Laminate and display device

The laminate with horizontally oriented light-absorbing anisotropic films and a retardation plate enables easy three-dimensional display in flat panel devices by outputting different hues per pixel, addressing the lack of three-dimensional capabilities in existing technologies.

JP2024143509APending Publication Date: 2024-10-11SUMITOMO CHEM CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023056232
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing flat panel display devices lack the capability for easy three-dimensional display, which is necessary for enhancing realism and immersion.

Method used

A laminate comprising horizontally oriented light-absorbing anisotropic films with different absorption axis directions and maximum absorption wavelengths, combined with a retardation plate, to output light of different hues per pixel, enabling three-dimensional display.

Benefits of technology

The laminate facilitates easy realization of three-dimensional displays by generating sufficient parallax and allowing images to be visually recognized even with tilted viewing angles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143509000001_ABST
    Figure 2024143509000001_ABST
Patent Text Reader

Abstract

To provide a laminate body and a display device which easily allows a three-dimensional display.SOLUTION: A laminate body 3 includes: a horizontal orientation light absorption anisotropic film A with a dichroism pigment compound A; and a horizontal orientation light absorption anisotropic film B with a dichroism pigment compound B. The absorption axis direction and the maximum absorption wavelength in the horizontal orientation light absorption anisotropic film A and the absorption axis direction and the maximum absorption wavelength in the horizontal orientation light absorption anisotropic film B are different.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a laminate and a display device. [Background technology]

[0002] Conventionally, laminates that function as polarizers, for example, have been known for use in flat panel displays such as liquid crystal displays and organic electroluminescence displays. An example of such a laminate is the polarizing film described in Patent Document 1. This conventional polarizing film includes a light-absorbing anisotropic film that contains a dichroic dye compound. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-211770 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, research and development has been progressing on 3D imaging technology that can provide a high sense of realism and presence in the above-mentioned display devices. For this reason, there is a demand for technology that enables easy 3D display.

[0005] The present disclosure has been made to solve the above problems, and has an object to provide a laminate and a display device that enable easy three-dimensional display. [Means for solving the problem]

[0006] A laminate according to one aspect of the present disclosure includes a horizontally aligned optically absorptive anisotropic film A having a dichroic dye compound A, and a horizontally aligned optically absorptive anisotropic film B having a dichroic dye compound B, in which the absorption axis direction and maximum absorption wavelength in the horizontally aligned optically absorptive anisotropic film A are different from the absorption axis direction and maximum absorption wavelength in the horizontally aligned optically absorptive anisotropic film B.

[0007] In this laminate, horizontally aligned optically absorptive anisotropic films A and B having different absorption axis directions and maximum absorption wavelengths are combined. Therefore, when white light is input to the laminate as one pixel, light of different hues can be output from the single pixel according to the absorption axis directions of the horizontally aligned optically absorptive anisotropic films. Therefore, for example, by arranging the laminate so that the absorption axis directions of the horizontally aligned optically absorptive anisotropic films A and B are different for each pixel, a three-dimensional display can be easily realized.

[0008] The dichroic dye compound A and the dichroic dye compound B may be selected from different hues in the group of cyan, magenta, and yellow or the group of red, green, and blue. In this case, sufficient parallax can be generated in the light output from the laminate. Therefore, a three-dimensional display can be realized more easily.

[0009] The dichroic dye compound A and the dichroic dye compound B may each be selected from two different hues from the group of cyan, magenta, and yellow, or the group of red, green, and blue. In this case, sufficient parallax can be generated in the light output from the laminate. Therefore, a three-dimensional display can be realized more easily.

[0010] The horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B may each be a cured product of an optically absorptive anisotropic film-forming composition having a polymerizable liquid crystal compound. In this case, the alignment state of the dichroic dye compound can be suitably fixed.

[0011] The polymerizable liquid crystal compound may be a liquid crystal compound that forms a smectic phase in at least one of the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B. This makes it possible to obtain higher polarization characteristics.

[0012] In both the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B, the polymerizable liquid crystal compound may be a liquid crystal compound that forms a smectic phase. This makes it possible to obtain higher polarization characteristics.

[0013] The laminate may further include a retardation plate having a phase difference of π / 2 and a slow axis in an orientation of 45°±5° with respect to the absorption axes of the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B. By combining a retardation plate, the function of the laminate can be expanded.

[0014] The front retardation value Re(λ) of the retardation plate may satisfy the following formula (1): Thereby, a retardation plate having desired optical characteristics is obtained. Re(450) <Re(550)<Re(650)…(1)

[0015] In the laminate, a horizontally aligned optically absorptive anisotropic film A, a horizontally aligned optically absorptive anisotropic film B, and a retardation film may be laminated in this order. In this case, the retardation film can function as an anti-reflection film for light input from the horizontally aligned optically absorptive anisotropic film A.

[0016] In the laminate, a retardation plate, a horizontally aligned optically absorptive anisotropic film A, and a horizontally aligned optically absorptive anisotropic film B may be laminated in this order. In this case, the light output from the laminate can be made circularly polarized. Therefore, even if the line of sight to the laminate is tilted to some extent, the image can be viewed.

[0017] A display device according to one aspect of the present disclosure includes the above-described laminate and a light source that outputs light toward the laminate.

[0018] In this display device, horizontally aligned optically absorptive anisotropic films A and B, which have different absorption axis directions and maximum absorption wavelengths, are combined in a laminate. Therefore, when white light is input to the laminate as one pixel, light of different hues can be output from the single pixel according to the absorption axis directions of the horizontally aligned optically absorptive anisotropic films. Therefore, for example, by arranging the laminate so that the absorption axis directions of the horizontally aligned optically absorptive anisotropic films A and B are different for each pixel, a three-dimensional display can be easily realized. Effect of the Invention

[0019] According to the present disclosure, three-dimensional display can be easily achieved. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a schematic diagram illustrating a configuration of a display device according to a first embodiment of the present disclosure. [Diagram 2] FIG. 4 is a schematic diagram showing a configuration of a display device according to a second embodiment of the present disclosure. [Diagram 3] FIG. 11 is a diagram showing evaluation results of the display device according to the example. [Figure 4] FIG. 11 is a diagram showing an evaluation result of a display device according to a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, preferred embodiments of a laminate and a display device according to one aspect of the present disclosure will be described in detail with reference to the drawings.

[0022] [First embodiment] Fig. 1 is a schematic diagram showing the configuration of a display device according to a first embodiment of the present disclosure. The display device 1A shown in Fig. 1 is composed of a light source 2 and a laminate 3. Examples of the display device 1A include a liquid crystal display device, an organic EL display device, an inorganic EL display device, an electron emission display device, electronic paper, and a piezoelectric ceramic display.

[0023] The display device 1A is configured as a device for displaying a three-dimensional image. The light source 2 is a portion that outputs light toward the laminated body 3. The light source 2 is configured by a device that outputs white light L, such as a white LED. The laminated body 3 in FIG. 1 corresponds to one pixel in the display device 1A. In this embodiment, when viewed from the side opposite to the light source 2, the laminated body 3 is configured by laminating a polarizing plate 11A (a polarizing plate including a horizontally aligned optically absorbing anisotropic film A described later), a polarizing plate 11B (a polarizing plate including a horizontally aligned optically absorbing anisotropic film B described later), and a retardation plate 12 in this order. That is, in this embodiment, the retardation plate 12 is disposed between the polarizing plate 11B and the light source 2.

[0024] The polarizing plates 11A and 11B are members having a function of absorbing light of a predetermined wavelength in a predetermined direction. The polarizing plates 11A and 11B are formed, for example, by laminating an alignment film and a horizontally aligned light absorbing anisotropic film on a glass substrate. The glass substrate is particularly transparent to visible light, and has a transmittance of 80% or more for light with a wavelength of 380 nm to 780 nm. The thickness of the glass substrate is, in consideration of practical handling and processability, for example, 5 μm to 300 μm, preferably 20 μm to 200 μm, and more preferably 20 μm to 100 μm.

[0025] The substrate of the polarizing plate 11A and the polarizing plate 11B may be a resin substrate. In this case, examples of the resin material include polyolefins such as polyethylene, polypropylene, and norbornene-based polymers; cyclic olefin-based resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide; and polyphenylene oxide. Among these, a film substrate selected from triacetyl cellulose, cyclic olefin-based resins, polymethacrylic acid esters, and polyethylene terephthalate is more preferable from the viewpoint of transparency when used in optical film applications.

