Co2 absorption and fixation method, and construction joint method

By forming successive absorption and fixation layers using a hydraulic composition with a specific water-cement ratio and exposing them to the atmosphere, the method efficiently captures and fixes CO2 in concrete and mortar structures, addressing the need for carbon neutral solutions.

JP2024143279APending Publication Date: 2024-10-11SUMITOMO OSAKA CEMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023055866
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Concrete and mortar structures do not absorb carbon dioxide (CO2) from the atmosphere, leading to neutralization and reduced alkalinity, and there is a need for a method to efficiently absorb and fix CO2 to align with carbon neutral initiatives.

Method used

A method involving the formation of multiple absorption and fixation layers using a hydraulic composition with a specific water-cement ratio, exposing each layer to the atmosphere to absorb and fix CO2, with each layer being overlaid on the previous one to enhance CO2 capture efficiency.

Benefits of technology

The method effectively captures and fixes CO2, enhancing the efficiency of CO2 removal by forming successive absorption and fixation layers, thereby improving the CO2 absorption capacity and fixation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143279000001
    Figure 2024143279000001
  • Figure 2024143279000002
    Figure 2024143279000002
Patent Text Reader

Abstract

To provide a CO2 absorption and fixation method capable of efficiently performing CO2 absorption and fixation, and a construction joint method.SOLUTION: The CO2 absorption and fixation method according to the present invention is a CO2 absorption and fixation method for absorbing and fixing CO2, and has the following steps (1)-(4), and a hydraulic composition includes cement and water, and the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) A step of forming a first absorption fixing layer with a thickness of 1 mm or more and 100 mm or less using a hydraulic composition (2) A step of exposing the first absorption and fixation layer to the atmosphere to absorb and fix CO2 on the first absorption fixation layer (3) A step of using a hydraulic composition, layering on the first absorption and fixation layer to form a second absorption and fixation layer with a thickness of 1 mm or more and 100 mm or less (4) A step of exposing the second absorption and fixation layer to the atmosphere to absorb and fix CO2 in the second absorption and fixation layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a CO2 absorption and fixation method and a joint construction method. [Background technology]

[0002] Conventionally, methods for repairing deteriorated concrete pavements include the overlay method, in which a new surface layer is laid on top of the existing pavement surface, and the replacement method, in which part or all of the existing pavement is removed and new pavement is laid. Among these methods, the overlay method is used not only to repair worn or damaged pavement surfaces, but also to repair uneven settlement in aprons at airports, etc.

[0003] For example, Non-Patent Document 1 discloses that when the flatness of the pavement at an airport is reduced due to longitudinal irregularities, depressions, etc., repairs are carried out using an overlay method to improve the flatness. [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] Airport Civil Engineering Facility Design Guidelines (Pavement Design Edition) Civil Aviation Bureau, Ministry of Land, Infrastructure, Transport and Tourism, April 2019 Summary of the Invention [Problem to be solved by the invention]

[0005] Meanwhile, a phenomenon called neutralization (carbonation) is known in which concrete or mortar structures absorb carbon dioxide (CO2) from the atmosphere and reduce the alkalinity of the structure. In recent years, with the rise in carbon neutral momentum, technologies aimed at reducing CO2 emissions and absorbing and fixing CO2 have been attracting attention. Therefore, there is a demand for a method of efficiently absorbing and fixing CO2 by utilizing the absorption and fixation of CO2 in concrete or mortar structures.

[0006] The present invention has been made in consideration of the above circumstances, and an objective of the present invention is to provide a CO2 absorption and fixation method and a joint construction method that can efficiently absorb and fix CO2 by jointing a CO2 absorption and fixation layer that absorbs and fixes CO2 on existing concrete. [Means for solving the problem]

[0007] The CO2 absorption and fixation method according to the present invention is a CO2 absorption and fixation method for absorbing and fixing CO2, The method includes the following steps (1) to (4): The hydraulic composition comprises cement and water, The water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) A step of forming a first absorbent fixing layer having a thickness of 1 mm to 100 mm using a hydraulic composition. (2) A step of exposing the first fixed absorbent layer to the atmosphere to absorb and fix CO2 in the first fixed absorbent layer. (3) A step of forming a second absorbent fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and overlapping the first absorbent fixing layer. (4) A step of exposing the second absorbent layer to the atmosphere to absorb and fix CO2 in the second absorbent layer.

