Etching method and etching apparatus

A two-stage etching process using fluorine-containing gases addresses the issue of residue and unwanted etching in silicon germanium films, achieving selective etching and reduced Ge residue on silicon films.

JP2024143369AActive Publication Date: 2024-10-11TOKYO ELECTRON LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023056011
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing etching methods for silicon germanium films result in excessive residue and unwanted etching of adjacent films, particularly silicon films, due to the lack of selective etching techniques.

Method used

An etching method involving two stages of fluorine-containing gases, where a first gas is supplied for a prolonged period to etch the silicon germanium film, followed by a second gas for a shorter duration to minimize residue and suppress etching of adjacent films.

Benefits of technology

This method effectively reduces residue and suppresses etching of adjacent films, ensuring high selectivity and minimizing Ge residue on silicon films while maintaining etching efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143369000001_ABST
    Figure 2024143369000001_ABST
Patent Text Reader

Abstract

To reduce residues after etching a silicon germanium film while suppressing etching of a film adjacent to the silicon germanium film when etching the silicon germanium film.SOLUTION: An etching method is a method for etching a silicon germanium film formed on a substrate, includes: a first step of supplying a first etching gas which is a fluorine-containing gas to the substrate for a first period of time; and a second step of supplying, after the first step, a second etching gas which is a fluorine-containing gas different in type from the first etching gas to the substrate for a second period of time shorter than the first period of time.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an etching method and an etching apparatus. [Background technology]

[0002] In manufacturing a semiconductor device, a SiGe film formed on the surface of a semiconductor wafer (hereinafter, referred to as a wafer) serving as a substrate may be etched. Patent Document 1 discloses that a laminated film consisting of a Si film and a SiGe film is formed on a wafer, and that HF ​​gas and ClF3 gas are supplied simultaneously to selectively etch the SiGe film of the laminated film. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-170380 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present disclosure provides a technique that, when etching a silicon germanium film, can reduce post-etching residues while suppressing etching of a film adjacent to the silicon germanium film. [Means for solving the problem]

[0005] The etching method disclosed herein is a method for etching a silicon germanium film formed on a substrate, comprising the steps of: a first step of supplying a first etching gas, which is a fluorine-containing gas, to the substrate for a first time; a second step of supplying a second etching gas, which is a fluorine-containing gas different in type from the first etching gas, to the substrate for a second time period shorter than the first time period after the first step; Includes. Effect of the Invention

[0006] ADVANTAGEOUS EFFECTS OF THE DISCLOSURE In etching a silicon germanium film, the present disclosure can reduce post-etch residues while suppressing etching of films adjacent to the silicon germanium film. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a vertical cross-sectional side view of a wafer undergoing an etching process according to an embodiment of the present disclosure. [Diagram 2] FIG. 4 is a flow chart showing the etching process. [Diagram 3] 5 is a chart showing timings of supply and interruption of gas used in the etching process and change in pressure in the processing vessel. FIG. [Figure 4] FIG. 2 is a vertical cross-sectional side view of the wafer after the etching process. [Diagram 5] FIG. 2 is a vertical sectional side view of an embodiment of an apparatus for performing the etching process. [Figure 6] FIG. 11 is a graph showing the results of an evaluation test. [Figure 7] 1A to 1C are explanatory diagrams showing images of chips on a substrate obtained in an evaluation test and various test results. [Figure 8] FIG. 11 is a graph showing the results of an evaluation test. [Figure 9] FIG. 11 is a graph showing the results of an evaluation test. [Figure 10] 1A to 1C are explanatory diagrams showing images of chips on a substrate obtained in an evaluation test and various test results. [Figure 11] 1A to 1C are explanatory diagrams showing images of chips on a substrate obtained in an evaluation test and various test results. [Figure 12] FIG. 2 is a vertical sectional side view of a substrate used in an evaluation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Before describing an embodiment of the etching method of the present disclosure, a film structure formed on a wafer W, which is a substrate to be etched, will be described. Fig. 1 is a longitudinal sectional front view of the film structure. In the figure, two mutually orthogonal directions in the surface direction of the wafer W are indicated as the X direction and the Y direction, and a thickness direction of the wafer W, which is orthogonal to each of the X direction and the Y direction, is indicated as the Z direction. In the following description, the wafer W is placed horizontally, and the X direction may be described as the left-right direction, the Y direction as the front-rear direction, and the Z direction as the vertical direction.

