Inorganic red pigment and use of the same
A lithium manganese composite oxide-based inorganic red pigment with controlled particle sizes and a safe manufacturing process addresses the issues of unsafe and unsuitable pigments, achieving vivid red colors in paints and ceramic coatings.
Patent Information
- Application Number
- JP2023056073
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing inorganic red pigments either have large particle sizes leading to rough surfaces and poor color development or contain harmful substances like cadmium and chromic acid, making them unsafe and unsuitable for applications requiring vivid red colors.
Development of a lithium manganese composite oxide-based inorganic red pigment with controlled particle sizes (1 μm to 5 μm) and a specific particle diameter ratio (D50/DSEM of 1 to 4), ensuring it does not contain harmful substances, and a manufacturing process that includes mixing Li and Mn sources with a molar ratio exceeding 2 and a cleaning step to remove excess Li.
The resulting pigment achieves a vivid red color with improved surface smoothness and safety, suitable for use in paints and ceramic coatings without harmful components.
Smart Images

Figure 2024143412000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an inorganic red pigment, a red paint containing the inorganic red pigment, a ceramic product having a coating film containing the inorganic red pigment, and a method for producing the inorganic red pigment. [Background technology]
[0002] Inorganic pigments are more heat-resistant and weather-resistant than organic pigments, and are therefore widely used to color products that may be exposed to high temperatures or that are installed outdoors. Inorganic pigments such as cadmium red and chrome vermilion are widely used as red coloring pigments. However, these inorganic pigments contain cadmium, chromate, lead, and other harmful substances that adversely affect the human body and the environment. In recent years, safer inorganic red pigments have been studied. For example, Patent Documents 1-2 and Non-Patent Documents 1-5 each study pigments that use various inorganic compounds to produce red color. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 2923558 [Patent Document 2] Patent No. 6410806 [Non-patent literature]
[0004] [Non-Patent Document 1] Dyes and Pigments, 136, January 2017, 219-223 [Non-Patent Document 2] RSC Adv., 5, 2015, 44886-44894 [Non-Patent Document 3] Applied Surface Science, 387,2016, 1147-1153 [Non-Patent Document 4] ACS Omega 2020, 5, 13108-13114 [Non-Patent Document 5] Z. Anorg. Allg. Chem. 2020, 1722-1729 Summary of the Invention [Problem to be solved by the invention]
[0005] The pigments disclosed in Non-Patent Documents 1 and 2 are pigments that exhibit a brighter red color than red iron oxide, but their particle size is large, and when used as a paint, the surface becomes rough and the desired color cannot be obtained. On the other hand, the pigments disclosed in Patent Documents 1 and 2 have a relatively small particle size and are suitable for use as a paint, but the color value is closer to orange.
[0006] In addition, the pigment disclosed in Non-Patent Document 3 has a bright red color and a relatively small particle size, making it suitable for use as a paint, but it is described that cerium sulfide is used. For this reason, harmful gases such as hydrogen sulfide and carbon sulfide must be used when producing the pigment, which is undesirable from the viewpoint of safety. Here, as described in Non-Patent Documents 4 and 5, oxides containing at least lithium and manganese as constituent elements (e.g., Li2MnO3) are highly safe inorganic red pigments that can be produced without using highly harmful raw materials. The pigment disclosed in Non-Patent Document 4 has a low color value (especially the a* value) and is close to a dull red or orange. In addition, the pigment disclosed in Non-Patent Document 5 has a relatively good color value, but has a large particle size, making it unsuitable for use as a paint.
[0007] The present invention has been made in view of the above circumstances, and has an object to provide an inorganic red pigment that is highly safe and has a vivid red color. Another object of the present invention is to provide a paint containing such an inorganic red pigment, a ceramic product having a coating film containing such an inorganic red pigment, and a method for producing such an inorganic red pigment. [Means for solving the problem]
[0008] In order to achieve the above object, an inorganic red pigment is disclosed herein. The inorganic red pigment disclosed herein contains a lithium manganese composite oxide and has an average particle diameter (D 50 ) is 1 μm or more and 5 μm or less, and the above D 50 and the average particle size (D SEM ) and D 50 / D SEM is between 1 and 4 inclusive.
[0009] By adjusting the particle size of the inorganic red pigment to fall within a specified range, it is possible to suppress orange and yellow coloring and realize a vivid red color. In addition, since the particle size of the inorganic red pigment is adjusted to be smaller than that of the conventional inorganic red pigment, the surface roughness is suppressed when the inorganic red pigment is made into a coating film, and a more vivid coloring is realized. Furthermore, the inorganic red pigment does not contain any harmful components that have adverse effects on the human body and the environment, making it a safer inorganic red pigment.
[0010] In a preferred embodiment of the inorganic red pigment disclosed herein, D in the volume-based particle size distribution based on a laser diffraction scattering method 90 The particle size is 30 μm or less. According to this configuration, particles with large diameters are suppressed, and better color development is achieved.
[0011] In a preferred embodiment of the inorganic red pigment disclosed herein, the a* value in the L*a*b* color system measured by the SCE method is 32 or more, and the h value in the L*C*h color system measured by the SCE method is 20 or more and 40 or less. According to this configuration, it is possible to provide an inorganic red pigment that realizes a more vivid red color.
[0012] In a preferred embodiment of the inorganic red pigment disclosed herein, the content of the lithium manganese composite oxide is 80 wt % or more when the total weight of the inorganic red pigment is taken as 100 wt %. According to this configuration, it is possible to provide an inorganic red pigment that is highly safe and exhibits a vivid red color.
[0013] In one preferred embodiment of the inorganic red pigment disclosed herein, the pigment further contains an aluminum component, and the aluminum content is 10 wt % or less when the total weight of the inorganic red pigment is taken as 100 wt %. With this configuration, a more vivid red color can be achieved.
[0014] In accordance with another aspect of the present invention, there is provided a red paint comprising the inorganic red pigment described above. According to this configuration, it is possible to realize a red paint that is highly safe and has a more vivid red color.
[0015] In accordance with another aspect of the present invention, there is provided a ceramic product comprising the above-described inorganic red pigment. According to this configuration, a ceramic product can be obtained that has a coating film with less surface roughness and a more vivid red color.
[0016] Also, from another aspect, there is provided a method for producing the inorganic red pigment disclosed herein. The method disclosed herein includes the steps of mixing a Li source and a Mn source such that the molar ratio of the Li amount to the Mn amount (Li / Mn) exceeds 2, calcining the mixture of the Li source and the Mn source, and washing the calcined product after the calcination step. In the washing step, washing is carried out so as to remove excess Li components.
[0017] According to this configuration, by making the amount of Li excessive relative to the amount of Mn, it is possible to suitably suppress grain growth during firing. This allows the particle size of the inorganic red pigment to be adjusted within a predetermined range, and an inorganic red pigment exhibiting a vivid red color can be suitably produced. In addition, this manufacturing method does not use any harmful substances that have adverse effects on the human body and the environment, making it a safer manufacturing method.