[0008] With this configuration, the CO2 absorption and fixation method of the present invention forms a new second absorbing and fixating layer on top of the first absorbing and fixating layer that has absorbed and fixed CO2, and further absorbs and fixes CO2, thereby enabling efficient absorption and fixation of CO2.

[0009] In the CO2 absorption and fixation method according to the present invention, in the step (2), the first absorption and fixation layer may be exposed to the atmosphere for a period of 1 year or more and 15 years or less.

[0010] In the CO2 absorption and fixation method according to the present invention, due to such a configuration, the first absorption and fixation layer absorbs and fixes a large amount of CO2, and therefore, CO2 can be absorbed and fixed more efficiently.

[0011] In the CO2 absorption and fixation method according to the present invention, in the step (4), the second absorption and fixation layer may be exposed to the atmosphere for a period of 1 year or more and 15 years or less.

[0012] In the CO2 absorption and fixation method according to the present invention, due to such a configuration, the second absorption and fixation layer absorbs and fixes a large amount of CO2, and therefore, CO2 can be absorbed and fixed more efficiently.

[0013] The CO2 absorption and fixation method according to the present invention may further include the following steps (5) and (6). (5) A step of forming an n-th absorbent-fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and superposing it on the n-1th absorbent-fixing layer (n is any natural number of 3 or more, and the n-th absorbent-fixing layer is the n-th absorbent-fixing layer). (6) A step of exposing the nth absorbent layer to the atmosphere to absorb and fix CO2 in the nth absorbent layer.

[0014] In the CO2 absorption and fixation method according to the present invention, the nth absorption and fixation layer is formed over the (n-1)th absorption and fixation layer in such a configuration, so that more efficient absorption and fixation of CO2 can be performed.

[0015] The CO2 absorption and fixation method according to the present invention may further include the following step (7). (7) increasing the natural number n by 1 and repeating steps (5) and (6) at least once.

[0016] According to the CO2 absorption and fixation method of the present invention, the absorption and fixation layer is repeatedly formed by the above-mentioned configuration, so that efficient absorption and fixation of CO2 can be continuously performed.

[0017] In the CO2 absorption and fixation method according to the present invention, in the step (1), the first absorption and fixation layer may be formed on the existing concrete.

[0018] With such a configuration, the CO2 absorption and fixation method according to the present invention forms the first absorption and fixation layer after the existing concrete absorbs and fixes CO2, so that it is possible to more efficiently absorb and fix CO2.

[0019] The jointing method according to the present invention is a jointing method for concrete or mortar that absorbs and fixes CO2, and has the following steps (1) to (4), the hydraulic composition contains cement and water, and the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) A step of forming a first absorption and fixation layer having a thickness of 1 mm or more and 100 mm or less using the hydraulic composition (2) A step of exposing the first absorption and fixation layer to the atmosphere to absorb and fix CO2 in the first absorption and fixation layer (3) A step of forming a second absorption and fixation layer having a thickness of 1 mm or more and 100 mm or less on top of the first absorption and fixation layer using the hydraulic composition (4) A step of exposing the second absorption and fixation layer to the atmosphere to absorb and fix CO2 in the second absorption and fixation layer

[0020] According to the present invention, with such a configuration, a new second absorption and fixation layer is formed on top of the first absorption and fixation layer that has absorbed and fixed CO2, and further CO2 is absorbed and fixed, so that CO2 can be efficiently absorbed and fixed.

Advantages of the Invention

[0021] According to the present invention, it is possible to provide a CO2 absorption and fixation method and a jointing method that can efficiently absorb and fix CO2.

Embodiments for Carrying Out the Invention

[0022] Hereinafter, the CO2 absorption and fixation method and the jointing method according to the present embodiment will be described.

