Visible light-transmitting infrared absorbing material

A curable resin composition with specific components forms a cured product that addresses reflow resistance, adhesion, and low haze, ensuring durability and functionality in electronic devices under harsh conditions.

JP2024143016AInactive Publication Date: 2024-10-11TAIYO HOLDINGS CO LTD

Patent Information

Application Number
JP2023055466
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing infrared absorbing materials lack reflow resistance, adhesion with other layers and substrates, moisture and heat resistance, and maintain low haze, which are essential for electronic device functionality in harsh environments.

Method used

A curable resin composition containing a carboxyl group-containing resin with a glass transition temperature of 180°C or higher, an inorganic infrared absorber like cesium-containing tungsten oxide, and an epoxy resin, such as hydrogenated bisphenol A epoxy resin, with optional melamine and a silane coupling agent, to form a cured product with improved adhesion, heat and moisture resistance, and low haze.

Benefits of technology

The cured product exhibits excellent reflow resistance, adhesion, and low haze, maintaining performance under high temperatures and humidity, suitable for electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143016000001
    Figure 2024143016000001
  • Figure 2024143016000002
    Figure 2024143016000002
Patent Text Reader

Abstract

To provide a cured product, particularly an infrared absorbing material, which exhibits superior reflow resistance, superior adhesion to other layers and substrates, superior moist-heat resistance, and low Haze.SOLUTION: A curable resin composition contains a carboxyl group-containing resin, an inorganic infrared absorber, and an epoxy resin, where the carboxyl group-containing resin has a glass transition point (Tg) of 180°C or higher.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a visible light transmitting infrared absorbing material that transmits visible light while absorbing infrared light, and a curable resin composition therefor. [Background technology]

[0002] Today, mobile phones, smartphones, wireless earbuds, LiDAR (Light Detection And Ranging), and other electronic devices are widespread. These electronic devices usually incorporate various optical components because they use electromagnetic waves of specific wavelengths, especially infrared rays. For example, the camera module in a mobile phone or smartphone contains optical components such as an image sensor, a lens, an anti-reflective coating, and a color filter array (CFA). In addition to these optical components, electronic devices usually have infrared absorbing materials to remove infrared rays that have entered from the outside or that have been diffusely reflected inside the device, which can interfere with the electronic device's proper functioning.

[0003] As such an infrared absorbing material, for example, Patent Document 1 proposes a near-infrared absorbing adhesive film that can prevent a decrease in absorptivity in the near-infrared region and simplify the structure of filters for plasma displays. Moreover, Patent Document 2 proposes a near-infrared absorbing hard coat film in which a near-infrared absorbing layer is formed on the surface of a film substrate. Moreover, Patent Document 3 proposes a photosensitive resin composition containing an infrared absorbing agent. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-265638 A [Patent Document 2] JP 2010-164713 A [Patent Document 3] International Publication No. 2011 / 118171 Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, the infrared absorbing material is usually mounted on an adherend such as a substrate by using solder reflow together with the substrate, optical components, and other functional layers such as a resist layer. That is, the infrared absorbing material must have the property of being resistant to the high temperatures in the reflow process, that is, it must have reflow resistance. At the same time, it is desirable for the infrared absorbing material to have a property of high adhesion to other functional layers and the substrate. Furthermore, the infrared absorbing material is also required to have excellent moisture and heat resistance so that its performance is not deteriorated even when used in the harsh environment of an electronic device, which can be hot and humid. Furthermore, it is desirable for the infrared absorbing material to have a low haze value as a characteristic. By maintaining a low haze value, incident light is not scattered on the material surface and leaks out, but is attenuated internally, thereby reducing noise. However, in light of this situation, none of Patent Documents 1 to 3 envisages an infrared absorbing material that has all of these properties.