[0018] In a preferred embodiment of the production method disclosed herein, an Al source is further added in the mixing step, and the Li source and the Al source are mixed together so that the molar ratio of the Li amount to the Al amount (Li / Al) is 4 or more. According to this configuration, the grain growth can be more suitably suppressed, and an inorganic red pigment that realizes a vivid red color can be more suitably produced. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is an FE-SEM image (10,000x) of the pigment of Example 1. [Diagram 2] FIG. 2 is an FE-SEM image (10,000x) of the pigment of Comparative Example 2. [Diagram 3] FIG. 3 is an FE-SEM image (10,000x) of the pigment of Comparative Example 3. [Figure 4] FIG. 4 is an FE-SEM image (1000x) of the pigment of Example 1. [Diagram 5] FIG. 5 is an FE-SEM image (1000x) of the pigment of Comparative Example 2. [Figure 6] FIG. 6 is an FE-SEM image (1000x) of the pigment of Comparative Example 3. [Figure 7] FIG. 7 is an XRD chart of the pigment of Example 1. [Figure 8] FIG. 8 is an XRD chart of the pigment of Comparative Example 3. [Figure 9] FIG. 9 is an FE-SEM image (10,000x) of the pigment of Example 16. [Figure 10] FIG. 10 is a FE-SEM image (1000x) of the pigment of Example 16. [Figure 11] FIG. 11 is an XRD chart of the pigment of Example 11. [Figure 12] FIG. 12 is an XRD chart of the pigment of Example 16. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Preferred embodiments of the present invention will be described below. Matters other than those specifically mentioned in this specification that are necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field. In this specification, the expression "A to B" indicating a numerical range means "A or more and B or less" unless otherwise specified.
[0021] <Inorganic red pigment> The inorganic red pigment disclosed herein contains a lithium manganese composite oxide. The inorganic red pigment has an average particle diameter in a volume-based particle size distribution based on a laser diffraction scattering method (hereinafter, simply referred to as "D 50 ") is 1μm or more and 5μm or less, and D 50 and the average particle size based on field emission scanning electron microscope (FE-SEM) images (hereinafter simply referred to as "D SEM " is also called.) 50 / D SEM is between 1 and 4 inclusive.
[0022] The inorganic red pigment may contain, for example, a metal compound. Examples of metal compounds that the inorganic red pigment may contain include metal compounds containing at least one or more metal elements selected from the group consisting of Li, Mn, Al, Si, Na, K, Mg, and Ca. The inorganic red pigment disclosed herein contains at least a lithium manganese composite oxide (typically Li2MnO3). The inorganic red pigment may contain not only primary particles of lithium manganese composite oxide, but also secondary particles formed by aggregation of the primary particles. Such lithium manganese composite oxide can be produced without using any component that adversely affects the human body or the environment, such as cadmium or lead. Therefore, an inorganic red pigment containing lithium manganese composite oxide can realize a safer inorganic red pigment. In this specification, the phrase "the inorganic red pigment contains a lithium manganese composite oxide" refers to the inclusion of a compound whose crystal structure is identified as Li2MnO3 when a fitting analysis is performed between an XRD pattern of the inorganic red pigment obtained by XRD (X-ray Diffraction) and a Li2MnO3 pattern in a database.
[0023] The inorganic red pigment contains lithium manganese composite oxide as a main component. Specifically, when the total weight of the inorganic red pigment is 100 wt%, the content of lithium manganese composite oxide (Li2MnO3) is preferably 80 wt% or more, more preferably 90 wt% or more, may be 95 wt% or more, or may be 99 wt% or more. The content of Li2MnO3 in the inorganic red pigment may be 100 wt%, but may be 99.5 wt% or less from the viewpoint of production efficiency, for example. In this specification, the "content of Li2MnO3 in the inorganic red pigment" can be obtained as follows. First, a quantitative analysis of the Mn content of the inorganic red pigment is performed using inductively coupled plasma (ICP) emission spectroscopy. Then, using the determined Mn content (wt%), the molar mass of Li2MnO3 (116.82 g / mol), and the molar mass of Mn (54.94 g / mol), it can be calculated from the formula: Li2MnO3 content (wt%) = (Mn content × 116.82) / 54.94.
[0024] As described above, the inorganic red pigment disclosed herein is preferably substantially free of harmful components that may have adverse effects on the human body or the environment, such as arsenic, lead, and cadmium components. In this specification, "substantially free" refers to the fact that the above-mentioned harmful components are not intentionally added. Therefore, when a component that may be interpreted as a harmful component is contained in a small amount due to raw materials or a manufacturing process, etc., it is included in the concept of "substantially free" in this specification. For example, when the content of harmful components in the inorganic red pigment is 0.01 wt% or less (preferably 0.005 wt% or less, more preferably 0.001 wt% or less, even more preferably 0.0005 wt% or less, and particularly preferably 0.0001 wt% or less), it can be said to be "substantially free."
[0025] Although not particularly limited, the inorganic red pigment preferably contains an aluminum component in addition to the lithium manganese composite oxide. This makes it possible to provide an inorganic red pigment that exhibits a more vivid red color. The aluminum component in the inorganic red pigment may be contained, for example, as lithium aluminate. It is more preferable that such lithium aluminate is present on the surface of the lithium manganese composite oxide. The presence of the aluminum component can be confirmed by using FE-SEM images and SEM-EDX images of the inorganic red pigment.
[0026] The aluminum component (more preferably lithium aluminate) may be attached to the entire surface of the lithium manganese composite oxide, or may be attached partially to the surface of the lithium manganese composite oxide. Preferably, the aluminum component is attached partially to the surface of the lithium manganese composite oxide. For example, as shown in FIG. 9, the aluminum component is present in the form of particles (i.e., scattered) on the surface of the lithium manganese composite oxide.
[0027] When the inorganic red pigment contains an aluminum component, the aluminum content is preferably 10 wt% or less, may be 5 wt% or less, or may be 1 wt% or less, when the total weight of the inorganic red pigment is 100 wt%. The lower limit of the aluminum content is not particularly limited, but is preferably 0.1 wt% or more, and more preferably 0.25 wt% or more, when the total weight of the inorganic red pigment is 100 wt%. The "aluminum content (wt%) in the inorganic red pigment" can be determined by quantitatively analyzing the Al element of the inorganic red pigment using inductively coupled plasma optical emission spectroscopy.
[0028] It is generally known that the particle size of a pigment affects the color development. In the case of a red pigment, the color development changes from red to orange to yellow as the particle size becomes smaller. In addition, in a coating film containing a pigment, if the particle size of the pigment is large, the surface becomes rough, and the amount of diffuse reflected light from the surface changes, and the desired color development may not be obtained. In other words, by adjusting the particle size of the inorganic red pigment to within a specified range, an inorganic red pigment that shows a vivid red color can be realized.
[0029] The inorganic red pigment disclosed herein has an average particle diameter (D 50 As described above, the inorganic red pigment may contain not only primary particles of the lithium manganese composite oxide, but also secondary particles formed by aggregation of the primary particles. The average particle diameter (D 50 ) is closest to the average particle size of the secondary particles of lithium manganese composite oxide. 50 By controlling the value of D to a predetermined value or less, the roughness of the coating surface is improved and good color development can be achieved. 50 By controlling the value of to a predetermined value or more, it is possible to provide an inorganic red pigment that exhibits a vivid red color without developing a yellow or orange color.
[0030] Inorganic red pigment D 50 is 1 μm or more, preferably 2 μm or more, and may be 3 μm or more. 50 is 5 μm or less, preferably 4.9 μm or less, and may be 4.5 μm or less. 50 The "D of inorganic red pigment" can be measured by a wet method using a general laser diffraction particle size distribution measuring device (e.g., Mastersizer 3000 manufactured by Spectris Co., Ltd.). 50 " refers to the particle size that corresponds to the cumulative 50% particle size from the smallest particle size in the volume-based particle size distribution based on such measurements.
