa) and a structure derived from the polyisocyanate (Ab). [3] The polyurethane resin composition further contains an aqueous medium (C), The polyurethane resin (A) further has a structure derived from the acidic group-containing polyol (Ac), The polyurethane resin composition according to [2], wherein the 60 μm-thick film of the polyurethane resin (A) is obtained by heating a composition containing the polyurethane resin (A) and an aqueous medium (C) at 60° C. for 2 hours and then at 120° C. for 2 hours. [4] The polyurethane resin composition according to [2] or [3], wherein the polyurethane resin (A) further has a structure derived from a compound (Ad) having one acidic group and one hydroxyl group in one molecule. [5] The polyurethane resin composition according to [4], wherein the compound (Ad) having one acidic group and one hydroxyl group in one molecule is a hydroxycarboxylic acid. [6] The polyurethane resin composition according to any one of claims [2] to [5], wherein the polyurethane resin (A) further has a structure derived from a chain extender (Ae). [7] The polyurethane resin composition according to any one of [2] to [6], wherein the acidic group-free polyol (Aa) is a polycarbonate polyol and / or a polyester polyol. [8] The polyurethane resin composition according to any one of [2] to [7], wherein the polyisocyanate (Ab) is an aliphatic polyisocyanate and / or an alicyclic polyisocyanate. [9] The polyurethane resin composition according to any one of [1] to [8], comprising a polyurethane resin (A) and a carbodiimide compound (B), and the blending ratio (B / A) of the carbodiimide compound (B) to the polyurethane resin (A) is in the range of 0.005 to 0.300.
[10] A laminate having an elastomer substrate and a urethane resin film (D) on the elastomer substrate, The urethane resin film (D) has a structure derived from a polyurethane resin (A) and a structure derived from a carbodiimide compound (B), The elastic modulus of a film of the polyurethane resin (A) having a thickness of 60 μm is more than 0 MPa and not more than 100 MPa, A laminate, wherein the elastomer substrate has an Asker C hardness of 40 to 80.
[11] A method for producing the laminate according to
[10] , comprising the steps of applying the polyurethane resin composition according to any one of [1] to [9] onto an elastomer substrate, and drying the composition. Effect of the Invention
[0012] The present invention provides a polyurethane resin composition for use as a coating agent for elastomer substrates, which has excellent adhesion and solvent resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In this specification, a numerical range indicated using "~" indicates a range including the numerical values before and after "~" as the minimum and maximum values, respectively. Furthermore, when a composition contains multiple substances corresponding to each component, the amount of each component in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified. In this specification, the term "process" does not only include independent processes, but also includes processes that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.
[0014] [Polyurethane resin composition] The polyurethane resin composition for coating an elastomer substrate (sometimes simply referred to as "polyurethane resin composition" in this specification) contains a polyurethane resin (A) and a carbodiimide compound (B), and the polyurethane resin (A) has a modulus of elasticity of a 60 μm-thick film exceeding 0 MPa and not more than 100 MPa, and the elastomer substrate has an Asker C hardness of 40 to 80.
[0015] The polyurethane resin composition exhibits high adhesion to elastomer substrates and can provide coatings with excellent solvent resistance. Here, "adhesion" refers to adhesion to elastomer substrates having an Asker C hardness of 40 or more and 80 or less. Furthermore, "solvent resistance" preferably refers to resistance to ethanol, acetone, and toluene, and particularly preferably refers to resistance to ethanol.
[0016] In addition, by using an aqueous dispersion of polyurethane resin (A) in which the polyurethane resin (A) is combined with an aqueous medium (C) described below, the polyurethane resin composition can reduce the amount of solvent used in coating applications, and therefore can contribute to the achievement of Goal 7 of the SDGs, etc.
[0017] <Polyurethane resin (A)> The polyurethane resin (A) is not particularly limited as long as it is a resin having a urethane bond. Examples of structures contained in the polyurethane resin (A) include a structure derived from an acidic group-free polyol (Aa), a structure derived from a polyisocyanate (Ab), a structure derived from an acidic group-containing polyol (Ac), a structure derived from a compound (Ad) having one acidic group and one hydroxyl group in one molecule, a structure derived from a chain extender (Ae), and a structure derived from a neutralizer (Af).
[0018] (Polyol (Aa) containing no acidic groups) As the acidic group-free polyol (Aa), a known one can be used. For example, a high molecular weight polyol such as polycarbonate polyol, polyester polyol, polyether polyol, polyurethane polyol, polyesteramide polyol, acrylic polyol, etc. (however, all have a hydroxyl group at the end), or a low molecular weight polyol such as ethylene glycol, propylene glycol, diethylene glycol, butylene glycol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, trimethylolpropane, glycerin, etc. can be used. From the viewpoint of further improving the solvent resistance, the acidic group-free polyol (Aa) is preferably a polycarbonate polyol and / or a polyester polyol, and is particularly preferably a polycarbonate polyol. The acidic group-free polyol (Aa) may be used alone or in combination of two or more kinds.
[0019] Polycarbonate polyols are obtained by reacting one or more polyol components with a carbonate ester or phosgene. From the viewpoints of safety and handling of reagents, etc., polycarbonate polyols obtained by reacting one or more polyol monomers with a carbonate ester are preferred because they are easy to produce and do not produce by-products of terminal chlorinated products.
[0020] As the polyol monomer constituting the polycarbonate polyol, known ones can be used. For example, aliphatic polyols such as linear aliphatic diols such as 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, and 1,9-nonanediol, branched aliphatic diols such as 2-methyl-1,3-propanediol, 1,5-hexanediol, 2-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 2-methyl-1,8-octanediol, and neopentyl glycol; polyhydric alcohols having three or more functional groups such as trimethylolpropane and pentaerythritol; 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanediol, 1,3-cyclopentanediol, 1,4-cycloheptanediol, 2,5-bis(hydroxymethyl)- ... alicyclic polyols such as diols having an alicyclic structure in the main chain, such as 1,4-dioxane, 2,7-norbornanediol, tetrahydrofuran dimethanol, and 1,4-bis(hydroxyethoxy)cyclohexane; aromatic diols such as 1,4-benzene dimethanol, 1,3-benzene dimethanol, 1,2-benzene dimethanol, 4,4'-naphthalenedimethanol, and 3,4'-naphthalenedimethanol; polyester polyols of hydroxycarboxylic acids and diols, such as polyester polyols of 6-hydroxycaproic acid and hexane diol; polyester polyols of dicarboxylic acids and diols, such as polyester polyols of adipic acid and hexane diol; and polyether polyols, such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol. Among these, from the viewpoint of improving adhesion, alicyclic polyols and / or aliphatic polyols are preferred, aliphatic polyols are more preferred, linear aliphatic diols and / or branched aliphatic diols are even more preferred, and linear aliphatic diols are particularly preferred. The polyol monomers may be used alone or in combination of two or more kinds.
[0021] The carbonate ester is not particularly limited, but examples thereof include aliphatic carbonate esters such as dimethyl carbonate and diethyl carbonate; aromatic carbonate esters such as diphenyl carbonate; and cyclic carbonate esters such as ethylene carbonate. In addition, phosgene capable of producing polycarbonate polyol can also be used. Among them, aliphatic carbonate esters are preferred, and dimethyl carbonate is more preferred, from the viewpoint of ease of production of polycarbonate polyol.
[0022] Known polyester polyols can be used as the polyester polyol. For example, polyester polyols obtained by esterification reaction of low molecular weight polyols (e.g., polyols having a molecular weight of 50 to 500) with polycarboxylic acids; polyester polyols obtained by ring-opening polymerization reaction of cyclic ester compounds such as ε-caprolactone; and copolymer polyester polyols thereof. Specifically, polyester polyols include polyester diols such as polyethylene adipate diol, polybutylene adipate diol, polyethylene butylene adipate diol, polyhexamethylene isophthalate adipate diol, polyethylene succinate diol, polybutylene succinate diol, polyethylene sebacate diol, polybutylene sebacate diol, poly-ε-caprolactone diol, poly(3-methyl-1,5-pentylene adipate) diol, and polycondensates of 1,6-hexanediol and dimer acid.
[0023] As the low molecular weight polyol, for example, the above-mentioned polyol monomers can be used. The low molecular weight polyols may be used alone or in combination of two or more kinds.
[0024] Examples of polycarboxylic acids include aliphatic polycarboxylic acids such as succinic acid, adipic acid, sebacic acid, and dodecanedicarboxylic acid; aromatic polycarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and naphthalenedicarboxylic acid; and anhydrides of the aliphatic polycarboxylic acids and aromatic polycarboxylic acids. The polycarboxylic acids may be used alone or in combination.
[0025] The number average molecular weight (Mn) of the acidic group-free polyol (Aa) is preferably 400 to 5,000. When the number average molecular weight of the acidic group-free polyol (Aa) is 400 or more, the performance as a soft segment is good, and it is preferable from the viewpoint of improving adhesion. When the number average molecular weight of the acidic group-free polyol (Aa) is 5,000 or less, the reactivity between the acidic group-free polyol (Aa) and the polyisocyanate (Ab) is not reduced, and problems such as the production process of the urethane prepolymer, which is a synthetic intermediate, taking a long time or the reaction not proceeding sufficiently in the production of the polyurethane resin (A), or the viscosity of the acidic group-free polyol (Aa) becoming high and difficult to handle do not occur. In this specification, Mn is defined as the hydroxyl value and 1 The value is calculated by H-NMR or a value calculated from the quantitative value of the polyol by gas chromatography after alkaline hydrolysis.