[0026] The alignment film is a film having a regulating force for aligning the dichroic dye compound contained in the horizontally aligned optically absorptive anisotropic film in a predetermined direction. The alignment film adjusts the absorption axis directions of the polarizing plates 11A and 11B to a desired direction by aligning the dichroic dye compound contained in the composition (composition for forming an optically absorptive anisotropic film) that forms the horizontally aligned optically absorptive anisotropic film. The absorption axis direction of the horizontally aligned optically absorptive anisotropic film is, for example, the same direction as the regulating force direction of the alignment film.

[0027] The alignment film has resistance to dissolution when the composition for forming an optically absorptive anisotropic film is applied, and also has resistance to heat treatment for removing the solvent and for orienting the dichroic dye. The thickness of the alignment film is, for example, 10 nm to 1200 nm, preferably 10 nm to 1000 nm, more preferably 10 nm to 500 nm, further preferably 10 nm to 200 nm, and particularly preferably 50 nm to 150 nm, in consideration of sufficient expression of the alignment control force.

[0028] Examples of the alignment film include an alignment film containing an orientable polymer, a photoalignment film, a groove alignment film having a concave-convex pattern or a plurality of grooves on the surface, and a stretched film stretched in the alignment direction.

[0029] Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and their hydrolyzates such as polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. The oriented polymers can be used alone or in combination of two or more kinds.

[0030] An alignment film containing an alignment polymer is usually obtained by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter referred to as an "alignment polymer composition") to a substrate and then removing the solvent, or by applying an alignment polymer composition to a substrate, removing the solvent, and rubbing the substrate (rubbing method).

[0031] The solvent is preferably an organic solvent, and examples of the organic solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; and chlorinated hydrocarbon solvents such as chloroform and chlorobenzene. The solvents can be used alone or in combination of two or more. The content of the solvent is preferably 100 to 1900 parts by mass, more preferably 150 to 900 parts by mass, and further preferably 180 to 600 parts by mass, based on 100 parts by mass of the orientable polymer composition.

[0032] The concentration of the oriented polymer in the oriented polymer composition may be within a range in which the oriented polymer material can be completely dissolved in the solvent, and is preferably 0.1 to 20% in terms of solid content relative to the solution, and more preferably 0.1 to 10%. As the oriented polymer composition, a commercially available oriented film material may be used as is. Examples of commercially available oriented film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).

[0033] Examples of the method for applying the oriented polymer composition to a substrate include known methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography. Examples of the method for removing the solvent contained in the oriented polymer composition include natural drying, ventilation drying, heat drying, and reduced pressure drying.

[0034] In order to impart an orientation regulating force to the orientation film, a rubbing treatment can be carried out as necessary (rubbing method). A method for imparting an orientation regulating force by the rubbing method includes a method in which an orientation polymer film formed on the surface of a substrate by applying an orientation polymer composition to the substrate and annealing the composition is brought into contact with a rotating rubbing roll wrapped with a rubbing cloth.

[0035] A photo-alignment film is usually obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter referred to as a "photo-alignment film-forming composition") to a substrate and irradiating the substrate with polarized light (preferably polarized UV). A photo-alignment film is more preferable in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the polarized light to be irradiated.

[0036] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that are the origin of liquid crystal alignment ability, such as molecular alignment induction caused by light irradiation or isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) is particularly preferred.

[0037] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.

[0038] Among them, photoreactive groups involved in photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film having excellent thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred.

[0039] A photo-alignment-inducing layer can be formed on a substrate by applying the composition for forming a photo-alignment film onto the substrate. The solvent contained in the composition can be the same as the solvent described in the "alignment polymer composition", and can be appropriately selected depending on the solubility of the polymer or monomer having a photoreactive group.

[0040] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted depending on the type of polymer or monomer and the thickness of the desired photo-alignment film, but is preferably at least 0.2% by mass or more, and more preferably in the range of 0.3 to 10% by mass, based on the mass of the composition for forming a photo-alignment film. The composition for forming a photo-alignment film may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, as long as the properties of the photo-alignment film are not significantly impaired.

[0041] The method of applying the composition for forming a photo-alignment film to a substrate may be the same as the method of applying the alignment composition to a substrate. The method of removing the solvent from the applied composition for forming a photo-alignment film may be natural drying, ventilation drying, heat drying, reduced pressure drying, etc.

[0042] The polarized light may be irradiated directly with polarized UV light after removing the solvent from the composition for forming a photo-alignment film applied on the substrate, or may be irradiated from the substrate side with polarized light and then transmitted through the substrate. It is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength in the range of 250 to 400 nm is particularly preferable.

[0043] Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferred. Among these, high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are preferred because of the high emission intensity of ultraviolet light with a wavelength of 313 nm. Polarized UV can be irradiated by irradiating light from the light source through an appropriate polarizer. As such a polarizer, a polarizing filter, a polarizing prism such as Glan-Thompson or Glan-Taylor, or a wire grid type polarizer can be used. It should be noted that if masking is performed when rubbing or polarized light irradiation is performed, multiple regions (patterns) with different liquid crystal alignment directions can also be formed.

[0044] A groove alignment film is a film that has a concave-convex pattern or multiple grooves on the film surface. When a polymerizable liquid crystal compound is applied to a film that has multiple linear grooves arranged at equal intervals, the liquid crystal molecules are aligned in the direction along the grooves.

[0045] Methods for obtaining a groove alignment film include a method in which the surface of a photosensitive polyimide film is exposed to light through an exposure mask having slits in a pattern shape, followed by development and rinsing to form a concave-convex pattern; a method in which a layer of uncured UV-curable resin is formed on a plate-shaped master having grooves on its surface, the formed resin layer is transferred to a substrate and then cured; and a method in which a roll-shaped master having multiple grooves is pressed against an uncured UV-curable resin film formed on a substrate to form concave-convex patterns, and then cured.

[0046] The horizontally aligned optically absorptive anisotropic film is configured to contain a dichroic dye compound. The dichroic dye compound is a dye compound having different absorbance in the long axis direction of the molecule and absorbance in the short axis direction of the molecule. The polarizing plates 11A and 11B including the horizontally aligned optically absorptive anisotropic film configured to contain the dichroic dye compound have an absorption direction in a predetermined direction and a maximum absorption wavelength in a predetermined wavelength range.

[0047] The dichroic dye compound A and the dichroic dye compound B may each be selected from different hues in the group of cyan, magenta, and yellow, or the group of red, green, and blue. The dichroic dye compound A and the dichroic dye compound B may each be selected from different hues in the group of cyan, magenta, and yellow, or the group of red, green, and blue, by two kinds.

[0048] Examples of the dichroic dye include an acridine dye, an oxazine dye, a cyanine dye, a naphthalene dye, an azo dye, and an anthraquinone dye, among which an azo dye is preferred. Examples of the azo dye include a monoazo dye, a bisazo dye, a trisazo dye, a tetrakisazo dye, and a stilbene azo dye, among which a bisazo dye and a trisazo dye are preferred.

[0049] The azo dye includes a compound represented by formula (I) (hereinafter sometimes referred to as "compound (I)"). K 1 (-N=NK 2 ) p -N=NK 3 (I) [In formula (I), K 1 and K 3 each independently represents a phenyl group which may have a substituent, a naphthyl group which may have a substituent, or a monovalent heterocyclic group which may have a substituent. 2 represents a p-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, or a divalent heterocyclic group which may have a substituent. p represents an integer of 1 to 4. When p is an integer of 2 or more, a plurality of K 2 may be the same or different. The -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO-, or -N=CH- bond as long as the compound exhibits absorption in the visible region.

[0050] Examples of the monovalent heterocyclic group include groups in which one hydrogen atom has been removed from a heterocyclic compound such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, benzoxazole, etc. Examples of the divalent heterocyclic group include groups in which two hydrogen atoms have been removed from the above-mentioned heterocyclic compounds.

[0051] K 1 and K 3 Phenyl, naphthyl and monovalent heterocyclic groups in 2 Examples of the substituent that the p-phenylene group, the naphthalene-1,4-diyl group, and the divalent heterocyclic group in the formula (I) may optionally have include an alkyl group having 1 to 4 carbon atoms; an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, or a butoxy group; a fluorinated alkyl group having 1 to 4 carbon atoms, such as a trifluoromethyl group; a cyano group; a nitro group; a halogen atom; and a substituted or unsubstituted amino group, such as an amino group, a diethylamino group, or a pyrrolidino group (the substituted amino group refers to an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. An unsubstituted amino group is -NH2).