[0009] A large number of laminates 15 each composed of a Si (silicon) film 12, a SiGe (silicon germanium) film 13, and a porous film 14 are provided on an undercoat film 11 formed on a wafer W. The SiGe film 13 in the laminates 15 is the film to be etched. A plurality of laminates 15 are provided at intervals in the front-rear and left-right directions, and are arranged in a matrix in a plan view. The porous film 14 is, for example, an insulating film, and more specifically, a low-k film composed of, for example, SiOC (carbon-added silicon oxide), SiCOH, SiOCN (a film composed of Si, oxygen, nitrogen, and carbon), or the like.

[0010] The structure of the laminate 15 will be described further. The porous films 14 are formed adjacent to the left and right sides of the SiGe film 13. Therefore, the direction in which the SiGe film 13 and the Si film 12 are arranged and the direction in which the SiGe film 13 and the porous film 14 are arranged cross each other. If the SiGe film 13 and the porous film 14 adjacent to it on the left and right are called adjacent bodies, the laminate 15 is formed by stacking a plurality of adjacent bodies and a plurality of Si films 12, and the adjacent bodies and the Si films 12 are alternately positioned when viewed in the vertical direction (Z direction). The upper end of the laminate 15 is formed by the Si film 12 out of the adjacent bodies and the Si film 12. A semiconductor film 16 is provided between the laminates 15 arranged on the left and right, and the laminate 15 and the semiconductor film 16 are adjacent to each other. The semiconductor film 16 is a film that forms a source or drain in a semiconductor product manufactured from the wafer W, and is formed of, for example, Si or SiGe.

[0011] In addition, an upper layer film 17 is provided on the stacked body 15 and the semiconductor film 16. A plurality of grooves 18 extending in the front-rear direction are formed in the upper layer film 17 at intervals in the left-right direction, dividing the upper layer film 17 into left and right parts, and each groove 18 is provided at a position overlapping the SiGe film 13 in the vertical direction (Z direction). The lower side of the upper layer film 17 extends toward between the stacked bodies 15 arranged in the front-rear direction, forming a recessed portion (not shown). A recessed portion 10 is formed, the side walls of which are the recessed portion and the Si film 12 and the SiGe film 13 in the stacked body 15, and the recessed portion 10 is connected to the groove 18. That is, the recessed portion 10 opens between the upper layer films 17 in the left-right direction (X direction) and extends in the Z direction. Therefore, the Si film 12 and the SiGe film 13 are exposed to the surface of the wafer W as the side walls of the recessed portion 10, and are exposed to the etching gas supplied above the wafer W. The semiconductor film 16 is covered with the upper film 17 and is not exposed on the surface of the wafer W.

[0012] Although detailed description of the structure is omitted, the upper layer 17 is composed of a plurality of types of films, such as a silicon oxide (SiO2) film and an insulating film composed of SiOCN. The upper layer 17 is resistant to an etching gas described later, and prevents the semiconductor film 16 from being etched from above by the etching gas.

[0013] Due to the above-mentioned film structure, the etching gas supplied above the wafer W flows into the recess 10 through the groove 18, and the SiGe film 13 can be etched sideways. More specifically, the gas flowing into the recess 10 flows in the Y direction of the paper surface of FIG. 1, and etches the SiGe film 13 at each stage. The Si film 12 and the SiGe film 13 are adjacent to each other, and it is required to selectively etch the SiGe film 13 and suppress the roughness (surface roughness) of the Si film 12 after etching. Furthermore, it is also required to prevent any residue of Ge (germanium) derived from the SiGe film 13 from remaining on the surface of the Si film 12 after etching.

[0014] In addition, the SiGe film 13 is adjacent to the semiconductor film 16 via the porous film 14, and even during etching of the SiGe film 13, the semiconductor film 16 is covered by the upper film 17 and the porous film 14 and is not exposed on the surface of the wafer W. However, during this etching, the etching gas can pass through the holes in the porous film 14 and be supplied to the semiconductor film 16. There is also a demand for etching the SiGe film 13 so as to suppress the etching of the semiconductor film 16. The etching in this embodiment can meet these demands.

[0015] The etching process of this embodiment will be specifically described below with reference to the flow chart of Fig. 2 and the timing chart of Fig. 3. This etching process is performed by supplying two types of fluorine-containing etching gases to a processing vessel in which a vacuum atmosphere is formed, with the wafer W described in Fig. 1 stored therein. The timing chart shows the timing of supplying and cutting off each etching gas into the processing vessel, and the timing of changing the pressure in the processing vessel.

