Co2 absorption and fixation method, and cross-section repair construction method
By forming absorption fixation layers using a specific hydraulic composition and exposing them to the atmosphere, the method addresses the challenge of CO2 absorption in concrete and mortar structures, achieving efficient CO2 removal and fixation.
Patent Information
- Application Number
- JP2023055867
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Concrete and mortar structures do not absorb carbon dioxide (CO2) from the atmosphere, leading to neutralization and alkalinity reduction, which is a concern in the context of carbon neutrality efforts, necessitating a method for CO2 absorption and fixation.
A method involving the use of a hydraulic composition with a water-cement ratio of 40% to 60% to form absorption fixation layers by chiseling existing concrete based on neutralization depth, exposing these layers to the atmosphere to absorb and fix CO2, and repeating this process to enhance CO2 removal efficiency.
The method effectively forms new layers that absorb and fix CO2, reducing the amount of CO2 in existing concrete structures, enabling continuous and efficient CO2 removal.
Smart Images

Figure 2024143280000001 
Figure 2024143280000002 
Figure 2024143280000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a CO2 absorption and fixation method and a cross-section repair method. [Background technology]
[0002] A cross-section repair method is known as a repair method for repairing deterioration of a concrete or mortar structure, loss of the cross-section of the structure, spalling, etc. The cross-section repair method is a method in which the deteriorated part of the structure is chipped off and removed, and the structure is restored to a sound state using a cross-section repair material.
[0003] As disclosed in Non-Patent Document 1, for example, there are three cross-section repair methods: the plastering method, the filling method, and the spraying method. The plastering method does not require the installation of formwork, so it is applied when the cross-section repair locations are small or scattered. The filling method is a method in which formwork is installed and highly fluid concrete or mortar is poured into the formwork, and is applied to medium- to large-scale repairs. The spraying method is a method in which concrete or mortar is applied using compressed air, centrifugal force, etc., without installing formwork, and is applied to medium- to large-scale repairs like the filling method. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Immediately useful basic knowledge of cement-based repair and reinforcement materials, 2nd edition, Cement Association, August 25, 2011 Summary of the Invention [Problem to be solved by the invention]
[0005] Meanwhile, a phenomenon called neutralization (carbonation) is known in which concrete or mortar structures absorb carbon dioxide (CO2) from the atmosphere and reduce the alkalinity of the structure. In recent years, with the rise in carbon neutral momentum, technologies aimed at reducing CO2 emissions and absorbing and fixing CO2 have been attracting attention. Therefore, there is a demand for a method of efficiently absorbing and fixing CO2 by utilizing the absorption and fixation of CO2 in concrete or mortar structures.
[0006] The present invention has been made in consideration of the above circumstances, and has an objective to provide a CO2 absorption and fixation method and a cross-section repair method using concrete or mortar, which efficiently absorbs and fixes CO2 by forming a CO2 absorption and fixation layer that absorbs and fixes CO2 after chipping the structure when repairing the cross-section of a concrete or mortar structure. [Means for solving the problem]
[0007] The CO2 absorption and fixation method according to the present invention is a CO2 absorption and fixation method for absorbing and fixing CO2, The method includes the following steps (1) to (4): The hydraulic composition comprises cement and water, The water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) The process of determining the thickness of existing concrete chipping based on the carbonation depth to which CO2 has been absorbed and fixed in the existing concrete. (2) The existing concrete is chipped to the thickness determined in step (1). (3) A step of forming a first absorbent fixing layer on the portion removed in the step (2) using a hydraulic composition. (4) A step of exposing the first fixed absorbent layer to the atmosphere and allowing the first fixed absorbent layer to absorb and fix CO2
[0008] With this configuration, the CO2 absorption and fixation method of the present invention chips away the areas of existing concrete where CO2 has been absorbed and fixed, and forms a new layer in the chipped-off area to absorb and fix CO2, thereby enabling efficient absorption and fixation of CO2.