[0052] Among the compounds (I), compounds represented by any one of formulas (I-1) to (I-8) are preferred, compounds represented by any one of formulas (I-1) to (I-3) are more preferred, and compounds represented by any one of formulas (I-1) and (I-3) are even more preferred. [ka] [In formulas (I-1) to (I-8), B 1 ~B 30 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the definitions of a substituted amino group and an unsubstituted amino group are as described above), a chlorine atom, or a trifluoromethyl group. n1 to n4 each independently represent an integer of 0 to 3. When n1 is 2 or more, multiple B 2 may be the same or different, and when n2 is 2 or more, a plurality of B 6 may be the same or different, and when n3 is 2 or more, a plurality of B 9 may be the same or different, and when n4 is 2 or more, a plurality of B 14 may be the same or different.] [ka] [In formula (I-9), R 1 ~R 8 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.

[0053] The oxazone dye is preferably a compound represented by formula (I-10). [ka] [In formula (I-10), R9 ~R 15 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.

[0054] The acridine dye is preferably a compound represented by formula (I-11). [ka] [In formula (I-11), R 16 ~R 23 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.

[0055] In the above formulas (I-9), (I-10), and (I-11), R x Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a toluyl group, a xylyl group, and a naphthyl group.

[0056] As the cyanine dye, the compounds represented by formula (I-12) and formula (I-13) are preferred. [ka] [In formula (I-12), D 1 and D. 2 represent, independently of each other, a group represented by any one of formulae (I-12a) to (I-12d). [ka] n5 represents an integer from 1 to 3. [ka] [In formula (I-13), D 3 and D. 4 represent, independently of each other, a group represented by any one of formulas (I-13a) to (I-13h). [ka] n6 represents an integer from 1 to 3.

[0057] Among these dichroic dyes, azo dyes are preferred from the viewpoint of alignment.

[0058] The polarizing plate 11A is provided with a horizontally aligned optically absorptive anisotropic film A having a dichroic dye compound A, and the polarizing plate 11B is provided with a horizontally aligned optically absorptive anisotropic film B having a dichroic dye compound B different from the dichroic dye compound A. The absorption axis direction and maximum absorption wavelength of the horizontally aligned optically absorptive anisotropic film A are different from the absorption axis direction and maximum absorption wavelength of the horizontally aligned optically absorptive anisotropic film B. In the example of FIG. 1, the absorption axis direction of the polarizing plate 11A is 90°±5°, and the maximum absorption wavelength is, for example, 600 nm to 680 nm. The absorption axis direction of the polarizing plate 11B is 0°±5°, and the maximum absorption wavelength is 500 nm to 580 nm.

[0059] The maximum absorption wavelength of a horizontally aligned optically absorptive anisotropic film can be determined by dissolving the dichroic dye compound contained in the horizontally aligned optically absorptive anisotropic film in a solvent to prepare a measurement sample, measuring the absorption spectrum of the measurement sample using an ultraviolet-visible spectrophotometer, and measuring the wavelength at which the maximum absorbance occurs from the obtained absorption spectrum.

[0060] The horizontally aligned optically absorptive anisotropic film can be formed by applying an optically absorptive anisotropic film-forming composition containing a dichroic dye compound onto an alignment film and drying it. The application method can be the same as the application method of the composition for forming an alignment film described above. The content of the dichroic dye compound in the optically absorptive anisotropic film-forming composition is preferably 0.1 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, even more preferably 0.1 to 10 parts by mass, and particularly preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the solid content of the optically absorptive anisotropic film-forming composition, from the viewpoint of improving the alignment of the dichroic dye. Here, the solid content is the total amount of components excluding the solvent from the optically absorptive anisotropic film-forming composition.

[0061] The light absorbing anisotropic film forming composition constituting at least one of the dichroic dye compound A and the dichroic dye compound B, preferably both, may contain a polymerizable liquid crystal compound, a solvent, a polymerization initiator, a sensitizer, a polymerization inhibitor, a leveling agent, and a polymerizable non-liquid crystal compound. In a horizontally aligned light absorbing anisotropic film containing a polymerizable liquid crystal compound, the strength is improved and color unevenness is reduced. When the light absorbing anisotropic film forming composition contains a polymerizable liquid crystal compound, the light absorbing anisotropic film forming composition may be dried to obtain a dried film, which is then cured. Curing refers to polymerizing the polymerizable liquid crystal compound contained in the dried film. Examples of polymerization methods include heating and light irradiation. The orientation state of the dichroic dye contained in the dried film can be fixed by curing.

[0062] The polymerizable liquid crystal compound is a compound having a polymerizable group and exhibiting liquid crystallinity. The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. The photopolymerizable group is a group that can undergo a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Examples of the compound exhibiting liquid crystallinity include a thermotropic liquid crystal and a lyotropic liquid crystal, and the thermotropic liquid crystal is preferred in terms of the ability to precisely control the film thickness. The compound exhibiting liquid crystallinity may be a nematic liquid crystal or a smectic liquid crystal in a thermotropic liquid crystal.

[0063] The polymerizable liquid crystal compound is preferably a liquid crystal compound that forms a smectic phase from the viewpoint of obtaining higher polarization characteristics. Examples of the smectic phase include smectic B phase, smectic D phase, smectic E phase, smectic F phase, smectic G phase, smectic H phase, smectic I phase, smectic J phase, smectic K phase, and smectic L phase, and smectic B phase, smectic F phase, or smectic I phase is preferable, and smectic B phase is more preferable. These smectic phases may be higher-order smectic phases.

[0064] When the liquid crystal phase formed by the polymerizable liquid crystal compound is one of these higher order smectic phases, a horizontally aligned optically absorptive anisotropic film with higher alignment order can be obtained. In the horizontally aligned optically absorptive anisotropic film with a high degree of alignment order, a Bragg peak derived from a higher order structure such as a hexatic phase or a crystalline phase is obtained in X-ray diffraction measurement. The Bragg peak is a peak derived from the periodic structure of molecular alignment. When the liquid crystal phase formed by the polymerizable liquid crystal compound is one of these higher order smectic phases, a horizontally aligned optically absorptive anisotropic film with a periodic interval of molecular alignment of, for example, 3.0 Å to 6.0 Å can be obtained.

[0065] Examples of the polymerizable liquid crystal compound include a compound represented by the following formula (B1) and a polymer of the compound (hereinafter, the compound and the polymer are collectively referred to as "polymerizable liquid crystal compound (B1)"). U 1 -V 1 -W 1 -X 1 -Y 1 -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (B1) [In formula (B1), X 1 , X 2 and X 3 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. A hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. However, X 1 , X 2 and X 3 At least one of Y is an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group. 1 and Y 2 are each independently a single bond or a divalent linking group. 1 represents a hydrogen atom or a polymerizable group. 2 represents a polymerizable group. 1 and W 2 are each independently a single bond or a divalent linking group. 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH2- constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or NH-.]

[0066] In the polymerizable liquid crystal compound (B1), X 1, X 2 and X 3 At least one of X is an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group. 1 and X 3 is preferably a cyclohexane-1,4-diyl group which may have a substituent, and the cyclohexane-1,4-diyl group is more preferably a trans-cyclohexane-1,4-diyl group. Examples of the optional substituent of the 1,4-phenylene group which may have a substituent or the cyclohexane-1,4-diyl group which may have a substituent include an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, and a butyl group, a cyano group, and a halogen atom such as a chlorine atom or a fluorine atom. It is preferably unsubstituted. Also, Y 1 and Y 2 If X is the same structure, 1 , X 2 and X 3 It is preferable that at least one of X has a different structure. 1 , X 2 and X 3 When at least one of the above has a different structure, smectic liquid crystallinity tends to be easily exhibited.

[0067] Y 1 and Y 2 are each independently -CH2CH2-, -CH2O-, -CH2CH2O-, -COO-, -OCOO-, a single bond, -N=N-, -CR a =CR b -, -C≡C-, -CR a =N- or CO-NR a - is preferred. a and R b each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 is more preferably -CH2CH2-, -COO-, or a single bond, and Y 2 More preferably, X is -CH2CH2- or CH2O-. 1 , X 2 and X 3If all have the same structure, Y 1 and Y 2 It is preferable that Y have different structures. 1 and Y 2 When the structures are different from each other, smectic liquid crystallinity tends to be easily exhibited.

[0068] U 2 is a polymerizable group. 1 is a hydrogen atom or a polymerizable group, and is preferably a polymerizable group. 1 and U 2 are preferably both polymerizable groups, and more preferably both photopolymerizable groups. The photopolymerizable group means a group that can be involved in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator described later.

