Cast iron pipe
A solvent-based paint with acrylic resin and epoxy resin components uniformly coats the outer and inner surfaces of cast iron pipes, addressing corrosion and weather resistance issues and simplifying application on large diameters.
Patent Information
- Application Number
- JP2023055753
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing cast iron pipes face issues with insufficient corrosion resistance and weather resistance due to different paints being used on the outer and inner surfaces, and water-based paints are difficult to apply to large diameters, leading to challenging coating conditions.
A solvent-based paint with acrylic resin and epoxy resin components is applied uniformly on both the outer and inner surfaces of the pipe, including the socket, providing corrosion resistance, weather resistance, and improved adhesion to epoxy powder coating.
The solution ensures that the same paint meets the required characteristics for both surfaces, enhancing corrosion resistance, weather resistance, and adhesion, while being easier to apply to large diameters without heating, thus improving manufacturing efficiency.
Smart Images

Figure 2024143207000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a cast iron pipe having a coating film formed by applying the same paint to the outer surface of the pipe and the inner surface of the pipe receiving portion, and more particularly to a cast iron pipe in which the paint is a solvent-based paint. [Background technology]
[0002] Ductile iron pipes, which are mainly used as water pipes, are coated on the outer and inner surfaces to protect the pipes. Paint that takes into consideration corrosion resistance during burial and weather resistance during storage is generally used on the outer surface of the pipe. In addition, epoxy resin powder coating is often used on the inner surface of the pipe to prevent corrosion and improve water sanitation. On the other hand, some of these cast iron pipes have a socket at at least one end into which the socket of an adjacent pipe body is inserted. In these cast iron pipes, the inner surface of the straight pipe section is coated with the above-mentioned powder coating, and a different coating from the powder coating that takes into consideration corrosion resistance and water sanitation is generally used on the inner surface of the socket.
[0003] Specifically, it is disclosed that an acrylic resin paint or an epoxy resin paint is applied to the outer surface of a pipe by spray coating or roller coating (Patent Document 1).
[0004] For the inner surface of the receiving hole, painting with a solvent-based epoxy resin paint (Patent Document 2) or painting with a paint containing a water-based epoxy ester resin, an acrylic resin emulsion, and an acrylic resin dispersion has been disclosed (Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-148330 A [Patent Document 2] JP 2010-209967 A [Patent Document 3] JP 2019-158113 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the acrylic resin paint used on the outer surface of such pipes may not have sufficient corrosion resistance, and the epoxy resin paint may not have sufficient weather resistance.
[0007] In addition, different paints are used for painting the outer surface of the pipe and the inner surface of the pipe receiving section due to the different required characteristics.The paint for the inner surface of the pipe receiving section needs to be corrosion-resistant, have water hygiene properties, and adhere to the epoxy resin powder coating that is applied to the straight pipe section before painting the inner surface of the pipe receiving section.This makes it difficult to apply paint to the outer surface of the pipe, and there is a problem that many types of paint are used.
[0008] Furthermore, it is difficult to heat pipes with a large nominal diameter, making it difficult to use water-based paints. Also, with two-component paints, which are used by mixing the base agent and hardener, the viscosity of the paint increases due to the hardening reaction after mixing, making it difficult to control the painting conditions when spraying.
[0009] Therefore, an objective of the present invention is to provide a cast iron pipe in which the same paint is applied to the outer surface of the pipe and the inner surface of the pipe receiving portion, thereby forming a coating film that satisfies the required characteristics of both the outer surface of the pipe and the inner surface of the pipe receiving portion. [Means for solving the problem]
[0010] The applicant therefore discovered that by using a solvent-based paint whose resin components are acrylic resin and epoxy resin on the outer surface of the pipe and the inner surface of the pipe receiving mouth, a coating film having good corrosion resistance, weather resistance, and water hygiene properties can be formed on the outer surface of the pipe and the inner surface of the pipe receiving mouth using the same solvent-based paint, and thus completed the present invention.