[0009] In the method for absorbing and fixing CO2 according to the present invention, the n-th absorbing and fixing layer (n is a natural number, and the n-th absorbing and fixing layer is the absorbing and fixing layer formed for the nth time) is exposed to the atmosphere for a period of 1 year or more and 15 years or less, The method may further include the following steps (5) to (7). (5) A process of chipping at least the portion of the existing concrete on which the nth absorbent layer has been formed, including the nth absorbent layer, to a thickness of 1 mm or more and 15 mm or less. (6) A step of forming an (n+1)th absorbing and fixing layer on the chipped portion in the step (5) using a hydraulic composition. (7) A step of exposing the (n+1)th fixed absorbent layer to the atmosphere to allow the (n+1)th fixed absorbent layer to absorb and fix CO2
[0010] With such a configuration, the CO2 absorption and fixation method according to the present invention forms the nth absorption and fixation layer in the existing concrete to absorb and fix CO2, and therefore, efficient absorption and fixation of CO2 can be continuously performed.
[0011] In the CO2 absorption and fixation method according to the present invention, the nth absorption and fixation layer may be exposed to the atmosphere for a period of one year or more and eight years or less.
[0012] In the CO2 absorption and fixation method according to the present invention, due to such a configuration, the nth absorption and fixation layer absorbs and fixes a large amount of CO2, and therefore, CO2 can be absorbed and fixed more efficiently.
[0013] The cross-section repair method according to the present invention is a cross-section repair method using concrete or mortar that absorbs and fixes CO2, The method includes the following steps (1) to (4): The hydraulic composition comprises cement and water, The water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) The process of determining the thickness of existing concrete chipping based on the carbonation depth to which CO2 has been absorbed and fixed in the existing concrete. (2) The existing concrete is chipped to the thickness determined in step (1). (3) A step of forming a first absorbent fixing layer on the portion removed in the step (2) using a hydraulic composition. (4) A step of exposing the first fixed absorbent layer to the atmosphere and allowing the first fixed absorbent layer to absorb and fix CO2
[0014] With this configuration, the cross-section repair method of the present invention chips away the areas of the existing concrete that have absorbed and fixed CO2, and forms a new layer in the chipped-off area to absorb and fix the CO2, thereby enabling efficient absorption and fixation of CO2.
[0015] In the cross-section repair method according to the present invention, the period during which the n-th absorption fixation layer (n is any natural number, and the n-th absorption fixation layer is the absorption fixation layer formed for the nth time) is exposed to the atmosphere is 1 year or more and 15 years or less, The method may further include the following steps (5) to (7). (5) A process of chipping at least the portion of the existing concrete on which the nth absorbent layer has been formed, including the nth absorbent layer, to a thickness of 1 mm or more and 15 mm or less. (6) A step of forming an (n+1)th absorbing and fixing layer on the chipped portion in the step (5) using a hydraulic composition. (7) A step of exposing the (n+1)th fixed absorbent layer to the atmosphere to allow the (n+1)th fixed absorbent layer to absorb and fix CO2
[0016] The cross-section repair method according to the present invention, which has such a configuration, forms an nth absorption and fixation layer in the existing concrete to absorb and fix CO2, and therefore can continuously and efficiently absorb and fix CO2. Effect of the Invention
[0017] According to the present invention, it is possible to provide a CO2 absorption and fixation method and a cross-section repair method that can efficiently absorb and fix CO2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The CO2 absorption and fixation method and cross-section repair method according to this embodiment will be described below.
[0019] <CO2 Absorption and Fixation Method> The CO2 absorption and fixation method according to this embodiment is a CO2 absorption and fixation method for absorbing and fixing CO2, and has the following steps (1) to (4). The hydraulic composition includes cement and water, and the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) A step of determining the hanging thickness of the existing concrete based on the neutralization depth at which CO2 in the existing concrete is absorbed and fixed (2) A step of hanging the existing concrete with the hanging thickness determined in step (1) (3) A step of forming a first absorption and fixation layer on the part removed by hanging using a hydraulic composition in step (2) (4) A step of exposing the first absorption and fixation layer to the atmosphere and absorbing and fixing CO2 in the first absorption and fixation layer
[0020] In the CO2 absorption and fixation method according to this embodiment, the hydraulic composition used for forming the absorption and fixation layer that absorbs and fixes CO2 includes cement and water.