[0016] First, the wafer W described in FIG. 1 is loaded into the processing vessel. Then, the processing vessel is evacuated to form a vacuum atmosphere of a predetermined first pressure in the processing vessel. Then, for example, F2 (fluorine) gas is supplied into the processing vessel as a first etching gas (time t1, step S1). This selectively etches the SiGe film 13 out of the Si film 12 and the SiGe film 13. When a preset first time has elapsed from time t1 and it becomes time t2, the supply of F2 gas into the processing vessel is stopped, while the supply of ClF3 (chlorine trifluoride) gas, which is a second etching gas, into the processing vessel is started. Furthermore, the exhaust flow rate in the processing vessel is adjusted to reduce the pressure in the processing vessel to a second pressure lower than the first pressure (step S2). The supplied ClF3 gas purges the F2 gas remaining in the processing vessel from the processing vessel, and etches the remaining part of the SiGe film 13.

[0017] When a preset second time has elapsed from time t2 and it becomes time t3, the supply of ClF3 gas into the processing chamber is stopped. This second time (time from time t2 to t3) is shorter than the first time (time from time t1 to t2). Figure 4 shows a longitudinal sectional front view of the wafer W after the etching process is completed. An inert gas is supplied into the processing chamber to purge the ClF3 gas from the processing chamber, completing the etching process, and the wafer W is unloaded from the processing chamber.

[0018] In this way, in the etching process of this embodiment, the type of gas is changed and two-stage etching is performed. The reason for this is that, when etching the SiGe film of a structure in which a Si film and a SiGe film are adjacent to each other, when ClF3 gas is used, the adhesion of Ge residue to the Si film and the roughness of the Si film after etching can be suppressed compared to when F2 gas is used, as shown in the evaluation test described later. However, this ClF3 gas has a high etching property for the Si film, and the Si film is easily etched. In other words, it is difficult to selectively etch the SiGe film.

[0019] Therefore, first, F2 gas is supplied for a relatively long time to the wafer W in Fig. 1. As shown in the evaluation test described later, the Si film 12 is difficult to etch with F2 gas. In other words, the SiGe film 13 can be etched with high selectivity to the Si film 12. Then, after the SiGe film 13 is almost completely removed by the F2 gas, ClF3 gas is supplied for a relatively short time. This makes it possible to suppress etching of the Si film 12 while reducing the roughness of the Si film 12 and reducing Ge residues adhering to the Si film 12.

[0020] Incidentally, as described above, ClF3 gas has a relatively high etching ability for Si films, but as shown in the evaluation test described later, it also has a relatively high etching ability for SiGe films. Therefore, the semiconductor film 16 formed on the wafer W is made of Si or SiGe as described above, but whether it is made of Si or SiGe, it is highly etchable by this ClF3 gas. However, since the supply time of ClF3 gas in this embodiment is relatively short, the supply of the ClF3 gas to the semiconductor film 16 through the holes of the porous film 14 is suppressed. Therefore, the etching of the semiconductor film 16 can also be suppressed.

[0021] Also, due to exhausting the inside of the processing vessel, the second pressure at times t2 to t3 when ClF3 gas is supplied is lower than the first pressure at times t1 to t2 when F2 gas is supplied. The relatively low pressure inside the processing vessel prevents ClF3 gas from remaining in the processing vessel for a long time. Therefore, etching of the Si film 12 and the semiconductor film 16 is more reliably suppressed. On the other hand, the relatively high pressure inside the processing vessel prevents F2 gas from remaining in the processing vessel for a long time and acting on the SiGe film 13. Therefore, a decrease in the etching rate is prevented.

[0022] Next, an etching apparatus 2, which is an example of an etching apparatus capable of performing the etching process described in FIG. 2 and FIG. 3, will be described. FIG. 5 is a vertical cross-sectional side view of the etching apparatus 2. In the figure, reference numeral 21 denotes the processing vessel described above, which constitutes the etching apparatus 2. In the figure, reference numeral 22 denotes a transfer port for the wafer W that opens in the side wall of the processing vessel 21, and is opened and closed by a gate valve 23. A stage 31 on which the wafer W is placed is provided in the processing vessel 21, and the stage 31 is provided with lift pins (not shown). The wafer W is transferred between the stage 31 and a substrate transfer mechanism arranged outside the processing vessel 21 via the lift pins.

[0023] A temperature adjustment unit 22 is embedded in the stage 31, and adjusts the temperature of the wafer W placed on the stage 31. This temperature adjustment unit 22 is configured as a flow path that is part of a circulation path through which a temperature adjustment fluid such as water flows, and adjusts the temperature of the wafer W by heat exchange with the fluid. However, the temperature adjustment unit 22 is not limited to being a flow path for such a fluid, and may be configured, for example, by a heater for performing resistance heating.