[0011] That is, the present invention provides [1] An iron pipe having a socket at at least one end, The outer surface of the pipe and the inner surface of the pipe receiving portion are provided with a coating film formed of a solvent-based paint whose resin components are an acrylic resin and an epoxy resin, A cast iron pipe, characterized in that the coating film provided on the outer surface of the pipe and the inner surface of the pipe receiving portion is formed from the same solvent-based paint. [2] The cast iron pipe according to the above [1], wherein the epoxy resin contains an epoxy ester resin. [3] The cast iron pipe according to the above [1] or [2], wherein the content of the epoxy resin in the solvent-based paint is 0.5 to 15 mass% in terms of solid content with respect to the total resin components. [4] A method for preventing corrosion of an outer surface and an inner surface of a cast iron pipe having a socket at at least one end, comprising the steps of: (a) applying a solvent-based paint having a resin component consisting of an acrylic resin and an epoxy resin to the inner surface of the pipe receiving portion; and (b) applying the same solvent-based paint to the outer surface of the pipe as to the inner surface of the pipe receiving portion; A corrosion prevention method comprising: [5] The corrosion prevention method according to the above [4], wherein the step (a) and the step (b) are carried out successively. [6] The corrosion prevention method according to the above [4], wherein the epoxy resin contains an epoxy ester resin; and [7] The corrosion prevention method according to the above [4], wherein the content of the epoxy resin in the solvent-based paint is 0.5 to 15 mass% in terms of solid content based on the total resin components. Regarding. Effect of the Invention
[0012] According to the present invention, by using a solvent-based paint whose resin components are acrylic resin and epoxy resin on the outer surface of the pipe and the inner surface of the pipe socket, it is possible to obtain a cast iron pipe that satisfies the required characteristics of both the outer surface of the pipe and the inner surface of the pipe socket (weather resistance, corrosion resistance, and adhesion to epoxy powder paint) using the same paint. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic cross-sectional view illustrating a coating region formed on the outer surface of a cast iron pipe and the inner surface of a pipe receiving portion. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] <Cast iron pipes> One aspect of the present invention is a cast iron pipe having a socket at least at one end, characterized in that the outer surface of the pipe and the inner surface of the socket are provided with a coating film formed by a solvent-based paint whose resin components are acrylic resin and epoxy resin, and the coating film provided on the outer surface of the pipe and the inner surface of the socket are formed by the same solvent-based paint. Referring to the drawings, the coating film formation area will be described. As shown in FIG. 1, a pipe body (e.g., a ductile iron pipe) P has a coating film formed by a solvent-based paint whose resin components are acrylic resin and epoxy resin on its outer surface 2 and inner surface 3 of the socket (area B). In addition, a coating film made of the same solvent-based paint can be formed on the pipe end surface 5. An epoxy resin powder coating is applied to the inner surface 4 of the straight pipe section (area A), for example, but the coating of this epoxy resin powder coating usually extends beyond area A to a part of area B. In such a case, the coating applied to area B is also required to have adhesion to the epoxy resin powder coating.
[0015] (Solvent-based paint) The solvent-based paint used in the present invention is a paint whose resin component is composed of an acrylic resin and an epoxy resin, and whose medium is an organic solvent. For cast iron pipes for water supply, a paint conforming to the provisions of JWWA K 139 "Synthetic Resin Paint for Ductile Cast Iron Pipes for Water Supply" of the Japan Water Works Association standard can be used. The terms "solvent-based paint" and "solvent-based" are used to distinguish from water-based paints, and mean a paint that does not substantially contain water as a solvent. By using a solvent-based paint, the solvent is more easily evaporated and a film is more easily formed than in water-based paints, so that it can be applied to pipes with large nominal diameters that are difficult to heat.
[0016] (Resin component) The solvent-based paint used in the present invention contains only acrylic resin and epoxy resin as resin components. The acrylic resin and epoxy resin can be any resin that is commercially available for use as a paint for cast iron pipes, and are not particularly limited. When used for water pipes, for example, acrylic resin and epoxy resin used in paints specified in JWWA K 139 "Synthetic resin paint for ductile cast iron pipes for water supply" of the Japan Water Works Association standard can be suitably used.
[0017] The total content of the resin components in the solvent-based coating material used in the present invention is preferably 60% by mass or more in terms of solid content. By making the total content of the resin components 60% by mass or more in terms of solid content, the smoothness of the coating surface tends to be improved.
[0018] (Acrylic resin) The acrylic resin is not particularly limited, but copolymers mainly composed of acrylic acid, methacrylic acid, acrylic acid alkyl esters, and / or methacrylic acid alkyl esters can be used. Also usable are acrylate or methacrylate copolymers containing styrene, vinyl acetate, or butadiene, as specified in the Japan Ductile Iron Pipe Association standard JDPA Z 2010-2009 "Synthetic Resin Coating for Ductile Cast Iron Pipes."