[0023] <CO2 Absorption and Fixation Method> The CO2 absorption and fixation method according to the present embodiment is a CO2 absorption and fixation method for absorbing and fixing CO2, and has the following steps (1) to (4). The hydraulic composition contains cement and water, and the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) A step of forming a first absorbent fixing layer having a thickness of 1 mm to 100 mm using a hydraulic composition. (2) A step of exposing the first fixed absorbent layer to the atmosphere to absorb and fix CO2 in the first fixed absorbent layer. (3) A step of forming a second absorbent fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and overlapping the first absorbent fixing layer. (4) A step of exposing the second absorbent layer to the atmosphere to absorb and fix CO2 in the second absorbent layer.

[0024] In the CO2 absorption and fixation method according to the present embodiment, the hydraulic composition used to form the absorption and fixation layer that absorbs and fixes CO2 contains cement and water.

[0025] The cement is not particularly limited, and for example, Portland cement such as ordinary Portland cement, high-early-strength Portland cement, ultra-high-early-strength Portland cement, moderate-heat Portland cement, sulfate-resistant Portland cement, and white Portland cement as specified in JIS R 5210:2019; mixed cement such as blast furnace cement, fly ash cement, and silica cement; ultra-fast-hardening cement, alumina cement, and other known cements can be used. Note that one type of cement may be used alone, or two or more types may be used in combination.

[0026] The water is not particularly limited, and may be, for example, tap water, industrial water, recycled water, groundwater, river water, rainwater, etc. It is preferable that the water does not contain organic matter, chloride ions, sodium ions, potassium ions, etc., which have an adverse effect on the hydration reaction of the concrete composition and the pavement concrete, or if they are contained, they are contained in extremely small amounts. It is more preferable that the water is tap water or industrial water of stable quality.

[0027] The hydraulic composition may also contain aggregate. As the aggregate, fine aggregate and / or coarse aggregate can be used. Note that fine aggregate refers to aggregate that passes entirely through a 10 mm mesh sieve and passes 85% or more by mass through a 5 mm mesh sieve, and coarse aggregate refers to aggregate that remains on a 5 mm mesh sieve at 85% or more by mass (JIS A 0203:2019).

[0028] Examples of fine aggregates include river sand, land sand, mountain sand, sea sand, crushed sand, limestone crushed sand, and other natural sands as specified in JIS A 5308:2019 Appendix A Aggregates for Ready-Mixed Concrete, blast furnace slag, etc. Note that one type of fine aggregate may be used alone, or two or more types may be used in combination.

[0029] Examples of coarse aggregates include natural aggregates such as river gravel, mountain gravel, and sea gravel, as specified in JIS A 5308:2019 Appendix A Aggregates for Ready-Mixed Concrete, artificial aggregates such as crushed stone such as sandstone, hard limestone, basalt, and andesite, and recycled aggregates. In addition, silica sand produced by crushing and classifying silica may be used. Note that one type of coarse aggregate may be used alone, or two or more types may be used in combination.

[0030] The hydraulic composition may also contain an admixture. Examples of the admixture include inorganic fine powders such as fly ash, silica fume, cement kiln dust, blast furnace fume, ground granulated blast furnace slag, ground cooled blast furnace slag, ground converter slag, hemihydrate gypsum, expanding material, ground limestone, ground quicklime, and ground dolomite, and inorganic fillers such as sodium bentonite, calcium bentonite, attapulgite, sepiolite, activated clay, acid clay, allophane, imogolite, shirasu (volcanic ash), shirasu balloon, kaolinite, metakaolin (calcined clay), synthetic zeolite, artificial zeolite, artificial zeolite, mordenite, and clinoptilolite. The admixture may be used alone or in combination of two or more kinds.

[0031] The hydraulic composition may also contain an admixture. Examples of the admixture include air-entraining agents, air-entraining water-reducing agents, high-performance water-reducing agents, high-performance air-entraining water-reducing agents, fluidizing agents, separation-reducing agents, setting retarders (e.g., tartaric acid, etc.), setting accelerators (e.g., aluminum sulfate, etc.), quick-setting agents, shrinkage-reducing agents, foaming agents, foaming agents, waterproofing agents, etc. The admixtures may be used alone or in combination of two or more.