[0006] From the above viewpoints, the present inventors aimed to provide a cured product, particularly an infrared absorbing material, which has excellent reflow resistance, excellent adhesion to other layers and a substrate, excellent moisture and heat resistance, and further exhibits low haze. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted intensive research in view of the above problems and have found that the above problems can be solved by a curable resin composition containing a resin having a specific functional group in its structure and also having a glass transition temperature of 180°C or higher, an inorganic infrared absorber, and an epoxy resin, and have thus completed the present invention.

[0008] That is, the above object of the present invention is to The above-mentioned problem can be solved by a curable resin composition which contains a carboxyl group-containing resin, an inorganic infrared absorbing agent, and an epoxy resin in its structure, and the carboxyl group-containing resin has a glass transition point (Tg) of 180° C. or higher. Another preferred embodiment of the present invention relates to a curable resin composition, wherein the inorganic infrared absorbing agent is cesium-containing tungsten oxide. Among these, a more preferred embodiment relates to a curable resin composition, wherein the average particle size of the cesium-containing tungsten oxide is 200 nm or less. Another aspect of the present invention relates to a curable resin composition, wherein the epoxy resin is a hydrogenated bisphenol A type epoxy resin. Another preferred embodiment of the present invention relates to a curable resin composition further comprising melamine. Furthermore, another preferred embodiment of the present invention relates to a curable resin composition further comprising a silane coupling agent. Another preferred embodiment of the present invention relates to a dry film having a resin layer made of the curable resin composition. Yet another aspect of the present invention relates to a cured product obtained from the above curable resin composition, and the cured product is an infrared absorbing material. Effect of the Invention

[0009] The cured product obtained from the curable resin composition of the present invention not only has excellent reflow resistance as an infrared absorbing material, but also has excellent adhesion to other functional layers, excellent moisture and heat resistance, and exhibits low haze. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The curable resin composition of the present invention forms a cured product as an infrared absorbing material after curing. Such a curable resin composition of the present invention is characterized in that it also contains, as the resin that is the main component of the cured product, a resin that contains a carboxyl group in its structure and has a glass transition temperature (Tg) of 180° C. or higher, an inorganic infrared absorber, and an epoxy resin. As a result, the cured product obtained from the curable resin composition is a visible light transmitting infrared absorbing material that has excellent adhesion to other functional layers, exhibits low haze, and is also excellent in reflow resistance.

[0011] Specifically, such a cured product of the present invention has a transmittance of less than 3% at a wavelength of 940 nm and a transmittance of 80% or more in the visible region at a film thickness of approximately 11 μm, and further has a haze value of less than 1.0%. Furthermore, the cured product of the present invention is not likely to peel off from other functional layers or the substrate even after heat treatment at 260° C. for 5 minutes. Furthermore, the cured product of the present invention is not likely to peel off from other functional layers or the substrate even after treatment at 85° C. and 85% RH for 500 hours.

[0012] Each of the components used in the present invention will now be described in detail.

[0013] [Carboxyl group-containing resin] The carboxyl groups of the carboxyl-containing resin undergo an addition reaction with the epoxy groups of the epoxy resin, which is contained as another component and will be described later, so that both added resins ultimately become the main components of the cured product.

[0014] As such a carboxyl group-containing resin, a conventionally known resin having a carboxyl group in its structure can be used. Furthermore, the glass transition temperature of the carboxyl group-containing resin must be specifically equal to or higher than 180° C. This allows the resulting cured product to exhibit high reflow resistance.

[0015] In order to provide a more excellent heat resistance, the carboxyl group-containing resin in the present invention preferably has a polymerizable ethylenically unsaturated double bond in its structure. The ethylenically unsaturated double bond is preferably derived from acrylic acid, methacrylic acid, or a derivative thereof.

[0016] Examples of such carboxyl group-containing resins in the present invention include the following compounds (which may be either oligomers or polymers), and examples of such compounds have a glass transition temperature of 180° C. or higher.

[0017] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, alkyl (meth)acrylate, isobutylene, etc.

[0018] (2) Carboxylic acid-containing urethane resins obtained by the polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.