[0021] The cement is not particularly limited. For example, Portland cement such as ordinary Portland cement, early-strength Portland cement, ultra-early-strength Portland cement, medium-heat Portland cement, sulfate-resistant Portland cement, and white Portland cement specified in JIS R 5210:2019; blast furnace cement, fly ash cement, silica cement, etc. Mixed cement; known cements such as super-fast hard cement and alumina cement can be used. Note that the cement may be used alone or in combination of two or more.
[0022] The water is not particularly limited. For example, tap water, industrial water, recycled water, groundwater, river water, rainwater, etc. can be used. It is preferable that the water does not contain organic substances, chloride ions, sodium ions, potassium ions, etc. that have an adverse effect on the hydration reaction of the concrete composition and the pavement concrete, or that the content is extremely small even if it is contained. The water is more preferably tap water or industrial water with stable quality.
[0023] The hydraulic composition may also contain aggregate. As the aggregate, fine aggregate and / or coarse aggregate can be used. Note that fine aggregate refers to aggregate that passes entirely through a 10 mm mesh sieve and passes 85% or more by mass through a 5 mm mesh sieve, and coarse aggregate refers to aggregate that remains on a 5 mm mesh sieve at 85% or more by mass (JIS A 0203:2019).
[0024] Examples of fine aggregates include river sand, land sand, mountain sand, sea sand, crushed sand, limestone crushed sand, and other natural sands as specified in JIS A 5308:2019 Appendix A Aggregates for Ready-Mixed Concrete, and blast furnace slag. Silica sand produced by crushing and classifying silica may also be used. Note that one type of fine aggregate may be used alone, or two or more types may be used in combination.
[0025] Examples of coarse aggregates include natural aggregates such as river gravel, mountain gravel, and sea gravel, as specified in JIS A 5308:2019 Appendix A Aggregates for Ready-Mixed Concrete, artificial aggregates such as crushed stone such as sandstone, hard limestone, basalt, andesite, and recycled aggregates. Note that one type of coarse aggregate may be used alone, or two or more types may be used in combination.
[0026] The hydraulic composition may also contain an admixture. Examples of the admixture include inorganic fine powders such as fly ash, silica fume, cement kiln dust, blast furnace fume, ground granulated blast furnace slag, ground cooled blast furnace slag, ground converter slag, hemihydrate gypsum, expanding material, ground limestone, ground quicklime, and ground dolomite, and inorganic fillers such as sodium bentonite, calcium bentonite, attapulgite, sepiolite, activated clay, acid clay, allophane, imogolite, shirasu (volcanic ash), shirasu balloon, kaolinite, metakaolin (calcined clay), synthetic zeolite, artificial zeolite, artificial zeolite, mordenite, and clinoptilolite. The admixture may be used alone or in combination of two or more kinds.
[0027] The hydraulic composition may also contain an admixture. Examples of the admixture include air-entraining agents, air-entraining water-reducing agents, high-performance water-reducing agents, high-performance air-entraining water-reducing agents, fluidizing agents, separation-reducing agents, setting retarders (e.g., tartaric acid, etc.), setting accelerators (e.g., aluminum sulfate, etc.), quick-setting agents, shrinkage-reducing agents, foaming agents, foaming agents, waterproofing agents, etc. The admixtures may be used alone or in combination of two or more.
[0028] The water-cement ratio of the hydraulic composition is 40% or more and 60% or less. The water-cement ratio is the mass percentage of water to cement. From the viewpoint of improving the CO2 absorption and fixation amount of the absorption and fixation layer described later, the water-cement ratio is 40% or more, preferably 45% or more. From the viewpoint of improving the strength of the absorption and fixation layer, the water-cement ratio is 60% or less, preferably 55% or less.
[0029] In step (1), the chipping thickness of existing concrete is determined based on the carbonation depth to which CO2 has been absorbed and fixed in the existing concrete.
[0030] In step (1), the carbonation depth of the existing concrete where CO2 has been absorbed and fixed can be determined by measurement or prediction. The carbonation depth can be measured, for example, by taking a core from the existing concrete by the method specified in JIS A 1107:2012, and using the core by the method specified in JIS A 1152:2018. The carbonation depth can be predicted, for example, by using the following formula (1).