[0069] U 1 and a photopolymerizable group represented by U 2 The polymerizable groups represented by may be different from each other, but are preferably the same type of group. Examples of the polymerizable group include vinyl group, vinyloxy group, 1-chlorovinyl group, isopropenyl group, 4-vinylphenyl group, acryloyloxy group, methacryloyloxy group, oxiranyl group, and oxetanyl group. Among them, radical polymerizable groups are preferred, acryloyloxy group, methacryloyloxy group, vinyl group, and vinyloxy group are more preferred, acryloyloxy group and methacryloyloxy group are even more preferred, and acryloyloxy group is particularly preferred.

[0070] V 1 and V 2 Examples of the alkanediyl group represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group, and an icosane-1,20-diyl group. 1 and V 2is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms.

[0071] Examples of the substituent that the alkanediyl group may optionally have include a cyano group and a halogen atom. The alkanediyl group is preferably unsubstituted, and more preferably an unsubstituted, linear alkanediyl group.

[0072] W 1 and W 2 are each independently preferably a single bond, -O-, -S-, -COO-, or -OCOO-, and more preferably a single bond or -O-.

[0073] Examples of the polymerizable liquid crystal compound (B1) include compounds represented by the following formulae (B-1) to (B-25). When the polymerizable liquid crystal compound (B1) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans form. [ka] [ka] [ka] [ka] [ka]

[0074] Among these, at least one selected from the group consisting of compounds represented by formula (B-2), formula (B-3), formula (B-4), formula (B-5), formula (B-6), formula (B-7), formula (B-8), formula (B-13), formula (B-14), formula (B-15), formula (B-16), and formula (B-17) is preferred.

[0075] The exemplified polymerizable liquid crystal compounds can be used alone or in combination. When two or more polymerizable liquid crystal compounds are combined, it is preferable that at least one of them is a polymerizable liquid crystal compound, and more preferable that two or more of them are polymerizable liquid crystal compounds. By combining them, liquid crystallinity may be temporarily maintained even at a temperature below the liquid crystal-crystal phase transition temperature. When two polymerizable liquid crystal compounds are combined, the mixing ratio is usually 1:99 to 50:50, preferably 5:95 to 50:50, and more preferably 10:90 to 50:50.

[0076] The polymerizable liquid crystal compound can be produced by a known method such as that described in Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996) and Japanese Patent No. 4719156.

[0077] The content of the polymerizable liquid crystal compound in the solid content of the composition for forming an optically absorptive anisotropic film is preferably 50% by mass or more, more preferably 70% by mass or more, and preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less. In this specification, the solid content in the composition for forming an optically absorptive anisotropic film refers to the total amount of components excluding volatile components such as solvents from the composition for forming an optically absorptive anisotropic film.

[0078] Examples of the solvent include the same solvents as those described in the "Orientable polymer composition" section, and the content of the solvent is preferably 100 to 1900 parts by mass, more preferably 150 to 900 parts by mass, and even more preferably 180 to 600 parts by mass, relative to 100 parts by mass of the composition for forming an optically absorptive anisotropic film.

[0079] As the polymerization initiator, a photopolymerization initiator is preferable. As the photopolymerization initiator, a photopolymerization initiator having light absorption at a wavelength of 300 nm to 380 nm is usually used. The photopolymerization initiator is a compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound, and can initiate a polymerization reaction at a lower temperature. Specifically, a photopolymerization initiator capable of generating active radicals or acids by the action of absorbed light can be mentioned, and among them, a photopolymerization initiator that generates radicals by the action of light is preferable.

[0080] Examples of the photopolymerization initiator include benzoin compounds, benzophenone compounds, alkylphenone compounds, acylphosphine oxide compounds, triazine compounds, iodonium salts, and sulfonium salts. These polymerization initiators can be used alone or in combination.

[0081] Benzoin compounds include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether. Benzophenone compounds include benzophenone, o-benzoyl methyl benzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.

[0082] Examples of alkylphenone compounds include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethan-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.

[0083] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0084] The triazine compounds include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethenyl] ]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine.

[0085] Commercially available photopolymerization initiators can be used. Commercially available photopolymerization initiators include "Irgacure (registered trademark) 907", "Irgacure (registered trademark) 184", "Irgacure (registered trademark) 651", "Irgacure (registered trademark) 819", "Irgacure (registered trademark) 250", "Irgacure (registered trademark) 369" (Ciba Japan Co., Ltd.); "Seikuol (registered trademark) BZ", "Seikuol (registered trademark) Z", "Seikuol (registered trademark) 100", "Seikuol (registered trademark) 200", "Seikuol (registered trademark) 1 ... Examples of such compounds include "Kayacure (registered trademark) BEE" (Seiko Chemical Co., Ltd.); "Kayacure (registered trademark) BP100" (Nippon Kayaku Co., Ltd.); "Kayacure (registered trademark) UVI-6992" (Dow Chemicals); "ADEKA Optomer SP-152", "ADEKA Optomer SP-170" (ADEKA Corporation); "TAZ-A", "TAZ-PP" (Nippon SiberHegner Co., Ltd.); and "TAZ-104" (Sanwa Chemical Co., Ltd.).

[0086] The content of the polymerization initiator can be appropriately adjusted according to the type and amount of the polymerizable liquid crystal compound contained in the composition for forming an optically absorptive anisotropic film, but is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, and is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization initiator is equal to or more than the above lower limit, the polymerizable liquid crystal compound can be polymerized without disturbing the alignment. When the content of the polymerization initiator is equal to or less than the above upper limit, the long-term storage stability can be improved, and the occurrence of alignment defects in the obtained polarizing film can be more easily suppressed or prevented.

[0087] The sensitizer is preferably a photosensitizer. Examples of the photosensitizer include xanthone compounds such as xanthone and thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and alkoxy group-containing anthracene (e.g., dibutoxyanthracene); phenothiazine and rubrene. The sensitizer can be used alone or in combination of two or more kinds.

[0088] When the composition for forming an optically absorptive anisotropic film contains a sensitizer, the polymerization reaction of the polymerizable liquid crystal compound contained in the composition can be further promoted. The amount of the sensitizer used can be appropriately adjusted depending on the type and amount of the polymerization initiator and the polymerizable liquid crystal compound, but is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.

[0089] In order to make the polymerization reaction of the composition for forming an optically absorptive anisotropic film proceed more stably, the composition may contain an appropriate amount of a polymerization inhibitor, which makes it easier to control the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound.

[0090] Examples of the polymerization inhibitor include radical scavengers such as hydroquinone, alkoxy group-containing hydroquinone, alkoxy group-containing catechol (for example, butylcatechol, etc.), pyrogallol, and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenols; β-naphthylamines, and β-naphthols.

[0091] When the composition for forming an optically absorptive anisotropic film contains a polymerization inhibitor, its content can be appropriately adjusted depending on the type and amount of the polymerizable liquid crystal compound, the amount of the sensitizer used, etc., but is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. If the content of the polymerization inhibitor is within this range, the polymerizable liquid crystal compound can be polymerized without disturbing the alignment.

[0092] The optically absorptive anisotropic film-forming composition may contain one or more leveling agents. The leveling agent has the function of adjusting the fluidity of the optically absorptive anisotropic film-forming composition and making the coating film obtained by applying the composition flatter, and specifically includes a surfactant. As the leveling agent, at least one selected from the group consisting of a leveling agent mainly composed of a polyacrylate compound and a leveling agent mainly composed of a fluorine atom-containing compound is preferable.

[0093] Leveling agents based on polyacrylate compounds include "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-358N", "BYK-361N", "BYK-380", "BYK-381" and "BYK-392" [BYK Chemie].

[0094] Leveling agents containing fluorine-containing compounds as the main component include "Megafac (registered trademark) R-08", "R-30", "R-90", "F-410", "F-411", "F-443", "F-445", "F-470", "F-471", "F-477", "F-479", "F-482" and "F-483" [DIC Corporation]; "Surflon (registered trademark) S-381" and "S-3 Examples of such compounds include "82", "S-383", "S-393", "SC-101", "SC-105", "KH-40" and "SA-100" [AGC Seimi Chemical Co., Ltd.]; "E1830", "E5844" [Daikin Fine Chemical Research Institute Ltd.]; "F-TOP EF301", "F-TOP EF303", "F-TOP EF351" and "F-TOP EF352" [Mitsubishi Materials Electronic Chemicals Co., Ltd.].

[0095] When the composition for forming an optically absorptive anisotropic film contains a leveling agent, the content thereof is preferably 0.05 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, the obtained polarizing film tends to be smoother and less prone to unevenness.