[0024] One end of an exhaust pipe 24 opens into the processing vessel 21, and the other end of the exhaust pipe 24 is connected to an exhaust mechanism 26, which is, for example, a vacuum pump, via a valve 25, which is a pressure changing mechanism. By adjusting the aperture of the valve 25, the exhaust flow rate in the processing vessel 21 is adjusted, and the pressure in the processing vessel 21 is set to a desired vacuum pressure. That is, as described above, the first pressure and the second pressure can be switched by changing the aperture of the valve 25.

[0025] A shower plate 32 is provided at the upper side of the processing vessel 21 so as to face the stage 31. The shower plate 32 is connected to the downstream side of gas supply paths 41-44, and the upstream side of the gas supply paths 41-44 is connected to gas supply sources 51-54 via flow rate adjustment units 40. Each flow rate adjustment unit 40 includes a valve and a mass flow controller. The gases supplied from the gas supply sources 51-54 are supplied to the downstream side by opening and closing a valve included in the flow rate adjustment unit 40. The flow rate of each gas supplied to the downstream side is adjusted by each flow rate adjustment unit 40. Each gas supplied to a gas flow path provided in the shower plate 32 is discharged downward from a number of discharge ports provided on the lower surface of the shower plate 32.

[0026] Gas supply sources 51, 52, 53, and 54 supply F2 gas, ClF3 gas, N2 gas, and Ar gas, respectively, and each of these gases is supplied into the processing vessel 21 through the shower plate 32. Each of the flow rate adjustment units 40 allows each of these gases to be supplied independently of each other. During the etching process, N2 gas, which is an inert gas, is supplied into the processing vessel 21 through the shower plate 32 together with the etching gas (F2 gas and ClF3 gas) as a carrier gas. It is also supplied into the processing vessel after the supply of the etching gas is completed, and also acts as a purge gas for purging the processing vessel. In addition, Ar gas, which is an inert gas, is a gas for adjusting the partial pressure of each etching gas, and is supplied into the processing vessel together with the etching gas. A first gas supply section is formed by a gas supply passage 41 through which F2 gas flows, a flow rate adjustment section 40 provided in the gas supply passage 41, and a shower plate 32, and a second gas supply section is formed by a gas supply passage 42 through which ClF3 gas flows, and a flow rate adjustment section 40 provided in the gas supply passage 42, and a shower plate 32.

[0027] The etching apparatus 2 also includes a control unit 20, which is a computer, and the control unit 20 includes a program, a memory, and a CPU. The program includes commands (each step) for performing the above-mentioned processing of the wafer W and transport of the wafer W, and the program is stored in a storage medium, such as a compact disc, a hard disk, a magneto-optical disc, a DVD, etc., and is installed in the control unit 20. The control unit 20 outputs control signals to each part of the etching apparatus 2 according to the program, and controls the operation of each part. Specifically, the operations of the etching apparatus 2 thus controlled include, for example, each operation such as adjustment of the temperature of the fluid supplied to the stage 31 (i.e., the processing temperature of the wafer W), supply and cut-off of each gas from the shower plate 32, and adjustment of the exhaust flow rate by the valve 25 (i.e., adjustment of the pressure inside the processing vessel 21).

[0028] By adjusting the aperture of the valve 25 of the etching device 2, the first pressure from time t1 to t2 is set to, for example, 1.33 Pa (10 mTorr) to 133 Pa (1000 mTorr), and the second pressure from time t2 to t3 is set to, for example, 0 Pa to 133 Pa. The temperature adjustment unit 22 sets the temperature of the wafer W to, for example, -50°C to 150°C from time t1 to t3. The flow rates of the gases supplied into the processing chamber are within the ranges of 1 to 500 sccm for F2 gas, 0.1 to 10 sccm for ClF3 gas, 50 to 1000 sccm for N2 gas, and 10 to 1000 sccm for Ar gas.

[0029] As described above, inert gas (N2 gas and Ar gas) is supplied into the processing vessel together with F2 gas and ClF3 gas. The relationship between the flow rates of F2 gas, ClF3, and inert gas supplied into the processing vessel is, for example, that the flow rate of F2 gas / flow rate of inert gas is greater than the flow rate of ClF3 gas / flow rate of inert gas. In other words, when supplying F2 gas and ClF3 gas to the wafer W, ClF3 gas may be supplied with a higher dilution rate with inert gas than F2 gas. By adjusting the flow rates of each gas in this manner, the etching effect of ClF3 gas on the Si film 12 and the semiconductor film 16 is more reliably suppressed.