[0032] The water-cement ratio of the hydraulic composition is 40% or more and 60% or less. The water-cement ratio is the mass percentage of water to cement. From the viewpoint of improving the CO2 absorption and fixation amount of the absorption and fixation layer described later, the water-cement ratio is 40% or more, preferably 45% or more. From the viewpoint of improving the strength of the absorption and fixation layer, the water-cement ratio is 60% or less, preferably 55% or less.

[0033] In step (1), a first absorbent fixing layer is formed using a hydraulic composition. The first absorbent fixing layer is formed by pouring or applying a kneaded hydraulic composition to a work area and then hardening the composition. When forming the first absorbent fixing layer, a self-leveling material may be used to level the surface of the first absorbent fixing layer.

[0034] The thickness of the first absorbing and fixing layer is 1 mm or more and 100 mm or less. In general, in a concrete or mortar structure, CO2 is absorbed and fixed from the surface exposed to the atmosphere toward the inside, so that in the early period of exposure to the atmosphere, the amount of CO2 absorbed and fixed per unit time is large, and the longer the exposure period, the smaller the amount of CO2 absorbed and fixed per unit time. Therefore, if the thickness of the first absorbing and fixing layer is increased, the amount of CO2 that can be absorbed and fixed increases, but in order to absorb and fix CO2 in the entire first absorbing and fixing layer, the period of exposure to the atmosphere becomes long. Therefore, by setting the thickness of the first absorbing and fixing layer to 1 mm or more and 100 mm or less, taking into consideration the amount of CO2 absorbed and fixed in the first absorbing and fixing layer and the period of exposure to the atmosphere, etc., CO2 can be efficiently absorbed and fixed in the first absorbing and fixing layer. The thickness of the first absorbing and fixing layer is preferably 1 mm or more and 50 mm or less, more preferably 1 mm or more and 20 mm or less, from the viewpoint of improving the efficiency of CO2 absorption and fixation.

[0035] The thickness of the first absorbing fixed layer is the distance from the top of the portion where the first absorbing fixed layer is formed to the top of the first absorbing fixed layer in the cross section in the thickness direction of the first absorbing fixed layer. For example, the thickness of the first absorbing fixed layer can be measured using a laser displacement meter. In addition, when the surface of the portion where the first absorbing fixed layer is formed and / or the surface of the first absorbing fixed layer is rough, the thickness of the first absorbing fixed layer refers to the distance from the average line that equalizes the roughness of the portion where the first absorbing fixed layer is formed in the cross section in the thickness direction of the first absorbing fixed layer to the average line that equalizes the roughness on the surface side of the first absorbing fixed layer. In this specification, the average line refers to the line where the total area of ​​the convex parts and the total area of ​​the concave parts per unit length are the same, and the measurement can be performed using a surface roughness meter.

[0036] The location where the first absorbent fixing layer is formed is not particularly limited as long as the hydraulic composition can be poured or applied. For example, the first absorbent fixing layer may be formed by overlapping it on existing concrete. By overlapping the first absorbent fixing layer on the existing concrete, a new surface layer can be formed on the existing concrete, so that when the existing concrete is deteriorated, it is possible to repair the existing concrete.

[0037] In step (2), the first absorbing fixed layer is exposed to the atmosphere to absorb and fix CO2 in the first absorbing fixed layer. The period for which the first absorbing fixed layer is exposed to the atmosphere is not particularly limited as long as the first absorbing fixed layer can absorb and fix CO2.

[0038] As described above, when a concrete or mortar structure is exposed to the atmosphere, the amount of CO2 absorbed and fixed per unit time changes depending on the period of exposure to the atmosphere. Therefore, it is preferable to expose the first absorbing and fixing layer to the atmosphere during a period when the amount of CO2 absorbed and fixed per unit time is large. From the viewpoint of improving the efficiency of CO2 absorption and fixation, the period for exposing the first absorbing and fixing layer to the atmosphere is preferably 1 year or more and 15 years or less, more preferably 1 year or more and 8 years or less.

[0039] In step (3), a hydraulic composition is used and is superimposed on the first absorbent fixing layer to form a second absorbent fixing layer. The second absorbent fixing layer is formed by pouring or applying the kneaded hydraulic composition onto the first absorbent fixing layer and then hardening it. When forming the second absorbent fixing layer, a self-leveling material may be used to level the surface of the n-th absorbent fixing layer.

