Plastic refractory, manufacturing method of plastic refractory, and spraying application method of plastic refractory

By integrating coarse aggregates with specific particle sizes and controlled kneading, the issue of plastic refractories sticking to discharge hoses is mitigated, ensuring continuous spraying and enhanced work efficiency.

JP2024143085APending Publication Date: 2024-10-11SHINAGAWA REFRACTORIES CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023055580
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Plastic refractories used in spray construction tend to stick to the inner surface of discharge hoses, leading to clogging and reduced discharge, which affects work efficiency and necessitates time-consuming cleaning.

Method used

Incorporating coarse aggregates with a particle size of 3 mm or more into the plastic refractory composition, along with specific kneading and granulating processes, enhances anti-sticking properties and maintains excellent compressed air conveyance.

Benefits of technology

Prevents the plastic refractory from sticking to the discharge hose, ensuring continuous spraying and improved work efficiency by maintaining hose integrity and reducing rebound loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143085000001
    Figure 2024143085000001
  • Figure 2024143085000002
    Figure 2024143085000002
Patent Text Reader

Abstract

To provide a plastic refractory, in performing spraying application, excellent in compressed air conveyability though having viscosity and hard to adhere to an inner face of a discharge hose.SOLUTION: A plastic refractory has a base material containing a refractory raw material and a binder, and further has a coarse grain aggregate having a grain size of 3 mm or larger.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plastic refractory for spray application. [Background technology]

[0002] Plastic refractories generally refer to refractories in the form of wet clay, which are made by mixing refractory aggregate with plastic raw materials such as clay and adding water and other ingredients (see Non-Patent Document 1). Unlike castable refractories, which are applied in a slurry form, plastic refractories have a low water content, so there is no risk of explosion and the furnace temperature can be raised in a short time after application is completed. In addition, plastic refractories have excellent spalling resistance compared to castable refractories and firebricks made of the same material.

[0003] As shown in the following Patent Documents 1 and 2, for example, plastic refractories can be sprayed using compressed air, which makes them more efficient to apply than conventional ramming applications. They are therefore widely used as lining materials for heating furnaces, soaking furnaces, and torpedo cars, as well as for the lining and repair of various industrial furnaces. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 57-073388 [Patent Document 2] Japanese Utility Model Application Publication No. 61-038498 [Non-patent literature]

[0005] [Non-Patent Document 1] Eiji Motoki, "Unshaped Refractories and Powder Technology (Part 12) Chapter 3 Rheology and Multiphase Flow of Unshaped Refractories - Application Edition: Plastic Refractories -", ​​Refractories, Refractories Technology Association, 2004, Vol. 56, No. 7, pp. 361-366 Summary of the Invention [Problem to be solved by the invention]

[0006] Plastic refractories for spray application have a certain degree of viscosity to ensure spray properties, but because of this, during application, the plastic refractories gradually adhere to the inner surface of the discharge hose, narrowing the flow path and reducing the discharge rate, eventually causing blockage, i.e., so-called hose clogging, which may make spraying impossible.

[0007] It takes a lot of time to remove the clogged plastic refractory material and resume construction, which may significantly reduce work efficiency.

[0008] The present invention has been made in consideration of the above-mentioned circumstances, and its object is to provide a plastic refractory material which, even though it has viscosity, has excellent compressed air transport properties when used for spray application, and is also unlikely to adhere to the inner surface of a discharge hose. [Means for solving the problem]

[0009] The plastic refractory according to the present invention is characterized in that the plastic refractory has a base material containing refractory raw materials and a binder, and further has coarse aggregate having a grain size of 3 mm or more.

[0010] In the plastic refractory material according to the present invention, it is preferable that the grain size of the coarse aggregate is 3 mm or more and 8 mm or less.

[0011] In the plastic refractory material according to the present invention, it is preferable that the grain size of the coarse aggregate is 3 mm or more and 5 mm or less.

[0012] In the plastic refractory material according to the present invention, it is preferable that the coarse aggregate is 15% by weight or more and 30% by weight or less with respect to 100% by weight of the base material.