[0026] The hydroxyl value of the acidic group-free polyol (Aa) is preferably 20 to 500 mgKOH / g, more preferably 30 to 300 mgKOH / g. When the hydroxyl value is within the above range, the adhesion is further improved. In this specification, the hydroxyl value is the number of milligrams (mg) of potassium hydroxide equivalent to the hydroxyl groups in 1 g of a sample, and can be measured by JIS K 1557 Method A.
[0027] (Polyisocyanate (Ab)) As the polyisocyanate (Ab), known compounds can be used. For example, aromatic polyisocyanate compounds such as 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate (TDI), 2,6-tolylene diisocyanate, and 4,4'-diphenylmethane diisocyanate (MDI) can be used; aliphatic polyisocyanates such as ethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate (PDI), and hexamethylene diisocyanate (HDI) can be used. alicyclic polyisocyanate compounds such as isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-dicyclohexene-1,2-dicarboxylate, 2,5-norbornane diisocyanate, 2,6-norbornane diisocyanate, etc. The structure of the polyisocyanate (b) may be partially or entirely derivatized by isocyanuration, carbodiimidization, biuretization, or the like.
[0028] From the viewpoint of controlling reactivity, etc., the polyisocyanate (Ab) is preferably an aliphatic polyisocyanate compound and / or an alicyclic polyisocyanate compound, and from the viewpoint of further improving solvent resistance, isophorone diisocyanate (IPDI), 4,4'-diphenylmethane diisocyanate (MDI) and 4,4'-dicyclohexylmethane diisocyanate (hydrogenated MDI) are particularly preferred. The polyisocyanate (Ab) may be used alone or in combination of two or more kinds.
[0029] From the viewpoint of efficiently making the elastic modulus of a 60 μm-thick film of the polyurethane resin (A) more than 0 MPa and not more than 100 MPa, the polyisocyanate (Ab) is particularly preferably any one of the following: 1. When the polyurethane resin (A) contains a structure derived from a compound (Ad) having one acidic group and one hydroxyl group in one molecule, the polyisocyanate (Ab) is preferably an alicyclic polyisocyanate compound, and isophorone diisocyanate (IPDI) and 4,4'-dicyclohexylmethane diisocyanate (hydrogenated MDI) are particularly preferred. 2. When the polyurethane resin (A) does not contain a structure derived from a compound (Ad) having one acidic group and one hydroxyl group in one molecule, it is particularly preferable that the polyisocyanate (Ab) contains isophorone diisocyanate (IPDI). 3. When the polyurethane resin (A) does not contain a structure derived from a compound (Ad) having one acidic group and one hydroxyl group in one molecule, it is particularly preferable that the content of the alicyclic structure in the polyurethane resin (A) is 5.0 to 15.0 mass%. In this specification, the content of the alicyclic structure in the polyurethane resin (A) is defined as follows: 1 It can be measured by H-NMR.
[0030] (Blocked isocyanate structure) When the polyurethane resin (A) has a structure derived from the polyisocyanate (Ab), the polyurethane resin (A) may have a blocked isocyanate structure. The blocked isocyanate structure refers to a structure in which a blocking agent is added to an isocyanate group. The blocked isocyanate structure in the polyurethane resin is a structure in which a blocking agent is added to an isocyanate group of a part of the structure derived from the polyisocyanate (Ab), and is usually present at the terminal of the polyurethane resin (A).
[0031] The blocking agent means a compound capable of reacting with an isocyanate group to convert the isocyanate group to another group, and capable of reversibly converting the other group to an isocyanate group by heat treatment. The heat treatment temperature is not particularly limited, but is preferably 80 to 180°C.
[0032] Examples of blocking agents include phenol-based agents such as phenol; aliphatic alcohol-based agents such as methanol; active methylene-based agents such as dimethyl malonate; mercaptan-based agents such as butyl mercaptan; acid amide-based agents such as acetanilide; lactam-based agents such as ε-caprolactam; acid imide-based agents such as succinimide; oxime-based agents such as acetaldoxime, acetoneoxime, and methylethylketoxime; and amine-based agents such as diphenylaniline, aniline, ethyleneimine, and dimethylpyrazole. The blocking agents may be used alone or in combination. The blocked isocyanate structures may be used alone or in combination.
[0033] (Acidic Group-Containing Polyol (Ac)) The acidic group-containing polyol (Ac) contains two or more hydroxyl groups and one or more acidic groups in one molecule. Examples of the acidic group include a carboxy group, a sulfonic acid group, a phosphoric acid group, and a phenolic hydroxyl group, and the carboxy group is preferred. The acidic group-containing polyol (Ac) may be used alone or in combination of two or more kinds.
[0034] As the acidic group-containing polyol (Ac), known polyols can be used. For example, dimethylolalkanoic acids such as 2,2-dimethylolpropionic acid and 2,2-dimethylolbutanoic acid; N,N-bishydroxyethylglycine, N,N-bishydroxyethylalanine, 3,4-dihydroxybutanesulfonic acid, 3,6-dihydroxy-2-toluenesulfonic acid, etc. can be mentioned. Among them, from the viewpoint of easy availability, dimethylolalkanoic acids having 4 to 12 carbon atoms and containing two methylol groups are preferred, and among dimethylolalkanoic acids, 2,2-dimethylolpropionic acid is particularly preferred.
[0035] (Compounds with one acidic group and one hydroxyl group in one molecule (Ad)) The compound (Ad) having one acidic group and one hydroxyl group in one molecule is a compound having one acidic group and one hydroxyl group in one molecule. The acidic group is as described above for the acidic group-containing polyol (Ac). The compound (Ad) having one acidic group and one hydroxyl group in one molecule may be used alone or in combination of two or more kinds.
[0036] As the compound (Ad) having one acidic group and one hydroxyl group in one molecule, known compounds can be used. For example, hydroxycarboxylic acids such as glycolic acid, hydroxypivalic acid, lactic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 10-hydroxydecanoic acid, 12-hydroxydodecanoic acid, 16-hydroxyhexadecanoic acid, trichlorolactic acid, salicylic acid, hydroxybenzoic acid, 1-hydroxy-2-naphthoic acid, 3-hydroxypropionic acid, 2-hydroxyoctanoic acid, 3-hydroxyundecanoic acid, 12-hydroxystearic acid, and 12-hydroxyoleic acid, and hydroxysulfonic acid can be mentioned. Among them, hydroxycarboxylic acids are preferred from the viewpoint of further improving adhesion, and 12-hydroxystearic acid is particularly preferred.
[0037] In the polyurethane resin (A), the total hydroxyl equivalent number of the acidic group-free polyol (Aa), the acidic group-containing polyol (Ac) and the compound (Ad) having one acidic group and one hydroxyl group in one molecule is preferably 50 to 4,000. If the hydroxyl equivalent number is within this range, the polyurethane resin composition containing the aqueous medium (C) can be easily produced. From the viewpoint of the storage stability of the polyurethane resin composition, the hydroxyl equivalent number is preferably 100 to 3,500, more preferably 120 to 3,000, and even more preferably 130 to 2,500.
[0038] The hydroxyl group equivalent number can be calculated by the following formulas (1) and (2). Hydroxyl equivalent number of each polyol component = molecular weight of each polyol component / number of hydroxyl groups of each polyol component (1) Total hydroxyl equivalent number of polyol components = M / total mole number of polyol components (2) In formula (2), M represents [[hydroxyl equivalent number of acidic group-free polyol (Aa) × number of moles of acidic group-free polyol (Aa)] + [hydroxyl equivalent number of acidic group-containing polyol (Ac) × number of moles of acidic group-containing polyol (Ac)] + [hydroxyl equivalent number of compound (Ad) having one acidic group and one hydroxyl group per molecule × number of moles of compound (Ad) having one acidic group and one hydroxyl group per molecule]].
[0039] (Chain extender (Ae)) The chain extender (Ae) is a component that increases the molecular weight of the polyurethane resin (A). The chain extender (Ae) is a compound other than the acidic group-free polyol (Aa), the acidic group-containing polyol (Ac) and the compound (Ad) having one acidic group and one hydroxyl group in one molecule, and is a compound that is reactive with the isocyanato group of the polyurethane prepolymer, which is a synthetic intermediate in the production of the polyurethane resin (A).
[0040] The chain extender (Ae) may be a known one. The chain extender (Ae) may be used alone or in combination of two or more. Examples of the chain extender (Ae) include amine compounds such as ethylenediamine, 1,4-tetramethylenediamine, 2-methyl-1,5-pentanediamine, 1,4-butanediamine, 1,6-hexamethylenediamine, 1,4-hexamethylenediamine, 3-aminomethyl-3,5,5-trimethylcyclohexylamine, 1,3-bis(aminomethyl)cyclohexane, xylylenediamine, piperazine, hydrazine, adipodihydrazide, 2,5-dimethylpiperazine, diethylenetriamine, triethylenetetramine, polyetheramine, and water. Amine compounds are preferred, and polyamine compounds having two or more functional groups in one molecule are particularly preferred. Here, the functional group in the polyamine compound means a primary amino group or a secondary amino group.