[0031] The inorganic red pigment disclosed herein has an average particle diameter (D SEM ) based on the volume-based particle size distribution based on the laser diffraction scattering method (D 50 ) ratio (D 50 / D SEM ) is 1 or more and 4 or less. Here, the average particle diameter (D SEM ) is closest to the average particle size of the primary particles of lithium manganese composite oxide. That is, D 50 / D SEM D indicates how large the secondary particle size is compared to the primary particle size. For example, when the secondary particle size becomes coarser than the primary particle size, D 50 / D SEM Therefore, the value of D 50 / D SEM By controlling the value of D to be 1 or more and 4 or less, the lithium manganese composite oxide does not become excessively coarse, and an inorganic red pigment having good color development properties can be provided. SEM " can be measured using a general field emission scanning electron microscope (e.g., Hitachi High-Technologies Corporation, SU-8230, etc.) and image processing software (ImageJ, etc.). SEM " is the particle diameter calculated by measuring the horizontal Feret diameter of multiple particles (at least 50 or more, for example 100 particles) and averaging the results.
[0032] As described above, if the particle size of a red pigment is too small, it will exhibit a yellow or orange color. From this perspective, the average particle size (D SEM ) is, for example, preferably 0.5 μm or more, more preferably 0.8 μm or more, and may be 1 μm or more. On the other hand, D SEM If becomes too large, the D of inorganic red pigment 50From this point of view, the inorganic red pigment D SEM It is preferable that the thickness is 3 μm or less, and more preferable that the thickness is 2.5 μm or less.
[0033] Although not particularly limited, the inorganic red pigment has a particle size distribution based on volume based on a laser diffraction scattering method of D 90 The particle size is preferably 30 μm or less, more preferably 20 μm or less, may be 15 μm or less, or may be 10 μm or less. 90 By having a particle size of the specified value or less, there are few coarse particles, so that even when the coating film is formed, the surface is less rough and the color development is good. 90 The lower limit of the particle diameter is not particularly limited, but may be, for example, 5.5 μm or more, or 6 μm or more. 90 The "particle size" refers to the particle size that corresponds to the cumulative 90% particle size from the smallest particle size in the volume-based particle size distribution based on the measurement of the inorganic red pigment by a wet method using the general laser diffraction particle size distribution measuring device described above.
[0034] Although not particularly limited, the inorganic red pigment has a particle size distribution based on volume based on a laser diffraction scattering method of D 10 The particle size is preferably 0.8 μm or more, and more preferably 1 μm or more. 10 By making the particle size equal to or larger than a predetermined value, the coloring of yellow or orange can be suppressed. 10 The upper limit of the particle size is not particularly limited, but is preferably 3 μm or less, more preferably 2.5 μm or less, and may be 2 μm or less. 10 The "particle size" refers to the particle size that corresponds to the cumulative 10% particle size from the smallest particle size in the volume-based particle size distribution based on the measurement of the inorganic red pigment by a wet method using the general laser diffraction particle size distribution measuring device described above.
[0035] The inorganic red pigment disclosed herein has an a* value of 32 or more in the L*a*b* color system when measured by the SCE method, and an h value of 20 to 40 in the L*C*h color system when measured by the SCE method. This configuration realizes an inorganic red pigment that exhibits a more vivid red color. Here, the SCE (Specular Components Exclude) method is a method in which regular reflected light is removed and only diffuse reflected light is measured. The SCE method can obtain measurement results that are close to those obtained when the color is recognized visually. In this specification, the "a* value, b* value, and L* value of the inorganic red pigment" and the "C* value and h value of the inorganic red pigment" can be measured using a commercially available spectrophotometer (for example, CM-5 manufactured by Konica Minolta Sensing Co., Ltd.).
[0036] In the L*a*b* color system based on JIS Z8729 (2004), the L* value indicates lightness, and the a* and b* values indicate hue and saturation. a* indicates the red direction, -a* indicates the green direction, b* indicates the yellow direction, and -b* indicates the blue direction. The larger the value (farther away from the center of the chromaticity diagram), the more vivid the color, and the smaller the value (closer to the center of the chromaticity diagram), the more dull the color. In other words, the higher the a* value, the more vivid the red color. When the a* value is less than 32, it is the so-called "red ocher," a red color with a slight brownish tinge. From this perspective, the a* value of the inorganic red pigment measured by the SCE method is preferably 32 or more, more preferably 33 or more, and may be 34 or more. There is no particular limit to the upper limit of the a* value, but it may be, for example, 50 or less, or 45 or less. The b* value of the inorganic red pigment is not particularly limited, but is preferably, for example, 20 to 40, and more preferably 20 to 36. The L* value of the inorganic red pigment is not particularly limited, but is preferably, for example, 40 to 55, and more preferably 40 to 51.
[0037] In the L*C*h color system, the L* value indicates lightness, the C* value indicates saturation, and the h value indicates the hue angle. The higher the C* value, the more outside the circle of the chromaticity diagram, and the more vivid the color. The h value is the angle shifted from the a*red axis at 0° to the hue in the counterclockwise direction, for example, 90° indicates the yellow direction, and 180° indicates the green direction. That is, by the h value being within a predetermined range, yellowish and purple hues are sufficiently suppressed, and a more vivid red color is displayed without developing orange or yellow. From this viewpoint, the h value of the inorganic red pigment measured by the SCE method is preferably 20 to 40, more preferably 30 to 38. The C* value of the inorganic red pigment is not particularly limited, but is preferably 35 to 56, more preferably 40 to 56, for example.
[0038] <Red paint> The red paint disclosed herein contains at least the inorganic red pigment described above. The red paint is applied, for example, to the surface of a ceramic object to be decorated, to form a coating film containing the inorganic red pigment on the surface of the ceramic. The red paint is, for example, a paste containing the inorganic red pigment described above and a solvent. In this specification, "paste" refers to a mixture in which a part or all of the solid content is dispersed in a solvent, and includes so-called "slurry", "ink", etc.
[0039] The red paint preferably contains a solvent for dispersing the inorganic red pigment. The solvent may be any of various solvents that are usually used in this type of paint. The solvent may be either aqueous or organic. As the aqueous solvent, water or a mixed solution mainly containing water (for example, a mixed solution of water and ethanol) may be used. As the organic solvent, terpineol, ether solvents, ester solvents, ketone solvents, alcohol solvents, etc. may be used.
[0040] The red paint may contain a resin as a binder. The resin may be any of various resins that are usually used in this type of paint. Examples of such resins include acrylic resin, silicone resin, acrylic silicone resin, styrene-acrylic copolymer resin, polyester resin, fluororesin, rosin resin, phenolic resin, urethane resin, melamine resin, epoxy resin, and cellulose resin.
[0041] The ratio of the inorganic red pigment in the red paint is not particularly limited, but is preferably 10 wt% to 40 wt%, and more preferably 15 wt% to 30 wt%, when the entire red paint is 100 wt%. Also, the ratio of the binder in the red paint is not particularly limited, but is preferably 20 wt% to 50 wt%, and more preferably 30 wt% to 40 wt%, when the entire red paint is 100 wt%.
[0042] The red paint disclosed herein may additionally contain other components as appropriate, for example, in a range of approximately less than 10 wt% when the entire red paint is taken as 100 wt%, so long as the effects of the present invention are not significantly impaired. Examples of additional components include reaction accelerators, surfactants, dispersants, thickeners, pH adjusters, preservatives, defoamers, plasticizers, stabilizers, antioxidants, etc.
[0043] <Ceramics products> The ceramic product disclosed herein is provided with a coating film containing the above-mentioned inorganic red pigment. As described above, the inorganic red pigment disclosed herein has a particle size (e.g., D 50 Or D SEM ) is adjusted, the surface roughness is reduced, and a coating film with improved color development can be provided. As a result, the coating film of this embodiment achieves a unique, vivid red color development. Note that the "ceramic products" referred to here include pottery, porcelain, earthenware, stoneware, glass, and the like. Specific products include, for example, tableware, decorative utensils, various tiles, sanitary ware, roofing tiles, bricks, clay pipes, ceramic pipes, and the like.