[0019] (Epoxy resin) The epoxy resin is not particularly limited, and examples thereof include bisphenol type epoxy resins such as bisphenol A type epoxy resin and bisphenol F type epoxy resin, naphthalene type epoxy resin, biphenyl type epoxy resin, novolac type epoxy resin, cyclic aliphatic epoxy resin, glycidylamine type resin, heterocyclic epoxy resin, polyfunctional epoxy resin, epoxy ester resin, etc. Among these, epoxy ester resin is preferably used from the viewpoint that the coating film formed becomes hard and the adhesion with the epoxy resin powder coating applied to the inner surface of the cast iron pipe is further improved.
[0020] Examples of epoxy ester resins include, but are not limited to, unsaturated fatty acid modified epoxy ester resins, and vinyl modified epoxy ester resins obtained by bulk polymerization of vinyl monomers having a terminal carboxyl group-containing structure and other vinyl monomers.
[0021] The content of the epoxy resin in the solvent-based paint used in the present invention is preferably 0.5 mass% or more, more preferably 1.5 mass% or more, based on the total resin components, based on the solid content. By making the content of the epoxy resin 0.5 mass% or more, based on the total resin components, based on the solid content, there is a tendency for the corrosion resistance to be improved. In addition, the content of the epoxy resin is preferably 15 mass% or less, more preferably 10 mass% or less, based on the total resin components, based on the solid content. By making the content of the epoxy resin 15 mass% or less, based on the total resin components, based on the solid content, there is a tendency for the corrosion resistance to be improved without decreasing the weather resistance.
[0022] (solvent) As the solvent, toluene, xylene, ethylbenzene, isobutanol, n-butanol, methanol, methyl isobutyl ketone, propylene glycol monoethyl ether, etc. can be used alone or in combination of two or more kinds.
[0023] (Pigments) The solvent-based paint used in the present invention may contain a pigment in order to impart sufficient coloring and rust prevention properties. Specific examples of pigments include color pigments such as titanium dioxide, iron oxide, carbon black (e.g., trade name MA100, manufactured by Mitsubishi Chemical Corporation), cyanine blue, and cyanine green; extender pigments such as calcium carbonate, talc, barium sulfate, and clay; and rust prevention pigments such as zinc phosphate, calcium phosphate, and aluminum phosphomolybdate. These may be used alone or in a mixture of two or more types as necessary.
[0024] (Other Ingredients) In addition to the above components, known additives can be added to the solvent-based paint as needed. Other additives include known additives such as antifoaming agents made of silicone or organic polymers; surface conditioners made of silicone or organic polymers; viscosity adjusters (anti-sagging agents) made of amide wax, organic bentonite, etc.; matting agents made of silica, alumina, etc.; dispersants made of polycarboxylates, etc.; ultraviolet absorbers made of benzophenone, etc.; hindered amine light stabilizers; phenolic antioxidants; waxes, etc. These can be used alone or in combination as needed.
[0025] The solvent-based paint is produced using equipment commonly used for paint production. The production method is not particularly limited, but for example, the desired paint can be obtained by adding pigments, additives (pigment dispersants, viscosity modifiers, etc.), solvents, etc. to commercially available resin components, and then dispersing them with a roll mill, SG mill, disperser, etc.
[0026] The formation of a coating film using a solvent-based paint is not particularly limited, but is usually performed at room temperature without heating the cast iron pipe. When heating the cast iron pipe, it is heated to a temperature at which the solvent does not boil. The coating method is not particularly limited, but it can be applied by a method such as brush coating, roller coating, air spray coating, airless spray coating, dip coating, and shower coat coating. Since the solvent-based paint of the present invention is a one-component type, it is easier to manage the coating conditions even in spray coating compared to two-component epoxy resin paint, and it can be applied stably.
[0027] The thickness of the coating film formed by the solvent-based paint is appropriately set depending on the application of the cast iron pipe to be coated, and is not particularly limited. For example, in the case of a cast iron pipe used for water supply and sewerage, the coating film on the outer surface of the pipe can be appropriately set in the range of approximately 100 to 150 μm, and the coating film on the inner surface of the pipe receiving part can also be appropriately set in the range of approximately 100 to 150 μm.