[0096] <Polarizing film> The horizontally aligned optically absorbing anisotropic film A and the horizontally aligned optically absorbing anisotropic film B used in the laminate of the present disclosure function as a polarizing film (hereinafter, also simply referred to as "polarizing film"). The polarizing film is a film having a polarizing function, and preferably has a dichroic dye encapsulated in an aligned polymerizable liquid crystal. The polarizing film used in the laminate of the present disclosure is preferably formed from the polarizing film-forming composition, has little or no alignment defects, and has excellent polarizing performance.

[0097] The polarizing film used in the laminate of the present disclosure can be produced, for example, by a method including a step (ii) of forming a coating film of the composition for forming a polarizing film, and drying and removing the organic solvent from the coating film, and a step (iii) of aligning and curing the polymerizable liquid crystal compound in a smectic liquid crystal phase state.

[0098] In step (ii), the composition for forming a polarizing film is applied onto the substrate, alignment film, or other layer (e.g., functional layer) to form a coating film, and the organic solvent is removed by drying under conditions in which the polymerizable liquid crystal compound contained in the resulting coating film does not polymerize, to obtain a dry film. The polarizing film may be directly applied onto the substrate or other layer (e.g., functional layer), but is preferably applied onto an alignment film having alignment regularity.

[0099] In step (ii), the drying method includes natural drying, ventilation drying, heat drying and reduced pressure drying. When the polymerizable liquid crystal compound is a polymerizable smectic liquid crystal compound, it is preferable to make the liquid crystal state of the polymerizable smectic liquid crystal compound contained in the dried film a nematic phase (nematic liquid crystal state) and then transition to a smectic phase. In order to form a smectic phase via a nematic phase, for example, a method is adopted in which the dried film is heated to a temperature at which the polymerizable smectic liquid crystal compound contained in the dried film transitions to a nematic liquid crystal state or higher, and then cooled to a temperature at which the polymerizable smectic liquid crystal compound shows a smectic liquid crystal state.

[0100] Step (iii) is a step of orienting and curing the polymerizable liquid crystal compound in the dried film in the state of a smectic liquid crystal phase. Hereinafter, a method of photopolymerizing the polymerizable liquid crystal compound while maintaining the liquid crystal state of the smectic phase after the liquid crystal state of the polymerizable liquid crystal compound in the dried film is changed to a smectic phase in step (ii) will be described. In the photopolymerization, the light irradiated to the dried film is appropriately selected according to the type of photopolymerization initiator contained in the dried film, the type of polymerizable liquid crystal compound (particularly, the type of photopolymerizable group possessed by the polymerizable liquid crystal compound) and the amount thereof.

[0101] Specific examples of the light include at least one light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays, and γ-rays, and active electron beams. Among them, ultraviolet light is preferred because it is easy to control the progress of the polymerization reaction and photopolymerization devices widely used in the field can be used. It is preferable to select the type of polymerizable liquid crystal compound and photopolymerization initiator contained in the polymerizable liquid crystal composition so that the composition can be photopolymerized by ultraviolet light. In addition, the polymerization temperature can be controlled by irradiating the dried film with light while cooling it with an appropriate cooling means during polymerization. By adopting such a cooling means, if the polymerization of the polymerizable liquid crystal compound is carried out at a lower temperature, a polarizing film can be appropriately formed even if a substrate having a relatively low heat resistance is used. During photopolymerization, a patterned polarizing film can also be obtained by performing masking or development.

[0102] Examples of the light source of the active energy rays include a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, and a metal halide lamp.

[0103] The UV irradiation intensity is usually 10 to 3,000 mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photopolymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 to 3,000 mJ / cm. 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 It is.

[0104] By carrying out photopolymerization, the polymerizable liquid crystal compound is polymerized while maintaining the liquid crystal state of the smectic phase, preferably the high-order smectic phase, to form a polarizing film. The polarizing film obtained by polymerizing the polymerizable liquid crystal compound while maintaining the liquid crystal state of the smectic phase has an advantage of having higher polarization performance due to the action of the dichroic dye, compared to conventional host-guest type polarizing films, i.e., polarizing films made of a liquid crystal state of a nematic phase. Furthermore, it has an advantage of having superior strength compared to films coated with only a dichroic dye or a lyotropic liquid crystal.

[0105] The thickness of the polarizing film can be appropriately selected depending on the display device to which it is applied, and is preferably 0.1 to 5 μm, more preferably 0.3 to 4 μm, and further preferably 0.5 to 3 μm.

[0106] The composition for forming a polarizing film used in the present disclosure has excellent long-term storage stability and can be used after long-term storage. Therefore, in step (ii), the composition for forming a polarizing film after storage may be used. When the composition for forming a polarizing film after storage is used, it is preferable to further perform step (i) from the viewpoint of effectively suppressing or preventing alignment defects in the resulting polarizing film.

[0107] Step (i) is a step of storing the composition for forming a polarizing film. In step (i), the storage temperature is preferably 15 to 35°C, more preferably 20 to 30°C. The composition for forming a polarizing film is usually stored in a sealed state so that the organic solvent does not evaporate. The container containing the composition for forming a polarizing film can be shielded, but the composition for forming a polarizing film used in the present disclosure has excellent long-term storage stability even without shielding, especially because the dichroic dye in the composition can absorb ultraviolet light (wavelength 380 nm) that can generate radicals caused by the photopolymerization initiator.

[0108] The retardation plate 12 is a member having a function as, for example, a quarter-wave plate. The retardation plate 12 is formed by, for example, laminating a photo-alignment film and a retardation film on a glass substrate. The retardation plate 12 has a phase difference of π / 2 and a slow axis in an orientation of 45°±5° with respect to the absorption axes of the dichroic dye compound A and the dichroic dye compound B. The retardation plate 12 preferably has optical characteristics represented by the following formula (1), more preferably satisfies the following formula (1) and has optical characteristics represented by the following formulas (2), (4), and (5), and further preferably satisfies the following formula (1) and has optical characteristics represented by the following formulas (3), (4), and (5). In the following formulas (1) to (5), Re(λ) is a front retardation value for light having a wavelength of λ nm. Re(450) <Re(550)<Re(650)…(1) 100nm <Re(550)<160nm …(2) 130nm <Re(550)<150nm …(3) Re(450) / Re(550)≦1.00 …(4) 1.00≦Re(650) / Re(550) …(5)

[0109] The front retardation value is determined by the following formula (6). In formula (6), d represents the thickness, and Δn(λ) represents the birefringence at a wavelength of λ nm. In order to obtain a desired front retardation value, d and Δn(λ) should be adjusted. By adjusting the front retardation value, the retardation plate 12 can be obtained as a quarter-wave plate. Re(λ)=d×Δn(λ) …(6)

[0110] In the display device 1A having the above configuration, white light L output from the light source 2 is input to the retardation plate 12. The white light L input to the retardation plate 12 becomes light whose vibration direction is aligned with the slow axis direction of the retardation plate 12, and is input to the polarizing plate 11B and the polarizing plate 11A in this order. The light output from the polarizing plate 11A through the polarizing plate 11B contains light La of a hue corresponding to the dichroic dye compound A of the polarizing plate 11A in the absorption axis direction of the polarizing plate 11B (0°±5° in this case), and contains light Lb of a hue corresponding to the dichroic dye compound B of the polarizing plate 11B in the absorption axis direction of the polarizing plate 11A (90°±5° in this case).

[0111] As described above, the laminate 3 applied to the display device 1A combines horizontally aligned optically absorptive anisotropic films A and B having different absorption axis directions and maximum absorption wavelengths. Therefore, when white light L is input to the laminate 3 as one pixel, light La and Lb of different hues can be output from one pixel according to the absorption axis directions of the horizontally aligned optically absorptive anisotropic films A and B. Therefore, for example, by arranging the laminate 3 so that the absorption axis directions of the horizontally aligned optically absorptive anisotropic films A and B are different for each pixel, a three-dimensional display can be easily realized.

[0112] In this embodiment, the dichroic dye compound A and the dichroic dye compound B are each selected from different hues in the group of cyan, magenta, and yellow, or the group of red, green, and blue. Alternatively, the dichroic dye compound A and the dichroic dye compound B are each selected from different hues in the group of cyan, magenta, and yellow, or the group of red, green, and blue, by two kinds. This allows sufficient parallax to be generated in the light output from the laminate 3. Therefore, three-dimensional display can be realized more easily.

[0113] In this embodiment, both the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B are cured products of optically absorptive anisotropic film-forming compositions having a polymerizable liquid crystal compound. This allows the alignment state of the dichroic dye compound to be suitably fixed. In this embodiment, the polymerizable liquid crystal compound in at least one or both of the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B is a liquid crystal compound that forms a smectic phase. This allows for higher polarization characteristics to be obtained.