[0013] The method for producing a plastic refractory according to the present invention is characterized in that it includes the steps of: kneading and granulating at least the refractory raw material and the binder to produce the base material; and kneading and granulating the base material by further adding the coarse aggregate having a particle size of 3 mm or more.

[0014] In the method for producing a plastic refractory material according to the present invention, it is preferable that the step of further adding, kneading and granulating the coarse aggregate having a particle size of 3 mm or more is carried out for 15 seconds or more and 70 seconds or less. Effect of the Invention

[0015] The plastic refractory according to the present invention contains coarse aggregate that does not have "stickiness that causes adhesion," so that when spraying is performed using a discharge hose, the plastic refractory is less likely to stick to the inner surface of the discharge hose. Therefore, even if the plastic refractory does stick to the inner surface of the discharge hose once, the coarse aggregate that does not have the stickiness that causes adhesion acts to scrape off the stuck matter that has stuck to the inner surface of the discharge hose, thereby preventing clogging of the discharge hose. Therefore, when spraying is performed using the plastic refractory according to the present invention, even though it has viscosity, it has excellent compressed air transportability and is less likely to stick to the inner surface of the discharge hose. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] An embodiment of the plastic refractory material according to the present invention will be described below. (Plastic refractories) The plastic refractory according to the present invention has a base material containing a refractory raw material and a binder, and further contains coarse aggregate having a grain size of 3 mm or more.

[0017] Examples of refractory raw materials for constituting the base material that can be applied to the present invention include known refractory raw materials such as alumina-based, spinel-based, alumina-silica-based, SiC-based, magnesia-based, and carbon-based materials, and only one of these may be used, or two or more may be used in combination.

[0018] The particle size of the refractory raw material is preferably less than 3 mm to suppress rebound loss during spray application, and is preferably smaller than the coarse aggregate added to the base material. A particle size equal to or larger than the coarse aggregate described below is not preferable because it weakens the anti-adhesion effect of the coarse aggregate. Note that rebound loss refers to the phenomenon in which, when a plastic refractory is sprayed onto a work surface with a spraying device, part of it falls off without adhering to the work surface.

[0019] Examples of binders for constituting the base material that can be applied to the present invention include sodium silicate, sodium phosphate, aluminum sulfate, cement, clay, etc., and only one of these may be used, or two or more may be used in combination.

[0020] Coarse aggregates applicable to the present invention include coarse refractory aggregates having a grain size of 3 mm or more, such as alumina, spinel, alumina-silica, SiC, magnesia, and carbon.

[0021] The particle size of the coarse aggregate applicable to the present invention is 3 mm or more, preferably 3 mm or more and 8 mm or less, more preferably 3 mm or more and 5 mm or less. When the particle size of the coarse aggregate is 5 mm or less, rebound loss during spray application is reduced and the adhesion rate can be increased, which is preferable. On the other hand, when the particle size of the coarse aggregate is less than 3 mm, the effect of preventing adhesion to the inner surface of the discharge hose is weak, which is not preferable.

[0022] The particle size of the coarse aggregate in the present invention can be measured using a sieve commonly used in the technical field of the present invention. For example, sieves having openings of 8 mm, 5 mm, 3 mm, and 1 mm are stacked in order of the widest opening, and the coarse aggregate is placed on the top sieve and measured while vibrating. The particle size of the coarse aggregate that passes through the 8 mm sieve and is captured on the 5 mm sieve is defined as 5 to 8 mm, and the particle size of the coarse aggregate that passes through the 5 mm sieve and is captured on the 3 mm sieve is defined as 3 to 5 mm.

[0023] The content of the coarse aggregate in the plastic refractory is preferably 15% by weight or more and 30% by weight or less, and more preferably 20% by weight or more and 30% by weight or less, relative to 100% by weight of the base material.

[0024] The amount of coarse aggregate added is preferably 15% by weight or more, since it is more effective in preventing adhesion to the inner surface of the discharge hose, and is preferably 30% by weight or less, since it reduces rebound loss during spray application and improves adhesion rate.