[0030] Although F2 gas is used as the first etching gas, other fluorine-containing gases capable of selectively etching the SiGe film 13 with respect to the Si film 12 may be used, for example, a mixed gas of HF gas and F2 gas may be used instead of F2 gas. Also, a fluorine-containing gas having a relatively large etching effect on the SiGe film 13 may be used as the second etching gas instead of the ClF3 gas. For example, IF7 (iodine heptafluoride) gas or NF3 (nitrogen trifluoride) gas may be used as the second etching gas. Incidentally, "containing fluorine" here means that fluorine is included as a constituent, not that fluorine is included as an impurity.

[0031] In the processing example shown in the chart of Fig. 3, ClF3 gas is supplied when the supply of F2 gas is stopped, and F2 gas is purged from the processing vessel 21 by ClF3 gas, but there may be an interval between the time when the supply of F2 gas is stopped and the time when the supply of ClF3 gas is started. During that interval, the F2 gas in the processing vessel may be purged with an inert gas such as N2 gas. However, in order to shorten the processing time, it is preferable to supply ClF3 gas when the supply of F2 gas is stopped, and to purge the F2 gas by ClF3 gas, as shown in Fig. 3.

[0032] Incidentally, the etching technique described in this embodiment suppresses the roughness of the Si film 12 adjacent to the SiGe film 13 as described above, and is therefore particularly effective when applied to a substrate in which the SiGe film 13 and the Si film 12 are adjacent to each other. However, this etching technique can reduce the amount of Ge remaining after etching the SiGe film, and therefore may be used when etching the SiGe film 13 that is not adjacent to the Si film 12.

[0033] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, modified, or combined in various forms without departing from the scope and spirit of the appended claims.

[0034] [Evaluation test 1] Each evaluation test performed in relation to the technology of the present disclosure will be described. In evaluation test 1, a plurality of wafers W with two chips fixed on the surface were prepared. Then, the etching apparatus 2 shown in the embodiment was used to perform processing by changing the type of etching gas and the etching time for each wafer W. One of the two chips has a SiGe film laminated as an upper film on the upper side of a lower film that is a Si film. The thickness of this SiGe film is 50 nm, and the Ge content in the film is 25%. The other chip is a polysilicon film. After etching, the chip on which the SiGe film was formed was subjected to measurement of the amount of Ge by XPS (X-ray photoelectron spectroscopy), measurement of RMS (root mean square roughness) by AFM (atomic force microscope), acquisition of images by SEM (scanning electron microscope), and measurement of the etching amount of the SiGe film. The etching amount was also measured for the chip of the polysilicon film.

[0035] Etching was performed by supplying F2 gas, ClF3 gas, F2 gas, and ClF3 gas to the wafer W as etching gas. The tests using F2 gas, ClF3 gas, F2 gas, and ClF3 gas are referred to as evaluation tests 1-1, 1-2, and 1-3, respectively. In the evaluation test 1-3, the timings of the start and end of the supply of F2 gas and ClF3 gas were aligned and the gases were supplied simultaneously. In each of the evaluation tests 1-1 to 1-3, the supply time (etching time) of the etching gas was changed for each wafer W. In the etching, the temperature of the wafer W, the pressure in the processing vessel 21, and the flow rate of each gas supplied into the processing vessel were set to values ​​within the ranges shown in the embodiment.

[0036] In explaining the test results, the etching time set so that the etching amount of the SiGe film of the above chip becomes 50 nm, which is the same as the thickness of the SiGe film (i.e., the SiGe film is just removed), may be expressed as the time to perform JE (just etching). The time to perform additional etching on the 50 nm SiGe film by extending the etching time from that may be expressed as the time to perform OE (over etching). Specifically, assuming that the thickness of the SiGe film of the chip is 100 nm, 150 nm, 300 nm, or 550 nm, the time to perform 100%, 200%, 500%, or 1000% OE, respectively, is the time to perform the etching amount of the SiGe film to become the same as the thickness of the SiGe film. The time to perform each OE is calculated based on the relationship between the etching amount of the SiGe film of 50 nm or less and the etching time corresponding to this etching amount (see the graph in Figure 6).