[0031]
number
[0032] Then, the chipping thickness of the existing concrete is determined based on the carbonation depth. At this time, the chipping thickness to be determined is not particularly limited as long as it includes the carbonated area where CO2 is absorbed and fixed. The chipping thickness may be, for example, the same as the calculated carbonation depth, a thickness smaller than the calculated carbonation depth, or a thickness larger than the calculated carbonation depth. The chipping thickness is preferably ±50 mm relative to the carbonation depth, and more preferably ±20 mm relative to the carbonation depth.
[0033] In addition, since carbonation of a concrete or mortar structure progresses from the surface of the structure exposed to the atmosphere toward the inside, the chipping thickness may be determined based on the depth to which carbonation is estimated to have progressed, i.e., the carbonation depth, depending on the age of the existing concrete. For example, the chipping thickness may be determined as follows: if the age of the existing concrete is less than 1 year, 1 to 3 mm if 1 to 2 years, 1 to 4 mm if 2 to 3 years, 1 to 6 mm if 3 to 4 years, 2 to 7 mm if 4 to 5 years, 2 to 7 mm if 5 to 6 years, 2 to 8 mm if 6 to 7 years, 2 to 9 mm if 7 to 8 years, 3 to 11 mm if 8 to 9 years, 3 to 11 mm if 9 to 10 years, 3 to 12 mm if 10 to 11 years, 3 to 13 mm if 11 to 12 years, 3 to 13 mm if 12 to 13 years, 3 to 14 mm if 13 to 14 years, 4 to 14 mm if 14 to 15 years. In this specification, the existing concrete includes not only concrete but also mortar.
[0034] In step (2), the existing concrete is chipped to the chipping thickness determined in step (1). There is no particular limitation on the method for chipping the existing concrete, and it can be done using known tools such as a chipping hammer, a breaker, a water jet, etc. Also, for example, a disk grinder can be used to make the surface exposed after chipping smooth. The chipped thickness of the existing concrete refers to the distance from the surface of the existing concrete exposed before chipping to the surface exposed after chipping. The chipped thickness can be measured using a laser displacement meter.
[0035] In addition, when chipping the existing concrete in step (2), the surface of the existing concrete and / or the surface exposed after chipping may be rough. In this case, the chipping thickness is the distance from the average line that equalizes the roughness of the existing concrete surface in the cross section in the chipping thickness direction to the average line that equalizes the roughness of the surface exposed after chipping. In this specification, the average line refers to the line where the total area of the convex parts and the total area of the concave parts per unit length are the same, and the measurement can be performed using a surface roughness meter.
[0036] By chipping the existing concrete to the thickness determined in step (1), the areas where CO2 has been absorbed, fixed, and neutralized are removed from the existing concrete.
[0037] In step (3), a first absorbing and fixing layer is formed on the chipped portion in step (2) using a hydraulic composition. The first absorbing and fixing layer is formed by pouring, applying, or the like the kneaded hydraulic composition on the chipped portion and then hardening it.
[0038] The first absorbent-fixing layer is formed on the portion of the existing concrete that has been chipped off. In this case, the thickness of the first absorbent-fixing layer is not particularly limited, and may be the same as the thickness of the portion chipped off from the existing concrete, or may be smaller or larger than the thickness of the portion chipped off from the existing concrete. When the thickness of the first absorbent-fixing layer is the same as the thickness of the portion chipped off from the existing concrete, the sum of the thickness of the chipped existing concrete and the thickness of the first absorbent-fixing layer can be the same as the thickness of the existing concrete before chipping. Note that the thickness of the first absorbent-fixing layer being the same as the thickness of the portion chipped off means a thickness within ±10 mm of the thickness of the portion chipped off.
[0039] The thickness of the first absorbing fixed layer is the distance from the top of the existing concrete that has been chipped to the top of the first absorbing fixed layer in the cross section in the thickness direction of the first absorbing fixed layer. For example, the thickness of the first absorbing fixed layer can be measured using a laser displacement meter. In addition, when the surface of the chipped existing concrete and / or the surface of the first absorbing fixed layer are rough, the thickness of the first absorbing fixed layer is the distance from the average line of the uniform roughness of the surface side of the chipped existing concrete in the cross section in the thickness direction of the first absorbing fixed layer to the average line of the uniform roughness of the surface side of the first absorbing fixed layer.