[0044] Specifically, the ceramic product has a coating film containing the inorganic red pigment on a substrate mainly composed of ceramics. The substrate is a molded body mainly composed of ceramics (for example, a molded body with a ceramic content of 50 mass% or more). Examples of ceramics constituting the substrate include silica (SiO2), alumina (Al2O3), zirconia (ZrO2), magnesia (MgO), titania (TiO2), ceria (CeO2), and yttria (Y2O3). The thickness, shape, hardness, color, and the like of the substrate can be appropriately changed depending on the application of the ceramic product, and the technology disclosed herein is not limited thereto, so detailed explanations are omitted. Note that the chemical formulas shown in parentheses after the above substance names indicate the representative compositions of the substances, and are not intended to limit the compositions of actual ceramics to those of the chemical formulas.
[0045] <Method of manufacturing inorganic red pigment> The above-mentioned inorganic red pigment contains a lithium manganese composite oxide, 50 is 1 μm or more and 5 μm or less, and D SEM D 50 Ratio of (D 50 / D SEM ) is 1 or more and 4 or less, it is possible to realize a more vivid red color without containing any components harmful to the human body or the environment. An inorganic red pigment exhibiting such characteristics can be suitably produced, for example, by the production method disclosed herein. A preferred embodiment of such a production method will be described below.
[0046] The manufacturing method disclosed herein may include at least a step (mixing step) of mixing a Li source and a Mn source so that the molar ratio of the Li amount to the Mn amount (Li / Mn) exceeds 2, a step (firing step) of firing the mixture of the Li source and the Mn source, and a step (cleaning step) of washing the mixture after the firing step. In the above-mentioned washing step, washing is performed to remove excess Li components. Note that the manufacturing method disclosed herein may further include other steps at any stage.
[0047] In the mixing step, a lithium source (Li source) and a manganese source (Mn source) are mixed so that the molar ratio of the Li amount to the Mn amount (Li / Mn) exceeds 2. The Li source is not particularly limited as long as it contains Li, and may be Li or a compound containing Li. Examples of the Li source include lithium carbonate, lithium hydroxide, lithium nitrate, and lithium acetate. The Mn source is not particularly limited as long as it contains Mn, and may be Mn or a compound containing Mn. Examples of the Mn source include manganese dioxide, manganese carbonate, and manganese sulfate. The mixing method is not particularly limited, and may be performed using, for example, a mortar or a powder mixer.
[0048] Even if the amount of Li is excessively added relative to the amount of Mn during mixing, lithium manganese composite oxide (Li2MnO3) rarely exceeds the stoichiometric ratio (Li / Mn=2) in the product. By adding a Li source so that the amount of Li is excessive relative to the amount of Mn during mixing of the raw materials, it is possible to suitably suppress grain growth during firing. This reduces the particle size (especially D 50 It is possible to realize an inorganic red pigment that exhibits a vivid red color without the increase in particle size (particle size). Moreover, such an inorganic red pigment can be produced without using substances that are harmful to the environment and the human body, such as cadmium and lead. In other words, according to the production method disclosed herein, it is possible to provide an inorganic red pigment that does not contain harmful substances and exhibits a vivid red color.
[0049] In the mixing step, the molar ratio of Li to Mn (Li / Mn) may be greater than the stoichiometric ratio of lithium manganese composite oxide (Li2MnO3). Li / Mn may be greater than 2, and may be, for example, 2.1 or more, 3 or more, 4 or more, or 5 or more. It is presumed that a large Li / Mn value can suppress grain growth during firing, thereby suppressing the grain size of the lithium manganese composite oxide from becoming coarse, but the amount of Li consumed increases. From the viewpoint of cost, Li / Mn is preferably 7 or less, and may be 6 or less.
[0050] Although not particularly limited, it is preferable to further add an aluminum source (Al source) in the mixing step. The Al source is not particularly limited as long as it contains Al, and may be Al or a compound containing Al. For example, the Al source is preferably a compound containing Al as a constituent element and not containing Li. Examples of the Al source include aluminum hydroxide, alumina (Al2O3), and aluminum nitrate. By further adding an Al source in the mixing step, the grain growth of the lithium manganese composite oxide can be more suitably suppressed.
[0051] When an Al source is further included in the mixing step, if the molar ratio of Li to Al (Li / Al) falls below 4 and the Al amount becomes excessive relative to Li, the effect of suppressing grain growth of the lithium manganese composite oxide is not exhibited, which is undesirable. From this viewpoint, the molar ratio of Li to Al (Li / Al) is preferably 4 or more, and may be 6 or more. The upper limit of the molar ratio of Li to Al (Li / Al) when an Al source is included in the mixing step is not particularly limited, but may be, for example, 12 or less, preferably 10 or less.
[0052] In the firing step, the mixture produced in the mixing step is fired. In the mixing step, the raw materials are mixed so that the molar ratio of the Li amount to the Mn amount (Li / Mn) exceeds 2, and thus excessive grain growth of the lithium manganese composite oxide is suppressed in the firing step. Although there is no intention to limit the technology disclosed herein, the reason why such an effect is obtained is presumed to be as follows. Since the molar ratio of the Li amount to the Mn amount (Li / Mn) exceeds 2, an excess Li component (Li salt) is present around the Li2MnO3 particles during firing. In the presence of this Li salt, multiple Li2MnO3 particles are unlikely to aggregate, and as a result, excessive grain growth is suppressed, and it is presumed that the coarsening of the inorganic red pigment after firing is suppressed.
[0053] The firing temperature in the firing step is not particularly limited as long as a lithium manganese composite oxide can be produced. For example, the firing temperature is preferably 850°C to 1100°C, and more preferably 900°C to 1050°C. This allows an inorganic red pigment having an appropriate particle size to be suitably produced. The firing time is not particularly limited, but may be, for example, about 30 minutes to 12 hours (preferably 1 hour to 6 hours). The firing atmosphere may be an air atmosphere, an oxidizing atmosphere, an inert gas atmosphere, or the like.
[0054] When the mixing step further includes an Al source, the grain growth of the lithium manganese composite oxide in the firing step can be more suitably suppressed. As described above, the raw materials are mixed so that the molar ratio of the Li amount to the Mn amount (Li / Mn) exceeds 2, so that excess Li salt is present around the Li2MnO3 particles during firing. It is presumed that the Al source reacts with the excess Li salt and precipitates as lithium aluminate around the Li2MnO3 particles. This can further suppress the grain growth of the lithium manganese composite oxide. It is presumed that the Al source reacts only with the excess Li salt, and its effect on the crystal structure of Li2MnO3 has not been confirmed by the XRD chart.
[0055] In the washing step, the fired product after the firing step is washed. The washing step is carried out so as to remove the excess Li component (Li salt) described above. In the washing step, the fired product may be washed with an acid or with water (e.g., distilled water). From the viewpoint of suitably removing the excess Li component, washing with an acid is preferred. Examples of the acid include nitric acid, hydrochloric acid, and sulfuric acid. When washing with an acid is carried out, after washing with the acid, the product is washed with distilled water until the pH becomes about 7, and then dried to obtain an inorganic red pigment with a suitably adjusted particle size.
[0056] The concentration of the acid in the cleaning step is not particularly limited. From the viewpoint of suitably removing the excess Li component, the concentration of the acid in the cleaning step is preferably 0.1 mol / L or more, may be 0.2 mol / L or more, or may be 0.5 mol / L or more. The upper limit of the acid concentration is not particularly limited, but is preferably 1.5 mol / L or less, and more preferably 1 mol / L or less.