[0114] In this embodiment, a retardation plate 12 having a phase difference of π / 2 and a slow axis in an orientation of 45°±5° with respect to the absorption axes of the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B is further provided. By combining the retardation plate 12, the function of the laminate 3 is expanded. In this embodiment, the horizontally aligned optically absorptive anisotropic film A, the horizontally aligned optically absorptive anisotropic film B, and the retardation plate 12 are laminated in this order in the laminate 3. This allows the retardation plate 12 to function as an anti-reflection film for light input from the horizontally aligned optically absorptive anisotropic film A.

[0115] In this embodiment, the front retardation value Re(λ) of the retardation plate 12 satisfies the above formula (1), thereby obtaining a retardation plate 12 having desired optical characteristics.

[0116] [Second embodiment] 2 is a schematic diagram showing the configuration of a display device according to a second embodiment of the present disclosure. As shown in FIG. 2, the display device 1B according to the second embodiment is different from the display device 1A according to the first embodiment in the arrangement position of the retardation plate 12 in the laminate 3. Specifically, in this embodiment, the retardation plate 12, the polarizing plate 11A (horizontally aligned optically absorptive anisotropic film A), and the polarizing plate 11B (dichroic dye compound B) are laminated in this order in the laminate 3 when viewed from the side opposite to the light source 2. That is, in this embodiment, the retardation plate 12 is arranged as the outermost surface of the display device 1B.

[0117] In the display device 1B having such a configuration, similarly to the display device 1A, when white light L is input to the laminate 3 as one pixel, light La, Lb of different hues can be output from one pixel according to the absorption axis directions of the horizontally aligned optically absorptive anisotropic films A, B. Therefore, for example, by arranging the laminate 3 so that the absorption axis directions of the horizontally aligned optically absorptive anisotropic films A, B are different from each other for each pixel, a three-dimensional display can be easily realized.

[0118] In the display device 1B, the light output from the polarizing plate 11A through the polarizing plate 11B, i.e., the light La and the light Lb having different hues, are both circularly polarized light by passing through the retardation plate 12. Therefore, even if the line of sight to the laminate 3 is tilted to some extent, the image can be viewed.

[0119] [Example] The present disclosure will be described in more detail below with reference to examples. In the following examples, "%" and "parts" are "mass%" and "parts by mass" unless otherwise specified. The configurations and evaluation results of the laminates in each example and comparative example are summarized in Figures 3 and 4.

[0120] [Production of polymerizable liquid crystal compounds] Polymerizable liquid crystal compounds (A-6) to (A-8) having the structures shown below were prepared. Polymerizable liquid crystal compounds (A-6) and (A-7) were prepared according to the method described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996). Polymerizable liquid crystal compound (A-8) was prepared in the same manner as described in JP-A-2010-31223. [ka] (A-6) [ka] (A-7) [ka] (A-8)

[0121] [Production of dichroic dye compounds] As the dichroic dye compound, azo dichroic dye compounds (D-1) to (D-3) having the structures shown below, which are described in the examples of JP2013-101328A, were used. [ka] (D-1) [ka] (D-2) [ka] (D-3)

[0122] [Measurement of maximum absorption wavelength of dichroic dye compounds] A solution was obtained as a measurement sample by dissolving 1 mg of a dichroic dye compound in 50 mL of chloroform. The measurement sample was placed in a measurement cell with an optical path length of 1 cm, and the measurement sample was set in an ultraviolet-visible spectrophotometer (UV-2450, manufactured by Shimadzu Corporation) to measure the absorption spectrum, and the wavelength at which the maximum absorbance was obtained was measured from the obtained absorption spectrum. The measurement results are shown in Table 1. [Table 1]

[0123] <Example 1> [Preparation of optically absorptive anisotropic film-forming composition (1)] The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming an optically absorptive anisotropic film (1). ·Polymerizable liquid crystal compound: (A-6) 75 parts ·Polymerizable liquid crystal compound: (A-7) 25 parts ·Dichroic dye: (D-1) 4.0 parts Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) 6 parts Leveling agent [polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)]: 1.2 parts Solvent: o-xylene 250 parts

[0124] [Preparation of optically absorptive anisotropic film-forming composition (2)] The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming an optically absorptive anisotropic film (2). ·Polymerizable liquid crystal compound: (A-6) 75 parts ·Polymerizable liquid crystal compound: (A-7) 25 parts ·Dichroic dye: (D-2) 4.0 parts Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) 6 parts Leveling agent [polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)]: 1.2 parts Solvent: o-xylene 250 parts

[0125] [Preparation of alignment film for polarizing plate] A glass substrate was used as the transparent substrate. A 2% by mass aqueous solution (composition for forming an alignment film) of polyvinyl alcohol (polyvinyl alcohol 1000 fully saponified type, manufactured by Wako Pure Chemical Industries, Ltd.) was applied onto the glass substrate by spin coating to form a dry film having a thickness of 100 nm. Subsequently, an alignment film was formed by subjecting the surface of the obtained film to a rubbing treatment. The rubbing treatment was performed using a semi-automatic rubbing device (product name: LQ-008 type, manufactured by Joyo Engineering Co., Ltd.) with a cloth (product name: YA-20-RW, manufactured by Yoshikawa Kako Co., Ltd.) under the conditions of a pressing amount of 0.15 mm, a rotation speed of 500 rpm, and 16.7 mm / s. A laminate (1) in which an alignment film was formed on the glass substrate was obtained by the rubbing treatment.

[0126] [Preparation of polarizing plate (1)] The optically absorptive anisotropic film-forming composition (1) was applied onto the alignment film of the laminate (1) by spin coating, and the composition was dried by heating on a hot plate at 120°C for 1 minute, and then quickly cooled to room temperature to form a dry film on the alignment film. The liquid crystal state of the polymerizable liquid crystal compound contained in this dry film was a smectic B phase. Next, ultraviolet light was irradiated at an exposure dose of 1000 mJ / cm using a UV irradiation device (Unicure VB-15201BY-A, manufactured by Ushio Inc.). 2 The dry film was irradiated with light of 365 nm (reference wavelength), which allowed the polymerizable liquid crystal compound contained in the dry film to polymerize while maintaining its liquid crystal state. This resulted in the production of a polarizing plate (1) consisting of a glass substrate / alignment film / horizontally aligned optically absorptive anisotropic film (1).

[0127] [Preparation of polarizing plate (2)] A polarizing plate (2) consisting of a glass substrate / alignment film / horizontally aligned optically absorptive anisotropic film (2) was obtained in the same manner as above, except that the optically absorptive anisotropic film-forming composition (2) was used.

[0128] [Preparation of composition for forming retardation film] The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming a retardation film. ·Polymerizable liquid crystal compound: (A-8) 100 parts Polymerization initiator: Irgacure OXE-03 (manufactured by Chiba Specialty Chemicals) 3 parts Leveling agent: 0.1 part polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) Solvent: Cyclopentanone 690 parts

[0129] [Preparation of photo-alignment film for retardation plate] A photo-alignment material (weight average molecular weight: 50,000, m:n = 50:50) having the structure shown below was produced in accordance with the method described in JP 2021-196514 A. Two parts of the photo-alignment material and 98 parts of cyclopentanone (solvent) were mixed as components, and the resulting mixture was stirred at 80°C for 1 hour to prepare a composition for forming a photo-alignment film for a retardation plate. [ka]

[0130] [Preparation of retardation plate] A glass substrate was used as the transparent substrate. A composition for forming a photo-alignment film for a retardation plate was applied onto the glass substrate by spin coating, and dried at 80°C for 1 minute to form a dry film. Next, the dry film was exposed to polarized UV light with an integrated light amount of 100 mJ / cm2 using a polarized UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.), to obtain a laminate (2) in which a photo-alignment film was formed on a glass substrate. The thickness of the photo-alignment film measured with a laser microscope (LEXT, manufactured by Olympus Corporation) was 100 nm.

[0131] The above-mentioned retardation film-forming composition was applied by spin coating onto the photo-alignment film of the laminate (2), and then heated and dried on a hot plate at 120°C for 1 minute, and then quickly cooled to room temperature to form a dry film on the photo-alignment layer. The liquid crystal state of the polymerizable liquid crystal compound contained in the dry film was a nematic phase. A high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.) was used to irradiate the dry film with ultraviolet light at an exposure dose of 500 mJ / cm2 (based on 365 nm) under a nitrogen atmosphere to form a retardation film, and a retardation plate consisting of a glass substrate / photo-alignment film / retardation film was obtained. The thickness of the retardation film measured using a laser microscope LEXTOLS4100 manufactured by Olympus Corporation was 2.0 μm.