[0019] (3) Carboxylic acid-containing urethane resins obtained by polyaddition reaction of diisocyanates with bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins and biphenol type epoxy resins, and monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, (meth)acrylates or partially acid anhydride modified products thereof, carboxyl group-containing dialcohol compounds and diol compounds.

[0020] (4) A carboxyl group-containing urethane resin obtained by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3) described above, to thereby obtain a terminal (meth)acrylated carboxyl group-containing urethane resin.

[0021] (5) A carboxyl group-containing urethane resin having a terminal (meth)acryloyl group added during the synthesis of the resin (2) or (3) above with a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate.

[0022] (6) A carboxyl group-containing resin obtained by reacting a difunctional or more polyfunctional (solid) epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride to the hydroxyl group present in the side chain.

[0023] (7) A carboxyl group-containing resin obtained by reacting a multifunctional epoxy resin with (meth)acrylic acid, which is further epoxidized with epichlorohydrin to form hydroxyl groups of a bifunctional (solid) epoxy resin, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.

[0024] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.

[0025] (9) A carboxyl group-containing resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or another such polybasic acid anhydride.

[0026] (10) A carboxyl group-containing resin obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid or an unsaturated group-containing monocarboxylic acid ester, and reacting the resulting reaction product with a polybasic acid anhydride.

[0027] (11) A carboxyl group-containing resin obtained by reacting a reaction product obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product with an unsaturated group-containing monocarboxylic acid or an unsaturated group-containing monocarboxylic acid ester, and reacting the resulting reaction product with a polybasic acid anhydride.

[0028] (12) A carboxyl group-containing resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to the resins (1) to (11) above.

[0029] From the viewpoint of obtaining a higher glass transition temperature as a carboxyl group-containing resin, those having at least one structure selected from a norbornyl structure, an adamantyl structure, a cardo structure, a tricyclodecane structure, an isobornyl structure and a dicyclopentanyl structure in their structure are preferred.

[0030] The glass transition temperature of the carboxyl group-containing resin in the present invention is preferably 180° C. or higher, more preferably 190° C. or higher, from the viewpoints of dimensional stability and dispersion stability of the absorbent. The upper limit of the glass transition temperature is not particularly limited, but is preferably 500° C. or lower. The method for adjusting the glass transition temperature of the carboxyl group-containing resin is not particularly limited, and examples thereof include a method of adjusting the composition ratio or polymerization ratio of the resin when synthesizing the compounds (1) to (12), and an appropriate selection of the structure of the resin when synthesizing the compounds (1) to (12).

[0031] Of course, commercially available carboxyl group-containing resins can also be used, such as Artcure RA-4101 (product name; manufactured by Negami Chemical Industries, Ltd.).

[0032] These carboxyl group-containing resins may be used alone or in combination of two or more.

[0033] From the viewpoint of improving the reflow resistance of the cured product, the carboxyl group-containing resin is blended in the curable resin composition in an amount of preferably 30 to 60 mass %, and more preferably about 50 to 60 mass %, calculated as the solid content of the curable resin composition.

[0034] [Inorganic infrared absorbers] The curable resin composition of the present invention contains an infrared absorbing agent, particularly a material that absorbs near-infrared light, due to its characteristics. However, in the curable resin composition of the present invention, from the viewpoint of high heat resistance, low haze and high adhesion of the cured product, organic infrared absorbing agents are avoided in principle, and inorganic infrared absorbing agents, that is, infrared absorbing agents composed of inorganic compounds, which can impart the characteristic of a transmittance of less than 3% at a wavelength of 940 nm to the cured product are selected.

[0035] Examples of inorganic infrared absorbing agents that can be suitably used in the present invention include lanthanum hexaboride, tin-containing indium oxide, antimony-containing tin oxide, and cesium-containing tungsten oxide.