[0040] The second absorbing and fixing layer is formed on the first absorbing and fixing layer. The second absorbing and fixing layer, which serves as a new surface layer, is formed on the first absorbing and fixing layer in which CO2 has been absorbed and fixed, so that the second absorbing and fixing layer can absorb and fix CO2.

[0041] The thickness of the second absorbent fixed layer is 1 mm or more and 100 mm or less. It is the same as the first absorbent fixed layer described above, and the thickness of the second absorbent fixed layer is preferably 1 mm or more and 50 mm or less, more preferably 1 mm or more and 20 mm or less, from the viewpoint of improving the efficiency of CO2 absorption and fixation. The thickness of the second absorbent fixed layer is the same as the first absorbent fixed layer, and is the distance from the top of the first absorbent fixed layer to the top of the second absorbent fixed layer in the cross section in the thickness direction of the second absorbent fixed layer, and the thickness when the surface of the first absorbent fixed layer and / or the second absorbent fixed layer is rough is also the same as the first absorbent fixed layer.

[0042] In step (4), the second absorbing fixed layer is exposed to the atmosphere to absorb and fix CO2 in the second absorbing fixed layer. The period for which the second absorbing fixed layer is exposed to the atmosphere is the same as that for the first absorbing fixed layer, and is not particularly limited as long as the second absorbing fixed layer can absorb and fix CO2. From the viewpoint of improving the efficiency of CO2 absorption and fixation, the period for which the second absorbing fixed layer is exposed to the atmosphere is preferably 1 year or more and 15 years or less, more preferably 1 year or more and 8 years or less.

[0043] The CO2 absorption and fixation method according to this embodiment forms a new second absorbing and fixating layer on top of the first absorbing and fixating layer that has absorbed and fixed CO2, and further absorbs and fixes CO2, thereby enabling efficient absorption and fixation of CO2.

[0044] The CO2 absorption and fixation method according to this embodiment may further include the following steps (5) and (6). (5) A step of forming an n-th absorbent-fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and superposing it on the n-1th absorbent-fixing layer (n is any natural number of 3 or more, and the n-th absorbent-fixing layer is the n-th absorbent-fixing layer). (6) A step of exposing the nth absorbent layer to the atmosphere to absorb and fix CO2 in the nth absorbent layer.

[0045] In step (5), the hydraulic composition is used and is superimposed on the (n-1)th absorbent fixing layer to form the (n)th absorbent fixing layer. The (n)th absorbent fixing layer is formed by pouring or applying the kneaded hydraulic composition onto the (n-1)th absorbent fixing layer and then hardening it. When forming the (n)th absorbent fixing layer, the surface of the (n)th absorbent fixing layer may be leveled using a self-leveling material.

[0046] The n-th absorbing fixed layer (n is any natural number equal to or greater than 3) in step (5) is the n-th absorbing fixed layer formed after the second absorbing fixed layer. The n-th absorbing fixed layer is formed on the (n-1)th absorbing fixed layer formed as the (n-1)th layer.

[0047] Since the nth absorbing fixed layer, which serves as a new surface layer, is formed on the (n-1)th absorbing fixed layer in which CO2 has been absorbed and fixed, it is possible to cause the nth absorbing fixed layer to absorb and fix CO2.

[0048] The thickness of the nth absorbent fixed layer is 1 mm or more and 100 mm or less. Similar to the above-mentioned first absorbent fixed layer, the thickness of the nth absorbent fixed layer is preferably 1 mm or more and 50 mm or less, more preferably 1 mm or more and 20 mm or less, from the viewpoint of improving the efficiency of CO2 absorption and fixation. The thickness of the nth absorbent fixed layer is similar to that of the first absorbent fixed layer, and is defined as the distance from the top of the n-1th absorbent fixed layer to the top of the nth absorbent fixed layer in the cross section in the thickness direction of the nth absorbent fixed layer, and the thickness when the surface of the n-1th absorbent fixed layer and / or the nth absorbent fixed layer is rough is also similar to that of the first absorbent fixed layer.