[0037] FIG. 7 shows the SEM images, Ge detection amount, RMS, and etching amount of the polysilicon film obtained by the JE and each OE process for each of the evaluation tests 1-1 to 1-3. As described above, the SEM images, Ge detection amount, and RMS were obtained from the chip on which the SiGe film was formed (i.e., the chip on which the surface was formed of Si by removing the SiGe film). Note that the Ge detection amount is actually obtained as a percentage value, and the RMS and etching amount of the polysilicon film are obtained as values ​​in nm units, but the values ​​shown in the table are normalized by dividing the values ​​obtained in this way by a predetermined coefficient. The larger the value in the figure for the Ge detection amount, the larger the amount remaining on the Si film, the larger the value in the figure for the RMS, the larger the roughness, and the larger the value in the figure for the etching amount of the polysilicon film, the larger the etching amount. Note that in FIG. 7, for comparison, the image of the surface of the chip on which the SiGe film was formed before etching and the normalized RMS are also shown in the lower right of the figure.

[0038] FIG. 8 shows a graph showing the relationship between the etching time by ClF3 gas and the etching amount of the SiGe film and the polysilicon film, which was the basis for performing the evaluation test 1-2. FIG. 9 shows a graph showing the relationship between the etching time by F2 gas and ClF3 gas and the etching amount of the SiGe film and the polysilicon film, which was the basis for performing the evaluation test 1-3. As in the evaluation test 1-1, the JE and OE times were determined from the correspondence between the etching amount of the SiGe film and the etching time, and the evaluation tests 1-2 and 1-3 were performed. The vertical axis of each graph shows the etching amount of each film, and the obtained value is divided by a predetermined coefficient to show a standardized value. Note that this predetermined coefficient is the same as the coefficient used to standardize and express the etching amount of the polysilicon film in FIG. 6.

[0039] The results of evaluation test 1-1 using F2 gas will be described. In this evaluation test 1-1 shown in FIG. 7, the specific etching times of JE, OE100%, OE200%, OE500%, and OE1000% are 82 seconds, 145 seconds, 208 seconds, 397 seconds, and 712 seconds, respectively. As shown in FIG. 6, the etching amount of the SiGe film increases as the etching time with F2 gas increases. On the other hand, as shown in FIG. 7, the etching amount of the polysilicon film is generally constant and relatively low for the etching times of JE and each OE. Therefore, as described in the embodiment, it can be seen that when etching the Si film and the SiGe film using F2 gas, the SiGe film can be etched with high selectivity.

[0040] However, the amount of Ge detected is relatively large. As the percentage of OE increases, the amount of Ge detected decreases, but it was confirmed that Ge remains even at 1000% OE. In addition, the RMS value decreases as the percentage of OE increases, but when this percentage is low and in the case of JE, the value is relatively large (i.e., the roughness is relatively large).

[0041] Next, the results of evaluation test 1-2 using ClF3 gas will be described. In this evaluation test 1-2 shown in FIG. 7, the specific etching times for JE, OE100%, and OE200% are 50 seconds, 115 seconds, and 179 seconds, respectively. The amount of Ge detected was relatively low in the case of JE, and no Ge was detected in the cases of OE100% and OE200%. In terms of RMS, the RMS values ​​of JE, OE100%, and OE200% were approximately the same as the RMS values ​​before etching, and were lower than the RMS values ​​of JE, OE100%, and OE200% in evaluation test 1-1. The RMS values ​​of OE100% and OE200% were particularly low.

[0042] However, when ClF3 gas is used, as shown in Fig. 8, as the etching time increases, not only the etching amount of the SiGe film but also the etching amount of the polysilicon film increases. And, the etching amount of each of the polysilicon films of JE, OE100%, and OE200% in Evaluation Test 1-2 was larger than the etching amount of each of the polysilicon films of JE and each OE in Evaluation Test 1-1.

[0043] Next, the results of evaluation test 1-3 using F2 gas + ClF3 gas will be described. In this evaluation test 1-3 shown in Figure 7, the specific etching times for JE, OE100%, and OE200% are 24 seconds, 54 seconds, and 85 seconds, respectively. As for the amount of Ge detected, as in test 1-2, the value was relatively low in the case of JE, and no Ge was detected in the cases of OE100% and OE200%. In addition, the RMS values ​​were particularly low in the cases of OE100% and OE200%, and were approximately the same as the RMS values ​​before etching.

[0044] However, even when F2 gas + ClF3 gas is used, as the etching time increases, not only the etching amount of the SiGe film but also the etching amount of the polysilicon film increases as shown in Figure 9. The etching amount of each polysilicon film with JE, OE100%, and OE200% in Evaluation Test 1-3 was greater than the etching amount of each polysilicon film with JE and each OE in Evaluation Test 1-1.