[0036] Among these, a preferred inorganic infrared absorbent is cesium-containing tungsten oxide from the viewpoints of high visible light transmittance and high infrared absorbing ability. In addition, from the viewpoint of further increasing the adhesion of the cured product to the adherend and further suppressing an increase in the haze value, the cesium-containing tungsten preferably has an average particle size of 200 nm or less. This is because the infrared absorption of composite tungsten oxide, an inorganic infrared absorber, is based on the light absorption and scattering characteristic of nanoparticles, known as "localized surface plasmon resonance." That is, when the average particle size of the composite tungsten oxide is 800 nm or less, localized surface plasmon resonance occurs, and the inorganic infrared absorber efficiently absorbs the near-infrared rays irradiated to the curable resin composition of the present invention, making it easier to convert them into thermal energy. If the average particle size is 200 nm or less, the localized surface plasmon resonance will be stronger and the irradiated near-infrared light will be absorbed more strongly, which is more preferable, and if the average particle size is 100 nm or less, the infrared absorption properties and transparency can be maintained, which is even more preferable. Of course, commercially available inorganic infrared absorbing agents can be used, and examples thereof include CWO (registered trademark) (manufactured by Sumitomo Metal Mining Co., Ltd.).

[0037] These inorganic infrared absorbing agents can be used alone or in combination of two or more kinds.

[0038] The inorganic infrared absorbing agent is blended in the curable resin composition in such an amount that the transmittance of the cured product at 940 nm is less than 3%. For example, the inorganic infrared absorbing agent is blended in an amount of preferably about 0.1 to 40 mass %, more preferably about 5 to 25 mass %, calculated as solid content, relative to the curable resin composition.

[0039] [Epoxy resin] The epoxy resin used in the present invention is selected from those having a structure in which the epoxy group undergoes an addition reaction with the carboxyl group of the carboxyl group-containing resin. Through the addition reaction, the epoxy resin becomes a main component of the cured product together with the carboxyl group-containing resin.

[0040] From the viewpoint of homogeneity in the curable resin composition, the epoxy resin preferably has the property of being soluble in the inorganic infrared absorbing agent or the property of being able to easily disperse the inorganic infrared absorbing agent.

[0041] Examples of such epoxy resins include the following: Bisphenol A type epoxy resins;hydroquinone type epoxy resins;bisphenol type epoxy resins;thioether type epoxy resins;brominated epoxy resins;novolac type epoxy resins;biphenol novolac type epoxy resins;bisphenol F type epoxy resins;hydrogenated bisphenol A type epoxy resins;glycidylamine type epoxy resins;hydantoin type epoxy resins;alicyclic epoxy resins;trihydroxyphenylmethane type epoxy resins;bixylenol type or biphenol type epoxy resins or mixtures thereof;bisphenol S type epoxy resins;bisphenol A novolac type epoxy resins;tetraphenylolethane type epoxy resins;heterocyclic epoxy resins;diglycidyl phthalate resins;tetraglycidylxylenoylethane resins;naphthalene group-containing epoxy resins;glycidyl methacrylate copolymer epoxy resins;copolymer epoxy resins of cyclohexylmaleimide and glycidyl methacrylate;epoxy-modified polybutadiene rubber derivatives;CTBN-modified epoxy resins. Of these, from the viewpoint of being able to impart better optical properties to the cured product, the epoxy resin is preferably a hydrogenated type, and more preferably a hydrogenated bisphenol A type epoxy resin.

[0042] In addition, commercially available products can also be used as the epoxy resin. Examples of such products include jER 828, 806, 807, YX8000, YX8034, and 834 (all manufactured by Mitsubishi Chemical Corporation), YD-128, YDF-170, ZX-1059, ST-3000, 4000D, and 6100 (all manufactured by Nippon Steel Chemical & Material Co., Ltd.), EPICLON 830, 835, 840, 850, N-730A, and N-695 (all manufactured by DIC Corporation), and RE-306 (manufactured by Nippon Kayaku Co., Ltd.), of which YX8034 is more preferred. These epoxy resins can be used alone or in combination of two or more.