[0049] In step (6), the nth absorbent fixed layer is exposed to the atmosphere to absorb and fix CO2 in the nth absorbent fixed layer. The period for which the nth absorbent fixed layer is exposed to the atmosphere is the same as that for the first absorbent fixed layer, and is not particularly limited as long as the nth absorbent fixed layer can absorb and fix CO2. From the viewpoint of improving the efficiency of CO2 absorption and fixation, the period for which the nth absorbent fixed layer is exposed to the atmosphere is preferably 1 year or more and 15 years or less, more preferably 1 year or more and 8 years or less.

[0050] The CO2 absorption and fixation method according to this embodiment includes steps (5) and (6), and thus the nth absorption and fixation layer is formed over the (n-1)th absorption and fixation layer, thereby enabling more efficient absorption and fixation of CO2.

[0051] The CO2 absorption and fixation method according to this embodiment may further include the following step (7). (7) increasing the natural number n by 1 and repeating steps (5) and (6) at least once.

[0052] In step (7), the natural number n is increased by 1 and step (5) and step (6) are repeated at least once. By repeating step (5) and step (6), a new surface layer, the n-th absorbent fixed layer, is formed on the (n-1)-th absorbent fixed layer in which the natural number n is increased by 1 and in which CO2 has been absorbed and fixed, and the n-th absorbent fixed layer is exposed to the atmosphere.

[0053] The CO2 absorption and fixation method according to this embodiment includes the step (7), and thus can efficiently and continuously absorb and fix CO2.

[0054] <Joint construction method> The joint construction method according to the present embodiment is a joint construction method for concrete or mortar that absorbs and fixes CO2, and includes the following steps (1) to (4), in which the hydraulic composition contains cement and water, and the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) A step of forming a first absorbent fixing layer having a thickness of 1 mm to 100 mm using a hydraulic composition. (2) A step of exposing the first fixed absorbent layer to the atmosphere to absorb and fix CO2 in the first fixed absorbent layer. (3) A step of forming a second absorbent fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and overlapping the first absorbent fixing layer. (4) A step of exposing the second absorbent layer to the atmosphere to absorb and fix CO2 in the second absorbent layer. Any parts not specifically explained are the same as those in the CO2 absorption and fixation method described above.

[0055] The joint construction method according to this embodiment involves joint construction of concrete or mortar that absorbs and fixes CO2 in the same process as the above-mentioned CO2 absorption and fixation method. Therefore, the joint construction method according to this embodiment forms a new second absorption and fixation layer on top of the first absorption and fixation layer that absorbs and fixes CO2, and further absorbs and fixes CO2, so that CO2 can be efficiently absorbed and fixed.

[0056] The present invention includes the following aspects. [1] A method for absorbing and fixing CO2, comprising the steps of: The method includes the following steps (1) to (4): The hydraulic composition comprises cement and water, A method for absorbing and fixing CO2, wherein the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) A step of forming a first absorbent fixing layer having a thickness of 1 mm to 100 mm using a hydraulic composition. (2) A step of exposing the first fixed absorbent layer to the atmosphere to absorb and fix CO2 in the first fixed absorbent layer. (3) A step of forming a second absorbent fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and overlapping the first absorbent fixing layer. (4) A step of exposing the second absorbent layer to the atmosphere to absorb and fix CO2 in the second absorbent layer. [2] The method for absorbing and fixing CO2 according to the above [1], wherein in the step (2), the first absorbing and fixing layer is exposed to the atmosphere for a period of 1 year or more and 15 years or less. [3] The method for absorbing and fixing CO2 according to the above [1] or [2], wherein in the step (4), the second absorbing and fixing layer is exposed to the atmosphere for a period of 1 year or more and 15 years or less. [4] The method for absorbing and fixing CO2 according to any one of the above [1] to [3], further comprising the following steps (5) and (6): (5) A step of forming an n-th absorbent-fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and superposing it on the n-1th absorbent-fixing layer (n is any natural number of 3 or more, and the n-th absorbent-fixing layer is the n-th absorbent-fixing layer). (6) A step of exposing the nth absorbent layer to the atmosphere to absorb and fix CO2 in the nth absorbent layer. [5] The method for absorbing and fixing CO2 according to the above [4], further comprising the following step (7): (7) increasing the natural number n by 1 and repeating steps (5) and (6) at least once. [6] The method for absorbing and fixing CO2 according to any one of the above [1] to [5], wherein in the step (1), the first absorbing and fixing layer is formed on an existing concrete. [7] A method for joining concrete or mortar that absorbs and fixes CO2. The method includes the following steps (1) to (4): The hydraulic composition comprises cement and water, A joint construction method in which the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) A step of forming a first absorbent fixing layer having a thickness of 1 mm to 100 mm using a hydraulic composition. (2) A step of exposing the first fixed absorbent layer to the atmosphere to absorb and fix CO2 in the first fixed absorbent layer. (3) A step of forming a second absorbent fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and overlapping the first absorbent fixing layer. (4) A step of exposing the second absorbent layer to the atmosphere to absorb and fix CO2 in the second absorbent layer. EXAMPLES

