Resin composition, molded product, method for producing molded product, cosmetic container, sanitary material, foam and method for producing foam
A resin composition utilizing biomass-derived ionomers and ethylene polymers addresses environmental concerns by maintaining performance and moldability, offering a sustainable alternative to fossil fuel-derived resins.
Patent Information
- Application Number
- JP2023055621
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Resins containing ionomers derived from fossil fuels pose environmental concerns due to resource depletion and high carbon dioxide emissions, necessitating a shift to more sustainable alternatives without compromising performance.
Development of a resin composition using biomass-derived components for ionomers and ethylene polymers, maintaining performance balance in melt physical properties, injection moldability, and blow moldability.
The resin composition achieves environmental friendliness while retaining the same performance as conventional fossil fuel-derived resins, with improved moldability and sustainability.
Smart Images

Figure 2024143115000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a molded article, a method for producing a molded article, a cosmetic container, a sanitary material, a foam, and a method for producing a foam. [Background technology]
[0002] Ionomers, in which at least a portion of the carboxyl groups in ethylene-unsaturated carboxylic acid copolymers have been neutralized with metal cations, have excellent heat sealability, thermal adhesion, transparency, oil resistance, impact resistance, abrasion resistance, and low-temperature properties, and are therefore used in a wide range of applications, such as packaging films, adhesive films, automotive interior and exterior materials, golf ball shells, tools, and various parts. Examples of documents relating to resins containing an ionomer in which at least a portion of an ethylene-unsaturated carboxylic acid copolymer is neutralized with a metal cation include Patent Documents 1 to 4.
[0003] Patent Document 1 describes a base film for transfer decoration that has 5 to 60 mass % of ionomer resin relative to the total mass of the film, and it is said that when this base film for transfer decoration is used, by containing a specific amount of ionomer resin in the base film, the conformability (vacuum formability) of the transfer decoration film to molded products is good even under relatively low temperature conditions.
[0004] Patent Document 2 describes a heat-shrinkable film in which the inner surface layer in contact with the filling contains an ethylene-unsaturated carboxylic acid copolymer and an ionomer resin, and the content of the ethylene-unsaturated carboxylic acid copolymer is 70% by weight or more and 95% by weight or less, and the content of the ionomer resin is 5% by weight or more and 30% by weight or less, when the sum of the content of the ethylene-unsaturated carboxylic acid copolymer and the content of the ionomer resin is 100% by weight. It is said that the heat-shrinkable film provided has excellent self-weld properties and high sealing strength at low temperatures.
[0005] Patent Document 3 describes a resin composition (where the total of the resin components in the resin composition before neutralization is taken as 100 mass%) that contains an ionomer resin containing 25 mass% to 64 mass% of an ethylene-unsaturated carboxylic acid copolymer (A) and 36 mass% to 75 mass% of an olefin polymer (B), the degree of neutralization of the ionomer resin neutralized with a metal ion being 52% or more, and claims to be able to provide a resin composition, a molded article, and a method for producing a resin composition that are excellent in heat resistance and scratch resistance.
[0006] Patent Document 4 describes a substrate film for a tape for use in a semiconductor manufacturing process, which comprises A) an ionomer resin obtained by crosslinking a binary copolymer having ethylene and (meth)acrylic acid as polymer components with a metal ion, and B) a terpolymer having ethylene, (meth)acrylic acid, and a (meth)acrylic acid alkyl ester as polymer components, and in which the amount of component B) used is in the range of 5 mass % or more and 50 mass % or less based on the total amount of components A) and B), and it is said that a substrate film for a tape for use in a semiconductor manufacturing process having excellent dicing characteristics, expandability, flexibility, heat resistance, and formability can be provided. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2017-160339 A [Patent Document 2] International Publication No. 2017 / 169208 [Patent Document 3] International Publication No. 2019 / 044784 [Patent Document 4] JP 2012-089732 A Summary of the Invention [Problem to be solved by the invention]
[0008] On the other hand, resins containing ionomers, in which at least a portion of ethylene-unsaturated carboxylic acid copolymers are neutralized with metal cations, are generally derived from fossil fuels. However, there are concerns that petroleum, a fossil fuel, will soon be exhausted, and that it emits a large amount of carbon dioxide during the manufacturing process and disposal process after the product is made, raising concerns about its impact on global warming.
[0009] The present invention has been made in consideration of the above circumstances, and provides a resin composition that has improved environmental friendliness while having a performance balance of basic physical properties, melt properties, injection moldability and blow moldability equivalent to those of resin compositions produced using only resins obtained from conventional fossil fuels. [Means for solving the problem]
[0010] The present inventors have found that, in a resin composition containing an ionomer (A) of an ethylene-unsaturated carboxylic acid copolymer and an ethylene-based polymer (B) (excluding those corresponding to the above-mentioned ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer), by using components produced using raw materials derived from biomass for at least a part of each component, it is possible to obtain a resin composition having improved environmental friendliness while maintaining a performance balance of basic physical properties, melt properties, injection moldability and blow moldability equivalent to those of a resin composition produced using only raw materials derived from conventional fossil fuels.
[0011] The present invention provides the following resin composition, molded article, method for producing a molded article, cosmetic container, sanitary material, foam, and method for producing a foam.
[0012] [1] An ionomer (A) of an ethylene-unsaturated carboxylic acid copolymer, An ethylene-based polymer (B) (excluding those corresponding to the ionomer (A) of the ethylene-unsaturated carboxylic acid-based copolymer), A resin composition comprising: The resin composition has a biomass content of more than 0 mass % and not more than 100 mass % as measured in accordance with ASTM D6866 for the entire resin composition. [2] When the total resin component of the resin composition is 100 mass%, The resin composition according to [1], wherein the content of the ionomer (A) in the ethylene-unsaturated carboxylic acid copolymer is 1% by mass or more and 99% by mass or less. [3] When the total resin component of the resin composition is 100 mass%, The resin composition according to [1] or [2], wherein the content of the ethylene polymer (B) is from 1% by mass to 99% by mass. [4] The resin composition according to any one of [1] to [3], wherein a content of structural units derived from an unsaturated carboxylic acid in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is 1 mass% or more and 49 mass% or less, when the entire ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is taken as 100 mass%. [5] The resin composition according to any one of [1] to [4], wherein the ethylene-based polymer (B) contains a low-density polyethylene. [6] The resin composition according to any one of [1] to [5], wherein the ethylene-based polymer (B) comprises a biomass ethylene-based polymer obtained by polymerizing a monomer containing ethylene derived from biomass. [7] The resin composition according to any one of [1] to [6], wherein a total content of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer and the ethylene polymer (B) is 2 mass% or more and 100 mass% or less, when the entire resin composition is taken as 100 mass%. [8] The resin composition according to any one of [1] to [7], wherein the ionomer (A) of the ethylene-unsaturated carboxylic acid-based copolymer includes at least one selected from ionomers of biomass ethylene-unsaturated carboxylic acid-based copolymers obtained by polymerization of a monomer containing ethylene derived from biomass. [9] The resin composition according to any one of [1] to [8], wherein the unsaturated carboxylic acid of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer includes at least one selected from the group consisting of acrylic acid and methacrylic acid.
[10] The resin composition according to any one of [1] to [9], having a melt mass flow rate (MFR) of 0.1 g / 10 min or more and 300 g / 10 min or less, measured in accordance with JIS K 7210:1999 at 190°C under a load of 2160 g.
[11] A molded article obtained by molding the resin composition according to any one of [1] to
[10] .