[0043] The epoxy resin is blended in the curable resin composition such that the number of reactive epoxy functional groups is preferably 0.5 to 2.5 mol, more preferably 0.75 to 1.5 mol, per 1 mol of carboxyl groups contained in the carboxyl group-containing resin, calculated as solid content.

[0044] [melamine] The curable resin composition of the present invention may also contain melamine or a derivative thereof as a curing agent in order to increase the crosslink density of the resulting cured product and further increase the glass transition temperature. Examples of melamine and its derivatives include guanamines such as acetoguanamine and benzoguanamine; melamine; and triazine derivatives such as ethyldiamino-S-triazine, 2,4-diamino-S-triazine, and 2,4-diamino-6-xylyl-S-triazine, among which melamine is preferred. As the melamine, a commercially available product can be used, for example, Melamine (manufactured by Mitsui Chemicals, Inc.). Of course, these melamines can be used alone or in combination of two or more kinds.

[0045] The melamine or its derivative is preferably blended in the curable resin composition in an amount of about 0.1 to 5 mass % in terms of solid content based on the curable resin composition.

[0046] [Silane coupling agents] The curable resin composition of the present invention may further contain a silane coupling agent in order to further improve the adhesion of the cured product to an adherend. Examples of such silane coupling agents include halogen-containing silane coupling agents such as γ-chloropropylmethoxysilane, vinyl group-containing silane coupling agents such as vinylethoxysilane, vinylmethoxysilane, vinyltris(β-methoxyethoxy)silane, vinyltriacetoxysilane, and vinyltrichlorosilane, (meth)acryloyl-containing silane coupling agents such as (meth)acryloxypropyltrimethoxysilane, glycidyl group-containing silane coupling agents such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, mercapto-containing silane coupling agents such as γ-mercaptopropyltrimethoxysilane, and amino group-containing silane coupling agents such as γ-aminopropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane. Of course, it is also possible to use a commercially available silane coupling agent, such as KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd.). Of course, these silane coupling agents can be used alone or in combination of two or more kinds.

[0047] The silane coupling agent is preferably blended in the curable resin composition in an amount of about 0.1 to 2 mass % in terms of solid content relative to the curable resin composition.

[0048] [Other ingredients] Furthermore, various other components can be further added to the curable resin composition of the present invention depending on the application or purpose and within the range that does not impair the effects of the present invention. Examples of such other components include solvents, colorants, release agents, flame retardants, flame retardant assistants, surfactants, antioxidants, defoamers, emulsifiers, leveling agents, anti-repellents, ion trapping agents, thixotropy imparting agents, storage stability improving agents, ozone degradation inhibitors, light stabilizers, thickeners, plasticizers, reactive diluents, electrical conductivity imparting agents, antistatic agents, radiation shielding agents, nucleating agents, lubricants, pigments, metal deactivators, thermal conductivity imparting agents, and physical property adjusters.

[0049] [Dry film] The dry film of the present invention can be produced by applying the above-mentioned curable resin composition onto a first film, drying the composition, and forming a resin layer as a dry coating film. If necessary, a second film may be laminated onto the resin layer.

[0050] The first film has a role of supporting the resin layer of the dry film, and is a film to which a resin composition is applied when forming the resin layer. As the first film, for example, polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyimide films, polyamideimide films, polyethylene films, polytetrafluoroethylene films, polypropylene films, polystyrene films, and other thermoplastic resin films, and surface-treated paper can be used. Among these, polyester films can be preferably used from the viewpoints of heat resistance, mechanical strength, handling, and the like. The thickness of the first film is not particularly limited, but is appropriately selected in the range of about 10 to 150 μm depending on the application. The surface of the second film on which the resin layer is provided may be subjected to a release treatment.