[0041] Of the chain extenders (Ae), polyamines having a number average molecular weight (Mn) of 600 or less are preferred. The number average molecular weight of the chain extender (Ae) of 600 or less can increase the cohesive force of the polyurethane resin (A) in the polyurethane resin composition containing the aqueous medium (C). In addition, when the chain extender (Ae) is a polyamine compound, the weight average molecular weight of the polyurethane resin (A) can be increased, and the solvent resistance can be further improved.
[0042] (Neutralizer (Af)) When the polyurethane resin (A) has a structure derived from an acidic group-containing polyol (Ac) and / or a structure derived from a compound (Ad) having one acidic group and one hydroxyl group in one molecule, the polyurethane resin (A) has an acidic group. In this case, the polyurethane resin may further have a structure derived from a neutralizing agent (Af) to neutralize the acidic group. The neutralizing agent (Af) may be used alone or in combination.
[0043] As the neutralizing agent (Af), known neutralizing agents can be used, such as organic amines such as trimethylamine, triethylamine, triisopropylamine, tributylamine, triethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, N-phenyldiethanolamine, 2-dimethylaminoethanol, 2-(dimethylamino)-2-methyl-1-propanol, diethylethanolamine, N-methylmorpholine, and pyridine; inorganic alkalis such as sodium hydroxide and potassium hydroxide; and ammonia.
[0044] The neutralizing agent (Af) preferably has a boiling point of 200° C. or lower, and particularly preferably in the range of −50° C. to 180° C., because when a resin film is formed from a polyurethane resin composition containing an aqueous medium (C), the neutralizing agent volatilizes at the temperature (usually 40° C. to 200° C.) when the polyurethane resin composition is dried, and disappears from the polyurethane resin film, thereby obtaining even better adhesion. When a dry coating film is obtained at a low temperature of 100° C. or lower in a short period of time from a few seconds to an hour, the boiling point is preferably 130° C. or lower, and particularly preferably 100° C. or lower.
[0045] <Preferable structure of polyurethane resin (A)> The polyurethane resin (A) preferably has a structure derived from an acidic group-free polyol (Aa) and a structure derived from a polyisocyanate (Ab). The polyurethane resin (A) preferably further has a structure derived from an acidic group-containing polyol (Ac). When the polyurethane resin (A) has a structure derived from an acidic group-containing polyol (Ac), the dispersibility in the aqueous medium (C) described below can be improved. The polyurethane resin (A) preferably further has a structure derived from a compound (Ad) having one acidic group and one hydroxyl group in one molecule. When the polyurethane resin (A) has a structure derived from a compound (Ad) having one acidic group and one hydroxyl group in one molecule, the solvent resistance tends to be further improved. Here, the compound (Ad) having one acidic group and one hydroxyl group in one molecule is particularly preferably a hydroxycarboxylic acid. It is preferable that the polyurethane resin (A) further has a structure derived from the chain extender (Ae). When the polyurethane resin (A) has a structure derived from the chain extender (Ae), it is easy to adjust the molecular weight of the polyurethane resin (A) to a desired high molecular weight.
[0046] <Characteristics of polyurethane resin (A)> The weight average molecular weight (Mw) of the polyurethane resin (A) is preferably 10,000 to 10,000,000, more preferably 15,000 to 5,000,000, and even more preferably 20,000 to 2,000,000. The weight average molecular weight is measured by gel permeation chromatography (GPC), and a converted value obtained from a calibration curve of a standard polystyrene prepared in advance can be used. By making the weight average molecular weight of the polyurethane resin (A) 10,000 or more, a good coating film tends to be obtained. By making the weight average molecular weight of the polyurethane resin (A) 10,000,000 or less, the drying property of the aqueous dispersion tends to be improved.
[0047] The acid value of the polyurethane resin (A) is preferably 5 to 40 mgKOH / g based on the solid content, more preferably 8 to 35 mgKOH / g, and particularly preferably 10 to 30 mgKOH / g. By setting the acid value of the polyurethane resin (A) in the range of 5 to 40 mgKOH / g based on the solid content, the storage stability tends to be improved. The acid value of the polyurethane resin (A) can be measured in accordance with the indicator titration method of JIS K 1557. When the polyurethane resin (A) contains a structure derived from the neutralizing agent (Af), the neutralizing agent (Af) is removed before measuring the acid value of the polyurethane resin (A). For example, when an organic amine is used as the neutralizing agent (Af), for example, an aqueous dispersion of the polyurethane resin (A) described later is applied onto a glass plate, and the coating film obtained by drying at a temperature of 60°C and under a reduced pressure of 20 mmHg for 24 hours is dissolved in N-methylpyrrolidone (NMP), and the acid value can be measured according to the indicator titration method of JIS K 1557. The acid value of the polyurethane resin (A) can be controlled by the content of the acidic group-containing polyol (Ac) and the chain extender (Ad) which is a compound having one acidic group and one hydroxyl group in one molecule.
[0048] <Composition of polyurethane resin (A)> The content of each structure in the polyurethane resin is preferably as follows. In this specification, the content of each structure in the polyurethane resin (A) is a value calculated from the blending amount (charged amount). The blending amount indicates the amount of the component that is the raw material of each structure used when producing the polyurethane resin (A). In the production of the polyurethane resin (A), each component is almost completely reacted, so the blending amount of each component is taken as the content of each structure in the polyurethane resin (A).
[0049] The structure derived from the acidic group-free polyol (Aa) is contained in the polyurethane resin (A) in an amount of preferably from 30 to 85% by mass, and particularly preferably from 40 to 80% by mass.
[0050] The structure derived from the polyisocyanate (Ab) is contained in the polyurethane resin (A) in an amount of preferably 10 to 50 mass%, particularly preferably 15 to 40 mass%. When the polyurethane resin (A) has a blocked isocyanate structure, the content of the structure derived from the polyisocyanate (Ab) includes the content of the blocked isocyanate structure.
[0051] The structure derived from the acidic group-containing polyol (Ac) is contained in the polyurethane resin (A) in an amount of preferably 0.5 to 20 mass %, and particularly preferably 1.0 to 15 mass %.
[0052] The total amount of the structure derived from the compound (Ad) having one acidic group and one hydroxyl group in one molecule, the structure derived from the chain extender (Ae), and the structure derived from the neutralizer (Af) is preferably 0 to 59.5 mass%, and particularly preferably 5.0 to 30.0 mass%, in the polyurethane resin (A). It is more preferable that the respective contents of the structure derived from the compound (Ad) having one acidic group and one hydroxyl group in one molecule, the structure derived from the chain extender (Ae), and the structure derived from the neutralizer (Af) are as follows.
[0053] The structure derived from the compound (Ad) having one acidic group and one hydroxyl group in one molecule is contained in the polyurethane resin (A) in an amount of preferably 0 to 30.0 mass %, particularly preferably 3.0 to 15.0 mass %.
[0054] The structure derived from the chain extender (Ae) is contained in the polyurethane resin (A) in an amount of preferably from 0 to 15.5% by mass, and particularly preferably from 1.0 to 8.0% by mass. The amount of the chain extender (Ae) used is preferably equal to or less than the equivalent of the isocyanato group that is the chain extension starting point in the polyurethane prepolymer, which is a synthetic intermediate of the polyurethane resin (A), and more preferably 0.70 to 0.99 equivalents of the isocyanato group in the polyurethane prepolymer. By adding the chain extender (Ae) in an amount equal to or less than the equivalent of the isocyanato group in the polyurethane prepolymer, there is a tendency that the molecular weight of the chain-extended polyurethane resin (A) is not reduced and the solvent resistance can be improved.
[0055] When the neutralizing agent (Af) is used, the amount used is preferably in the range of 0.8 to 1.2 times the number of moles of the acidic groups contained in the polyurethane resin (A). When the amount of the neutralizing agent (Af) used is 0.8 times or more the number of moles of the acidic groups, the stability of the resulting dispersion is high, and when it is 1.2 times or less, a coating film with higher adhesion can be obtained in a short time of several seconds to 1 hour under low-temperature drying at 100°C or less.
[0056] In the polyurethane resin (A), the content of urethane bonds is preferably 4.0 to 12.0 mass %, more preferably 5.0 to 10.0 mass %, and even more preferably 6.0 to 9.0 mass %, based on the solid content.
[0057] By setting the content of the urethane bond within the above range, the viscosity of the polyurethane resin composition can be reduced.
[0058] In the polyurethane resin (A), the content of urea bonds is preferably from 0.8 to 5.0 mass %, more preferably from 1.0 to 4.5 mass %, and even more preferably from 2.0 to 4.0 mass %, based on the solid content.
[0059] By setting the content ratio of the urea bond within the above range, the viscosity of the polyurethane resin composition can be reduced.
[0060] In the polyurethane resin (A), the lower limit of the total content of urethane bonds and urea bonds is preferably 6.0 mass% or more, more preferably 7.0 mass% or more, and even more preferably 8.0 mass% or more, based on the solid content. The upper limit of the total content of urethane bonds and urea bonds is preferably 20.0 mass% or less, more preferably 14.0 mass% or less, even more preferably 12.0 mass% or less, and particularly preferably 11.0 mass% or less, based on the solid content. Specifically, it is preferably 6.0 to 20.0 mass%, preferably 7.0 to 14.0 mass%, and more preferably 8.0 to 12.0 mass%.