[0057] As described above, when the content of the Al component is about 10 wt% or less when the inorganic red pigment is 100 wt%, it can exhibit the effect of showing a more vivid red color. From this viewpoint, it is preferable to carry out the washing step so that the content of aluminum is 0.1 wt% to 10 wt% when the inorganic red pigment is 100 wt%. Even when an Al source is further added in the mixing step, washing may be carried out with an acid in the washing step, or washing may be carried out with water (e.g., distilled water). In this case, the concentration of the acid in the washing step is preferably 0.1 mol / L or more and 1 mol / L or less, and more preferably 0.1 mol / L or more and 0.8 mol / L or less. Alternatively, as described above, washing may be carried out with only distilled water.
[0058] In the manufacturing method disclosed herein, the molar ratio (Li / Mn) of the amount of Li to Mn in the mixing step is adjusted to exceed 2, so that grain growth in the firing step is suppressed, and the grain size (e.g., D 50 Or D SEM ) is suitably adjusted. Therefore, in this production method, it is not necessary to carry out a particle size adjustment step such as pulverization after the washing step. As a result, there is almost no generation of fine powder due to pulverization, and a vivid red color with less yellowness than in the past can be obtained.
[0059] The inorganic red pigment disclosed herein does not contain any components harmful to the human body or the environment, and can achieve a vivid red color. Such an inorganic red pigment can be used for various purposes, and can be suitably used, for example, for painting automobiles, exterior walls, notebook computers, mobile phones, etc. Furthermore, such an inorganic red pigment can be widely used not only in the above-mentioned red paints, but also in colorants used in cosmetics, stationery such as crayons, and daily necessities (e.g., plastics).
[0060] Hereinafter, examples of the technology disclosed herein will be described, but it is not intended that the technology disclosed herein be limited to those shown in these examples.
[0061] [First test] In the first test, the inorganic red pigment was prepared by varying the molar ratio of Li to Mn (Li / Mn) when mixing the raw materials. Then, a pigment paste was prepared using each of the prepared pigments. The pigment paste was applied to an alumina substrate to prepare a coating film.
[0062] 1. Preparation of Pigments <Example 1> 4.35 g of manganese (IV) oxide (Kanto Chemical Co., Ltd., Kagoshima Grade 1) and 7.39 g of lithium carbonate (Fujifilm Wako Pure Chemical Industries, Ltd., Wako Special Grade) were mixed in a mortar for 10 minutes or more so that the molar ratio of Li to Mn (Li / Mn) was 4. The mixed powder was then placed in an alumina crucible and fired at 1050°C for 6 hours. After firing, the mixture was washed with 1M nitric acid to remove excess lithium salt. The mixture was then further washed with distilled water until the pH of the solution reached 7, and the resulting precipitate was dried at 100°C. This resulted in the pigment of Example 1.
[0063] <Example 2> A pigment of Example 2 was prepared in the same manner as in Example 1, except that the amount of lithium carbonate was changed to 11.08 g so that the molar ratio of the amount of Li to the amount of Mn (Li / Mn) was 6.
[0064] <Example 3> A pigment of Example 3 was prepared in the same manner as in Example 1, except that the amount of lithium carbonate was 5.54 g so that the molar ratio of the Li amount to the Mn amount (Li / Mn) was 3.
[0065] <Example 4> The pigment of Example 4 was prepared in the same manner as in Example 1, except that the amount of lithium carbonate was 4.06 g so that the molar ratio of the Li amount to the Mn amount (Li / Mn) was 2.1.
[0066] <Example 5> The pigment of Example 5 was produced in the same manner as in Example 1, except that the firing temperature was 900°C.
[0067] <Comparative Example 1 and Comparative Example 2> In Comparative Example 1, commercially available red iron oxide (Toyo Bengara Kogyo Co., Ltd.) was prepared as a pigment. In Comparative Example 2, commercially available Li2MnO3 (Toshima Manufacturing Co., Ltd.) was prepared as a pigment.
[0068] <Comparative Example 3> A pigment of Comparative Example 3 was prepared in the same manner as in Example 1, except that the amount of lithium carbonate was 3.70 g so that the molar ratio of the amount of Li to the amount of Mn (Li / Mn) was 2.
[0069] 2. Evaluation of pigments <Observation of pigment particle shape> A field emission scanning electron microscope (SU-8230, Hitachi High-Technologies Corporation) was used to observe the particle shapes of the pigments of Example 1, Comparative Example 2, and Comparative Example 3. An FE-SEM image (10,000x) of Example 1 is shown in FIG. 1, an FE-SEM image (10,000x) of Comparative Example 2 is shown in FIG. 2, and an FE-SEM image (10,000x) of Comparative Example 3 is shown in FIG. 3.
[0070] <Average particle size based on field emission scanning electron microscope images (D SEM ) Measurement> For each of the pigments prepared above, the average particle diameter (D SEM) was measured. Specifically, first, FE-SEM observation images of each example were obtained using the above-mentioned field emission scanning electron microscope. The FE-SEM images of each example were obtained at a magnification of 5000x or 1000x. Then, using the image processing software "ImageJ", the horizontal Feret diameters of 100 particles with clear contours in the FE-SEM images were measured and the average value was calculated. This average value was used as the average particle diameter (D SEM ) The results are shown in Table 1. As an example, an FE-SEM image (1000x) of Example 1 is shown in FIG. 4, an FE-SEM image (1000x) of Comparative Example 2 is shown in FIG. 5, and an FE-SEM image (1000x) of Comparative Example 3 is shown in FIG. 6.
[0071] <Average particle size based on laser diffraction scattering method (D 50 ) Measurement> For each of the pigments prepared above, the average particle diameter (D 50 ) was measured. Specifically, the particle size of the pigment was measured by a wet method using a laser diffraction particle size distribution measuring device (Spectris Corporation, Mastersizer 3000). Water was used as the dispersion medium. When dispersibility was poor, a dispersant was added before measurement. In the volume-based particle size distribution based on the above measurement, the particle size corresponding to the cumulative 50% from the smallest particle size side was taken as the average particle size (D 50 In addition, the D 10 Particle size and D corresponding to the cumulative 90% from the smallest particle size in the above particle size distribution 90 The particle size and were measured, and the results are shown in Table 1.
[0072] <Color development evaluation> The color development of each example pigment was evaluated. Specifically, a spectrophotometer (CM-5, manufactured by Konica Minolta Sensing Co., Ltd.) was used to measure the lightness (L*) and chromaticity (a*, b*) of the L*a*b* color system, and the chroma (C*) and hue angle (h) of the L*C*h color system. First, 0.5 g of each example pigment was collected in a petri dish. Next, the petri dish was set in the above-mentioned spectrophotometer, and the lightness (L*), chromaticity (a*, b*), chroma (C*) and hue angle (h) of each example pigment were measured using the SCE (specular reflection excluded) method. The results are shown in Table 1. In the "Color development evaluation" column of Table 1, a* value higher than that of Comparative Example 1 (i.e., commercially available red iron oxide) and an h value of 20 to 40 were evaluated as having good color development (◯), and a* value lower than that of Comparative Example 1 or an h value not satisfying the range of 20 to 40 were evaluated as having poor color development (×). Here, when the a* value is lower than that of Comparative Example 1 (i.e., 31.9 or less), the color is a dull red. When the h value is less than 20, the color is reddish purple, and when it is more than 40, the color is close to orange.