[0045] As described above, the results of this evaluation test 1 confirmed that the amount of Ge remaining on the Si film after etching (amount of residue) can be reduced and the roughness of the Si film can be suppressed by using ClF3 gas as the etching gas. However, it was also shown that the amount of etching of the Si film becomes relatively large compared to the case of using F2 gas.

[0046] [Evaluation test 2] In evaluation test 2, a wafer W having the same configuration as evaluation test 1 was etched under the same conditions as evaluation test 1-1, where OE was 100%. That is, etching was performed using F2 gas. Following this etching with F2 gas, F2 gas and NH3 gas were supplied into the processing vessel to purge the F2 gas in the processing vessel and etch the wafer. The pressure in the processing vessel was lower during the period when F2 gas was supplied alone (the period when purging was performed) than during the period when F2 gas was supplied alone out of F2 gas and NH3 gas. After such etching, SEM images, Ge detection amounts, and RMS were obtained from the chips on which the SiGe film had been formed, as in evaluation test 1, and the etching amount was obtained from the chips on which the polysilicon film had been formed. The time for supplying F2 gas and NH3 gas (the time for purging) was changed for each wafer W, and tests performed with the time set to 5 seconds, 10 seconds, and 20 seconds were designated evaluation tests 2-1, 2-2, and 2-3, respectively.

[0047] [Evaluation test 3] As evaluation test 3, a test was performed under the same processing conditions as evaluation test 2, except that there was no period in which etching was performed by supplying only F2 gas out of F2 gas and NH3 gas. Therefore, in this evaluation test 3, etching was performed only during a period in which both F2 gas and NH3 gas were simultaneously supplied to the wafer W (the period corresponding to the purge in evaluation test 2). The supply times of F2 gas and NH3 gas were set to 5 seconds, 10 seconds, and 20 seconds, respectively, as in evaluation test 2, and the tests performed with these time settings were designated evaluation tests 3-1, 3-2, and 3-3, respectively. In this evaluation test 3, the etching amounts of the SiGe film and the polysilicon film were measured.

[0048] The results of evaluation tests 2 and 3 are shown in FIG. 10. The values ​​in the table are normalized in the same manner as in evaluation test 1. Looking at the results of evaluation test 2, the Ge detection amount and RMS were relatively large in each of evaluation tests 2-1 to 2-3. In addition, the longer the supply time of F2 gas and NH3 gas, the larger the etching amount of the polysilicon film became among evaluation tests 2-1 to 2-3. Looking at the results of evaluation test 3, there was no significant difference in the etching amount of the SiGe film among evaluation tests 3-1 to 3-3, but the etching amount of the polysilicon film became larger as the etching time became longer. Therefore, it can be seen from the results of evaluation tests 2 and 3 that the polysilicon film is etched relatively greatly by the action of F2 gas and NH3 gas.

[0049] [Evaluation test 4] As Evaluation Test 4, processing was performed under the same conditions as Evaluation Test 2, except that instead of purging with F2 gas and NH3 gas in Evaluation Test 2, ClF3 gas was supplied for purging, and the length of the purging period was different from the range of 5 to 20 seconds set in Evaluation Test 2. Therefore, in Evaluation Test 4, ClF3 gas was supplied after F2 gas was supplied, as in the embodiment. As for the pressure in the processing vessel, the pressure during the period during which ClF3 gas was supplied was lower than the pressure during the period during which F2 gas was supplied, as in the embodiment. The time period during which ClF3 gas was supplied was set to 5 seconds, 20 seconds, and 60 seconds, respectively, and the tests performed with these time settings are referred to as Evaluation Tests 4-1, 4-2, and 4-3, respectively.

[0050] [Evaluation test 5] Evaluation test 5 was performed under the same processing conditions as evaluation test 4, except that there was no period during which F2 gas was supplied to perform etching. Therefore, in evaluation test 5, etching was performed using only ClF3 gas. The time for supplying ClF3 gas was set to 5 seconds, 20 seconds, and 60 seconds, respectively, as in evaluation test 4, and the tests performed with these time settings are evaluation tests 5-1, 5-2, and 5-3, respectively. In evaluation test 5, as in evaluation test 3, the etching amounts of the SiGe film and the polysilicon film were measured.