[0132] [Laminated body production] The polarizing plate (1), polarizing plate (2), and retardation plate obtained as above were laminated to obtain laminates according to Examples 1 to 8. The polarizing plate (3), polarizing plate (4), and retardation plate obtained in a similar manner were laminated to obtain laminates according to Examples 9 to 12. The polarizing plate (5), polarizing plate (6), and retardation plate obtained in a similar manner were laminated to obtain laminates according to Examples 13 and 14. The polarizing plate (7) and retardation plate obtained in a similar manner were laminated to obtain laminates according to Comparative Examples 1 to 4. Details of the polarizing plates (3) to (7) will be described later.

[0133] [Appearance evaluation] The laminates according to Examples 1 to 14 and Comparative Examples 1 to 4 were placed on a backlight, and the hues of the laminates were visually observed through a polarizing plate having an absorption axis at 0° to the outermost polarizing plate, and similarly, the hues of the laminates were visually observed through a polarizing plate having an absorption axis at 90° to the outermost polarizing plate.

[0134] [Absorption spectrum measurement] The laminates according to Examples 1 to 14 and Comparative Examples 1 to 4 were set in an ultraviolet-visible spectrophotometer (UV-2450, manufactured by Shimadzu Corporation) so that the absorption axis of the outermost polarizing plate was oriented at 45° with respect to the incident light, and the absorption spectrum was measured. From the results of the absorption spectrum measurement, the maximum absorption wavelength λmax and half width of the laminates according to Examples 1 to 14 and Comparative Examples 1 to 4 were evaluated.

[0135] [Anti-reflective properties] The laminates according to Examples 1 to 14 and Comparative Examples 1 to 4 were placed on a plane mirror, and the laminates were visually observed from a distance of 50 cm to evaluate the antireflection properties. Those that displayed black and had good antireflection properties were marked with "○", those that displayed black but some light transmission was observed were marked with "△", and those that did not display black were marked with "×".

[0136] <Example 1> In Example 1, a laminate was prepared by laminating a polarizing plate (1), a polarizing plate (2), and a retardation plate in this order so that the absorption axis and the slow axis were as follows: The liquid crystal state of the polymerizable liquid crystal compound in the polarizing plate (1) and the polarizing plate (2) during the formation of the polarizing film (before photocuring) was a smectic B phase. Polarizing plate (1) 0° direction Polarizing plate (2) 90° direction ·Retardation plate 45° direction

[0137] In the appearance evaluation of Example 1, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (1), it exhibited a "blue" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (1), it exhibited a "red" color. From this result, it was confirmed that the laminate of Example 1 can output blue and red light per pixel, and that a three-dimensional display can be easily realized by arranging the laminate so that the absorption axis directions of the polarizing plate (1) and the polarizing plate (2) are different from each other for each pixel. In the spectrum measurement of Example 1, the maximum absorption wavelength was 582 nm and the half width was 124 nm. In addition, the antireflection property of Example 1 was "○".

[0138] <Example 2> In Example 2, a polarizing plate (1), a polarizing plate (2), and a retardation plate were laminated in this order to form a laminate so that the absorption axis and the slow axis were as follows. Polarizing plate (1) 90° direction Polarizing plate (2) 0° direction ·Retardation plate 45° direction

[0139] In the appearance evaluation of Example 2, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (1), it exhibited a "red" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (1), it exhibited a "blue" color. When the direction of polarization was confirmed using a UV-Vis spectrometer, it was confirmed that the light was circularly polarized in the opposite direction to that of Example 1. In the spectrum measurement of Example 2, the maximum absorption wavelength was 576 nm and the half-width was 122 nm. Furthermore, the antireflection property of Example 2 was "○".

[0140] <Example 3> In Example 3, a retardation plate, a polarizing plate (1), and a polarizing plate (2) were laminated in this order to form a laminate so that the absorption axis and the slow axis were as follows. Polarizing plate (1) 0° direction Polarizing plate (2) 90° direction ·Retardation plate 45° direction

[0141] In the appearance evaluation of Example 3, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (1), it exhibited a "blue" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (1), it exhibited a "red" color. In the spectrum measurement of Example 3, the maximum absorption wavelength was 578 nm and the half-width was 126 nm. In addition, the antireflection property of Example 3 was "x".

[0142] <Example 4> In Example 4, a retardation plate, a polarizing plate (1), and a polarizing plate (2) were laminated in this order to form a laminate so that the absorption axis and the slow axis were as follows. Polarizing plate (1) 90° direction Polarizing plate (2) 0° direction ·Retardation plate 45° direction

[0143] In the appearance evaluation of Example 4, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (1), it exhibited a "red" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (1), it exhibited a "blue" color. In the spectrum measurement of Example 4, the maximum absorption wavelength was 584 nm and the half-width was 122 nm. In addition, the antireflection property of Example 4 was "x".

[0144] <Example 5> In Example 5, a laminate was prepared by laminating a polarizing plate (2), a polarizing plate (1), and a retardation plate in this order so that the absorption axis and the slow axis were as follows. Polarizing plate (1) 90° direction Polarizing plate (2) 0° direction ·Retardation plate 45° direction

[0145] In the appearance evaluation of Example 5, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (1), it exhibited a "red" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (1), it exhibited a "blue" color. In the spectrum measurement of Example 5, the maximum absorption wavelength was 576 nm and the half-width was 122 nm. In addition, the antireflection property of Example 5 was "○".

[0146] <Example 6> In Example 6, a polarizing plate (2), a polarizing plate (1), and a retardation plate were laminated in this order to obtain a laminate having the following absorption axis and slow axis. Polarizing plate (1) 0° direction Polarizing plate (2) 90° direction ·Retardation plate 45° direction

[0147] In the appearance evaluation of Example 6, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (1), it exhibited a "blue" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (1), it exhibited a "red" color. In the spectrum measurement of Example 6, the maximum absorption wavelength was 582 nm and the half-width was 124 nm. In addition, the antireflection property of Example 6 was "○".

[0148] <Example 7> In Example 7, a retardation plate, a polarizing plate (2), and a polarizing plate (1) were laminated in this order to obtain a laminate having the following absorption axis and slow axis. Polarizing plate (1) 90° direction Polarizing plate (2) 0° direction ·Retardation plate 45° direction

[0149] In the appearance evaluation of Example 7, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (1), it exhibited a "red" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (1), it exhibited a "blue" color. In the spectrum measurement of Example 7, the maximum absorption wavelength was 584 nm and the half-width was 122 nm. In addition, the antireflection property of Example 7 was "x".

[0150] <Example 8> In Example 8, a retardation plate, a polarizing plate (2), and a polarizing plate (1) were laminated in this order to obtain a laminate having the following absorption axis and slow axis. Polarizing plate (1) 0° direction Polarizing plate (2) 90° direction ·Retardation plate 45° direction

[0151] In the appearance evaluation of Example 8, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (1), it exhibited a "blue" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (1), it exhibited a "red" color. In the spectrum measurement of Example 8, the maximum absorption wavelength was 578 nm and the half-width was 126 nm. In addition, the antireflection property of Example 8 was "x". [Production of polymerizable liquid crystal compounds] <Example 9>

[0152] In Example 9, a liquid crystal compound LC242 (registered trademark of BASF) represented by the following formula (LC242) was used as the polymerizable liquid crystal compound of the composition for forming an optically absorptive anisotropic film. [ka]

[0153] [Preparation of optically absorptive anisotropic film-forming composition (3)] The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming an optically absorptive anisotropic film (3). ·Polymerizable liquid crystal compound: LC242 100 parts ·Dichroic dye: (D-1) 4.0 parts Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) 6 parts Leveling agent [polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)]: 1.2 parts Solvent: o-xylene 250 parts

[0154] [Preparation of optically absorptive anisotropic film-forming composition (4)] The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming an optically absorptive anisotropic film (4). ·Polymerizable liquid crystal compound: LC242 100 parts ·Dichroic dye: (D-2) 4.0 parts Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) 6 parts Leveling agent [polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)]: 1.2 parts Solvent: o-xylene 250 parts

[0155] [Laminated body production] Similarly to Example 1, a polarizing plate (3) was prepared using the composition for forming an optically absorptive anisotropic film (3), and a polarizing plate (4) was prepared using the composition for forming an optically absorptive anisotropic film (4). In Example 9, a laminate was prepared by laminating the polarizing plate (3), the polarizing plate (4), and a retardation plate in this order so that the absorption axis and the slow axis were as follows. The liquid crystal state of the polymerizable liquid crystal compound in the polarizing plate (3) and the polarizing plate (4) during the formation of the polarizing film (before photocuring) was a nematic phase. Polarizing plate (3) 0° direction Polarizing plate (4) 90° direction ·Retardation plate 45° direction

[0156] In the appearance evaluation of Example 9, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (3), it exhibited a "blue" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (3), it exhibited a "red" color. In the spectrum measurement of Example 9, the maximum absorption wavelength was 526 nm and the half-width was 206 nm. In addition, the antireflection property of Example 9 was "△".