[0061] By making the total content of the urethane bond and the urea bond 7.0% by mass or more, the stickiness of the coating film surface may be reduced, and by making the total content of the urethane bond and the urea bond 25.0% by mass or less, the adhesion of the coating film to the substrate may be improved.
[0062] The content ratio of urethane bonds and the content ratio of urea bonds in the polyurethane resin (A) can be controlled by the molecular weights of each of the acidic group-free polyol (Aa), the polyisocyanate (Ab), the acidic group-containing polyol (Ac), the compound chain extender (Ad) having one acidic group and one hydroxyl group in one molecule, and the chain extender (Ae), the numbers of hydroxyl groups, isocyanato groups, and amino groups in one molecule, and the usage ratio of each raw material on a solid content basis when producing the polyurethane resin (A).
[0063] The content of urethane bonds, urea bonds, etc. in the polyurethane resin (A) can be roughly calculated from the blending amounts, the molecular weights of each raw material, and the molecular weights or mole numbers of the portions corresponding to each structure.
[0064] (Production method of polyurethane resin (A)) The polyurethane resin (A) can be obtained by any method as long as the desired polyurethane resin (A) can be obtained. For example, the polyurethane resin (A) can be obtained by a production method including a step of reacting an acid group-free polyol (Aa) and a polyisocyanate (Ab). In addition, the polyurethane resin (A) is preferably a polyurethane resin (A) obtained by the following production method for an aqueous polyurethane resin (A) dispersion.
[0065] <<Aqueous dispersion of polyurethane resin (A)>> The aqueous dispersion of polyurethane resin (A) is one in which polyurethane resin (A) is dispersed in an aqueous medium. The proportion (solid content) of polyurethane resin (A) in the aqueous dispersion of polyurethane resin (A) is preferably 5 to 60 mass%, particularly preferably 20 to 50 mass%.
[0066] <<Method for producing aqueous dispersion of polyurethane resin (A)>> The method for producing the aqueous dispersion of polyurethane resin (A) preferably includes the following steps. (I) a step of reacting an acidic group-free polyol (Aa), a polyisocyanate (Ab), an acidic group-containing polyol (Ac), and a compound (Ad) having one acidic group and one hydroxyl group in one molecule in the presence of an organic solvent to obtain a polyurethane prepolymer; (II) mixing the polyurethane prepolymer with an aqueous medium; and (III) A step of increasing the molecular weight of the polyurethane prepolymer with a chain extender (Ae). Furthermore, when a neutralizing agent (Af) is used, a step of neutralizing the acidic groups of the polyurethane prepolymer with the neutralizing agent (Af) may be included after step (I). In addition, a step of removing the organic solvent used in step (I) may be included as step (IV). When the polyurethane resin (A) does not contain a structure derived from the chain extender (Ae), the polyurethane prepolymer obtained in step (I) or step (II) can be used as the polyurethane resin (A). In addition, the aqueous dispersion of polyurethane resin (A) can be produced by known methods described in WO 2016 / 039396, WO 2016 / 163394, and the like.
[0067] ·Process (I) In step (I), the polyurethane prepolymer is obtained by reacting an acid group-free polyol (Aa), a polyisocyanate (Ab), an acid group-containing polyol (Ac), and the compound (Ad) having one acid group and one hydroxyl group in one molecule in the presence of an organic solvent. Examples of the organic solvent include the hydrophilic organic solvents and the same solvents as the film-forming assistants described below. Therefore, the polyurethane prepolymer has a structure derived from the acid group-free polyol (Aa), a structure derived from the polyisocyanate (Ab), a structure derived from the acid group-containing polyol (Ac), and a structure derived from the compound (Ad) having one acid group and one hydroxyl group in one molecule.
[0068] It is preferable that the polyurethane prepolymer has a free isocyanato group content in the range of 0.5 to 5.0% by mass based on the solid content of the polyurethane prepolymer, since this improves dispersibility in aqueous media.
[0069] The acid value (AV) of the polyurethane prepolymer is preferably 4 to 40 mgKOH / g, more preferably 6 to 32 mgKOH / g, and particularly preferably 8 to 29 mgKOH / g. By making the acid value of the polyurethane prepolymer 4 mgKOH / g or more, the dispersibility in an aqueous medium and the storage stability tend to be improved. In addition, by making the acid value of the polyurethane prepolymer 40 mgKOH / g or less, the flexibility of the coating film tends to be increased.
[0070] The "acid value of the polyurethane prepolymer" refers to the acid value of the so-called solid content excluding the solvent used in producing the polyurethane prepolymer and the neutralizing agent used to disperse the polyurethane prepolymer in an aqueous medium.
[0071] Specifically, the acid value of the polyurethane prepolymer can be calculated by the following formula (3).
[0072] [Acid value of polyurethane prepolymer]=[(number of millimoles of acidic group-containing polyol (Ac))×(number of acidic groups in one molecule of acidic group-containing polyol (Ac))+(number of millimoles of compound (Ad) having one acidic group and one hydroxyl group in one molecule)×(number of acidic groups of compound (Ad) having one acidic group and one hydroxyl group in one molecule)]×56.1 / [total mass of polyisocyanate (Ab), acidic group-containing polyol (Ac), blocking agent, non-acidic group-containing polyol (Aa), and compound (Ad) having one acidic group and one hydroxyl group in one molecule] (3)
[0073] In this way, the acid value of the polyurethane prepolymer is adjusted by the contents of the acidic group-containing polyol (Ac) and the compound (Ad) having one acidic group and one hydroxyl group in one molecule.
[0074] ·Process (II) In step (II), the polyurethane prepolymer is mixed with an aqueous medium. The aqueous medium may be a component (C) described later. The method for mixing the polyurethane prepolymer with the aqueous medium is not particularly limited, and may be, for example, a method in which the polyurethane prepolymer is added to an aqueous medium stirred by a homomixer or homogenizer, or a method in which the aqueous medium is added to a polyurethane prepolymer stirred by a homomixer or homogenizer. A mixture of the polyurethane prepolymer and the aqueous medium is obtained by step (II). The mixture of the polyurethane prepolymer and the aqueous medium is preferably a dispersion in which the polyurethane prepolymer is dispersed in the aqueous medium.
[0075] ·Process (III) In step (III), the polyurethane prepolymer is reacted with the chain extender (Ae) to bond the polyurethane prepolymers together, thereby adjusting the molecular weight of the polyurethane resin (A) to a desired range.
[0076] Step (III) may be carried out slowly under cooling, or in some cases, the reaction may be accelerated under heating conditions of 90° C. or less. The reaction time under cooling may be, for example, 0.5 to 24 hours, and the reaction time under heating conditions of 90° C. or less may be, for example, 0.1 to 6 hours.
[0077] The amount of each component used may be the amount that corresponds to the content of each component described above in the polyurethane resin (A).
[0078] <Elastic modulus of polyurethane resin (A) film with a thickness of 60 μm> The elastic modulus of a 60 μm thick film of polyurethane resin (A) (hereinafter also referred to as a "film of polyurethane resin (A)") (hereinafter also referred to as "elastic modulus of polyurethane resin (A)") is more than 0 MPa and not more than 100 MPa. From the viewpoint of further improving adhesion, the lower limit of the elastic modulus of polyurethane resin (A) is preferably 2 MPa or more, more preferably 3 MPa or more. The upper limit of the elastic modulus of polyurethane resin (A) is preferably 80 MPa or less, more preferably 40 MPa or less, further preferably 15 MPa or less, and preferably 10 MPa or less. Specifically, the elastic modulus of polyurethane resin (A) is preferably 2 to 80 MPa, more preferably 2 to 40 MPa. In this specification, the elastic modulus of polyurethane resin (A) is measured by a tensile test specified in JIS K7311. The elastic modulus of the polyurethane resin (A) can be increased by reducing the content of the compound (Ad) having one acidic group and one hydroxyl group in one molecule in the polyurethane resin (A), by adjusting the content of the alicyclic structure within the above-mentioned range, by adjusting the total content of the urethane bond and the urea bond within the above-mentioned range, and the like.
[0079] The film of polyurethane resin (A) is a film consisting of polyurethane resin (A) alone, or a film containing polyurethane resin (A) and, as an optional component, one or more components selected from the group consisting of wetting agents, film-forming assistants, and polymerization initiators, which are described below as other additives.
[0080] The method for producing the film of polyurethane resin (A) is not particularly limited. The method for producing the film of polyurethane resin (A) includes a step of applying polyurethane resin (A) or a composition containing polyurethane resin (A) to a substrate to obtain a substrate coated with polyurethane resin (A) or a composition containing polyurethane resin (A), a step of drying the substrate coated with polyurethane resin (A) or a composition containing polyurethane resin (A) to obtain a coating film of polyurethane resin (A), and a step of separating the coating film of polyurethane resin (A) from the substrate to obtain a film of polyurethane resin (A).