[0040] In step (4), the first absorbing and fixing layer is exposed to the atmosphere to absorb and fix CO2 in the first absorbing and fixing layer. In general, in a concrete or mortar structure, CO2 is absorbed and fixed from the surface exposed to the atmosphere toward the inside, so that in the early period of exposure to the atmosphere, the amount of CO2 absorbed and fixed per unit time is large, and the longer the exposure period, the smaller the amount of CO2 absorbed and fixed per unit time becomes. Therefore, it is preferable to expose the first absorbing and fixing layer to the atmosphere during a period when the amount of CO2 absorbed and fixed per unit time is large. From the viewpoint of improving the efficiency of CO2 absorption and fixation, the period for exposing the first absorbing and fixing layer to the atmosphere is 1 year or more and 15 years or less, preferably 1 year or more and 8 years or less.
[0041] The CO2 absorption and fixation method according to this embodiment involves chipping away the areas of existing concrete where CO2 has been absorbed and fixed, and forming a new layer in the chipped-away area to absorb and fix the CO2, thereby enabling efficient absorption and fixation of CO2.
[0042] The CO2 absorption and fixation method according to this embodiment may include exposing the n-th absorption and fixation layer (n is any natural number, and the n-th absorption and fixation layer is the absorption and fixation layer formed for the nth time) to the atmosphere for a period of 1 year or more and 15 years or less, and may further include the following steps (5) to (7). (5) A process of chipping at least the portion of the existing concrete on which the nth absorbent layer has been formed, including the nth absorbent layer, to a thickness of 1 mm or more and 15 mm or less. (6) A step of forming an (n+1)th absorbing and fixing layer on the chipped portion in the step (5) using a hydraulic composition. (7) A step of exposing the (n+1)th fixed absorbent layer to the atmosphere to allow the (n+1)th fixed absorbent layer to absorb and fix CO2
[0043] In step (5), at least a portion of the existing concrete on which the nth absorbing and fixing layer has been formed, including the nth absorbing and fixing layer, is chipped off to a thickness of 1 mm or more and 15 mm or less.
[0044] In step (5), the nth absorption and fixation layer is formed on the existing concrete for the nth time (n is any natural number) and is exposed to the atmosphere to absorb and fix CO2. The period for exposing the nth absorption and fixation layer to the atmosphere is 1 year or more and 15 years or less, and preferably 1 year or more and 8 years or less.
[0045] The method for chipping the nth absorbent fixing layer is the same as the method for chipping the existing concrete described above, and is not particularly limited, and can be performed using known tools such as a chipping hammer, a breaker, a water jet, etc. Also, for example, a disk grinder may be used to smooth the surface exposed after chipping.
[0046] The chipped thickness of the nth absorbent fixing layer is 1 mm or more and 15 mm or less. By setting the chipped thickness of the nth absorbent fixing layer to 1 mm or more and 15 mm or less, the part of the nth absorption step layer where CO2 is absorbed and fixed can be sufficiently removed. The chipped thickness of the nth absorbent fixing layer is the same as the chipped thickness of the existing concrete described above, and refers to the distance from the surface of the nth absorbent fixing layer exposed before chipping to the surface exposed after chipping. When chipping the nth absorbent fixing layer in step (5), the surface of the nth absorbent fixing layer and / or the surface exposed after chipping may be rough. In that case, the chipped thickness is the same as the chipped thickness of the existing concrete described above, and refers to the distance from the average line of the uniform roughness of the surface of the nth absorbent fixing layer in the cross section in the chipping thickness direction to the average line of the uniform roughness of the surface exposed after chipping.
[0047] In step (6), the (n+1)th absorbing and fixing layer is formed on the chipped portion in step (5) using a hydraulic composition. The (n+1)th absorbing and fixing layer is formed by pouring, applying, or the like the kneaded hydraulic composition on the chipped portion and then hardening it.
[0048] The (n+1)th absorbing fixed layer is formed in the portion of the nth absorbing fixed layer that has been chipped off. In this case, the thickness of the (n+1)th absorbing fixed layer is not particularly limited, and may be the same as the chipped thickness from the nth absorbing fixed layer, or may be smaller or larger than the chipped thickness from the nth absorbing fixed layer. The fact that the thickness of the nth absorbing fixed layer is the same as the chipped thickness is the same as in the first absorbing fixed layer described above.