[0051] The second film is provided on the opposite side of the resin layer to the first film for the purpose of preventing dust and the like from adhering to the surface of the resin layer of the dry film and improving handling. As the second film, for example, a film made of a thermoplastic resin exemplified as the first film, surface-treated paper, etc. can be used, among which polyester film, polyethylene film, and polypropylene film (biaxially oriented polypropylene film (OPP)) are preferred. The thickness of the second film is not particularly limited, but is appropriately selected within the range of about 10 to 150 μm depending on the application. The surface of the second film on which the resin layer is provided may be subjected to a release treatment.

[0052] [Cured product] The cured product of the present invention can be obtained by thermally curing the above-mentioned curable resin composition or dry film.

[0053] The method for obtaining a cured product from the curable resin composition of the present invention is not particularly limited, and may be a conventionally known method. For example, the composition may be cured by heating at 150 to 230°C. As an example, after applying a curable resin composition onto a substrate (including a board) (e.g., applying using an applicator, etc.), a drying step may be carried out as necessary to remove the organic solvent in the composition, and then a thermal curing step may be carried out to thermally crosslink the composition by heating.

[0054] Examples of the substrate include printed wiring boards and flexible printed wiring boards on which circuits have been formed in advance using copper or the like, as well as copper-clad laminates for high-frequency circuits using materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven cloth epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, fluororesin / polyethylene / polyphenylene ether, polyphenylene oxide / cyanate, etc., and include copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc. Among these, it is preferable to use a glass substrate for the curable resin composition of the present invention from the viewpoint of adhesion.

[0055] As a coating method, for example, an organic solvent is used to adjust the viscosity to a level suitable for the coating method, and the composition is applied onto a substrate by a method such as an inkjet method, a dip coating method, a flow coating method, a roll coating method, a bar coater method, a screen printing method, or a curtain coating method, and then the organic solvent contained in the composition is evaporated and dried at a temperature of about 60 to 100° C., thereby forming a tack-free resin layer.

[0056] Drying can be carried out using a hot air circulation drying oven, IR oven, hot plate, convection oven, etc. (a method in which hot air in the dryer is brought into countercurrent contact using a heat source that uses steam for air heating, or a method in which hot air is blown onto the support from a nozzle).

[0057] Examples of the heating method include heating with a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, a hot plate, a vacuum oven, a vacuum press, and the like.

[0058] In addition, when the above-mentioned dry film is used, the resin layer can be formed on the substrate by laminating the resin layer on the substrate with a laminator or the like so that the resin layer contacts the substrate, and then peeling off the first film. The dry film is preferably laminated to the substrate under pressure and heat using a vacuum laminator or the like. By using such a vacuum laminator, when a patterned substrate is used, even if the substrate surface is uneven, the dry film follows the pattern and adheres to the substrate, so that no air bubbles are mixed in, and the filling of the recesses on the substrate surface is also improved. The pressure condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.

[0059] Specifically, the cured product of the present invention has a transmittance of less than 3% at a wavelength of 940 nm and a transmittance of 80% or more in the visible region at a film thickness of approximately 11 μm, and further has a haze value of less than 1.0%. Furthermore, the cured product of the present invention is not likely to peel off from other functional layers or the substrate even after heat treatment at 260° C. for 5 minutes. Furthermore, the cured product of the present invention is not likely to peel off from other functional layers or the substrate even after treatment at 85° C. and 85% RH for 500 hours. Therefore, the cured product of the present invention is suitably used as an excellent infrared absorbing material whose performance degradation is suppressed even during its severe production process and in a severe usage environment. The shape of the cured product of the present invention is not particularly limited since it is selected according to the application, and examples of the shape include a film, sheet, rod, lens, etc.