[12] A method for producing the molded article according to
[11] , A method for producing a molded article, comprising the step of injection molding the resin composition.
[13] A method for producing the molded article according to
[11] , A method for producing a molded article, comprising the step of blow molding the resin composition.
[14] A cosmetic container comprising the resin composition according to any one of [1] to
[10] .
[15] A sanitary material comprising the resin composition according to any one of [1] to
[10] .
[16] A foam comprising the resin composition according to any one of [1] to
[10] .
[17] A method for producing a foam, comprising a step of foaming the resin composition according to any one of [1] to
[10] . Effect of the Invention
[0013] According to the present invention, it is possible to provide a resin composition which has improved environmental friendliness while having a balance of basic physical properties, melt properties, injection moldability and blow moldability equivalent to conventional resin compositions produced using only fossil fuel-derived resins. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, embodiments of the present invention will be described with reference to the drawings. In this specification, "A to B" indicating a range of values means A or more and B or less unless otherwise specified.
[0015] 1.Resin composition The resin composition according to this embodiment includes an ionomer (A) of an ethylene-unsaturated carboxylic acid copolymer and an ethylene-based polymer (B) (excluding those corresponding to the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer), and the biomass degree of the entire resin composition, as measured in accordance with ASTM D6866, is more than 0 mass% and 100 mass% or less.
[0016] According to the resin composition of the present embodiment, it contains an ionomer (A) of an ethylene-unsaturated carboxylic acid copolymer and an ethylene-based polymer (B) (excluding those corresponding to the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer), and by using components produced using raw materials derived from biomass for at least a part of each component, it is possible to provide a resin composition with improved environmental friendliness while having a performance balance of basic physical properties, melt properties, injection moldability and blow moldability equivalent to that of conventional resin compositions produced using only raw materials derived from fossil fuels.
[0017] In the resin composition according to the present embodiment, when the entire resin components of the resin composition are taken as 100% by mass, the content of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is, from the viewpoint of further improving the balance of the performance of the melt properties, injection moldability and blow moldability, preferably 1% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, even more preferably 30% by mass or more, even more preferably 40% by mass or more, and even more preferably 45% by mass or more, and from the viewpoint of improving the heat resistance, it is preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 95% by mass or less.
[0018] In the resin composition according to this embodiment, when the entire resin components of the resin composition are taken as 100% by mass, from the viewpoint of further improving heat resistance, the content of the ethylene-based polymer (B) is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, and even more preferably 8% by mass or more, and from the viewpoint of further improving the performance balance of flexibility, injection moldability and blow moldability, the content is preferably 99% by mass or less, more preferably 90% by mass or less, even more preferably 70% by mass or less, and even more preferably 60% by mass or less.
[0019] In the resin composition according to the present embodiment, when the entire resin components of the resin composition are taken as 100% by mass, the total content of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer and the ethylene polymer (B) is, from the viewpoint of further improving the performance balance of the basic physical properties, melt properties, injection moldability and blow moldability, preferably 2% by mass or more, more preferably 10% by mass or more, even more preferably 30% by mass or more, even more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 70% by mass or more, and even more preferably 90% by mass or more. There is no upper limit for the total content of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer and the ethylene polymer (B), but it is, for example, 100% by mass or less.
[0020] <Ionomer of ethylene-unsaturated carboxylic acid copolymer (A)> The ionomer of ethylene-unsaturated carboxylic acid copolymer (A) is an ionomer of a copolymer of ethylene and an unsaturated carboxylic acid. The ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer may be in the form of a block copolymer, a random copolymer or a graft copolymer. Taking into consideration the suitability for extrusion lamination, however, it is preferable to use a binary random copolymer, a ternary random copolymer, a graft copolymer of a binary random copolymer or a graft copolymer of a ternary random copolymer, and more preferably a binary random copolymer or a ternary random copolymer.
[0021] The unsaturated carboxylic acid in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer may be, for example, at least one selected from the group consisting of acrylic acid, methacrylic acid, 2-ethylacrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, maleic anhydride, fumaric anhydride, itaconic anhydride, monomethyl maleate, monoethyl maleate, and monoethyl maleate. Among these, the unsaturated carboxylic acid preferably includes at least one selected from the group consisting of acrylic acid and methacrylic acid, from the viewpoint of further improving the flexibility of the resulting molded article.
[0022] The ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is an ionomer of a copolymer in which at least ethylene and an unsaturated carboxylic acid are copolymerized, and may be a multicomponent copolymer of ternary or higher components in which a third copolymer component is further copolymerized. Examples of the third copolymerization component include unsaturated carboxylates (e.g., (meth)acrylic acid alkyl esters such as methyl acrylate, ethyl acrylate, isobutyl acrylate, n-butyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, isobutyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, 2-ethylhexyl methacrylate, dimethyl maleate, and diethyl maleate), vinyl esters (e.g., vinyl acetate, vinyl propionate, and the like), unsaturated hydrocarbons (e.g., propylene, butene, 1,3-butadiene, pentene, 1,3-pentadiene, 1-hexene, and the like), oxides such as vinyl sulfate and vinyl nitrate, halogen compounds (e.g., vinyl chloride, vinyl fluoride, and the like), vinyl group-containing primary and secondary amine compounds, carbon monoxide, and sulfur dioxide. Among these, from the viewpoint of further improving flexibility, the third copolymerization component is preferably an unsaturated carboxylic acid ester, more preferably a (meth)acrylic acid alkyl ester (the alkyl moiety preferably has 1 to 4 carbon atoms). These other copolymerization components may be used alone or in combination of two or more.
[0023] The ionomer (A) of an ethylene-unsaturated carboxylic acid copolymer preferably contains an ionomer of an ethylene-unsaturated carboxylic acid copolymer obtained by polymerizing a monomer containing ethylene derived from biomass. From the viewpoint of further improving environmental friendliness, the biomass degree of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is preferably more than 0 mass%, more preferably 0.01 mass% or more, even more preferably 0.1 mass% or more, even more preferably 1 mass% or more, even more preferably 5 mass% or more, even more preferably 10 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, even more preferably 40 mass% or more, even more preferably 50 mass% or more, even more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and there is no upper limit for the biomass degree of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer, but it is preferably 100 mass% or less. The method for producing ethylene derived from biomass and the biomass content will be described later.
[0024] The content of structural units derived from ethylene in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer, when the entire ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is taken as 100 mass%, from the viewpoint of further improving heat resistance, mechanical strength, etc., is preferably 50 mass% or more, more preferably 55 mass% or more, even more preferably 60 mass% or more, even more preferably 70 mass% or more, and even more preferably 80 mass% or more, and from the viewpoint of further improving transparency, it is preferably 99 mass% or less, more preferably 97 mass% or less, even more preferably 95 mass% or less, and even more preferably 93 mass% or less.
[0025] The content of constituent units derived from unsaturated carboxylic acid in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer, when the entire ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is taken as 100 mass%, from the viewpoint of further improving the flexibility of the obtained molded body, is preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, and even more preferably 7 mass% or more, and from the viewpoint of further improving the performance balance of processability and heat resistance, is preferably 49 mass% or less, more preferably 40 mass% or less, even more preferably 30 mass% or less, and even more preferably 20 mass% or less.
[0026] The content of the constituent units derived from monomers other than ethylene and unsaturated carboxylic acid in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and even more preferably 12% by mass or less, from the viewpoint of improving heat resistance, when the entire ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is taken as 100% by mass. There is no lower limit for the content of the constituent units derived from monomers other than ethylene and unsaturated carboxylic acid in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer, but it may be 0% by mass or more, 1% by mass or more, 5% by mass or more, or 8% by mass or more.