[0057] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0058] (Preparation of hydraulic composition) Table 1 shows the components contained in the hydraulic compositions 1 and 2. Details of each component shown in Table 1 are described below. Cement: Ordinary Portland cement (manufactured by Sumitomo Osaka Cement Co., Ltd.) Fine aggregate: Mountain sand (produced in Kakegawa City, Shizuoka Prefecture)

[0059] [Table 1]

[0060] (CO2 absorption and fixation) <Example 1> CO2 absorption and fixation was carried out in the following manner. [1] The kneaded hydraulic composition 1 was poured into a formwork (length 400 mm, width 100 mm, height 100 mm) to prepare a test specimen having a length of 400 mm, a width of 100 mm, and a thickness of 80 mm. [2] The first accelerated carbonation test was conducted by exposing the specimen to an atmosphere with a CO2 concentration of 5% for 28 days. At this time, only the top surface of the specimen was left open, and the other surfaces were sealed with aluminum tape so that CO2 absorption and fixation occurred only from the top surface. The first accelerated carbonation test was conducted in accordance with the method specified in JIS A 1153:2012. [3] After the first accelerated carbonation test, a part of the specimen was cut and the amount of CO2 absorbed and fixed by the specimen was measured using the cut specimen. The amount of CO2 absorbed and fixed by the specimen was measured by cutting 10 mm from the top surface in the thickness direction of the specimen, crushing it, and then using a STA 2500 (TG-DTA simultaneous measurement device) (manufactured by NETZSCH Japan) to measure the amount of CO2 absorbed and fixed by the specimen using simultaneous thermogravimetry and differential thermal analysis. The results are shown in Table 2. [4] A mark was made 20 mm above the top surface of the test specimen, and the kneaded hydraulic composition 1 was poured successively so as to be at the same height as the mark. A laminate having a layer of hydraulic composition 1 20 mm thick was formed on the top surface of the test specimen, and the specimen was allowed to cure in air for 28 days. [5] A second accelerated carbonation test was conducted by exposing the laminate to an atmosphere with a CO2 concentration of 5% for 28 days. At this time, only the top surface of the laminate was left open, and the other surfaces were sealed with aluminum tape so that CO2 absorption and fixation occurred only from the top surface. The second accelerated carbonation test was conducted in the same manner as the first accelerated carbonation test. [6] A part of the laminate was cut, and the amount of CO2 absorbed and fixed by the laminate was measured using the cut laminate. The amount of CO2 was measured by cutting 10 mm from the top surface of the laminate in the thickness direction, pulverizing it, and using the same method as above. The results are shown in Table 2.