[0028] (Cast Iron Pipe) The cast iron pipe of the present invention is not particularly limited to, for example, water supply and sewerage, water storage, etc., but from the viewpoint of being able to fully exert the effects of the present invention, a cast iron pipe for water supply and sewerage is preferable. In addition, the inner surface of the straight pipe part of the cast iron pipe is preferably subjected to mortar lining treatment or epoxy resin powder coating, and from the viewpoint of being able to fully exert the effects of the present invention, it is preferable that the epoxy resin powder coating is applied. Furthermore, since the paint applied to the cast iron pipe of the present invention is solvent-based and does not require a high temperature for evaporation of the solvent compared to water-based paint, a pipe with a large nominal diameter that is difficult to heat (for example, φ900 mm or more) is preferable because it can fully exert the effects of the present invention.
[0029] <Method of preventing corrosion on the outer surface of cast iron pipes and the inner surface of the pipe socket> In another aspect of the present invention, there is provided a method for preventing corrosion of the outer surface and the inner surface of a cast iron pipe having a receiving portion provided at least at one end after casting, the method comprising the steps of (a) applying a solvent-based paint, the resin components of which are an acrylic resin and an epoxy resin, to the inner surface of the pipe receiving portion, and (b) applying to the outer surface of the pipe the same solvent-based paint as the solvent-based paint applied to the inner surface of the pipe receiving portion.
[0030] In the corrosion prevention method of the present invention, from the viewpoint of workability during production of cast iron pipes, it is preferable that steps (a) and (b) are carried out successively. Here, "successively" specifically means that the steps are carried out simultaneously or as successive steps, and the interval between steps (a) and (b) is preferably within 5 minutes.
[0031] In the corrosion prevention method of the present invention, it is preferable that the inner surface of the straight pipe portion is coated with an epoxy resin powder prior to the step (a).
[0032] (Inner surface treatment of straight pipe section) In one embodiment, the cast iron pipe used in the corrosion prevention method of the present invention has a mortar lining treatment or epoxy resin powder coating applied to the inner surface 4 of the straight pipe section. The epoxy resin powder coating is performed by heating the cast iron pipe and forming an inner coating film on the inner surface of the cast iron pipe by, for example, spraying an epoxy resin powder paint on the inner surface of the cast iron pipe in order to impart corrosion resistance to the inner surface of the cast iron pipe. In addition, in order to impart corrosion resistance to the inner surface of the cast iron pipe, a mortar lining layer can be formed on the inner surface of the cast iron pipe instead of forming an inner coating film with an epoxy resin powder paint. Before the epoxy resin powder coating or the formation of the mortar lining layer, it is preferable to perform surface preparation such as polishing and cleaning of the inner surface of the pipe as necessary. The formation of the mortar lining layer is not particularly limited, and a known method can be used. For example, a method of forming a mortar lining on the inner surface of the pipe while moving an inner lining device in the axial direction of the pipe with a cement material containing aggregate such as silica sand, and then steam curing can be used. The thickness of the mortar lining layer is specified for each diameter in JWWA A 113 "Mortar lining for ductile cast iron pipes for water supply."
[0033] ((a) Step: Formation of coating film on the inner surface of the pipe socket) In the corrosion prevention method of the present invention, for example, after the straight pipe section inner surface treatment, a coating film is formed on the inner surface of the receiving portion 1 (the inner surface 3 of the receiving portion) in step (a) (area B). All of the above-mentioned contents regarding the cast iron pipe can be applied to the solvent-based paint used. When the pipe temperature is increased by the straight pipe section inner surface treatment, the coating film on the inner surface 3 of the receiving portion can be formed by utilizing the residual heat, and is preferably formed continuously after the straight pipe section inner surface treatment. The interval between the straight pipe section inner surface treatment step and the coating film formation step on the inner surface of the receiving portion is not particularly limited, but in the case of natural cooling, the coating film on the inner surface of the receiving portion is formed continuously after the inner surface treatment step, usually at an interval of 15 minutes or less, more preferably at an interval of 10 minutes or less. The surface temperature of the cast iron pipe at this time is preferably 50°C or less. If it is higher than 50°C, the solvent in the paint tends to boil.
[0034] The coating method for forming the coating film on the inner surface 3 of the pipe receiving portion (step (a)) is not particularly limited, and the coating can be applied to a desired thickness by spraying, brushing, or roller.