[0027] Here, the content of constituent units derived from ethylene, the content of constituent units derived from unsaturated carboxylic acid, and the content of constituent units derived from monomers other than ethylene and unsaturated carboxylic acid in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer can be measured, for example, by Fourier transform infrared absorption spectroscopy (FT-IR).
[0028] Examples of the ionomer (A) of an ethylene-unsaturated carboxylic acid copolymer include monovalent metal ions such as sodium, lithium, potassium, silver, and mercury, and polyvalent metal ions such as zinc, magnesium, calcium, cobalt, nickel, manganese, lead, titanium, strontium, barium, beryllium, aluminum, iron, cadmium, and tin. These metal ions may be used alone or in combination of two or more. Among these, from the viewpoint of easier availability of industrially manufactured products, the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer preferably contains one or more metal ions selected from the group consisting of sodium, lithium, potassium, zinc, magnesium, aluminum and barium, more preferably contains at least one or more metal ions selected from the group consisting of sodium, zinc and magnesium, and further preferably contains one or two metal ions selected from sodium and zinc. In addition to the above metal ions, the ionomer of the unsaturated carboxylic acid may contain amino compounds such as ammonia, methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, ethylenediamine, diethylenetriamine, triethylenetetramine, and 1,3-dimethylaminocyclohexane.
[0029] The degree of neutralization of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is preferably 80% or less, more preferably 70% or less, and even more preferably 60% or less, from the viewpoint of further improving the balance of the performance of the melt properties, injection moldability, and blow moldability. Although there is no lower limit for the degree of neutralization of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer, from the viewpoint of improving the transparency and mechanical strength, it is, for example, 1% or more, preferably 5% or more, more preferably 10% or more, even more preferably 20% or more, and even more preferably 40% or more. The degree of neutralization of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is the ratio (mol %) of the number of moles of carboxyl groups neutralized by metal ions to the number of moles of all carboxyl groups contained in the ethylene-unsaturated carboxylic acid copolymer. Here, the degree of neutralization of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer can be measured, for example, by an incineration residue analysis method.
[0030] The ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer can be obtained by radically polymerizing each polymerization component of the ethylene-unsaturated carboxylic acid copolymer under high temperature and pressure, and then reacting the obtained ethylene-unsaturated carboxylic acid copolymer with an oxide, hydroxide, carbonate, or the like containing a metal ion. Moreover, the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer may be a commercially available product.
[0031] The density of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer, measured in accordance with JIS K 7112:1999, is preferably 900 kg / m from the viewpoint of further improving the mechanical strength. 3 More preferably, it is 910 kg / m or more. 3 More preferably, 920 kg / m 3 From the viewpoint of improving extrusion lamination processability and flexibility, it is preferably 980 kg / m 3 Less than or equal to 960 kg / m 3 More preferably, 950 kg / m or less 3 The following is the result.
[0032] The melting point of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer, as measured by a differential scanning calorimeter (DSC), is preferably 70°C or higher, more preferably 80°C or higher, from the viewpoint of further improving heat resistance, and is preferably 130°C or lower, more preferably 120°C or lower, even more preferably 110°C or lower, and even more preferably 100°C or lower, from the viewpoint of further improving the balance of performance among the melt properties, injection moldability and blow moldability. The melt mass flow rate (MFR) of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer, measured according to JIS K 7210:1999 under conditions of 190°C and a load of 2160 g, is preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 0.3 g / 10 min or more, and even more preferably 0.5 g / 10 min or more, from the viewpoint of further improving the balance of melt properties, injection moldability, and blow moldability, and is preferably 100 g / 10 min or less, more preferably 80 g / 10 min or less, even more preferably 50 g / 10 min or less, even more preferably 30 g / 10 min or less, and even more preferably 10 g / 10 min or less, from the viewpoint of further improving the heat resistance, mechanical strength, and the like.
[0033] <Ethylene-based polymer (B)> The ethylene polymer (B) is polyethylene or a copolymer of ethylene and a polar monomer (excluding those corresponding to the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer described above). From the viewpoint of further improving the mechanical strength, the ethylene polymer (B) preferably contains polyethylene.
[0034] From the viewpoint of further improving the mechanical strength of the resulting molded article, the ethylene-based polymer (B) preferably contains polyethylene, more preferably contains at least one selected from the group consisting of low-density polyethylene (LDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), and even more preferably contains low-density polyethylene (LDPE). The ethylene polymer (B) is produced by a high pressure process, a medium pressure process or a low pressure process, preferably by a high pressure process. The ethylene polymer (B) may be a single polymer or a mixture of two or more kinds of ethylene polymers.
[0035] Copolymers of ethylene and polar monomers include ethylene-vinyl acetate copolymers.
[0036] The ethylene polymer (B) preferably includes a biomass ethylene polymer obtained by polymerizing a monomer containing ethylene derived from biomass. From the viewpoint of further improving environmental friendliness, the biomass degree of the ethylene-based polymer (B) is preferably more than 0 mass%, more preferably 10 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, even more preferably 40 mass% or more, even more preferably 50 mass% or more, even more preferably 60 mass% or more, even more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 93 mass% or more, and there is no upper limit for the biomass degree of the ethylene-based polymer (B), but it is preferably 100 mass% or less. The method for producing ethylene derived from biomass and the biomass content will be described later.
[0037] The density of the ethylene polymer (B), as measured in accordance with JIS K 7112:1999, is preferably 900 kg / m from the viewpoint of further improving the mechanical strength. 3 More preferably, 905 kg / m 3 More preferably, 910 kg / m 3 More preferably, 915 kg / m 3 From the viewpoint of further improving the balance of melt properties, injection moldability, blow moldability and heat resistance, it is preferably 940 kg / m 3 Less than or equal to 930 kg / m 3 More preferably, 925 kg / m or less 3 or less, i.e., in the range of low density polyethylene.
[0038] The melt mass flow rate (MFR) of the ethylene polymer (B), measured according to JIS K 7210:1999 under conditions of 190°C and a load of 2160 g, is not limited as long as it can be mixed with the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer and molded, but is preferably 0.01 g / 10 min or more, more preferably 0.1 g / 10 min or more, even more preferably 1 g / 10 min or more, even more preferably 1.5 g / 10 min or more, and is preferably 100 g / 10 min or less, more preferably 70 g / 10 min or less, even more preferably 50 g / 10 min or less, even more preferably 30 g / 10 min or less, and even more preferably 10 g / 10 min or less.
[0039] <Biomass-derived ethylene> The method for producing ethylene derived from biomass according to the present embodiment is not limited, and a known method can be used. Examples of the method for producing ethylene derived from biomass are given below.
[0040] "Biomass" refers to organic resources that are primarily derived from plants and animals, excluding fossil fuels. Methods for producing biomass-derived ethylene include, for example, a method in which plant raw materials are fermented by microorganisms to produce biomass-derived ethanol (bioethanol) and then dehydrated, and a method in which ethylene is extracted from biomass naphtha, which is produced using vegetable oil waste and residual oil as raw materials. The former raw materials include non-edible raw materials and edible raw materials. Examples of non-edible raw materials include cellulosic crops such as pulp, kenaf, and rice straw, waste paper, papermaking residues, wood, charcoal, compost, natural rubber, cotton, factory flue gas, waste gas, etc. Examples of edible raw materials include carbohydrate crops such as sugarcane, soybean pulp, corn, potatoes, wheat, and rice, buckwheat, and soybeans. As the former raw materials, one or more types selected from the group consisting of these can be used. As the latter raw material, various waste materials, unused resources, resource crops, etc. can be used. Specifically, oils and fats such as rapeseed oil and soybean oil, essential oils such as eucalyptus oil, vegetable oil cakes, etc. can be used. From the viewpoint of reducing the amount of carbon dioxide generated in the life cycle from the raw material to the disposal of the plastic product, it is preferable to use ethylene extracted from biomass naphtha.