[0073] <Observation of the crystal structure of pigments> Furthermore, for Example 1 and Comparative Example 3, the crystal structure of the pigment was evaluated using an X-ray diffractometer (Rigaku Corporation, SmartLab). The crystal structures of the pigments of Example 1 and Comparative Example 3 were identified by fitting analysis of the acquired XRD patterns of Example 1 and Comparative Example 3 with the Li2MnO3 pattern in the database. The XRD chart of Example 1 is shown in FIG. 7, and the XRD chart of Comparative Example 3 is shown in FIG. 8.
[0074] 3. Preparation of pigment paste and coating <Example 1> 0.2 g of the pigment of Example 1 prepared above, 0.36 g of Clarity LA2270 (Kuraray Co., Ltd.) as an acrylic resin, and 0.44 g of bis(2-ethoxyethyl)ether (Wako Grade 1, Fujifilm Wako Pure Chemical Industries, Ltd.) as a solvent were placed in an ointment jar. The mixture was mixed and dispersed using a centrifugal mixer to obtain a pigment paste containing the pigment of Example 1. The pigment paste was applied to an alumina substrate using a metal mask and metal squeegee measuring 2 cm long x 2 cm wide x 200 μm high to form a coating film. In this manner, the coating film of Example 1 was obtained.
[0075] <Examples 2 to 5 and Comparative Examples 1 to 3> The pigments of each example (Examples 2 to 5 and Comparative Examples 1 to 3) were used and prepared in the same manner as in Example 1. The pigment paste was applied to an alumina substrate in the same manner as in Example 1 to produce a coating film of each example (Examples 2 to 5 and Comparative Examples 1 to 3).
[0076] 4. Evaluation of coating film <Film forming properties> The film-forming properties of the coating films of each example were evaluated. Specifically, the uniformity of the coating films of each example was visually confirmed. In the "Film-forming properties evaluation" column of Table 1, coating films with a uniform surface were evaluated as good (○), and coating films with an uneven or rough surface were evaluated as poor (×).
[0077] [Table 1]
[0078] As shown in Table 1, the pigments of Examples 1 to 5, which were prepared by mixing so that the molar ratio of the Li amount to the Mn amount (Li / Mn) exceeded 2, were D 50 is 1 μm or more and 5 μm or less, and D SEM D 50 Ratio of (D 50 / D SEM It can be seen that the a* value of the pigments of Examples 1 to 5 is higher than that of Comparative Example 1 (a* value is 32 or more), the h value is 20 to 40, and the pigments exhibit a vivid red color. 50is 1 μm or more and 5 μm or less, and D SEM D 50 Ratio of (D 50 / D SEM ) is 1 or more and 4 or less, a vivid red color can be realized.
[0079] In addition, the pigments of Examples 1 to 5, which were prepared by mixing so that the Li / Mn ratio exceeded 2, had a D 50 The particle size is 5 μm or less, and D 90 It can be seen that the particle diameter is 30 μm or less, and the particles are not coarsened. On the other hand, in Comparative Example 3 in which the Li / Mn ratio is 2 (i.e., the stoichiometric ratio), D 50 Particle size and D 90 Both particle sizes exceeded 30 μm, and it was found that the particles were coarse. This is presumably because when the Li / Mn ratio was 2, the particle growth during firing was significant. For this reason, the coating film containing the pigment in Comparative Example 3 had a rough surface and was a dull red color. In Comparative Example 2, D 50 The particle size was 8.4 μm, which was coarse compared to Examples 1 to 5. The pigment of Comparative Example 2 exhibited a color close to orange.
[0080] Moreover, as shown in Figures 1 and 4, the primary particle size in Example 1 is 5 μm or less, and it is understood that the particles are hardly coarsened by sintering. On the other hand, as shown in Figures 2, 3, 5, and 6, the primary particle sizes in Comparative Examples 2 and 3 are equivalent to or smaller than the primary particle size in Example 1, but the primary particle size grows during sintering to form coarse secondary particles. In other words, by preparing a pigment with a Li / Mn ratio of more than 2, particle growth during sintering is suitably suppressed, and a pigment that exhibits a vivid red color can be provided.
[0081] 7 and 8, it is understood that Example 1, in which the Li / Mn ratio exceeds 2 when the pigment is produced, and Comparative Example 3, which was produced with Li / Mn=2 (i.e., the stoichiometric ratio), have the same crystal structure. In other words, it is understood that even if the Li / Mn ratio exceeds 2 when the pigment is produced, it does not affect the crystal structure of the lithium manganese composite oxide (Li2MnO3) contained in the pigment.
[0082] [Second test] In the second test, the molar ratio of Li to Mn (Li / Mn) was varied when mixing the raw materials for the inorganic red pigment, and an Al component was added to produce the pigment. Then, a pigment paste was prepared using each of the pigments produced. The pigment paste was applied to an alumina substrate to produce a coating film.
[0083] 1. Pigment Preparation <Example 11> 4.35g of manganese (IV) oxide (Kanto Chemical Co., Ltd., Kagoshima Grade 1), 7.39g of lithium carbonate (Fujifilm Wako Pure Chemical Industries, Ltd., Wako Special Grade), and 1.02g of alumina (Daimei Chemical Industry Co., Ltd., Taimicron TM-DA) were mixed in a mortar for 10 minutes or more so that the molar ratio of Li to Mn (Li / Mn) was 4 and the molar ratio of Li to Al (Li / Al) was 10. The mixed powder was then placed in an alumina crucible and fired at 1050°C for 6 hours. After firing, the mixture was washed with 1M nitric acid to remove excess lithium salt. The mixture was then further washed with distilled water until the pH of the solution became 7, and the resulting precipitate was dried at 100°C. This resulted in the pigment of Example 11.
[0084] <Example 12> The pigment of Example 12 was prepared in the same manner as in Example 11, except that the amount of alumina was 2.55 g so that the molar ratio of the amount of Li to the amount of Mn (Li / Mn) was 4 and the molar ratio of the amount of Li to the amount of Al (Li / Al) was 4.
[0085] <Example 13> The pigment of Example 13 was prepared in the same manner as in Example 11, except that the amount of lithium carbonate was 5.54 g and the amount of alumina was 1.28 g so that the molar ratio of the amount of Li to the amount of Mn (Li / Mn) was 3 and the molar ratio of the amount of Li to the amount of Al (Li / Al) was 6.
[0086] <Example 14> In Example 14, 1.85 g of lithium carbonate (Honjo Chemical Co., Ltd., industrial use), 1.63 g of manganese dioxide n-hydrate (Fujifilm Wako Pure Chemical Industries, Ltd.), and 0.255 g of alumina (Nippon Light Metals Co., Ltd., LS-711) were mixed in a mortar for 10 minutes or more so that the molar ratio of Li to Mn (Li / Mn) was 4 and the molar ratio of Li to Al (Li / Al) was 10. Except for this, the pigment of Example 14 was produced in the same manner as in Example 11.
[0087] <Example 15> In Example 15, 1.85 g of lithium carbonate (Honjo Chemical Co., Ltd., industrial use), 1.09 g of manganese dioxide (Tosoh Corporation, FMH), and 0.390 g of aluminum hydroxide (Fuji Film Wako Pure Chemical Industries, Ltd.) were mixed in a mortar for 10 minutes or more so that the molar ratio of Li to Mn (Li / Mn) was 4 and the molar ratio of Li to Al (Li / Al) was 10. Other than this, the pigment of Example 15 was prepared in the same manner as in Example 11.
[0088] <Example 16> The pigment of Example 16 was prepared in the same manner as in Example 11, except that 0.1 M nitric acid was used in washing after calcination.