[0025] The material of the coarse aggregate is preferably the same as that of the refractory material of the base material in order to avoid chemical reactions caused by heat during operation of the various heating furnaces.

[0026] The shape of the coarse aggregate preferably has one or more angular parts, and is preferably unpolished crushed particles of clinker or raw stone. A shape with angular parts is preferable because it makes it easier to scrape off stuck material, improving the sticking prevention effect.

[0027] (Method of manufacturing plastic refractories) The method for producing a plastic refractory according to the present invention includes the steps of kneading and granulating the above-mentioned refractory raw material and a binder to produce a base material, and further adding the above-mentioned coarse aggregate having a particle size of 3 mm or more to the base material, kneading and granulating the base material.

[0028] By adding coarse aggregate to a base material composed of at least refractory raw materials and a binder, which are mixed and granulated, the material has excellent compressed air transportability even for highly viscous plastic refractories, and can prevent adhesion to the inner surface of the discharge hose, greatly improving spray application properties.

[0029] In addition to the refractory raw material and the binder, other known additives such as reinforcing materials for improving strength and anti-explosion agents can be added to the base material as appropriate. These additives do not impair the effects of the present invention. It is preferable to knead and granulate these additives together when kneading and granulating the base material.

[0030] The coarse aggregate is desirably added after mixing and granulating at least one or more types of refractory raw materials as the base material with a binder. If the coarse aggregate is added after mixing and granulating the refractory raw materials with a binder, the fine powder of the refractory raw materials and the binder are less likely to adhere to the surface of the coarse aggregate, and as a result, a sufficient anti-sticking effect is easily achieved.

[0031] That is, the fine powder of the refractory raw material is granulated with a binder to achieve the viscosity required for a plastic refractory. The granules deformed by the impact during spraying are integrated with the wall surface and other granules due to their viscosity to form a lining. However, when the fine powder of the refractory raw material and the binder are attached to the surface of the coarse aggregate, they bounce back without being deformed by the impact during spraying, which makes it easy for the rebound loss to occur and makes it difficult to form a lining.

[0032] On the other hand, if the coarse aggregate is added and mixed after granulating the fine powder of the refractory raw material, the granules act as a cushion and the coarse aggregate can be incorporated into the lining. The coarse aggregate incorporated into the lining is expected to prevent cracks from progressing and improve abrasion resistance, which will extend the life of the lining.

[0033] In addition, the kneading time after adding the coarse aggregate to the granulated base material affects the sticking prevention effect and viscosity. The kneading time after adding the coarse aggregate to the base material is preferably 15 seconds to 70 seconds, more preferably 20 seconds to 50 seconds. If the kneading time is 15 seconds or more, the coarse aggregate is evenly dispersed in the base material, making it easier to achieve the sticking prevention effect. If the kneading time is 70 seconds or less, the granulated fine powder is less likely to be broken apart by the coarse aggregate, making it easier to achieve the viscosity required for a plastic refractory.

[0034] The coarse aggregate may be added, for example, not only in a refractory plant but also in a steelworks, etc. Only the base material may be transported from the refractory plant to the steelworks construction site, and the refractories generated in the steelworks after use may be crushed and subjected to particle size adjustment and sorting, after which they may be used as coarse aggregate and added to the base material at the construction site.

[0035] The amount of coarse aggregate added is preferably 15% to 30% by weight, more preferably 20% to 30% by weight, based on 100% by weight of the base material. The particle size of the coarse aggregate added is 3 mm or more, preferably 3 mm to 8 mm, more preferably 3 mm to 5 mm.

[0036] (Method of spraying plastic refractory material) The plastic refractory according to the present invention can be sprayed using a known spraying device, which is, for example, configured to include a material cutting device, a material conveying device, a spraying machine, an air hose for sending compressed air to the spraying machine, a discharge hose for sending the plastic refractory to the spraying nozzle, a spraying nozzle, etc.