[0041] Ethylene can be extracted from biomass naphtha by known methods such as heating, cracking, distillation, and purification, in the same manner as extraction from naphtha derived from fossil fuels.
[0042] The method for producing bioethanol is not limited, and for example, ethanol can be produced by contacting edible biomass raw materials such as sugarcane and corn with ethanol-producing microorganisms, such as yeast, or products derived from their crushed products to ferment sugar, and then purifying the ethanol. Ethanol can be purified by conventional methods such as distillation, membrane separation, and extraction. As a production method using non-edible raw materials as biomass raw materials, for example, ethanol can be obtained by using synthetic gas (gas mainly composed of carbon monoxide and hydrogen) generated by burning non-edible raw materials that are waste resources such as used paper and papermaking residues, and flue gas and waste gas emitted from factories, etc. as carbon sources and fermenting them with microorganisms.
[0043] The ethanol obtained as described above can be dehydrated to obtain biomass-derived ethylene. The dehydration reaction requires certain conditions, such as the type of catalyst, heating temperature, and pressure, but any of the conventional methods can be used.
[0044] In the process of producing the biomass ethylene obtained in this way, higher alcohol and higher alkene impurities may be produced during the ethanol fermentation and dehydration steps, and therefore these by-products can be removed before or after the dehydration of the ethanol.
[0045] <Biomass ratio> In the resin composition according to this embodiment, the biomass degree of the entire resin composition, measured in accordance with ASTM D6866, exceeds 0% by mass, from the viewpoint of improving environmental friendliness, and is preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 8% by mass or more, even more preferably 10% by mass or more, even more preferably 20% by mass or more, and even more preferably 40% by mass or more. There is no upper limit for the biomass degree of the entire resin composition, but it may be 100% by mass or less, or may be 90% by mass or less, 70% by mass or less, or may be 50% by mass or less. In ASTM D6866, radiocarbon from biomass ( 14 The biomass ratio is calculated by measuring the carbon concentration of fossil fuels. 14 C) shows a constant value, making it possible to distinguish it from biomass-derived carbon. For example, when polyethylene has a biomass content of more than 0 mass% but less than 100 mass%, it can be said to contain both biomass-derived ethylene and fossil fuel-derived ethylene.
[0046] In the present embodiment, the polymerization method for the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer containing biomass-derived ethylene and the ethylene polymer (B) containing biomass-derived ethylene is not limited, and a conventionally known method similar to that in the case where fossil fuel-derived ethylene is used as the raw material can be used.
[0047] <Other ingredients> The resin composition according to the present embodiment may contain various additives within the scope of the present invention. Examples of such additives include one or more additives selected from the group consisting of inorganic fillers such as silica and talc, antioxidants, weathering stabilizers, wavelength conversion agents, antistatic agents, antifogging agents, antiblocking agents, slip agents, pigments, etc. Furthermore, the resin composition according to this embodiment may contain resins other than the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer and the ethylene polymer (B) within the scope of the invention.
[0048] The resin composition according to the present embodiment can be prepared, for example, by simultaneously or continuously mixing the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer, the ethylene polymer (B) and any additives, and the mixing order is not limited. As a preparation method, it is preferable to melt mix them using a single screw extruder, a twin screw extruder, a Banbury mixer, a roll, various kneaders, etc.
[0049] Hereinafter, the physical properties of the resin composition according to this embodiment will be described.
[0050] In the resin composition according to the present embodiment, the melt mass flow rate (MFR), measured in accordance with JIS K 7210:1999 under conditions of 190°C and a load of 2160 g, is, from the viewpoint of further improving moldability, processability, and injection moldability, preferably 0.1 g / 10 min or more, more preferably 0.3 g / 10 min or more, even more preferably 0.5 g / 10 min or more, and is preferably 300 g / 10 min or less, more preferably 200 g / 10 min or less, even more preferably 100 g / 10 min or less, even more preferably 50 g / 10 min or less, even more preferably 30 g / 10 min or less, and even more preferably 10 g / 10 min or less.
[0051] In the resin composition according to the present embodiment, the density measured in accordance with JIS K 7112:1999 is preferably 910 kg / m from the viewpoint of further improving the balance of melt properties, injection moldability, and blow moldability. 3 More preferably, 915 kg / m 3 More preferably, 920 kg / m 3 More preferably, 925 kg / m 3 From the viewpoint of further improving processability, it is preferably 960 kg / m 3 Less than or equal to 955 kg / m 3 More preferably, 950 kg / m or less 3 More preferably, 945 kg / m or less 3 The following is the result.
[0052] In the resin composition according to the present embodiment, the melting point is preferably 80° C. or higher, more preferably 90° C. or higher, even more preferably 95° C. or higher, and even more preferably 100° C. or higher from the viewpoint of improving the balance of flexibility and processability, and is preferably 135° C. or lower, more preferably 125° C. or lower, even more preferably 120° C. or lower, and even more preferably 115° C. or lower from the viewpoint of further improving the performance balance of flexibility and processability. The melting point is measured, for example, by a differential scanning calorimeter (DSC) or the like.
[0053] In the resin composition according to this embodiment, from the viewpoint of further improving the balance of melt properties, injection moldability, blow moldability, and heat resistance, the freezing point is preferably 30° C. or higher, more preferably 35° C. or higher, even more preferably 40° C. or higher, and even more preferably 45° C. or higher, and is preferably 95° C. or lower, more preferably 90° C. or lower, even more preferably 85° C. or lower, and even more preferably 80° C. or lower. The freezing point is measured, for example, by a differential scanning calorimeter (DSC) or the like.
[0054] In the resin composition according to the present embodiment, the latent heat of fusion is preferably 10 J / g or more, more preferably 20 J / g or more, even more preferably 30 J / g or more, and is preferably 130 J / g or less, more preferably 120 J / g or less, even more preferably 110 J / g or less, from the viewpoint of further improving the balance of performance among melt properties, injection moldability, blow moldability, and heat resistance. The latent heat of fusion is measured, for example, by a differential scanning calorimeter (DSC) or the like.
[0055] In the resin composition according to this embodiment, the yield stress measured in accordance with JIS K 7127:1999 is preferably 5 MPa or more, more preferably 8 MPa or more, and even more preferably 10 MPa or more, from the viewpoint of further improving mechanical strength such as toughness. In the resin composition according to this embodiment, the upper limit of the yield stress measured in accordance with JIS K 7127:1999 is not limited, but may be, for example, 30 MPa or less, or 25 MPa or less.
[0056] In the resin composition according to this embodiment, the stress at break measured in accordance with JIS K 7161-1:2014 is preferably 5 MPa or more, more preferably 8 MPa or more, and even more preferably 10 MPa or more, from the viewpoint of further improving mechanical strength such as toughness. In the resin composition according to this embodiment, the upper limit of the stress at break measured in accordance with JIS K 7161-1:2014 is not limited, but may be, for example, 50 MPa or less, or 40 MPa or less.