[0081] The composition containing polyurethane resin (A) may contain only one or more components selected from the group consisting of an aqueous medium (C), a wetting agent, a film-forming aid, and a polymerization initiator. Here, the aqueous medium (C), the wetting agent, the film-forming aid, and the polymerization initiator are as described below as other additives. In addition, when the composition containing polyurethane resin (A) contains water and a film-forming aid, the component corresponding to the film-forming aid that also functions as a hydrophilic organic solvent is the hydrophilic organic solvent contained in the aqueous medium (C). In addition, the content of each component in the composition containing polyurethane resin (A) is as described below as the content of the aqueous medium (C) and other additives in the composition of the polyurethane resin composition.
[0082] Examples of methods for applying the polyurethane resin (A) or a composition containing the polyurethane resin (A) include dipping, roll coating, reverse roll coating, gravure roll coating, screen coating, spray coating, knife coating, air knife coating, bar coating, and spin coating.
[0083] In the method for producing a film of the polyurethane resin (A), the substrate is not particularly limited, and may be an inorganic substrate such as glass, or an elastomer substrate.
[0084] The method of drying the substrate coated with the polyurethane resin (A) or the composition containing the polyurethane resin (A) is not particularly limited, and includes a method using heating. The heating method includes a heating method using the heat of self-reaction and a heating method in which the substrate coated with the polyurethane resin (A) or the composition containing the polyurethane resin (A) is actively heated. The active heating method includes a method in which the substrate coated with the polyurethane resin (A) or the composition containing the polyurethane resin (A) is placed in a hot air oven, an electric furnace, or an infrared induction heating furnace and heated. The heating temperature is 40 to 200°C.
[0085] When the polyurethane resin composition contains an aqueous medium (C), the film of the polyurethane resin (A) is a film obtained by heating a composition containing the polyurethane resin (A) and the aqueous medium (C) at 60°C for 2 hours and then at 120°C for 2 hours. Here, the aqueous dispersion of the polyurethane resin (A) contains only the polyurethane resin (A) and the aqueous medium (C), or further contains only one or more components selected from the group consisting of a wetting agent, a film-forming assistant, and a polymerization initiator. Examples of the wetting agent, the film-forming assistant, and the polymerization initiator include the components described below as other additives. In addition, when the aqueous medium (C) contains a hydrophilic organic solvent, the film to be measured obtained from the aqueous dispersion of the polyurethane resin (A) may contain the hydrophilic organic solvent as a film-forming assistant.
[0086] <Carbodiimide compound (B)> As the carbodiimide compound (B), known compounds can be used.
[0087] Examples of the carbodiimide compound (B) include N,N'-di-o-toluylcarbodiimide, N,N'-diphenylcarbodiimide, N,N'-di-2,6-dimethylphenylcarbodiimide, N,N'-bis(2,6-diisopropylphenyl)carbodiimide, N,N'-dioctyldecylcarbodiimide, N-triyl-N'-cyclohexylcarbodiimide, N,N'-di-2,2-di-tert-butylphenylcarbodiimide, N-triyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N'-di-p-hydroxyphenylcarbodiimide, N,N'-dicyclohexylcarbodiimide, and N,N'-di-p-toluylcarbodiimide. Examples of such carbodiimides include the Carbodilite series manufactured by Nisshinbo Chemical Inc., but the present invention is not limited to these examples. The carbodiimide compound (B) may be used alone or in combination of two or more kinds.
[0088] <Other ingredients> The polyurethane resin composition may further contain one or more components selected from the group consisting of an aqueous medium (C) and other additives.
[0089] 《Aqueous medium (C)》 The aqueous medium (C) is water or a mixed medium of water and a hydrophilic organic solvent. Examples of water include tap water, ion-exchanged water, distilled water, and ultrapure water. Examples of hydrophilic organic solvents include ketones such as acetone and ethyl methyl ketone; pyrrolidones such as N-methylpyrrolidone (N-methyl-2-pyrrolidone (NMP)), N-ethylpyrrolidone, N-propylpyrrolidone, N-isopropylpyrrolidone, N-butylpyrrolidone, N-cyclohexylpyrrolidone, N-octylpyrrolidone, N-phenylpyrrolidone, and vinylpyrrolidone; ethers such as diethyl ether and dipropylene glycol dimethyl ether; methanol, ethanol, n-propanol, isopropanol, n-butanol, n-hexanol, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, and the like. Examples of suitable alkyl ethers include alcohols such as ethylene glycol, propylene glycol, and glycerin; polyhydric alcohol alkyl ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; amides such as β-alkoxypropionamide, typified by "KJCMPA(R)-100" manufactured by KJ Chemical Co.; and hydroxyl group-containing tertiary amines such as 2-(dimethylamino)-2-methyl-1-propanol (DMAP). The aqueous medium (C) may be used alone or in combination of two or more kinds.
[0090] Other Additives Other additives are other components other than the aqueous medium (C). As other additives, for example, other resins, surface conditioners, surfactants, emulsifiers, thickeners, urethane catalysts, fillers, foaming agents, oil repellents, pigments, dyes, wetting agents, film-forming assistants, polymerization initiators, hollow foams, flame retardants, defoamers, leveling agents, antiblocking agents, UV absorbers, light stabilizers, plasticizers, antisettling agents, polymerization inhibitors, dispersants, penetration promoters, moisturizing agents, fixing agents, preservatives, antioxidants, antifungal agents, chelating agents, sensitizers, pH adjusters, etc. can be used. Other additives may be used alone or in combination of two or more.
[0091] The film-forming assistant is generally a hydrophilic compound that has the effect of promoting film formation. For example, the film-forming assistant may be the component described above as the hydrophilic organic solvent. The film-forming assistant may also serve as the hydrophilic organic solvent in the aqueous medium (C). That is, the polyurethane resin composition may not contain water, but may contain a hydrophilic organic solvent as a film-forming assistant. Examples of wetting agents include anionic surfactants such as sulfate esters of higher alcohols, salts of sulfate esters of higher alcohols, alkylbenzene sulfonates, and polyoxyethylene alkylphenyl sulfonates; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, and oxyethylene-oxypropylene block polymers; and silicone-based surfactants. Examples of the polymerization initiator include persulfates such as ammonium persulfate, potassium persulfate, and sodium persulfate; azo compounds such as 2,2'-azobisisobutyronitrile and 2,2'-azobis(2,4-dimethylvaleronitrile); and peroxides such as hydrogen peroxide, t-butyl hydroperoxide, benzoyl peroxide, and lauroyl peroxide.
[0092] <Preferred embodiment of polyurethane resin composition> The polyurethane resin composition preferably further comprises an aqueous medium (C). When the polyurethane resin composition further comprises an aqueous medium (C), the combination of the polyurethane resin (A) and the aqueous medium (C) may constitute an aqueous polyurethane resin (A) dispersion. When the polyurethane resin composition further comprises an aqueous medium (C) and an additional additive, the combination of the polyurethane resin (A), the aqueous medium (C) and the additional additive may constitute an aqueous polyurethane resin (A) dispersion. Therefore, when the polyurethane resin composition further comprises an aqueous medium (C) or an aqueous medium (C) and an additional additive, the polyurethane resin composition may comprise an aqueous polyurethane resin (A) dispersion and a carbodiimide compound (B).
[0093] In addition, the polyurethane resin composition is preferably a mixture of a polyurethane resin (A) and a carbodiimide compound (B), and is particularly preferably a mixture of a polyurethane resin (A) and a carbodiimide compound (B) and further contains an aqueous medium (C).
[0094] In the present invention, the polyurethane resin (A) and the carbodiimide compound (B) may partially react with each other. Thus, a polyurethane resin composition containing the polyurethane resin (A) and the carbodiimide compound (B), and a polyurethane resin composition containing the polyurethane resin (A) and the carbodiimide compound (B) may contain a product (partial reaction product) in which a part of the polyurethane resin (A) and a part of the carbodiimide compound (B) have reacted with each other.
[0095] <Composition of Polyurethane Resin Composition> The blending ratio (B / A) of the carbodiimide compound (B) to the polyurethane resin (A) is preferably 0.005 to 0.300, particularly preferably 0.008 to 0.250, from the viewpoint of improving solvent resistance and adhesion. The blending ratio is based on the solid content weight of the polyurethane resin (A) and the carbodiimide compound (B). The aqueous medium (C) is preferably contained in the polyurethane resin composition in an amount of 0 to 80 mass%, more preferably 30 to 75 mass%, and particularly preferably 60 to 70 mass%. Here, the amount of the hydrophilic organic solvent in the aqueous medium (C) is preferably 0 to 20 mass%. The content of the hydrophilic organic solvent that also functions as a film-forming assistant is the amount of the hydrophilic organic solvent in the aqueous medium (C). The pH of the polyurethane resin composition containing the aqueous medium (C) is preferably 5.0 to 10.0. The other additives are contained in the polyurethane resin composition in an amount of preferably 0 to 15% by mass, and particularly preferably 1.0 to 10% by mass.
[0096] <Method of producing polyurethane resin composition> The polyurethane resin composition can be produced by a method of blending a polyurethane resin (A) and a carbodiimide compound (B).
[0097] When the polyurethane resin composition further contains other components (i.e., the aqueous medium (C) and / or other additives), the incorporation of the other components can be carried out at any stage. For example, the polyurethane resin composition may be produced by a method in which the aqueous dispersion of the polyurethane resin (A) and other additives are mixed in advance, and then the carbodiimide compound (B) is incorporated.