[0049] The thickness of the (n+1)th absorbing fixed layer is defined as the distance from the top of the nth chipped absorbing fixed layer to the top of the (n+1)th absorbing fixed layer in a cross section in the thickness direction of the (n+1)th absorbing fixed layer, as in the case of the first absorbing fixed layer described above. In addition, when the surface of the chipped nth absorbing fixed layer and / or the surface of the (n+1)th absorbing fixed layer is rough, the thickness is the same as that of the first absorbing fixed layer.
[0050] In step (7), the n+1th absorbent fixed layer is exposed to the atmosphere to absorb and fix CO2 in the n+1th absorbent fixed layer. The period during which the n+1th absorbent fixed layer is exposed to the atmosphere is the same as the period during which the nth absorbent fixed layer is exposed to the atmosphere described above.
[0051] The CO2 absorption and fixation method according to this embodiment includes steps (5) to (7) of exposing the nth absorption and fixation layer to the atmosphere for a period of 1 year or more and 15 years or less, thereby forming the nth absorption and fixation layer in the existing concrete and absorbing and fixing CO2, thereby enabling efficient continuous absorption and fixation of CO2.
[0052] <Cross-section repair method> The cross-section repair method according to this embodiment is a cross-section repair method using concrete or mortar that absorbs and fixes CO2, and includes the following steps (1) to (4), in which the hydraulic composition contains cement and water, and the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) The process of determining the thickness of existing concrete chipping based on the carbonation depth to which CO2 has been absorbed and fixed in the existing concrete. (2) The existing concrete is chipped to the thickness determined in step (1). (3) A step of forming a first absorbent fixing layer on the portion removed in the step (2) using a hydraulic composition. (4) A step of exposing the first fixed absorbent layer to the atmosphere and allowing the first fixed absorbent layer to absorb and fix CO2 Any parts not specifically explained are the same as those in the CO2 absorption and fixation method described above.
[0053] The cross-section repair method according to this embodiment repairs the cross-section with concrete or mortar that absorbs and fixes CO2 in the same process as the above-mentioned CO2 absorption and fixation method. Therefore, the cross-section repair method according to this embodiment chips off the part of the existing concrete that absorbed and fixed CO2, and forms a new layer in the chipped-off part to absorb and fix CO2, so that CO2 can be absorbed and fixed efficiently.
[0054] The cross-section repair method according to this embodiment may include exposing the n-th absorbing fixation layer (n is any natural number, and the n-th absorbing fixation layer is the absorbing fixation layer formed for the nth time) to the atmosphere for a period of 1 year or more and 15 years or less, and may further include the following steps (5) to (7). (5) A process of chipping at least the portion of the existing concrete on which the nth absorbent layer has been formed, including the nth absorbent layer, to a thickness of 1 mm or more and 15 mm or less. (6) A step of forming an (n+1)th absorbing and fixing layer on the chipped portion in the step (5) using a hydraulic composition. (7) A step of exposing the (n+1)th fixed absorbent layer to the atmosphere to allow the (n+1)th fixed absorbent layer to absorb and fix CO2
[0055] The cross-section repair method according to this embodiment includes steps (5) to (7) of exposing the nth absorption and fixation layer to the atmosphere for a period of 1 year or more and 15 years or less, thereby forming the nth absorption and fixation layer in the existing concrete and absorbing and fixating CO2, thereby enabling efficient continuous absorption and fixation of CO2. EXAMPLES
[0056] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0057] (Preparation of hydraulic composition) Table 1 shows the components contained in the hydraulic compositions 1 and 2. Details of each component shown in Table 1 are described below. Cement: Ordinary Portland cement (manufactured by Sumitomo Osaka Cement Co., Ltd.) Fine aggregate: Mountain sand (produced in Kakegawa City, Shizuoka Prefecture)
[0058] [Table 1]