[0057] In the resin composition according to this embodiment, the elongation at break measured in accordance with JIS K 7161-2:2014 is, from the viewpoint of further improving flexibility, preferably 80% or more, more preferably 100% or more, even more preferably 130% or more, and even more preferably 150% or more, and from the viewpoint of further improving the performance balance of mechanical strength and heat resistance, preferably 700% or less, more preferably 650% or less, even more preferably 600% or less, even more preferably 550% or less, and even more preferably 500% or less.
[0058] The stress at break (based on JIS K 7161-1:2014) and the elongation at break (based on JIS K 7161-2:2014) of the resin composition according to the present embodiment are measured using a tensile tester. The measurement can be performed by cutting a press sheet of the resin composition according to the present embodiment into a dumbbell shape according to the above JIS standard to prepare a test piece, and pulling it under the conditions of a chuck distance of 90 mm, a pulling speed of 50 mm / min, 23°C, and a relative humidity of 50% RH. The elongation at break represents the elongation of the test piece just before break between the designated gauge points in the tensile test. The stress at break is the value obtained by dividing the tensile force at the break point by the initial cross-sectional area of the test piece when the test piece breaks in the tensile test.
[0059] In the resin composition according to this embodiment, the flexural modulus at 23° C., measured in accordance with JIS K 7106:1995, is preferably 150 MPa or more, more preferably 180 MPa or more, and even more preferably 200 MPa or more, from the viewpoint of further improving the performance balance of heat resistance and mechanical properties, and is preferably 400 MPa or less, more preferably 380 MPa or less, more preferably 350 MPa or less, and even more preferably 320 MPa or less, from the viewpoint of further improving the performance balance of flexibility, conformability, processability, and handleability.
[0060] In the resin composition according to this embodiment, the Shore A hardness, measured in accordance with JIS K 7215:1986, is preferably 70 or more, more preferably 75 or more, even more preferably 80 or more, and even more preferably 85 or more, from the viewpoint of further improving the performance balance of moldability and flexibility, and is preferably 120 or less, more preferably 110 or less, and even more preferably 100 or less, from the viewpoint of further improving the performance balance of moldability and flexibility.
[0061] In the resin composition according to this embodiment, the Shore D hardness measured in accordance with JIS K 7215:1986 is preferably 30 or more, more preferably 40 or more, and even more preferably 50 or more from the viewpoint of further improving heat resistance, and is preferably 80 or less, more preferably 75 or less, and even more preferably 70 or less, from the viewpoint of further improving flexibility and processability.
[0062] The Shore A hardness and the Shore D hardness are measured in accordance with JIS K 7215:1986 using a type D durometer at 23°C.
[0063] In the resin composition according to this embodiment, the Vicat softening point measured under a load of 10 N in accordance with JIS K 7206:2016 is preferably 40°C or higher, more preferably 45°C or higher, and even more preferably 50°C or higher, from the viewpoint of further improving the performance balance of heat resistance, flexibility, processability, and handleability, and is preferably 100°C or lower, more preferably 95°C or lower, and even more preferably 90°C or lower.
[0064] The Vicat softening point is determined as follows. Using the resin composition according to this embodiment, a thermal deformation tester is used in accordance with JIS K 7206:2016, a needle indenter tool is placed at the top center of a test piece obtained from a press sheet of the resin composition so that the test piece is in contact with the test piece, and a load of 10 N is applied while the temperature of the heat transfer medium, silicone oil, is increased from 20°C at a heating rate of 50°C / h, and the temperature of the heat transfer medium is measured when the needle indenter penetrates 1 mm from the surface of the test piece.
[0065] The press sheet of the resin composition according to this embodiment used for the above physical properties is produced as follows. The resin composition of this embodiment is heated at 160°C for 4 minutes, during which degassing is performed 5 times, and then subjected to a compressive test at 160°C for 4 minutes under 9.8 MPa (100 kg / cm 2 ) conditions, then press molded at 20°C, 3 minutes, 14.7 MPa (150 kg / cm 2 ) and produce a pressed sheet with a thickness of 3 mm.
[0066] From the viewpoint of further improving processability, the melt tension at 160°C of the resin composition according to this embodiment is preferably 150 mN or more, more preferably 200 mN or more, even more preferably 250 mN or more, and is preferably 1000 mN or less, preferably 950 mN or less, even more preferably 900 mN or less, even more preferably 850 mN or less. From the viewpoint of further improving processability, the maximum take-up speed of the resin composition according to this embodiment at 160°C is preferably 10 m / min or more, more preferably 13 m / min or more, even more preferably 15 m / min or more, and is preferably 40 m / min or less, more preferably 35 m / min or less, even more preferably 30 m / min or less. From the viewpoint of further improving processability, the average take-up speed of the resin composition according to this embodiment at 160°C is preferably 10 m / min or more, more preferably 13 m / min or more, even more preferably 15 m / min or more, and is preferably 40 m / min or less, preferably 35 m / min or less, preferably 30 m / min or less.
[0067] From the viewpoint of further improving processability, the melt tension at 180°C of the resin composition according to this embodiment is preferably 50 mN or more, more preferably 80 mN or more, even more preferably 100 mN or more, even more preferably 120 mN or more, and is preferably 450 mN or less, more preferably 430 mN or less, even more preferably 400 mN or less, even more preferably 380 mN or less. From the viewpoint of further improving processability, the maximum take-up speed of the resin composition according to this embodiment at 180°C is preferably 20 m / min or more, more preferably 25 m / min or more, even more preferably 30 m / min or more, and is preferably 70 m / min or less, more preferably 65 m / min or less, even more preferably 60 m / min or less. From the viewpoint of further improving processability, the average take-up speed of the resin composition according to this embodiment at 180°C is preferably 20 m / min or more, more preferably 25 m / min or more, even more preferably 30 m / min or more, and is preferably 60 m / min or less, more preferably 55 m / min or less, even more preferably 50 m / min or less.
[0068] From the viewpoint of further improving processability, the melt tension at 200°C of the resin composition according to this embodiment is preferably 55 mN or more, more preferably 60 mN or more, even more preferably 65 mN or more, and is preferably 160 mN or less, more preferably 150 mN or less, even more preferably 145 mN or less. From the viewpoint of further improving processability, the maximum take-up speed of the resin composition according to this embodiment at 200°C is preferably 40 m / min or more, more preferably 50 m / min or more, even more preferably 60 m / min or more, and is preferably 130 m / min or less, more preferably 120 m / min or less, even more preferably 110 m / min or less. From the viewpoint of further improving processability, the average take-up speed of the resin composition according to this embodiment at 200°C is preferably 30 m / min or more, more preferably 20 m / min or more, even more preferably 50 m / min or more, and is preferably 110 m / min or less, more preferably 100 m / min or less, even more preferably 95 m / min or less.
[0069] The method for measuring the melt tension, maximum take-up speed, and average take-up speed of the resin composition according to this embodiment will be described below using the case at 160° C. as an example. Using a melt tension tester, the resin composition is filled into a barrel with a diameter of 9.55 mm heated to 160 ° C. The resin composition is extruded into a string shape from a capillary die with a diameter of 2.095 mm at a piston descending speed of 5 mm / min. The obtained string-like resin composition is passed through a pulley with a load cell installed at a position 300 mm below the capillary die, and the string-like resin composition is wound up with a winding roll. At this time, the winding speed of the string-like resin composition is linearly increased from an initial speed of 5.0 m / min to 200 m / min after 1 minute, and the load applied to the pulley with the load cell when the string-like resin composition breaks is defined as the melt tension [mN]. The value of the winding speed when the string-like resin composition breaks is defined as the maximum winding speed [m / min]. The average of the winding speed values from the start of winding the string-like resin composition to the breakage of the string-like resin composition is defined as the average winding speed [m / min]. The melt tension, maximum take-up speed and average take-up speed at 180°C and 200°C were measured in the same manner as above, except that the barrel heating temperature was changed to 180°C or 200°C.