[0098] When the polyurethane resin composition further contains an aqueous medium (C) or a combination of the aqueous medium (C) and further additives, the polyurethane resin composition can be produced by a method of blending an aqueous dispersion of the polyurethane resin (A) and a carbodiimide compound (B). Here, the aqueous dispersion of the polyurethane resin (A) is as described above.
[0099] <Elastomer base material> In this specification, the term "elastomer" is meant to include rubber and thermoplastic elastomers.
[0100] The Asker C hardness of the elastomer substrate is 40 to 80. When the Asker C hardness of the elastomer substrate is less than 40, the adhesion of the polyurethane resin composition is poor. When the Asker C hardness of the elastomer substrate is more than 80, the adhesion of the polyurethane resin composition is poor. The Asker C hardness of the elastomer substrate may be 50 to 80, 60 to 80, or 70 to 80. The Asker C hardness is measured in accordance with the spring hardness test type C test method described in Appendix 2 of "7. Hardness test" of JIS K7312. The Asker C hardness of the elastomer substrate can be reduced by using a plasticizer and increased by crosslinking (vulcanization). The Asker C hardness of the elastomer substrate can be changed by selecting the monomer used.
[0101] The elastomer substrate is not particularly limited as long as it has the above-mentioned Asker C hardness. Examples of the material of the elastomer substrate include chloroprene rubber, silicone rubber, thermoplastic polyurethane, gel, etc. These may be used alone or in combination of two or more kinds.
[0102] The shape of the elastomer substrate may be any shape. Specific examples of the shape of the elastomer substrate include sheet-shaped substrates and rod-shaped substrates formed by extrusion molding, press molding, injection molding, etc. Examples of elastomer substrates having such shapes include weather strips and wiper blades for automobiles, shoes, sandals, boots, vibration-proof members for machines and buildings, etc.
[0103] In addition, the elastomer base material contains fillers, antioxidants, vulcanization accelerators, UV absorbers, and lubricants. The composition may contain various additives such as a binder.
[0104] (Method of using polyurethane resin composition) The polyurethane resin composition is used as a coating agent for elastomeric substrates. The method for producing a coating on an elastomer substrate using a polyurethane resin composition is not particularly limited. For example, a resin film (coating) can be obtained by applying the polyurethane resin composition to an elastomer substrate and then drying it.
[0105] The resin film obtained by applying to a substrate and drying is also called a coating film, and the resin film separated from the substrate is also called a film. Therefore, the resin film is a concept including a coating film and a film. The resin film is a resin film containing a polyurethane resin (A).
[0106] Here, the method for applying the polyurethane resin composition and the method for drying the substrate to which the polyurethane resin composition has been applied are as described above for the film of the polyurethane resin (A).
[0107] The thickness of the resin film is not particularly limited, but is preferably adjusted to 0.1 to 200 μm, more preferably 1 to 100 μm, and particularly preferably 5 to 80 μm.
[0108] [Laminate] The laminate according to the present invention has an elastomer substrate and a urethane resin film (D) on the elastomer substrate. Here, the urethane resin film (D) has a structure derived from a polyurethane resin (A) and a structure derived from a carbodiimide compound (B). The elastic modulus of a film of the polyurethane resin (A) having a thickness of 60 μm is more than 0 MPa and 100 MPa or less. The Asker C hardness of the elastomer substrate is 40 to 80.
[0109] In the laminate, the elastic modulus of the elastomer substrate, the polyurethane resin (A), the carbodiimide compound (B), the polyurethane resin (A) film having a thickness of 60 μm, and the Asker C hardness of the elastomer substrate are as described above, including preferred embodiments.
[0110] The urethane resin film (D) has a structure derived from the polyurethane resin (A) and a structure derived from the carbodiimide compound (B). The polyurethane resin (A) and the carbodiimide compound (B) are as described above, including preferred embodiments. The urethane resin film (D) is as described above as a resin film that is a coating of a polyurethane resin composition, including preferred embodiments. Thus, the urethane resin film (D) may contain other components in addition to the structure derived from the polyurethane resin (A) and the structure derived from the carbodiimide compound (B). The other components are as described above for the polyurethane resin composition.
[0111] [Method of manufacturing laminate] The method for producing a laminate according to the present invention preferably includes a step of applying a polyurethane resin composition onto an elastomer substrate and drying the applied composition.
[0112] In the method for producing a laminate, the elastomer substrate and the polyurethane resin composition are as described above, including preferred embodiments. In the method for producing a laminate, the conditions for applying and drying the polyurethane resin composition are as described above, including preferred embodiments. Even if the polyurethane resin (A) contains a structure derived from the neutralizer (Af), when a resin film is formed from the polyurethane resin composition containing the aqueous medium (C), the neutralizer (Af) may volatilize and disappear from the polyurethane resin film, and therefore the urethane resin film (D) may not contain a structure derived from the neutralizer (Af). EXAMPLES
[0113] EXAMPLES Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these.
[0114] [Production Example 1] Polyurethane resin (A) aqueous dispersion (U1) Polycarbonate polyol (product name "UH200" manufactured by UBE Corporation; number average molecular weight 2,000; hydroxyl value 57 mgKOH / g; reaction product of 1,6-hexanediol and dimethyl carbonate, 370 g), 2,2-dimethylolpropionic acid (DMPA, 11.1 g), 12-hydroxystearic acid (HSA, 49.4 g), and isophorone diisocyanate (IPDI, 104 g) were heated in dipropylene glycol dimethyl ether (DMM, 213 g) in the presence of dibutyltin dilaurate (0.3 g) under a nitrogen atmosphere at 80 to 95°C for 5 hours. The reaction mixture was cooled to 80°C, and triethylamine (25.8 g) was added and mixed, of which 658 g was added to water (861 g) under strong stirring. Next, a 35% by mass aqueous solution of diethylenetriamine (DETA, 18.1 g) was added to obtain an aqueous dispersion (U1) of polyurethane resin (A). The solid content was 30% by mass.
[0115] [Production Example 2] Polyurethane resin (A) aqueous dispersion (U2) Polycarbonate polyol (product name "UH200" manufactured by UBE Corporation, 303 g), 2,2-dimethylolpropionic acid (DMPA, 16.2 g), and isophorone diisocyanate (IPDI, 84.5 g) were heated in dipropylene glycol dimethyl ether (DMM, 134 g) in the presence of dibutyltin dilaurate (0.3 g) under a nitrogen atmosphere at 80 to 95 ° C for 5 hours. The reaction mixture was cooled to 80 ° C, and triethylamine (12.3 g) was added and mixed, of which 394 g was added to water (583 g) under strong stirring. Next, a 35 mass % 2-methyl-1,5-pentanediamine aqueous solution (MPMD, 23.1 g) was added to obtain an aqueous dispersion (U2) of polyurethane resin (A). The solid content was 30 mass %.
[0116] [Production Example 3] Polyurethane resin (A) aqueous dispersion (U3) Polycarbonate polyol (product name "UH200" manufactured by UBE Corporation, 440g), 2,2-dimethylolpropionic acid (DMPA, 23.1g), and isophorone diisocyanate (IPDI, 124g) were heated in dipropylene glycol dimethyl ether (DMM, 193g) in the presence of dibutyltin dilaurate (0.3g) under a nitrogen atmosphere at 80-95°C for 5 hours. The reaction mixture was cooled to 80°C, and triethylamine (17.5g) was added and mixed, of which 320g was added to water (478g) under strong stirring. Next, a 35% by mass aqueous solution of 2-methyl-1,5-pentanediamine (MPMD, 10.3g) and adipodihydrazide (ADH, 4.64g) were added to obtain an aqueous dispersion (U3) of polyurethane resin (A). The solid content was 30% by mass.
[0117] [Production Example 4] Polyurethane resin (A) aqueous dispersion (U4) Polyester polyol (product name "Placcel 220N" manufactured by Daicel Corporation; number average molecular weight 2,000; hydroxyl value 57 mgKOH / g; polycaprolactone diol, 370 g), 2,2-dimethylolpropionic acid (DMPA, 11.1 g), 12-hydroxystearic acid (HSA, 49.4 g), and isophorone diisocyanate (IPDI, 104 g) were heated in dipropylene glycol dimethyl ether (DMM, 213 g) in the presence of dibutyltin dilaurate (0.3 g) under a nitrogen atmosphere at 80 to 95°C for 5 hours. The reaction mixture was cooled to 80°C, and triethylamine (25.8 g) was added and mixed, of which 658 g was added to water (861 g) under strong stirring. Next, a 35% by mass aqueous solution of diethylenetriamine (DETA, 18.1 g) was added to obtain an aqueous dispersion (U4) of polyurethane resin (A). The solid content was 30% by mass.