[0059] (CO2 absorption and fixation) <Example 1> [1] The mixed hydraulic composition 1 was poured into a formwork (length 400 mm, width 100 mm, height 100 mm) to prepare a test specimen (existing concrete) having a length of 400 mm, a width of 100 mm, and a thickness of 100 mm. [2] The first accelerated carbonation test was conducted by exposing the specimen to an atmosphere with a CO2 concentration of 5% for 28 days. At this time, only the top surface of the specimen was left open, and the other surfaces were sealed with aluminum tape so that CO2 absorption and fixation occurred only from the top surface. The first accelerated carbonation test was conducted in accordance with the method specified in JIS A 1153:2012. [3] After the first accelerated carbonation test, a part of the specimen was cut, and the carbonation depth and the amount of CO2 absorbed and fixed by the specimen were measured using the cut specimen. The carbonation depth was measured in accordance with the method specified in JIS A 1152:2018. The amount of CO2 absorbed and fixed by the specimen was measured by cutting 10 mm from the top surface in the thickness direction of the specimen, crushing it, and then using STA 2500 (TG-DTA simultaneous measurement device) (manufactured by NETZSCH Japan) to perform simultaneous thermogravimetry and differential thermal analysis. Furthermore, from the measurement results of the carbonation depth, the number of years equivalent to the test specimen being exposed to the atmosphere was calculated using the method described in the Architectural Institute of Japan's Guidelines for Durability Design and Construction of Reinforced Concrete Buildings and Commentary. The results are shown in Table 2. [4] Based on the results of the measurements of the carbonation depth in [3] above, the chipping thickness was determined to be 20 mm, including the carbonized area where CO2 was absorbed and fixed. [5] The specimen was chipped to a thickness of 20 mm from the top surface using an electric hammer (Makita) and a disc grinder (Makita). The chipped thickness was measured using a vernier caliper (Mitutoyo) before and after chipping, and the thickness after chipping was subtracted from the thickness before chipping. [6] Hydraulic composition 1 was poured into the chipped portion of the test specimen to a thickness of 20 mm to form a laminate, which was then cured in air for 28 days. [7] A second accelerated carbonation test was conducted by exposing the laminate to an atmosphere with a CO2 concentration of 5% for 28 days. At this time, only the top surface of the laminate was left open, and the other surfaces were sealed with aluminum tape so that CO2 absorption and fixation occurred only from the top surface. The second accelerated carbonation test was conducted in the same manner as the first accelerated carbonation test. [8] A part of the laminate was cut, and the amount of CO2 absorbed and fixed by the laminate was measured using the cut laminate. The amount of CO2 was measured by cutting 10 mm from the top surface of the laminate in the thickness direction, pulverizing it, and using the same method as above. The results are shown in Table 2.
[0060] <Comparative Example 1> [1] The kneaded hydraulic composition 1 was poured into a formwork (length 400 mm, width 100 mm, height 100 mm) to prepare a test specimen having a length of 400 mm, a width of 100 mm, and a thickness of 100 mm. [2] The first accelerated carbonation test was conducted by exposing the specimen to an atmosphere with a CO2 concentration of 5% for 28 days. At this time, only the top surface of the specimen was left open, and the other surfaces were sealed with aluminum tape so that CO2 was absorbed and fixed only from the top surface. The first accelerated carbonation test was conducted in the same manner as above. [3] After the first accelerated carbonation test, a portion of the test specimen was cut and the cut specimen was used to measure the carbonation depth and the amount of CO2 absorbed and fixed by the test specimen. The carbonation depth was measured in the same manner as above. The amount of CO2 was measured in the same manner as above, using a specimen that was cut 10 mm from the top in the thickness direction and crushed. Furthermore, from the carbonation depth measurement results, the number of years that would be equivalent if the test specimen was exposed to the atmosphere was calculated in the same manner as above. The results are shown in Table 2. [4] The specimens were left to cure in the air for 28 days. [5] The second accelerated carbonation test was conducted by exposing the air-cured specimen to an atmosphere with a CO2 concentration of 5% for 28 days. At this time, only the top surface of the specimen was left open, and the other surfaces were sealed with aluminum tape so that CO2 was absorbed and fixed only from the top surface. The second accelerated carbonation test was conducted in the same manner as above. [6] A part of the test specimen was cut, and the amount of CO2 absorbed and fixed by the test specimen was measured using the cut specimen. The amount of CO2 was measured by cutting 10 mm from the top surface of the test specimen in the thickness direction, crushing it, and using the same method as above. The results are shown in Table 2.