[0070] 2. Molded body The molded article of the present embodiment is obtained by molding the resin composition of the present embodiment. The molding method is not limited, and known molding methods such as extrusion molding, injection molding, compression molding, and blow molding can be used, and the molded article can be obtained by molding into various shapes such as a sheet shape, a film shape, a plate shape, and other three-dimensional shapes. The molded article of the present embodiment may be made only of the resin composition of the present embodiment, or may be made of the resin composition of the present embodiment and other components. The molded article of the present embodiment may be a part or the whole of a member.
[0071] Furthermore, the surface of the molded article of the present embodiment may be subjected to a frame treatment, a corona treatment, a plasma treatment, a hard coat treatment with an inorganic or organic compound, an antistatic treatment, an antireflection treatment, an electromagnetic shielding treatment, etc., within the scope of not impairing the effects of the present invention. These treatments can be performed on the surface of the molded article by deposition, sputtering, dipping, thermal transfer, etc.
[0072] The molded article of the present embodiment can be used in a wide range of fields, including, but not limited to, optical materials, electronic components, various machine components, foams, sheets, films, pipes, tubes, toys, and daily necessities.
[0073] 3. Manufacturing method of molded body The method for producing the molded article of the present embodiment may include a step of injection molding the resin composition of the present embodiment. The method for producing a molded article according to the present embodiment uses the resin composition according to the present embodiment, and therefore has an excellent balance of basic physical properties and melt properties, and is suitable for injection molding. By injection molding, molded articles of various shapes, particularly complex shapes, that can be used in fields such as automotive interior and exterior materials, home appliances, civil engineering and construction materials, daily necessities, sporting goods, and industrial goods can be produced.
[0074] The temperature of the injection molding is preferably in the range of about 150 to 250°C. In the injection molding, any of the additives described above can be blended into the resin composition. When blending these additives in the injection molding, a resin composition obtained by melt-mixing some or all of the additives in the resin composition in advance using a single-screw extruder, a twin-screw extruder, a Banbury mixer, a kneader, or the like can be used. In this case, some or all of the additives can be used in the form of a master batch. In the injection molding, it is preferable to use an injection molding die having a surface embossed shape in order to improve the releasability from the die and prevent the glass from cracking during lamination by applying an embossing treatment to the surface of the molded product. The embossed shape is arbitrary, and various shapes such as a matte finish, a diamond lattice shape, a continuous straight line, a continuous curved line, and a protrusion shape having a large number of convex parts can be used.
[0075] The method for producing the molded article of the present embodiment may include a step of blow molding the resin composition of the present embodiment. The method for producing a molded article according to the present embodiment uses the resin composition according to the present embodiment, and therefore has an excellent balance of basic physical properties and melt properties, making it suitable for blow molding. Small, thin products can be produced by blow molding. When used for blow molding, high-speed molding is possible, and the range of molding conditions is wide, allowing for increased productivity.
[0076] 4. Cosmetic containers The cosmetic container of the present embodiment contains the resin composition of the present embodiment. The cosmetic container is not limited to a specific shape, but may be, for example, a hollow molded body having a cylindrical body with a bottom and a neck opening. Examples of the cosmetic to be stored include liquid basic cosmetics such as lotion and serum, and liquid makeup cosmetics such as liquid foundation. Here, the term "liquid" refers to a cosmetic having fluidity, and includes low-viscosity liquids as well as high-viscosity suspensions and pastes. Furthermore, the cosmetic container of the present embodiment can also be used as a package for packaging the above-mentioned container such as the hollow molded body. A film can be formed using the resin composition of the present embodiment, and a resin layer or a paper layer other than the resin composition of the present embodiment can be laminated on one or both sides of the film to form a laminate, which can then be used as a package.
[0077] 5. Hygiene materials The sanitary material of the present embodiment contains the resin composition of the present embodiment. Examples of sanitary materials include gathers and back sheets of disposable diapers, sanitary products, medical disposable sheets, linings for surgical and treatment gowns, and medical sanitary materials such as bandages.
[0078] 6. Foam The foam of the present embodiment contains the resin composition of the present embodiment. When the resin composition of the present embodiment is used for a foam, the resin composition may contain a chemical foaming agent, a foaming assistant, and the like, as necessary. The foam of the present embodiment uses the resin composition of the present embodiment, and therefore has an excellent balance of basic physical properties, melt properties, injection moldability, blow moldability, and heat resistance, and is widely used in applications such as heat insulation materials, sound absorbing materials, shoe soles, buoys, automobile parts, and miscellaneous goods.
[0079] When the resin composition of the present embodiment is used for a foam, the resin composition can be melt-kneaded, and then, if necessary, pelletized, and molded into a shape suitable for the intended object, for example, into a sheet, using a T-die or roll, etc. The molding temperature for the resin composition varies depending on the composition of the resin composition and the molding method, but it is generally preferable to select a temperature suitable for the molding method within the temperature range of 100 to 200°C.
[0080] To form a foam from the molded article thus obtained, foaming may be performed using a press, a furnace, a foaming bath, or the like. When electron beam crosslinking is performed, the molded article may be irradiated with an electron beam before foaming to perform crosslinking. The foaming conditions vary depending on the types of chemical foaming agent, foaming assistant, etc., but generally, a temperature suitable for the foaming method should be selected from the temperature range of 150 to 250°C. The expansion ratio when foaming from the molded body is, for example, 2.1 times or more, and from the viewpoint of further improving cushioning properties, preferably 3.1 times or more, and from the viewpoint of further improving mechanical strength, preferably 10 times or less, more preferably 8 times or less.
[0081] 7. Foam manufacturing method The method for producing a foam of the present embodiment includes a step of foaming the resin composition of the present embodiment. In the foam production method of the present embodiment, a foam such as a crosslinked foam can be produced using the resin composition of the present embodiment. In producing the foam, one or more selected from the group consisting of a foaming agent and a crosslinking agent can be added to the resin composition of the present embodiment. The resin composition used for producing the foam is in an uncrosslinked and unfoamed state, and may be in a molten state, or may be in the form of pellets or sheets which have been cooled and solidified.
[0082] The method for producing the foam of the present embodiment is not limited, but is preferably one selected from the group consisting of press molding, extrusion molding, and injection molding. In the press molding, for example, a sheet made of the resin composition of the present embodiment can be obtained using a press molding machine. In the sheet molding, it is preferable to mold the sheet at a temperature equal to or lower than the decomposition temperature of the foaming agent and the crosslinking agent, and specifically, it is preferable to mold the sheet under temperature conditions, for example, 100°C to 130°C, where the resin components are in a molten state. The obtained sheet is cut and inserted into a mold heated to, for example, 130°C to 200°C, and pressed against, for example, 30 kgf / m 3 More than 300kgf / m 3 A foam can be produced by applying a pressure of about 10 minutes or more and 90 minutes or less. In the extrusion molding, the resin composition of the present embodiment is extruded from an extruder and released into the atmosphere, whereby a foam can be produced. That is, a foam can be produced by heat treatment. In the injection molding, the resin composition of the present embodiment is injected into a mold at a temperature equal to or lower than the decomposition temperature of the foaming agent and the crosslinking agent, and crosslinked and foamed by maintaining the temperature in the mold at, for example, about 130° C. to 200° C. That is, a foam can be produced by heat treatment.