[0061] <Comparative Example 1> [1] The kneaded hydraulic composition 1 was poured into a formwork (length 400 mm, width 100 mm, height 100 mm) to prepare a test specimen having a length of 400 mm, a width of 100 mm, and a thickness of 100 mm. [2] The first accelerated carbonation test was conducted by exposing the specimen to an atmosphere with a CO2 concentration of 5% for 28 days. At this time, only the top surface of the specimen was left open, and the other surfaces were sealed with aluminum tape so that CO2 was absorbed and fixed only from the top surface. The first accelerated carbonation test was conducted in the same manner as above. [3] After the first accelerated carbonation test, a part of the specimen was cut and the amount of CO2 absorbed and fixed by the specimen was measured. The amount of CO2 was measured by cutting 10 mm from the top surface of the specimen in the thickness direction, crushing it, and using the same method as above. The results are shown in Table 2. [4] The specimens were left to cure in the air for 28 days. [5] The second accelerated carbonation test was conducted by exposing the air-cured specimen to an atmosphere with a CO2 concentration of 5% for 28 days. At this time, only the top surface of the specimen was left open, and the other surfaces were sealed with aluminum tape so that CO2 was absorbed and fixed only from the top surface. The second accelerated carbonation test was conducted in the same manner as above. [6] A part of the test specimen was cut, and the amount of CO2 absorbed and fixed by the test specimen was measured using the cut specimen. The amount of CO2 was measured by cutting 10 mm from the top surface of the test specimen in the thickness direction, crushing it, and using the same method as above. The results are shown in Table 2.

[0062] <Comparative Example 2> The procedure was the same as Comparative Example 1, except that Hydraulic Composition 2 was used instead of Hydraulic Composition 1.

[0063] [Table 2]

[0064] In Table 2, the total amount of CO2 absorption and fixation is the sum of the values ​​after each accelerated carbonation test. The total amount of CO2 absorption and fixation is higher in Example 1 than in Comparative Examples 1 and 2. This shows that it is possible to efficiently absorb and fix CO2 by forming a new layer that absorbs and fixes CO2 on the layer that absorbs and fixes CO2.

Claims

1. CO 2 Absorbs and fixes CO 2 An absorption and fixation method comprising the steps of: The method includes the following steps (1) to (4): The hydraulic composition comprises cement and water, The water-cement ratio of the hydraulic composition is 40% or more and 60% or less. 2 Absorption fixation method. (1) A step of forming a first absorbent fixing layer having a thickness of 1 mm to 100 mm using a hydraulic composition. (2) Exposing the first fixed layer to the atmosphere to cause CO 2 The process of absorbing and fixing (3) A step of forming a second absorbent fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and superimposing it on the first absorbent fixing layer. (4) Exposing the second fixed layer to the atmosphere to cause CO 2 The process of absorbing and fixing

2. 2. The method according to claim 1, wherein in the step (2), the first absorbing fixed layer is exposed to the atmosphere for a period of 1 year or more and 15 years or less. 2 Absorption fixation method.

3. 3. The method according to claim 1 or 2, wherein in the step (4), the second absorbing fixed layer is exposed to the atmosphere for a period of 1 year or more and 15 years or less. 2 Absorption fixation method.

4. The CO method according to claim 1 or 2, further comprising the following steps (5) and (6): 2 Absorption fixation method. (5) A step of forming an n-th absorbent fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and superposing it on the n-1-th absorbent fixing layer (n is any natural number of 3 or more, and the n-th absorbent fixing layer is the n-th layer). (6) Exposing the nth fixed absorbent layer to the atmosphere to cause CO 2 The process of absorbing and fixing

5. The CO according to claim 4, further comprising the following step (7): 2 Absorption fixation method. (7) increasing the natural number n by 1 and repeating steps (5) and (6) at least once.

6. The CO2 absorbing and fixing layer according to claim 1 or 2, wherein in step (1), the first absorbing and fixing layer is formed on the existing concrete. 2 Absorption fixation method.

7. CO 2 A concrete or mortar jointing method that absorbs and fixes The method includes the following steps (1) to (4): The hydraulic composition comprises cement and water, A joint construction method in which the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) A step of forming a first absorbent fixing layer having a thickness of 1 mm to 100 mm using a hydraulic composition. (2) Exposing the first fixed layer to the atmosphere to cause CO 2 The process of absorbing and fixing (3) A step of forming a second absorbent fixing layer having a thickness of 1 mm to 100 mm by using a hydraulic composition and superimposing it on the first absorbent fixing layer. (4) Exposing the second fixed layer to the atmosphere to cause CO 2 The process of absorbing and fixing

Citation Information

Patent Citations

  • Method of repairing reinforced concrete structure

    JP2006124232A

  • Method for suppressing corrosion of reinforcing bar embedded in existing reinforced concrete

    JP2013117057A

  • Absorption method of carbon dioxide

    JP2020165276A