[0118] [Production Example 5] Polyurethane resin (A) aqueous dispersion (U5) Polycarbonate polyol (product name "UH200" manufactured by UBE Corporation, 280g), 2,2-dimethylolpropionic acid (DMPA, 8.20g), 12-hydroxystearic acid (HSA, 37.3g), and isophorone diisocyanate (IPDI, 78.0g) were heated in dipropylene glycol dimethyl ether (DMM, 162g) in the presence of dibutyltin dilaurate (0.3g) under a nitrogen atmosphere at 80-95°C for 5 hours. The reaction mixture was cooled to 80°C, and triethylamine (19.3g) was added and mixed, of which 430g was added to water (564g) under strong stirring. Next, a 35% by mass aqueous solution of diethylenetriamine (DETA, 9.20 g) and a 35% by mass aqueous solution of polyetheramine (product name "JEFFAMINE (registered trademark) D-400" manufactured by HUNTSMAN Corporation, 16.9 g) were added to obtain an aqueous dispersion (U5) of polyurethane resin (A). The solid content was 30% by mass.
[0119] [Production Example 6] Polyurethane resin (A) aqueous dispersion (U6) Polycarbonate polyol (product name "UH200" manufactured by UBE Corporation, 276 g), 2,2-dimethylolpropionic acid (DMPA, 18.2 g), and 4,4'-dicyclohexylmethane diisocyanate (H12MDI, 108 g) were heated in dipropylene glycol dimethyl ether (DMM, 134 g) in the presence of dibutyltin dilaurate (0.3 g) under a nitrogen atmosphere at 80 to 95 ° C for 5 hours. The reaction mixture was cooled to 80 ° C, and triethylamine (13.7 g) was added and mixed, and 395 g of the mixture was added to water (574 g) under strong stirring. Next, a 35 mass % aqueous solution of 2-methyl-1,5-pentanediamine (MPMD, 31.0 g) was added to obtain an aqueous dispersion (U6) of polyurethane resin (A). The solid content was 30 mass %.
[0120] [Production Example 7] Polyurethane resin (A) aqueous dispersion (U7) Polycarbonate polyol (product name "UH200" manufactured by UBE Corporation, 266 g), 2,2-dimethylolpropionic acid (DMPA, 18.6 g), and 4,4'-dicyclohexylmethane diisocyanate (H12MDI, 117 g) were heated in dipropylene glycol dimethyl ether (DMM, 134 g) in the presence of dibutyltin dilaurate (0.3 g) under a nitrogen atmosphere at 80 to 95 ° C for 5 hours. The reaction mixture was cooled to 80 ° C, and triethylamine (14.0 g) was added and mixed, and 392 g of the mixture was added to water (569 g) under strong stirring. Next, a 35 mass % aqueous solution of 2-methyl-1,5-pentanediamine (MPMD, 39.6 g) was added to obtain an aqueous dispersion (U7) of polyurethane resin (A). The solid content was 30 mass %.
[0121] [Production Example 8] Polyurethane resin (A) aqueous dispersion (U8) Polycarbonate polyol (product name "UH200" manufactured by UBE Corporation, 286g), 2,2-dimethylolpropionic acid (DMPA, 19.9g), and 4,4'-dicyclohexylmethane diisocyanate (H12MDI, 126g) were heated in N-methyl-2-pyrrolidone (NMP, 144g) in the presence of dibutyltin dilaurate (0.3g) under a nitrogen atmosphere at 80-95°C for 5 hours. Then, 3,5-dimethylpyrazole (DMPZ, 8.70g) was added and the mixture was stirred at the same temperature for 1.5 hours. The reaction mixture was cooled to 80°C, and triethylamine (15.0g) was added and mixed. Of the mixture, 402g was added to water (567g) under strong stirring. Next, a 35% by mass aqueous solution of 2-methyl-1,5-pentanediamine (MPMD, 30.5 g) was added to obtain an aqueous dispersion (U8) of polyurethane resin (A). The solid content was 30% by mass.
[0122] The number average molecular weight and hydroxyl value of the polycarbonate polyol and polyester polyol are catalog values.
[0123] [Evaluation of elastic modulus of polyurethane resin (A) film] The aqueous dispersions of polyurethane resin (A) obtained in Production Examples 1 to 8 were applied onto a glass plate and heated at 60°C for 2 hours and at 120°C for 2 hours to obtain a polyurethane resin (A) film having a thickness of 60 μm. The obtained polyurethane resin (A) film was punched out using a Super Dumbbell (registered trademark) cutter (SDK-300) manufactured by Dumbbell Co., Ltd. to prepare a test piece. The obtained test piece was subjected to a tensile test using a universal testing machine 5982 manufactured by Instron Co., Ltd. in accordance with a method of JIS K 7311. The measurement conditions were 23°C, 50% humidity, a 500N load cell, and a tensile speed of 100 mm / min.
[0124] [Carbodiimide compound (B) or isocyanate curing agent] The following carbodiimide compounds (B) or isocyanate curing agents were used. The abbreviations in Tables 1 and 2 are as follows. B1: Carbodilite V-02-L2 (carbodiimide compound, solid content 40% by mass) manufactured by Nisshinbo Chemical Inc. B2: Carbodilite V-10 (carbodiimide compound, solid content 40% by mass) manufactured by Nisshinbo Chemical Inc. B1': Vencorex EASAQUA XD870 (alicyclic isocyanate curing agent, solid content 70% by mass) B2': Vencorex EASAQUA L600 (linear aliphatic isocyanate curing agent, solid content 97% by mass)
[0125] [Elastomer base material] The following elastomer substrates were used. The abbreviations in Tables 1 and 2 are as follows. S1: Chloroprene rubber (70mm x 150mm, thickness 2.0mm, manufactured by Engineering Test Services Co., Ltd.) S2: Polyurethane thermoplastic elastomer film ESMER URS (70mm x 150mm, thickness 2.0mm, manufactured by Nihon Matai Co., Ltd.) S3: Urethane gel Hypergel sheet Asker C50 (70mm x 150mm, thickness 3.0mm, manufactured by Exseal Co., Ltd.) S4: Ethylene propylene diene rubber (70 mm x 150 mm, thickness 2.0 mm, manufactured by Engineering Test Services Co., Ltd.) S5: Natural rubber (70mm x 150mm, thickness 2.0mm, manufactured by Engineering Test Services Co., Ltd.) S6: Urethane gel Hypergel sheet Asker C30 (70mm x 150mm, thickness 3.0mm, manufactured by Exseal Co., Ltd.)
[0126] [Asker C hardness evaluation of elastomer substrate] For the elastomer substrates S1 to S6, the substrates were stacked to a thickness of 12 mm, and the Asker C hardness was evaluated in accordance with the spring hardness test type C test method described in Appendix 2 of "7. Hardness test" of JIS K7312. The hardness tester used was an Asker rubber hardness tester C1L type manufactured by Kobunshi Keiki Co., Ltd.
[0127] [Manufacturing method of test sample] For the evaluation test described later, test pieces were prepared by the method described below. Each of the polyurethane resin (A) aqueous dispersion compositions of Examples 1 to 10 and Comparative Examples 1 to 9 described later was applied to elastomer substrates S1 to S6 attached to a galvanized iron plate (70 mm x 150 mm, thickness 0.8 mm, manufactured by TP Giken Co., Ltd.) with double-sided tape (Nistack™ NW-K25, manufactured by Nichiban Co., Ltd.) using a #50 bar coater. When elastomer substrates S1, S2, S4, and S5 were used, they were heated at 150°C for 30 minutes, and when elastomer substrates S3 and S6 were used, they were heated at 100°C for 60 minutes, and then left to stand at 23°C for 24 hours to obtain test samples. The elastomer substrates S1 to S6 were previously degreased with a wafer soaked in acetone.
[0128] [Example 1] To 100 parts by mass of the polyurethane resin (A) aqueous dispersion U1, 4.0 parts by mass of the carbodiimide compound B1, 4.5 parts by mass of a red pigment (manufactured by Toyo Color Co., Ltd.; EMF Pink 2B-1), and 0.6 parts by mass of a surface conditioner (manufactured by BYK-Chemie; BYK-345) were mixed to produce an aqueous dispersion composition of polyurethane resin (A). A test sample was produced by the above-mentioned method using the elastomer substrate S1.
[0129] [Example 2] A test sample was produced in the same manner as in Example 1, except that the aqueous polyurethane resin (A) dispersion U2 was used instead of the aqueous polyurethane resin (A) dispersion U1.
[0130] [Example 3] A test sample was produced in the same manner as in Example 1, except that the aqueous polyurethane resin (A) dispersion U3 was used instead of the aqueous polyurethane resin (A) dispersion U1.
[0131] [Example 4] A test sample was produced in the same manner as in Example 1, except that the aqueous polyurethane resin (A) dispersion U4 was used instead of the aqueous polyurethane resin (A) dispersion U1.
[0132] [Example 5] A test sample was produced in the same manner as in Example 1, except that the aqueous polyurethane resin (A) dispersion U5 was used instead of the aqueous polyurethane resin (A) dispersion U1.
[0133] [Example 6] A test sample was produced in the same manner as in Example 1, except that carbodiimide compound B2 was used instead of carbodiimide compound B1.
[0134] [Example 7] A test sample was produced in the same manner as in Example 1, except that 20 parts by mass of the carbodiimide compound B1 was used per 100 parts by mass of the aqueous dispersion U1 of the polyurethane resin (A).
[0135] [Example 8] A test sample was produced in the same manner as in Example 1, except that 0.5 parts by mass of the carbodiimide compound B1 was used per 100 parts by mass of the aqueous dispersion U1 of the polyurethane resin (A).