[0083] Also, a crosslinked foam can be obtained by a crosslinking method using ionizing radiation irradiation. For example, an organic pyrolysis type foaming agent is added as a foaming agent to the resin composition of the present embodiment, and the mixture is melt-kneaded at a temperature lower than the decomposition temperature of the organic pyrolysis type foaming agent, and the resulting kneaded product is molded into, for example, a sheet to obtain a sheet-like foam. Next, the obtained sheet-like foam is irradiated with a predetermined amount of ionizing radiation to crosslink the sheet-like foam, and then the obtained crosslinked foam is heated to a temperature equal to or higher than the decomposition temperature of the organic pyrolysis type foaming agent to foam, thereby obtaining a sheet-like crosslinked foam. That is, a foam can be produced by heat treatment. As the ionizing radiation, α-rays, β-rays, γ-rays, electron beams, neutron beams, X-rays, etc. are used. Among these, γ-rays and electron beams of cobalt-60 are preferably used.
[0084] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES
[0085] Hereinafter, the present embodiment will be described in detail with reference to examples, etc. However, the present embodiment is not limited to the description of these examples.
[0086] [material] The following components were used. The melt flow rate (MFR) was measured at 190°C and a load of 2160 g in accordance with JIS K 7210:1999. The density was measured in accordance with JIS K 7112:1999. The biomass ratio was measured in accordance with ASTM D6866.
[0087] <Ionomer (A)> Ionomer 1: Content of ethylene-derived structural units: 85% by mass, Content of methacrylic acid-derived structural units: 15% by mass, Degree of neutralization: 54% (sodium), MFR (190°C, 2160g load): 0.9g / 10min, Degree of biomass: 0% by mass Ionomer 2: Content of structural units derived from ethylene: 90% by mass, Content of structural units derived from methacrylic acid: 10% by mass, Neutralization degree: 50% sodium, MFR (190°C, 2160g load): 1.6g / 10min, Biomass degree: 0% by mass
[0088] <Ethylene-based polymer (B)> Low-density polyethylene 1: Low-density polyethylene, Braskem, SEB818, MFR (190°C, 2160g load): 8.7g / 10min, density: 918kg / m 3 Biomass content: 95% by mass Low-density polyethylene 2: Low-density polyethylene, manufactured by Dow Mitsui Polychemicals, MFR (190°C, 2160g load): 7.2g / 10min, density: 918kg / m 3 , Biomass content: 0% by mass Low-density polyethylene 3: Low-density polyethylene, Braskem, SEB853, MFR (190°C, 2160g load): 2.7g / 10min, density: 923kg / m 3 Biomass content: 95% by mass Low-density polyethylene 4: Low-density polyethylene, manufactured by Dow Mitsui Polychemicals, MFR (190°C, 2160g load): 1.9g / 10min, density: 921kg / m 3 , Biomass content: 0% by mass
[0089] [Examples 1 to 6 and Comparative Examples 1 to 6] <Preparation of resin composition (P)> The materials were mixed in advance in the proportions shown in Table 1, fed into a twin-screw extruder with a screw diameter of 30 mmφ, melt-kneaded under the following extrusion conditions or melt-kneading conditions, and granulated to prepare pellets of resin composition (P).
[0090] The extrusion conditions and melt-kneading conditions in the twin-screw extruder are as follows. Screw effective length L / D: 35 ·Extruder setting temperature (℃): C1 (110), C2 (160), C3 (180), C4 (180), C5 (180), H (180), D (180) Screw speed: 200 rpm Screen mesh: 60 / 120 / 60 Output: 15kg / h
[0091] [Biomass content of resin composition (P)] The biomass degree (mass%) of the resin composition (P) obtained in each example was calculated from the biomass degree of the low-density polyethylene 1 or low-density polyethylene 3 used as the raw material and the content of the low-density polyethylene 1 or low-density polyethylene 3 when the entire resin composition (P) was taken as 100 mass%.
[0092] [Content of structural units derived from unsaturated carboxylic acid in resin composition (P)] The content (mass%) of structural units derived from unsaturated carboxylic acid in the resin composition (P) obtained in each example was calculated from the content of structural units derived from unsaturated carboxylic acid in the ionomer (A) used as a raw material and the content of the ionomer (A) when the entire resin composition (P) was taken as 100 mass%.
[0093] [MFR of resin composition (P)] The MFR (g / 10 min) of the resin composition (P) obtained in each example was measured under conditions of 190° C. and a load of 2160 g in accordance with JIS K 7210:1999.
[0094] [Density of resin composition (P)] The density (kg / cm) of the resin composition (P) obtained in each example 3 ) was measured in accordance with JIS K 7112:1999.
[0095] [Melting point, freezing point and latent heat of fusion of resin composition (P)] The melting point (° C.), solidification point (° C.) and latent heat of fusion (J / g) of the resin composition (P) obtained in each example were measured using a differential scanning calorimeter (DSC).
[0096] <Press sheet production> The resin composition (P) obtained in each example was heated at 160°C for 4 minutes, during which time it was degassed 5 times, and then it was heated at 160°C for 4 minutes and compressed under 9.8 MPa (100 kg / cm 2 ) conditions, then press molded at 20°C, 3 minutes, 14.7 MPa (150 kg / cm 2 ) and press molded into a 3 mm thick press sheet.
[0097] The obtained press sheets were evaluated for yield stress, breaking stress, breaking elongation, bending stiffness, Shore A hardness, Shore D hardness and Vicat softening point according to the following methods.
[0098] Yield stress The press sheets obtained in each example were subjected to a tensile test in accordance with JIS K 7127:1999 to measure the yield stress (MPa).
[0099] [Stress at break and elongation at break] The stress at break (based on JIS K 7161-1:2014) and elongation at break (based on JIS K 7161-2:2014) of the press sheets obtained in each example were measured using a tensile tester. The press sheets were cut into dumbbell shapes based on the above JIS standard to prepare test pieces, and the test pieces were pulled under the conditions of chuck distance: 90 mm, tensile speed: 50 mm / min, 23°C, and relative humidity of 50% RH. The elongation at break represents the elongation of the test piece just before break between the designated gauge points in the tensile test. The stress at break is the value obtained by dividing the tensile force at the break point by the initial cross-sectional area of the test piece when the test piece breaks in the tensile test.
[0100] [Flexural rigidity] The flexural modulus (MPa) of the press sheet obtained in each example was measured in accordance with JIS K 7106. The press sheet was cut into a test piece having a length of 100 mm, a width of 20 mm, and a thickness of 3 mm, and the test piece was measured at 23°C using an automatic reading type "Olsen type stiffness tester" manufactured by Toyo Seiki Seisakusho.
[0101] [Shore A hardness and Shore D hardness] The Shore A hardness and Shore D hardness of the pressed sheet obtained in each example were measured in accordance with JIS K 7215: 1986. The pressed sheet was cut into a test piece having a length of 100 mm, a width of 20 mm, and a thickness of 3 mm, and the hardness was measured at 23°C using a type D durometer.
[0102] [Vicat softening point] The Vicat softening point (°C) of the press sheet obtained in each example was measured in accordance with JIS K 7206: 2016. Using a thermal deformation tester, a needle indenter was placed at the center of the top of the press sheet so that it was in contact with the press sheet, and while applying a load of 10 N, the temperature of the heat transfer medium, silicon oil, was increased from 20°C at a heating rate of 50°C / h, and the temperature of the heat transfer medium was measured when the needle indenter penetrated 1 mm from the surface of the test piece.