[0037] The plastic refractory material cut out from the material cutting device is supplied into the spray machine via a material conveying device, and then transported from the spray machine to the discharge hose and spray nozzle by compressed air from an air hose, and sprayed onto the desired surface to form a workpiece (for example, lining material for various heating furnaces, torpedo cars, etc.). EXAMPLES

[0038] The refractory raw material, alumina-silica refractory aggregate, and the binder clay were mixed in a 1.5 ton batch mixer while adding water to moisten the mixture, and then mixed for 10 minutes to create the base material.

[0039] Aggregates with particle sizes of 1 to 3 mm, 3 to 5 mm, and 5 to 8 mm were prepared and added to the above-mentioned base material in the weight ratios shown in Examples 1 to 6 and Comparative Examples 1 to 4 in Table 1 below, and then kneaded for 30 seconds to granulate. The aggregates with particle sizes of 3 to 5 mm and 5 to 8 mm are coarse aggregates in the present invention.

[0040] The plastic refractories produced in Examples 1 to 6 and Comparative Examples 1 to 4 were evaluated for the degree of adhesion inside the hose and rebound loss.

[0041] The degree of adhesion inside the hose was evaluated by checking the inside of the hose after conducting a 500kg spray test, and was rated as A (excellent) for no adhesion, B (good) for adhesion area of ​​10% or less of the cross-sectional area, C (fair) for 11-20%, D for 21-30%, and E for 31% or more. The results are shown in Table 1 below.

[0042] The rebound loss was calculated by spraying 500 kg onto the wall, then collecting the refractory that had fallen to the floor and measuring its weight. For example, if 500 kg was sprayed and 150 kg of refractory fell to the floor, the rebound loss would be 30%. A rebound loss of 20% or less was rated A (excellent), 21-30% was rated B (good), 31-40% was rated C (passable), 41-50% was rated D, and 51% or more was rated E. The results are shown in Table 1 below. [Table 1]

[0043] As shown in Table 1, in all of Examples 1 to 6 of the present invention, the degree of adhesion to the inside of the hose was low, and good results were obtained.

[0044] In addition, for the plastic refractory of Example 2, seven types (2-1 to 2-7) were prepared by changing the mixing time after adding the coarse aggregate to the base material, and the degree of adhesion inside the hose and rebound loss were evaluated. The results are shown in Table 2 below. [Table 2]

[0045] As shown in Table 2, when the kneading time was set to 15 to 70 seconds, the degree of adhesion to the inside of the hose was low and good results were obtained. In particular, when the kneading time was set to 15 to 50 seconds, the rebound loss was suppressed to a low level. [Industrial Applicability]

[0046] The plastic refractory according to the present invention can be suitably used as a lining material for heating furnaces, soaking furnaces, torpedo cars, etc., and for lining and repair of various industrial furnaces.

Claims

1. A plastic refractory having a base material containing a refractory raw material and a binder, The plastic refractory further comprises coarse aggregate having a grain size of 3 mm or more.

2. 2. The plastic refractory according to claim 1, wherein the particle size of the coarse aggregate is 3 mm or more and 8 mm or less.

3. 3. The plastic refractory according to claim 2, wherein the particle size of the coarse aggregate is 3 mm or more and 5 mm or less.

4. 2. The plastic refractory material according to claim 1, wherein the coarse aggregate is present in an amount of 15% by weight or more and 30% by weight or less relative to 100% by weight of the base material.

5. A method for producing the plastic refractory according to any one of claims 1 to 4, comprising the steps of: A step of producing the base material by kneading and granulating at least the refractory raw material and the binder; and further adding the coarse aggregate having a grain size of 3 mm or more to the base material, and kneading and granulating the mixture.

6. The method according to claim 5, wherein the step of further adding the coarse aggregate having a grain size of 3 mm or more and kneading and granulating the mixture is carried out for 15 seconds or more and 70 seconds or less.

7. A method for spraying the plastic refractory material according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Application of plastic refractory

    JP1982073388A

  • Furnace wall structure reinforced insulation for industrial furnace

    JP1986038498U