[0035] ((b) Step: Formation of coating film on the outer surface of the tube) In the corrosion prevention method of the present invention, for example, after carrying out step (a), in step (b), the same paint as that used for the inner surface of the pipe receiving portion is applied to the outer surface 2 of the pipe to form a coating film. All of the above-mentioned contents regarding the cast iron pipe can be applied to the solvent-based paint used. There is no particular limitation on the method for painting the outer surface 2 of the pipe, and sprays, brushes, rollers, etc. can be used. In addition, the temperature of the pipe body during painting is usually room temperature, but if it is heated, it is preferably 50°C or lower. If the temperature of the pipe body is higher than 50°C, the solvent in the paint tends to boil.
[0036] (Formation of coating film on pipe end surface) In one embodiment of the corrosion prevention method of the present invention, after step (a) or step (b), a coating film may be formed on the pipe end surface 5 with the same solvent-based paint as on the outer surface of the pipe and the inner surface of the pipe receiving portion. The method of forming the coating film on the pipe end surface 5 is not particularly limited, and can be performed by spraying, brushing, rolling, dipping, or the like.
[0037] In addition, unless there is any particular contradiction, all of the contents described above in relation to the cast iron pipe of the present invention are applicable to the corrosion prevention method of the present invention, and all of the contents described above in relation to the corrosion prevention method of the present invention are applicable to the cast iron pipe of the present invention. EXAMPLES
[0038] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0039] First, the components used in the examples are shown below. <Solution-based paint> (resin) Acrylic resin varnish: Acrydic A9510 (DIC Corporation) Epoxy ester resin varnish: Arakid 9201N (Arakawa Chemical Industries, Ltd.) (Pigments) Carbon black: MA-100 (Mitsubishi Chemical Corporation) Titanium oxide: Anatase (manufactured by Sakai Chemical Industry Co., Ltd.) Calcium carbonate: NEOLIGHT SA-200 (Takehara Chemical Industry Co., Ltd.) Barium sulfate: Barium sulfate W-6 (Takehara Chemical Industry Co., Ltd.) Talc: T talc (Takehara Chemical Industry Co., Ltd.) <Powder paint> Epoxy resin powder paint: V-PET#1600 Kurimoto Gray FH (manufactured by Dai Nippon Paint Co., Ltd., JWWA G 112 standard product, powder)
[0040] Example 1 A cast iron pipe (φ900×6000mm) was heated to 240-330℃. Then, the inner surface of the pipe was powder-coated with epoxy resin powder paint to a target thickness of 300μm using a powder coating device that sprays paint onto the inner surface of the pipe (area A in Fig. 1). After that, the pipe was naturally cooled until the temperature of the pipe was 50℃ or less, and the inner surface of the pipe socket (area B in Fig. 1) was painted with paint A in Table 1 by airless spray (film thickness: 100μm). Then, the outer surface of the pipe (2 in Fig. 1) was painted with paint A in Table 1 by airless spray (film thickness: 100μm), and finally the end surface of the pipe socket (5 in Fig. 1) was painted with paint A in Table 1 by brush (film thickness: 100μm).
[0041] The resulting cast iron pipe was able to meet the required corrosion resistance and weather resistance requirements for the outer surface of the pipe and the inner surface of the pipe socket with just one type of paint, thereby reducing manufacturing labor while still meeting the required performance.
[0042] [Table 1]
[0043] Test example 1: Weather resistance (1) Preparation of test specimens Either Paint A, Paint B or Paint C shown in Table 1 was brush-painted onto a sandblasted steel plate (150 mm x 70 mm x 2 mm) to a film thickness of 100 μm, and then allowed to dry naturally.
[0044] (2) Test method Weather resistance was evaluated according to the JIS K 5600-7-7 xenon lamp method. The test piece prepared in (1) was set in an i-Super Xenon Tester XER-W75 (manufactured by Iwasaki Electric Co., Ltd.) and tested for 300 hours under the test conditions of cycle A specified in 9.5 of JIS K 5600-7-7.
[0045] (3) Evaluation The evaluation was carried out according to the following criteria. ○: No cracks, peeling, or rust are observed. ×: Cracks, peeling, and rust are observed.
[0046] Test example 2: Corrosion resistance (1) Preparation of test specimens The test specimen was prepared in the same manner as in Test Example 1.