[0089] <Comparative Example 11> In Comparative Example 11, the amount of lithium carbonate was 5.54 g and the amount of alumina was 2.55 g so that the molar ratio of the amount of Li to the amount of Mn (Li / Mn) was 3 and the molar ratio of the amount of Li to the amount of Al (Li / Al) was 3. The temperature during firing was set to 900° C. Other than these, the pigment of Comparative Example 11 was produced in the same manner as in Example 11.
[0090] <Comparative Example 12> In Comparative Example 12, the amount of alumina was 2.55 g so that the molar ratio of the Li amount to the Mn amount (Li / Mn) was 4 and the molar ratio of the Li amount to the Al amount (Li / Al) was 4. The firing temperature was set to 800° C. Other than these, the pigment of Comparative Example 12 was produced in the same manner as in Example 11.
[0091] <Reference example 11> In Reference Example 11, a pigment was prepared so that the LiAlO2 equivalent (wt%) was approximately equal to the LiAlO2 equivalent (wt%) of Example 11 described later. Specifically, 0.42 g of the pigment prepared in Example 11 and 0.08 g of lithium aluminate (Tokyo Chemical Industry Co., Ltd.) were mixed in a mortar for 10 minutes or more. This mixed powder was used as the pigment of Reference Example 11. The LiAlO2 equivalent of Reference Example 11 calculated from the amount added when the pigment was prepared was 16.1 wt%.
[0092] 2. Evaluation of pigments <Observation of pigment particle shape> The particle shape of the pigment of Example 16 was observed using the above-mentioned field emission scanning electron microscope (SU-8230, Hitachi High-Technologies Corporation). An FE-SEM image (10,000x) of Example 16 is shown in FIG.
[0093] <Average particle size based on field emission scanning electron microscope images (D SEM ) Measurement> For each of the pigments prepared above, the average particle diameter (D SEM ) was measured in the same manner as in the first test. The results are shown in Table 2. As an example, an FE-SEM image (1000x) of Example 16 is shown in FIG. 10. Table 2 also shows the results of Example 1 and Comparative Example 1.
[0094] <Average particle size based on laser diffraction scattering method (D 50 ) Measurement> For each of the pigments prepared above, the average particle diameter (D 50) was measured in the same manner as in the first test. The results are shown in Table 2. Note that Table 2 also shows the results of Example 1 and Comparative Example 1.
[0095] <Color development evaluation> The color development of each example pigment was evaluated in the same manner as in the first test. The results are shown in Table 2. Table 2 also shows the results of Example 1 and Comparative Example 1. In the "Color Development Evaluation" column of Table 2, a pigment having an a* value higher than that of Comparative Example 1 (i.e., commercially available red iron oxide) and an h value of 20 to 40 was evaluated as having good color development (◯), and a pigment having an a* value lower than that of Comparative Example 1 or an h value not satisfying the range of 20 to 40 was evaluated as having poor color development (×).
[0096] <Observation of the crystal structure of pigments> The crystal structures of Examples 11 and 16 were measured in the same manner as in the first test. The XRD chart of Example 11 is shown in FIG. 11, and the XRD chart of Example 16 is shown in FIG.
[0097] <Measurement of Al content in pigment> The Al content (wt%) in the pigment was measured using an inductively coupled plasma (ICP) optical emission spectrometer (Agilent Technologies, Inc. 5800 ICP-OES). 0.1 g of the pigment in each example was dissolved by heating in 10 ml of hydrochloric acid (hydrochloric acid:water = 1:1) and the volume was adjusted to 250 ml. After appropriate dilution, quantitative analysis of Al was performed using the above-mentioned ICP to determine the Al content (wt%). The results are shown in Table 2.
[0098] <Calculation of the LiAlO2 equivalent amount contained in the pigment> For Example 11, the LiAlO2 equivalent (wt%) was calculated from the Al content (wt%). Specifically, the LiAlO2 equivalent (wt%) was calculated from the above-obtained Al content (wt%), the molar mass of LiAlO2 (65.92 g / mol), and the molar mass of Al (26.98 g / mol) according to the formula: LiAlO2 equivalent (wt%) = (Al content x 65.92) / 26.98. As a result, the LiAlO2 equivalent of Example 11 was 16 wt%.
[0099] 3. Preparation of pigment paste and coating <Example 11> 0.2 g of the pigment of Example 11 prepared above, 0.36 g of Clarity LA2270 (Kuraray Co., Ltd.) as an acrylic resin, and 0.44 g of bis(2-ethoxyethyl)ether (Wako Grade 1, Fujifilm Wako Pure Chemical Industries, Ltd.) as a solvent were placed in an ointment jar. The mixture was mixed and dispersed using a centrifugal mixer to obtain a pigment paste containing the pigment of Example 11. The pigment paste was applied to an alumina substrate using a metal mask and metal squeegee measuring 2 cm long x 2 cm wide x 200 μm high to form a coating film. In this manner, the coating film of Example 11 was obtained.
[0100] <Examples 12 to 16, Comparative Examples 11 to 12, and Reference Example 11> The pigments of each example (Examples 12 to 16, Comparative Examples 11 to 12, and Reference Example 11) were used and prepared in the same manner as in Example 1. The pigment paste was applied to an alumina substrate in the same manner as in Example 11 to produce coating films of each example (Examples 12 to 16, Comparative Examples 11 to 12, and Reference Example 11).
[0101] 4. Evaluation of coating film <Film forming properties> The film-forming properties of the coating films of each example were evaluated in the same manner as in the first test. The results are shown in Table 2. Table 2 also shows the results of Example 1 and Comparative Example 1. In the "Film-forming properties evaluation" column in Table 2, coating films with a uniform surface were rated as good (◯), and coating films with an uneven or rough surface were rated as poor (×).
[0102] [Table 2]
[0103] As shown in Table 2, the pigments of Examples 1, 11 to 16, which were prepared by mixing so that the molar ratio of the Li amount to the Mn amount (Li / Mn) exceeded 2, were D 50 is 1 μm or more and 5 μm or less, and D SEM D 50Ratio of (D 50 / D SEM It can be seen that the molar ratio of the Li amount to the Al amount (Li / Al) is 1 or more and 4 or less. Furthermore, the pigments of Examples 11 to 16, which were prepared by mixing so that the molar ratio of the Li amount to the Al amount (Li / Al) was 4 or more, had a D 50 It can be seen that the a* value is smaller than that of Example 1. This is presumably because the presence of the Al component during firing causes the Al component to react with the excess Li component, resulting in the precipitation of lithium aluminate (LiAlO2) around the Li2MnO3, which suppresses the grain growth of Li2MnO3 more than in the case of Li salt alone. This shows that the coating films using the pigments of Examples 11 to 16 have a higher a* value and an h value of 20 to 40 than Comparative Example 1, and exhibit a vivid red color. That is, D 50 is 1 μm or more and 5 μm or less, and D SEM D 50 Ratio of (D 50 / D SEM ) is 1 or more and 4 or less, and further contains an aluminum component, and the aluminum content is 10 wt % or less, by using a pigment, a vivid red color can be realized. Moreover, as shown in Examples 14 and 15, it is understood that the Li source and the Al source are not particularly limited.
[0104] As shown in Table 2, even Example 1, in which no alumina was added during production, contained less than 1 wt% Al. This is presumably due to trace amounts of Al present in the alumina crucible or other raw materials used in producing the pigment.
[0105] As shown in Table 2, in Comparative Example 3, which further contains an Al component and is mixed so that the molar ratio of Li to Al (Li / Al) is 3, grain growth due to firing is remarkable, and D 50 This is presumably because when the amount of Al is excessive relative to the amount of Li during pigment production, the effect of suppressing particle growth due to the inclusion of the Al component is no longer obtained, and instead the particle diameter becomes larger.