[0051] The results of evaluation tests 4 and 5 are shown in FIG. 11. Each value in the table is normalized in the same manner as in evaluation test 1. Looking at the results of evaluation test 4, the amount of Ge detected was kept low in each of evaluation tests 4-1 to 4-3, and was lower than the amount of Ge detected in any of evaluation tests 2-1 to 2-3. In addition, the RMS was also kept low in each of evaluation tests 4-1 to 4-3, and was lower than the RMS in any of evaluation tests 2-1 to 2-3. In addition, the amount of etching of the polysilicon film was relatively low in each of evaluation tests 4-1 to 4-3, and was approximately the same as the values ​​in each of evaluation tests 2-1 to 2-3.

[0052] 1 by the method shown in the embodiment described above, it is possible to suppress the SiGe film 13 from being selectively etched to prevent Ge residue from remaining. It is also possible to suppress the roughness of the Si film 12 after etching.

[0053] The results of evaluation test 5 show that the etching amount of the SiGe film and the polysilicon film increases as the supply time of ClF3 gas increases, as in evaluation test 1. The etching amount of the polysilicon film is relatively large in evaluation test 5-2, but is relatively small in evaluation test 5-1. From these results, it is considered that the time (second time) from time t2 to time t3 during which ClF3 gas is supplied as shown in FIG. 3 is preferably shorter than 20 seconds, and more preferably 5 seconds or less.

[0054] [Evaluation test 6] As an evaluation test 6-1, a substrate having a film structure shown in FIG. 12 was prepared. This film structure includes a stack 62 in which a Si film 12 and a SiGe film 13 are alternately stacked upward, and a SiN (silicon nitride) film 61 is formed on the uppermost Si film 12. A porous film 63, which is a low-k film, is formed so as to cover the stack 62 from the sides to the top, and the porous film 63 is exposed on the surface of the substrate. That is, when the etching gas is supplied, the porous film 63 is exposed to the etching gas. After the etching gas is supplied to the substrate on which each film is formed in this way as described in FIG. 2 and FIG. 3 of the embodiment, the state of the SiGe film 13 was observed. In addition, as an evaluation test 6-2, a substrate having a film structure similar to that of the substrate except that the porous film 63 is not formed was supplied with the etching gas as described in FIG. 2 and FIG. 3, and the state of the SiGe film 13 was observed.

[0055] In evaluation test 6-2, the SiGe film 13 was etched from the side, but in evaluation test 6-1, no etching from the side of the SiGe film 13 was observed. From these test results, it is expected that etching of the semiconductor film 16 adjacent to the porous film 14 will be suppressed when etching is performed on the wafer W having the film structure of Figures 1 and 2 as described with reference to Figures 2 and 3. [Explanation of symbols]

[0056] W wafer 13. SiGe film

Claims

1. 1. A method for etching a silicon germanium film formed on a substrate, comprising: a first step of supplying a first etching gas, which is a fluorine-containing gas, to the substrate for a first time; a second step of supplying a second etching gas, which is a fluorine-containing gas different in type from the first etching gas, to the substrate for a second time period that is shorter than the first time period after the first step; An etching method comprising:

2. the first step is a step of selectively etching the silicon germanium film out of the silicon germanium film and the silicon film exposed on the surface of the substrate, 2. The etching method according to claim 1, wherein the second step is a step of etching the remaining portion of the silicon germanium film.

3. 3. The etching method according to claim 2, wherein the second etching gas is chlorine trifluoride gas.

4. The substrate includes: a silicon-containing film; a porous film interposed between the silicon-containing film and the silicon germanium film; 4. The method of claim 3, further comprising:

5. the first step and the second step are steps of supplying the first etching gas and the second etching gas to the substrate stored in a processing vessel, respectively; 2. The etching method according to claim 1, further comprising the step of setting a pressure in the processing vessel in the second step lower than a pressure in the processing vessel in the first step.

6. An apparatus for etching a silicon germanium film formed on a substrate, comprising: a processing vessel for storing the substrate; A first etching gas, which is a fluorine-containing gas, is supplied into the processing vessel for a first period of time. A gas supply unit; a second gas supply unit that supplies, after the supply of the first etching gas, a second etching gas, which is a fluorine-containing gas different in type from the first etching gas, into the processing chamber for a second time that is shorter than the first time; An etching apparatus comprising:

Citation Information

Patent Citations

  • Substrate processing method and storage medium

    JP2018170380A

  • Etching method

    JP2019129313A

  • Silicon-containing film etching method, computer storage medium, and silicon-containing film etching apparatus

    JP2019201102A

  • Etching method, etching apparatus, and storage medium

    JP2020053448A

  • Etching method and etching apparatus

    JP2022191045A