[0047] (2) Test method Corrosion resistance was evaluated according to JIS K 5600-7-1 Neutral Salt Spray Resistance. A cross cut was made with a cutter knife in the center of the coating surface of the above test piece so as to reach the base, and then the test was carried out in an environment where an ambient temperature of 35°C was used and a 5% aqueous solution of sodium chloride was sprayed.
[0048] (3) Evaluation The evaluation was performed on the area other than the 2 mm periphery of the crosscut portion according to the following criteria. ○: No red rust or blisters after 240 hours △: No red rust or blisters after 120 hours
[0049] Test example 3: Warm water resistance (1) Preparation of test specimens The test specimen was prepared in the same manner as in Test Example 1.
[0050] (2) Test method The test piece was immersed in boiling tap water for 10 minutes and the appearance of the coating was visually observed.
[0051] (3) Evaluation The evaluation was carried out according to the following criteria. ○: No blisters on the coating ×: Blisters occurred on the coating
[0052] Test Example 4: Adhesion to powder paint (1) Preparation of test specimens A ductile iron pipe (φ100 mm) with an epoxy resin powder coating (film thickness 300 μm) on the inside was cut to a length of 150 mm and further divided into four in the circumferential direction to obtain cast iron pieces (150 mm × 70 mm). Either Paint A, Paint B or Paint C listed in Table 1 was brush-painted onto the epoxy resin powder coating of this cast iron piece to a film thickness of 100 μm, and then it was allowed to dry naturally. (2) Test method The test pieces were subjected to adhesion tests according to the JIS K 5600-5-6 cross-cut method. After coating the test pieces with each paint, they were aged for 7 days in an environment of 23°C, and cross-cuts were made to the powder coating film, with 6 cuts in a grid pattern and 2mm intervals between cuts, as described in test methods 7.1.3 and 7.1.4. After cutting, a tape peel test was performed on the coating film at the cross-cut area, and the peeling condition was observed. (3) Evaluation The evaluation was carried out in accordance with the description in 8.3 Table 1 "Classification of test results" of JIS K 5600-5-6, and was classified as follows. ○:Classification 0~1 ×: Classification 2~5
[0053] From Table 1, it can be seen that when a solvent-based paint whose resin components are acrylic resin and epoxy resin is used, the corrosion resistance, hot water resistance, and adhesion to the powder coating are superior compared to when a solvent-based paint whose resin component is only acrylic resin is used, and it is possible to paint the outer surface of the pipe and the inner surface of the pipe socket with the same paint. [Explanation of symbols]
[0054] 1 Socket 2 Pipe outer surface 3 Inner surface of pipe socket 4. Inner surface of straight pipe 5 Pipe end face P Pipe body (cast iron pipe)
Claims
1. An iron pipe having a socket at at least one end, The outer surface of the pipe and the inner surface of the pipe receiving portion are provided with a coating film formed of a solvent-based paint whose resin components are an acrylic resin and an epoxy resin, A cast iron pipe, characterized in that the coating films provided on the outer surface of the pipe and the inner surface of the pipe receiving portion are formed from the same solvent-based paint.
2. 2. The cast iron pipe according to claim 1, wherein the epoxy-based resin comprises an epoxy ester resin.
3. 3. The cast iron pipe according to claim 1 or 2, wherein the content of the epoxy resin in the solvent-based paint is 0.5 to 15 mass % in terms of solid content with respect to the total resin components.
4. A method for preventing corrosion of an outer surface and an inner surface of a cast iron pipe having a socket at at least one end, comprising the steps of: (a) applying a solvent-based paint containing an acrylic resin and an epoxy resin to the inner surface of the pipe receiving portion; and (b) applying the same solvent-based paint to the outer surface of the pipe as to the inner surface of the pipe receiving portion; A corrosion prevention method comprising:
5. 5. The corrosion prevention method according to claim 4, wherein the steps (a) and (b) are carried out consecutively.
6. The corrosion prevention method according to claim 4, wherein the epoxy-based resin comprises an epoxy ester resin.
7. 5. The corrosion prevention method according to claim 4, wherein the content of the epoxy resin in the solvent-based paint is 0.5 to 15 mass % in terms of solid content based on the total resin components.
Citation Information
Patent Citations
Pipe protective cap
JP2010209967A
Cast iron pipe having coated film at inner surface of socket and its coating method
JP2019158113A
Cast iron pipe having joint portion and anticorrosion method for cast iron pipe joint portion
JP2020148330A