[0136] [Example 9] A test sample was produced in the same manner as in Example 1, except that the elastomer substrate S2 was used instead of the elastomer substrate S1.
[0137] [Example 10] A test sample was produced in the same manner as in Example 1, except that the elastomer substrate S3 was used instead of the elastomer substrate S1.
[0138] [Comparative Example 1] A polyurethane resin (A) aqueous dispersion composition was produced by blending 4.5 parts by mass of a red pigment (manufactured by Toyo Color Co., Ltd.; EMF Pink 2B-1) and 0.6 parts by mass of a surface conditioner (manufactured by BYK-Chemie; BYK-345) with 100 parts by mass of the polyurethane resin (A) aqueous dispersion U1. A test sample was produced by the above-mentioned method using the elastomer layer S1.
[0139] [Comparative Example 2] A test sample was produced in the same manner as in Example 1, except that the isocyanate curing agent B1' was used instead of the carbodiimide compound B1.
[0140] [Comparative Example 3] A test sample was produced in the same manner as in Example 1, except that the isocyanate curing agent B2' was used instead of the carbodiimide compound B1.
[0141] [Comparative Example 4] A test sample was produced in the same manner as in Example 1, except that the elastomer substrate S4 was used instead of the elastomer substrate S1.
[0142] [Comparative Example 5] A test sample was produced in the same manner as in Example 1, except that the elastomer substrate S5 was used instead of the elastomer substrate S1.
[0143] [Comparative Example 6] A test sample was produced in the same manner as in Example 1, except that the elastomer substrate S6 was used instead of the elastomer substrate S1.
[0144] [Comparative Example 7] A test sample was produced in the same manner as in Example 1, except that the aqueous polyurethane resin (A) dispersion U6 was used instead of the aqueous polyurethane resin (A) dispersion U1.
[0145] [Comparative Example 8] A test sample was produced in the same manner as in Example 1, except that the aqueous polyurethane resin (A) dispersion U7 was used instead of the aqueous polyurethane resin (A) dispersion U1.
[0146] [Comparative Example 9] A test sample was produced in the same manner as in Comparative Example 1, except that the aqueous polyurethane resin (A) dispersion U8 was used instead of the aqueous polyurethane resin (A) dispersion U1.
[0147] [Adhesion evaluation] The obtained test samples were used to carry out a cross-cut peel test to evaluate adhesion. In the cross-cut peel test, the coating film was cut at 2 mm intervals in an area of 20 mm x 20 mm, adhesive tape was applied, and the adhesive tape was peeled upward at a right angle to the substrate, and the proportion of the coating film that did not peel off was evaluated. For example, when 10 out of 100 pieces remained in the cross-cut peel test, it was recorded as 10 / 100. The larger the number, the higher the adhesion. Since all of the samples in the examples were 80 / 100 or more, it can be said that the adhesion was good.
[0148] [Solvent resistance evaluation] The obtained test samples were subjected to a solvent rubbing test to evaluate the solvent resistance. The solvent rubbing test was performed by applying a load of 900 g to a wafer impregnated with 80% by mass ethanol, rubbing the surface of each test sample back and forth, and measuring the number of back and forth strokes at the time when scratches were confirmed on the coating film. The larger the number of back and forth strokes, the higher the solvent resistance. Since all of the samples in the examples had 25 or more back and forth strokes, it can be said that the solvent resistance was good.
[0149] [Table 1]
[0150] [Table 2]
[0151] The abbreviations used in Tables 1 and 2 are as follows. UH200: Product name "UH200" manufactured by UBE Corporation; Number average molecular weight 2,000; Hydroxyl value 57 mgKOH / g; Polycarbonate polyol obtained by reacting 1,6-hexanediol with dimethyl carbonate 220N: Product name "Placcel 220N" manufactured by Daicel Corporation; Number average molecular weight 2,000; Hydroxyl value 57 mgKOH / g; Polycaprolactone diol IPDI: Isophorone diisocyanate H12MDI: 4,4'-Dicyclohexylmethane diisocyanate HSA: 12-hydroxystearic acid DETA: Diethylenetriamine MPMD: 2-methyl-1,5-pentanediamine ADH: Adipodihydrazide D-400: Product name "JEFFAMINE (registered trademark) D-400" manufactured by HUNTSMAN Corporation; polyetheramine In addition, the numerator of "weight ratio (B / A)" in the table for Comparative Examples 2 and 3 is the weight of the isocyanate curing agent.
[0152] From the results in Table 1, it can be seen that all the examples have both good adhesion and solvent resistance. That is, in all the examples, the adhesion is 75 / 100 or more, and the solvent resistance is 21 or more, and both are further improved. Specifically, it can be seen from Examples 1 to 5 that when the elastic modulus of the polyurethane resin (A) is 100 MPa or less, good adhesion and solvent resistance are exhibited. In addition, as in Example 4, good adhesion and solvent resistance were exhibited whether the acidic group-free polyol (Aa) was a polycarbonate polyol or a polyester polyol. Also, as in Example 6, good adhesion and solvent resistance were exhibited even when the type of carbodiimide compound (B) was changed. Furthermore, good adhesion and solvent resistance were exhibited even when the amount of the carbodiimide compound (B) was changed within the range of Examples 1, 7, and 8. In addition, from Examples 1, 9, and 10, when the Asker C hardness of the elastomer substrate was 40 to 80, good adhesion and solvent resistance were exhibited. On the other hand, the results in Table 2 reveal the following. Comparative Example 1 reveals that the solvent resistance is reduced when the carbodiimide compound (B) is not included. Comparative Examples 2 and 3 reveal that the adhesion is reduced when an isocyanate curing agent is used instead of the carbodiimide compound (B). Furthermore, Comparative Examples 4, 5, and 6 reveal that the adhesion and solvent resistance are reduced when the Asker C hardness of the elastomer substrate is not 40 to 80. In addition, Comparative Examples 7 and 8 reveal that the adhesion is reduced when the elastic modulus of the polyurethane resin (A) exceeds 100 MPa. Comparative Example 9 reveals that the solvent resistance is improved compared to the rubber laminate described in WO2014 / 038565.
Claims
1. 1. A polyurethane resin composition for coating an elastomeric substrate, comprising: The polyurethane resin composition contains a polyurethane resin (A) and a carbodiimide compound (B), The elastic modulus of a film of the polyurethane resin (A) having a thickness of 60 μm is more than 0 MPa and not more than 100 MPa, The Asker C hardness of the elastomer substrate is 40 to 80. A polyurethane resin composition for coating an elastomeric substrate.
2. The polyurethane resin composition according to claim 1 , wherein the polyurethane resin (A) has a structure derived from the acidic group-free polyol (Aa) and a structure derived from the polyisocyanate (Ab).
3. The polyurethane resin composition further contains an aqueous medium (C), The polyurethane resin (A) further has a structure derived from the acidic group-containing polyol (Ac), 3. The polyurethane resin composition according to claim 2, wherein the 60 μm-thick film of the polyurethane resin (A) is obtained by heating a composition containing the polyurethane resin (A) and the aqueous medium (C) at 60° C. for 2 hours and then at 120° C. for 2 hours.
4. The polyurethane resin composition according to claim 2 or 3, wherein the polyurethane resin (A) further has a structure derived from a compound (Ad) having one acidic group and one hydroxyl group in one molecule.
5. The polyurethane resin composition according to claim 4, wherein the compound (Ad) having one acidic group and one hydroxyl group in one molecule is a hydroxycarboxylic acid.
6. The polyurethane resin composition according to claim 2 or 3, wherein the polyurethane resin (A) further has a structure derived from a chain extender (Ae).
7. The polyurethane resin composition according to claim 2 or 3, wherein the acidic group-free polyol (Aa) is a polycarbonate polyol and / or a polyester polyol.
8. The polyurethane resin composition according to claim 2 or 3, wherein the polyisocyanate (Ab) is an aliphatic polyisocyanate and / or an alicyclic polyisocyanate.
9. The polyurethane resin composition according to claim 1 or 2, wherein the polyurethane resin composition is prepared by blending a polyurethane resin (A) and a carbodiimide compound (B), and a blending ratio (B / A) of the carbodiimide compound (B) to the polyurethane resin (A) is in the range of 0.005 to 0.
300.
10. A laminate having an elastomer substrate and a urethane resin film (D) on the elastomer substrate, The urethane resin film (D) has a structure derived from a polyurethane resin (A) and a structure derived from a carbodiimide compound (B), The elastic modulus of a film of the polyurethane resin (A) having a thickness of 60 μm is more than 0 MPa and not more than 100 MPa, A laminate, wherein the elastomer substrate has an Asker C hardness of 40 to 80.
11. A method for producing the laminate according to claim 10, comprising the steps of applying the polyurethane resin composition according to claim 1 onto an elastomer substrate and drying the applied composition.
Citation Information
Patent Citations
Method for forming slip coating on surface of rubber-made part
JP2007167704A
Photocurable aqueous resin dispersion and elastomer laminate
JP2018076532A
Rubber laminate and method for producing same
WO2014038565A1
Aqueous polyurethane resin dispersion and use of same
WO2014103689A1
Cited By
Aqueous polyurethane resin dispersion, coating composition, laminate, and polyurethane resin film
WO2025204296A1