[0060] [Infrared absorbing material] The cured product of the present invention can be molded into a desired shape as exemplified above and used as various infrared absorbing materials. More specifically, examples of the infrared absorbing agent include lenses having a function of absorbing and cutting near-infrared rays (camera lenses for digital cameras, mobile phones, car-mounted cameras, etc., optical lenses such as f-θ lenses and pickup lenses) and optical filters for semiconductor light receiving elements, coating agents for near-infrared absorbing films and near-infrared absorbing plates that block heat rays for energy saving, coating agents for agricultural near-infrared absorbing films for the purpose of selectively utilizing sunlight, recording media that utilize the absorption heat of near-infrared rays, near-infrared cut filters for electronic devices, near-infrared filters for photography, protective glasses, sunglasses, heat ray blocking films, dyes for optical recording, optical character reading and recording, for preventing confidential document duplication, electrophotographic photoreceptors, laser welding, noise cut filters for CCD cameras, filters for CMOS image sensors, and other optical members.

[0061] EXAMPLES The present invention will be specifically described below with reference to examples and comparative examples. However, it goes without saying that the present invention is not limited to the following examples. Unless otherwise specified, the "parts" and "%" shown are based on mass. EXAMPLES

[0062] [Preparation of Curable Resin Composition] According to the blending amounts shown in Table 1 below, each component was blended, mixed and stirred, and then kneaded in a three-roll mill to prepare curable resin compositions of Example 1 and Comparative Examples 1 and 2. The values ​​in the table represent parts by mass and indicate the solid content.

[0063] [Table 1] The details of the components corresponding to each number in Table 1 above are as follows: *1 Artcure RA-4101; acrylic acrylate resin; manufactured by Negami Chemical Industries, Ltd. (acid value of solid content: 90 mg KOH / g) *2 Zeffle GK-570; Tetrafluoroethylene-vinyl monomer copolymer; Daikin Industries, Ltd. *3 CWO (registered trademark); Cesium-containing tungsten; manufactured by Sumitomo Metal Mining Co., Ltd. *4 Near infrared absorbing agent: manufactured by Nippon Carlit Co., Ltd. *5 Hydrogenated epoxy resin: manufactured by Mitsubishi Chemical Corporation (epoxy equivalent: 270g / eq) *6 Melamine; manufactured by Mitsui Chemicals, Inc. *7 Hexamethylene diisocyanate-based polyisocyanate; manufactured by Asahi Kasei Corporation *8 3-Glycidoxypropyltrimethoxysilane; manufactured by Shin-Etsu Chemical Co., Ltd.

[0064] [Preparation of dry film for evaluation] The curable resin compositions prepared in the amounts shown in Table 1 were applied to a 25 μm-thick PET film (E-5041, manufactured by Toyobo Co., Ltd.) using an applicator, and dried for 30 minutes in a hot air circulation drying oven at 80°C to prepare dry films for evaluation with a film thickness of 10 μm.

[0065] [Test Example 1. Heat resistance test] To evaluate the heat resistance, the rate of change in transmittance before and after reflow was measured as follows. A soda lime glass having a glass thickness of 1 mm was washed with alcohol, dried, and then laminated with each of the dry films obtained in the above [Preparation of dry film for evaluation], and heated in a hot air circulation drying oven at 170°C for 60 minutes to cure the curable resin composition. The total light transmittance of each of the obtained test cured products was measured using a 1 mm soda lime glass as a reference. The total light transmittance was measured using an ultraviolet-visible light spectrophotometer (V-670EX, manufactured by JASCO Corporation) in accordance with JIS K 7361-1. Thereafter, the cured product for evaluation was passed through a reflow oven previously set at a maximum temperature of 260° C., and then the total light transmittance was measured in the same manner as above. Regarding the measurement results of the total light transmittance before and after reflow, the rate of change in transmittance at a wavelength of 940 nm was calculated and evaluated according to the following criteria. ○: Less than 2% △: 2% or more but less than 50% ×: 50% or more