[0103] <Melt tension, maximum take-off speed and average take-off speed> The melt tension and maximum take-up speed of the resulting resin composition (P) were measured by the following methods. Using a melt tension tester (manufactured by Toyo Seiki Seisakusho Co., Ltd.), the resin composition (P) was filled into a barrel with a diameter of 9.55 mm heated to 160 ° C. The resin composition (P) was extruded into a string shape from a capillary die with a diameter of 2.095 mm at a piston descending speed of 5 mm / min. The obtained string-like resin composition (P) was passed through a pulley with a load cell installed at a position 300 mm below the capillary die, and the string-like resin composition (P) was taken up by a take-up roll. At this time, the take-up speed of the string-like resin composition (P) was linearly increased from an initial speed of 5.0 m / min to 200 m / min after 1 minute, and the load applied to the pulley with the load cell when the string-like resin composition (P) broke was obtained as the melt tension [mN]. In addition, the value of the take-up speed when the string-like resin composition (P) broke was taken as the maximum take-up speed [m / min]. In addition, the average of the winding speeds from the start of winding the string-shaped resin composition (P) until the string-shaped resin composition (P) breaks was defined as the average take-up speed [m / min]. Using the same method as above, the barrel heating temperature was changed to 180°C and 200°C, and the same measurements were carried out. The melt tension, maximum take-off speed and average take-off speed at 160°C, 180°C and 200°C are shown in Table 1.
[0104] [Evaluation of injection moldability] <Making square plate sheets> The resin compositions (P) obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were injection molded under the following conditions using the following injection molding machine to obtain square plate sheets with a length of 150 mm, a width of 80 mm, and a thickness of 2 mm. The mold releasability of the obtained square plate sheets was evaluated. The color of the square plate sheets was also observed. The obtained evaluation results are shown in Table 1. <Injection molding machine and injection molding conditions> ·Injection molding machine: Toshiba Machine Co., Ltd., IS-220F ·Molding temperature: 250℃ Mold: Film gate Mold temperature (chiller temperature): 60℃
[0105] <Evaluation of mold releasability> The mold releasability of the resin composition (P) was evaluated according to the following criteria. (standard) A (Good): After removing the square plate sheet from the mold, no peeled resin residue is observed on the mold. B (Fail): After removing the square plate from the mold, peeled off resin remains on the mold.
[0106] [Evaluation of blow molding] The resin compositions (P) obtained in Examples 4 to 6 and Comparative Examples 4 to 6 were laminated and extruded under the conditions of a resin thickness of 20 μm from a die opening width of 500 mm, a take-up speed of 80 m / min, and a distance (air gap) from the tip of the die opening to the nip roll of 110 mm. The take-up speed (m / min) at which the edge of the molten film started to shake when the take-up speed was increased while keeping the extrusion amount constant was then defined as the draw-down. The color of the obtained molten film was also observed. The results are shown in Table 1.
[0107] <Evaluation of drawdown> The drawdown property of the resin composition (P) was evaluated according to the following criteria. (standard) A (Good): Drawdown exceeds 400m / min B (bad): Drawdown is less than 400m / min.
[0108] [Table 1]
[0109] As is clear from Table 1, the resin composition (P) of Example 1 contained biomass-derived raw materials, but the MFR, density, melting point, solidification point, latent heat of fusion, yield stress, break stress, break elongation, flexural modulus, Shore A hardness, Shore D hardness, and Vicat softening point were all equivalent to those of the resin composition (P) (Comparative Example 1) using only fossil fuel-derived raw materials. The same was true in the comparison between Example 2 and Comparative Example 2, between Example 3 and Comparative Example 3, between Example 4 and Comparative Example 4, between Example 5 and Comparative Example 5, and between Example 6 and Comparative Example 6. In addition, although the resin composition (P) of Example 1 contained raw materials derived from biomass, the mold releasability in injection molding and the appearance were both equivalent to those of the resin composition (P) (Comparative Example 1) that used only raw materials derived from fossil fuels. The same was true in comparisons between Example 2 and Comparative Example 2, and between Example 3 and Comparative Example 3. In addition, although the resin composition (P) of Example 4 contains raw materials derived from biomass, the drawdown in blow molding and the appearance were both equivalent to those of the resin composition (P) (Comparative Example 4) that uses only raw materials derived from fossil fuels. The same was true in the comparison between Example 5 and Comparative Example 5, and between Example 6 and Comparative Example 6.
Claims
1. An ionomer (A) of an ethylene-unsaturated carboxylic acid copolymer; An ethylene-based polymer (B) (excluding those corresponding to the ionomer (A) of the ethylene-unsaturated carboxylic acid-based copolymer), A resin composition comprising: The resin composition has a biomass content of more than 0 mass% and not more than 100 mass%, as measured in accordance with ASTM D6866 for the entire resin composition.
2. When the total resin component of the resin composition is 100 mass%, The resin composition according to claim 1, wherein the ionomer (A) content of the ethylene-unsaturated carboxylic acid copolymer is 1% by mass or more and 99% by mass or less.
3. When the total resin component of the resin composition is 100 mass%, The resin composition according to claim 1 or 2, wherein the content of the ethylene polymer (B) is from 1% by mass to 99% by mass.
4. The resin composition according to any one of claims 1 to 3, wherein the content of structural units derived from unsaturated carboxylic acids in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is 1 mass% or more and 49 mass% or less, when the entire ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is 100 mass%.
5. The resin composition according to any one of claims 1 to 4, wherein the ethylene-based polymer (B) contains a low-density polyethylene.
6. The resin composition according to any one of claims 1 to 5, wherein the ethylene-based polymer (B) comprises a biomass ethylene-based polymer obtained by polymerizing a monomer containing ethylene derived from biomass.
7. The resin composition according to any one of claims 1 to 6, wherein a total content of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer and the ethylene polymer (B) is 2 mass% or more and 100 mass% or less, when the entire resin composition is taken as 100 mass%.
8. The ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer comprises at least one selected from ionomers of biomass ethylene-unsaturated carboxylic acid copolymers obtained by polymerizing a monomer containing ethylene derived from biomass. The resin composition according to any one of claims 1 to 7.
9. The resin composition according to any one of claims 1 to 8, wherein the unsaturated carboxylic acid of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer includes at least one selected from the group consisting of acrylic acid and methacrylic acid.
10. The resin composition according to any one of claims 1 to 9, wherein the melt mass flow rate (MFR) measured in accordance with JIS K 7210:1999 under conditions of 190 ° C. and a load of 2160 g is 0.1 g / 10 min or more and 300 g / 10 min or less.
11. A molded article obtained by molding the resin composition according to any one of claims 1 to 10.
12. A method for producing the molded article according to claim 11, A method for producing a molded article, comprising the step of injection molding the resin composition.
13. A method for producing the molded article according to claim 11, A method for producing a molded article, comprising the step of blow molding the resin composition.
14. A cosmetic container comprising the resin composition according to any one of claims 1 to 10.
15. A sanitary material comprising the resin composition according to any one of claims 1 to 10.
16. A foam comprising the resin composition according to any one of claims 1 to 10.
17. A method for producing a foam, comprising a step of foaming the resin composition according to any one of claims 1 to 10.
Citation Information
Patent Citations
Base material film of tape for semiconductor manufacturing process
JP2012089732A
Substrate film for transferring and decorating
JP2017160339A
Heat-shrinkable film and method for producing heat-shrinkable film
WO2017169208A1
Resin composition, molded object, and production method for resin composition
WO2019044784A1