[0061] <Comparative Example 2> The procedure was the same as Comparative Example 1, except that Hydraulic Composition 2 was used instead of Hydraulic Composition 1.
[0062] [Table 2]
[0063] In Table 2, the total amount of CO2 absorption and fixation is the sum of the values after each accelerated carbonation test. In Example 1, the total amount of CO2 absorption and fixation is higher than in Comparative Examples 1 and 2. This shows that a new layer is formed in the chipped portion to absorb and fix CO2, and therefore it is possible to efficiently absorb and fix CO2. Furthermore, in Example 1, it was shown that the specimen after the first accelerated carbonation test has a life of 7.7 years when exposed to atmospheric concentrations. This shows that the chipping thickness of the specimen can be determined depending on the period of exposure of the specimen to the atmosphere.
Claims
1. CO 2 Absorbs and fixes CO 2 An absorption and fixation method comprising the steps of: The method includes the following steps (1) to (4): The hydraulic composition comprises cement and water, The water-cement ratio of the hydraulic composition is 40% or more and 60% or less. 2 Absorption fixation method. (1) CO from existing concrete 2 The process of determining the chipping thickness of existing concrete based on the carbonation depth to which the carbonation is absorbed and fixed. (2) The existing concrete is chipped to the thickness determined in step (1). (3) A step of forming a first absorbing and fixing layer on the part removed in the step (2) using a hydraulic composition. (4) Exposing the first absorbing fixed layer to the atmosphere to cause CO 2 The process of absorbing and fixing
2. The period during which the n-th absorbent fixed layer (n is any natural number, and the n-th absorbent fixed layer is the absorbent fixed layer formed for the nth time) is exposed to the atmosphere is 1 year or more and 15 years or less, The CO method according to claim 1, further comprising the following steps (5) to (7): 2 Absorption fixation method. (5) A process of chipping at least a portion of the existing concrete on which the nth absorbent fixing layer has been formed, the portion including the nth absorbent fixing layer, to a thickness of 1 mm to 15 mm. (6) A step of forming the (n+1)th absorbing and fixing layer on the chipped portion in the step (5) using a hydraulic composition. (7) Exposing the n+1th absorbent fixed layer to the atmosphere to absorb CO 2 The process of absorbing and fixing
3. 3. The CO absorbing fixed layer according to claim 2, wherein the period of exposure of the nth absorbing fixed layer to the atmosphere is 1 year or more and 8 years or less. 2 Absorption fixation method.
4. CO 2 A cross-section repair method using concrete or mortar to absorb and fix The method includes the following steps (1) to (4): The hydraulic composition comprises cement and water, A cross-section repair method, in which the water-cement ratio of the hydraulic composition is 40% or more and 60% or less. (1) CO from existing concrete 2 The process of determining the chipping thickness of existing concrete based on the carbonation depth to which the carbonation is absorbed and fixed. (2) The existing concrete is chipped to the thickness determined in step (1). (3) A step of forming a first absorbing and fixing layer on the part removed in the step (2) using a hydraulic composition. (4) Exposing the first absorbing fixed layer to the atmosphere to cause CO 2 The process of absorbing and fixing
5. The period during which the n-th absorbent fixed layer (n is any natural number, and the n-th absorbent fixed layer is the absorbent fixed layer formed for the nth time) is exposed to the atmosphere is 1 year or more and 15 years or less, The cross section repair method according to claim 4, further comprising the following steps (5) to (7). (5) A process of chipping at least a portion of the existing concrete on which the nth absorbent fixing layer has been formed, the portion including the nth absorbent fixing layer, to a thickness of 1 mm to 15 mm. (6) A step of forming the (n+1)th absorbing and fixing layer on the chipped portion in the step (5) using a hydraulic composition. (7) Exposing the n+1th absorbent fixed layer to the atmosphere to absorb CO 2 The process of absorbing and fixing
Citation Information
Patent Citations
Hollow floor slab member and floor slab repair method
JP2007063888A
Method for suppressing corrosion of reinforcing bar embedded in existing reinforced concrete
JP2013117057A
Absorption method of carbon dioxide
JP2020165276A
Cited By
Fluid automatic discharge device for high temperature and high pressure
KR1020250025900A