[0066] [Test Example 2. Moisture and heat resistance test] To evaluate the humidity and heat resistance, the rate of change in transmittance before and after a constant temperature and humidity test was measured as follows. Each dry film obtained in the above [Preparation of dry film for evaluation] was laminated on a 1 mm soda lime glass, and heated in a hot air circulation drying oven at 170°C for 60 minutes to cure the curable resin composition. The total light transmittance of each of the obtained cured products for evaluation was measured using a 1 mm soda lime glass as a reference. The total light transmittance was measured using an ultraviolet-visible light spectrophotometer (V-670EX, manufactured by JASCO Corporation) in accordance with JIS K 7361-1. Thereafter, the cured product for evaluation obtained above was placed in a thermo-hygrostat at 85° C. and 85% RH for 500 hours, after which it was taken out and the total light transmittance was measured in the same manner as above. Regarding the measurement results of the total light transmittance before and after the constant temperature and humidity test, the rate of change in transmittance at a wavelength of 940 nm was calculated and evaluated according to the following criteria. ○: Less than 2% △: 2% or more but less than 50% ×: 50% or more

[0067] [Test Example 3. Adhesion test] Each dry film obtained in the above [Preparation of dry film for evaluation] was laminated on a soda lime glass (16 cm x 11 cm, thickness 1 mm) and heated in a hot air circulation drying oven at 170 ° C for 60 minutes to cure the curable resin composition. Furthermore, an upper layer material was applied and cured to obtain a substrate for evaluation. The obtained cured product for evaluation was subjected to an adhesion test according to the procedure shown below, and the results were evaluated. The adhesion of the reflective layer (cured product) formed on the substrate as described below can be measured by a cross-cut test conforming to JIS K5600-5-6. Each evaluation substrate was scratched so that there were 100 1mm x 1mm squares. Peeling of the reflective layer was then confirmed using tape peeling. The peeling rate in the cross-cut test is the ratio of the "peeled" area to the area of ​​all squares. The "peeled" area is the total area of ​​the parts of the grid where the reflective layer (cured product) has peeled off. The adhesion was evaluated according to the following criteria. ○: The "peeling rate" was 0% (no peeling). ×: The "peeling rate" was more than 0% and less than 5%.

[0068] [Test Example 4. Haze test] Each dry film obtained in the above [Preparation of dry film for evaluation] was laminated on 1 mm soda lime glass, and heated in a hot air circulation drying oven at 170°C for 60 minutes to cure the curable resin composition. The haze value of each of the obtained cured products for evaluation was measured using 1 mm soda lime glass as a standard. The haze value was measured using a haze meter (Haze Meter NDH 7000II manufactured by Nippon Denshoku Industries Co., Ltd.) and was evaluated according to the following criteria. ○: Less than 1% △: 1% or more but less than 2% ×: 2% or more

[0069] [Table 2]

Claims

1. Carboxyl group-containing resin, Inorganic infrared absorbers, and Epoxy Resin A curable resin composition comprising: The glass transition point (Tg) of the carboxyl group-containing resin is 180° C. or higher. Curable resin composition.

2. The curable resin composition according to claim 1 , wherein the inorganic infrared absorbing agent is cesium-containing tungsten oxide.

3. The curable resin composition according to claim 2 , wherein the average particle size of the cesium-containing tungsten oxide is 200 nm or less.

4. The curable resin composition according to claim 1 , wherein the epoxy resin is a hydrogenated bisphenol A type epoxy resin.

5. The curable resin composition according to claim 1 , further comprising melamine.

6. The curable resin composition according to claim 1 , further comprising a silane coupling agent.

7. A dry film having a resin layer made of the curable resin composition according to claim 1.

8. A cured product obtained from the curable resin composition according to any one of claims 1 to 6.

9. The cured product according to claim 8 , wherein the cured product is an infrared absorbing material.

Citation Information

Patent Citations

  • Near infrared absorbing adhesive film, antireflection film with near infrared absorbing adhesive layer, electromagnetic wave shield film with near infrared absorbing adhesive layer, and filter for plasma display

    JP2009265638A

  • Near-infrared ray absorption hard coat film and antireflection film

    JP2010164713A

  • Photosensitive resin composition and light receiving device

    WO2011118171A1

Cited By

  • Retaining wall assembly of ecological type and method using thereof

    KR1020240083802A