[0106] In addition, as shown in Comparative Example 12 in Table 2, when the firing temperature is lowered (for example, when it is set to 800° C. or lower), D 50 The particle size tends to be excessively small. 50 If the particle size is less than 1 μm, the h value will be 40 or more, resulting in a color close to orange. 50 In Comparative Example 12, D 50 D SEM is larger, but this is because the particle size distribution has two peaks and there is a large variation.
[0107] In Example 16, cleaning was performed using nitric acid with a lower concentration than in Example 11, and therefore the content of Al component is high. As shown in FIG. 9, it can be seen that in Example 16, a large amount of white granular lithium aluminate is present on the surface of each lithium manganese composite oxide. In addition, as shown in FIGS. 9 and 10, no aggregation of primary particles was observed in Example 16, which may explain the D 50 It is presumed that the a* value is not coarsened. Example 16 is the same as Example 11 except that the nitric acid concentration during washing was changed, but as shown in Table 2, it can be seen that the a* value is improved.
[0108] Reference Example 11 is a powder material in which lithium aluminate is mixed into the pigment of Example 11. Since Reference Example 11 uses the pigment of Example 11, both the a* value and the h value are good. On the other hand, Reference Example 11 has almost the same amount of LiAlO2 equivalent as Example 16, but the a* value is lower than that of Example 11. This is presumed to be because Reference Example 11 does not have a form in which lithium aluminate exists on the surface of the lithium manganese composite oxide, since lithium aluminate powder is mixed with the pigment after firing. In other words, it is presumed that a more vivid red color can be realized by the presence of a large amount of aluminum components as lithium aluminate on the surface of the lithium manganese composite oxide. It is considered that the reason why the L* value of Example 16 and Reference Example 11 is improved in Table 2 is that the color of lithium aluminate is white, and becomes whitish by mixing.
[0109] Furthermore, as shown in FIG. 8 and FIG. 11, it is understood that the crystal structure is the same between Example 11, in which Li / Mn exceeds 2 when the pigment is produced, and Comparative Example 3, in which Li / Mn=2 (i.e., stoichiometric ratio) is produced. That is, even if Li / Mn exceeds 2 when the pigment is produced and alumina is added, most of the components derived from the excess lithium carbonate and alumina are removed by washing, and it is understood that there is no influence on the crystal structure of the lithium manganese composite oxide contained in the pigment. Furthermore, as shown in FIG. 12, in Example 16, a peak of LiAlO2 was confirmed along with a peak of Li2MnO3. It is presumed that in Example 16, the nitric acid concentration during washing was lowered, so that most of the excess lithium carbonate was removed, but the lithium aluminate was not removed and remained on the surface of the lithium manganese oxide.
[0110] Although specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.
[0111] The technology disclosed herein includes the following items 1 to 9. The following items 1 to 9 are not limited to the above-described embodiment.
[0112] Item 1 relates to an inorganic red pigment. The inorganic red pigment in item 1 is Lithium manganese composite oxide is included, The average particle size (D) in the volume-based particle size distribution based on the laser diffraction scattering method 50 ) is 1 μm or more and 5 μm or less, D 50 and the average particle size (D SEM ) and D 50 / D SEM is between 1 and 4 inclusive.
[0113] Item 2 is the inorganic red pigment according to item 1, D in volume-based particle size distribution based on laser diffraction scattering method 90 The particle size is 30 μm or less.
[0114] Item 3 is the inorganic red pigment according to item 1 or 2, The a* value of the L*a*b* color system measured using the SCE method is 32 or more, and the h value of the L*C*h color system measured using the SCE method is 20 or more and 40 or less.
[0115] Item 4 is an inorganic red pigment according to any one of Items 1 to 3, When the total weight of the inorganic red pigment is taken as 100 wt %, the content of the lithium manganese composite oxide is 80 wt % or more.
[0116] Item 5 is an inorganic red pigment according to any one of Items 1 to 4, Further comprising an aluminum component, When the total weight of the inorganic red pigment is taken as 100 wt %, the aluminum content is 10 wt % or less.
[0117] Item 6 is about red paint. The red paint in item 6 is: The inorganic red pigment according to any one of items 1 to 5 is contained.
[0118] Item 7 is about ceramic products. The ceramic products in item 7 are: The present invention is provided with a coating film containing the inorganic red pigment according to any one of items 1 to 5.
[0119] Item 8 relates to a method for producing an inorganic red pigment. The method for producing an inorganic red pigment in Item 8 is as follows: mixing a Li source and a Mn source such that the molar ratio of the amount of Li to the amount of Mn (Li / Mn) exceeds 2; calcining a mixture of the Li source and the Mn source; A step of washing the fired product after the firing step with an acid; Including, In the washing step, washing is carried out so as to remove excess Li components.
[0120] Item 9 is a method for producing the inorganic red pigment according to item 8, In the mixing step, an Al source is further added, The Li source and the Al source are mixed so that the molar ratio of the Li amount to the Al amount (Li / Al) is 4 or more.
Claims
1. 1. An inorganic red pigment comprising: Lithium manganese composite oxide is included, The average particle diameter (D) in the volume-based particle size distribution based on the laser diffraction scattering method 50 ) is 1 μm or more and 5 μm or less, The above D 50 and the average particle diameter (D SEM ) and D 50 / D SEM An inorganic red pigment, wherein
2. D in volume-based particle size distribution based on laser diffraction scattering method 90 2. The inorganic red pigment according to claim 1, having a particle size of 30 μm or less.
3. 2. The inorganic red pigment according to claim 1, wherein the a* value of the L*a*b* color system measured by the SCE method is 32 or more, and the h value of the L*C*h color system measured by the SCE method is 20 or more and 40 or less.
4. 2. The inorganic red pigment according to claim 1, wherein the content of the lithium manganese composite oxide is 80 wt % or more when the total weight of the inorganic red pigment is taken as 100 wt %.
5. Further comprising an aluminum component, 2. The inorganic red pigment according to claim 1, wherein the content of aluminum is 10 wt % or less when the total weight of the inorganic red pigment is taken as 100 wt %.
6. A red paint comprising the inorganic red pigment according to any one of claims 1 to 5.
7. A ceramic product provided with a coating film containing the inorganic red pigment according to any one of claims 1 to 5.
8. mixing a Li source and a Mn source such that a molar ratio of the amount of Li to the amount of Mn (Li / Mn) exceeds 2; calcining a mixture of the Li source and the Mn source; A step of washing the fired product after the firing step; Including, In the washing step, washing is performed so as to remove excess Li components.
9. In the mixing step, an Al source is further added, The method according to claim 8 , wherein the Li source and the Al source are mixed so that a molar ratio of Li to Al (Li / Al) is 4 or more.
Citation Information
Patent Citations
Positive electrode active material for nonaqueous electrolyte secondary battery and its manufacturing method
JP2003272629A
Lithium manganate for lithium secondary battery positive electrode secondary active material, and manufacturing method of lithium manganate, lithium secondary battery positive electrode active material, and lithium secondary battery
JP2008066028A
Method for manufacturing lithium-containing complex oxide, positive electrode active material, and secondary battery
JP2012252853A
Production method of lithium-manganese compound oxide, lithium-manganese compound oxide obtained by the production method, positive active material for secondary battery containing the same and lithium ion secondary battery using the same as positive active material
JP2013245114A
Orange inorganic pigment, covering pigment, and resin composition
JP2022114385A