[0157] <Example 10> In Example 10, a polarizing plate (3), a polarizing plate (4), and a retardation plate were laminated in this order to obtain a laminate having the following absorption axis and slow axis. Polarizing plate (3) 90° direction Polarizing plate (4) 0° direction ·Retardation plate 45° direction

[0158] In the appearance evaluation of Example 10, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (3), it exhibited a "red" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (3), it exhibited a "blue" color. In the spectrum measurement of Example 10, the maximum absorption wavelength was 526 nm and the half-width was 206 nm. In addition, the antireflection property of Example 10 was "△".

[0159] <Example 11> In Example 11, a retardation plate, a polarizing plate (3), and a polarizing plate (4) were laminated in this order to obtain a laminate having the following absorption axis and slow axis. Polarizing plate (3) 0° direction Polarizing plate (4) 90° direction ·Retardation plate 45° direction

[0160] In the appearance evaluation of Example 11, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (3), it exhibited a "blue" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (3), it exhibited a "red" color. In the spectrum measurement of Example 11, the maximum absorption wavelength was 524 nm and the half-width was 184 nm. In addition, the antireflection property of Example 11 was "x".

[0161] <Example 12> In Example 12, a retardation plate, a polarizing plate (3), and a polarizing plate (4) were laminated in this order to obtain a laminate having the following absorption axis and slow axis. Polarizing plate (3) 90° direction Polarizing plate (4) 0° direction ·Retardation plate 45° direction

[0162] In the appearance evaluation of Example 12, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (3), it exhibited a "red" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (3), it exhibited a "blue" color. In the spectrum measurement of Example 12, the maximum absorption wavelength was 528 nm and the half-width was 208 nm. In addition, the antireflection property of Example 12 was "x".

[0163] <Example 13> [Preparation of optically absorptive anisotropic film-forming composition (5)] The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming an optically absorptive anisotropic film (5). ·Polymerizable liquid crystal compound: (A-6) 75 parts ·Polymerizable liquid crystal compound: (A-7) 25 parts ·Dichroic dye: (D-1) 2.5 parts ·Dichroic dye: (D-3) 2.5 parts Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) 6 parts Leveling agent [polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)]: 1.2 parts Solvent: o-xylene 250 parts

[0164] [Preparation of optically absorptive anisotropic film-forming composition (6)] The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming an optically absorptive anisotropic film (6). ·Polymerizable liquid crystal compound: (A-6) 75 parts ·Polymerizable liquid crystal compound: (A-7) 25 parts ·Dichroic dye: (D-2) 2.5 parts ·Dichroic dye: (D-3) 2.5 parts Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) 6 parts Leveling agent [polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)]: 1.2 parts Solvent: o-xylene 250 parts

[0165] [Laminated body production] Similarly to Example 1, a polarizing plate (5) was prepared using the composition for forming an optically absorptive anisotropic film (5), and a polarizing plate (6) was prepared using the composition for forming an optically absorptive anisotropic film (6). In Example 13, a laminate was prepared by laminating a polarizing plate (5), a polarizing plate (6), and a retardation plate in this order so that the absorption axis and slow axis were as follows. The liquid crystal state of the polymerizable liquid crystal compound in the polarizing plate (5) and the polarizing plate (6) during the formation of the polarizing film (before photocuring) was a smectic B phase. Polarizing plate (5) 90° direction Polarizing plate (6) 0° direction ·Retardation plate 45° direction

[0166] In the appearance evaluation of Example 13, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (5), it exhibited a "green" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (5), it exhibited an "orange" color. In the spectrum measurement of Example 13, the maximum absorption wavelength was 580 nm and the half-width was 146 nm. In addition, the antireflection property of Example 13 was "○".

[0167] <Example 14> In Example 14, a polarizing plate (5), a polarizing plate (6), and a retardation plate were laminated in this order to obtain a laminate having the following absorption axis and slow axis. Polarizing plate (5) 0° direction Polarizing plate (6) 90° direction ·Retardation plate 45° direction

[0168] In the appearance evaluation of Example 14, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (5), it exhibited an "orange color," and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (5), it exhibited a "green color." In the spectrum measurement of Example 14, the maximum absorption wavelength was 586 nm and the half-width was 164 nm. In addition, the antireflection property of Example 14 was "○."

[0169] <Comparative Example 1> [Preparation of composition for forming polarizing film] The following components were mixed and stirred at 80° C. for 1 hour to obtain a composition for forming a polarizing film. ·Polymerizable liquid crystal compound: (A-6) 75 parts ·Polymerizable liquid crystal compound: (A-7) 25 parts ·Dichroic dye: (D-1) 2.5 parts ·Dichroic dye: (D-2) 2.5 parts ·Dichroic dye: (D-3) 2.5 parts Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) 6 parts Leveling agent [polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)]: 1.2 parts Solvent: o-xylene 250 parts

[0170] [Laminated body production] A polarizing plate (7) was produced using a polarizing film-forming composition in the same manner as in Example 1. The liquid crystal state of the polymerizable liquid crystal compound in the polarizing plate (7) during the formation of the polarizing film (before photocuring) was a smectic B phase. In Comparative Example 1, the polarizing plate (7) and the retardation plate were laminated in this order to form a laminate with the following absorption axis and slow axis: Polarizing plate (7) 0° direction ·Retardation plate 45° direction

[0171] In the appearance evaluation of Comparative Example 1, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (7), it exhibited a "black" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (7), it exhibited a "colorless" color. From this result, it was confirmed that the laminate of Comparative Example 1 was unable to output light of different hues per pixel. In the spectrum measurement of Comparative Example 1, the maximum absorption wavelength was 600 nm, and the half-width was >350 nm. In addition, the antireflection property of Comparative Example 1 was "○".

[0172] <Comparative Example 6> In Comparative Example 2, a polarizing plate (7) and a retardation plate were laminated in this order to obtain a laminate having the following absorption axis and slow axis. Polarizing plate (7) 90° direction ·Retardation plate 45° direction

[0173] In the appearance evaluation of Comparative Example 2, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (7), it appeared "colorless", and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (7), it appeared "black". In the spectrum measurement of Comparative Example 2, the maximum absorption wavelength was 600 nm and the half-width was >350 nm. In addition, the antireflection property of Comparative Example 2 was "○".

[0174] <Comparative Example 3> In Comparative Example 3, a retardation plate and a polarizing plate (7) were laminated in this order to form a laminate so that the absorption axis and the slow axis were as follows. Polarizing plate (7) 0° direction ·Retardation plate 45° direction

[0175] In the appearance evaluation of Comparative Example 3, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (7), it exhibited a "black" color, and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (7), it exhibited a "colorless" color. In the spectrum measurement of Comparative Example 3, the maximum absorption wavelength was 600 nm, and the half-width was >350 nm. In addition, the antireflection property of Comparative Example 3 was "x".

[0176] <Comparative Example 4> In Comparative Example 4, a polarizing plate (7) and a retardation plate were laminated in this order to obtain a laminate having the following absorption axis and slow axis. Polarizing plate (7) 0° direction ·Retardation plate 45° direction

[0177] In the appearance evaluation of Comparative Example 4, when observed through a polarizing plate having an absorption axis in the 0° direction relative to the polarizing plate (7), it appeared "colorless", and when observed through a polarizing plate having an absorption axis in the 90° direction relative to the polarizing plate (7), it appeared "black". In the spectrum measurement of Comparative Example 4, the maximum absorption wavelength was 600 nm and the half-width was >350 nm. In addition, the antireflection property of Comparative Example 2 was "x".

[0178] The gist of the present disclosure is as follows: [1] to

[11] . [1] A laminate comprising a horizontally aligned optically absorptive anisotropic film A having a dichroic dye compound A and a horizontally aligned optically absorptive anisotropic film B having a dichroic dye compound B, wherein the absorption axis direction and maximum absorption wavelength in the horizontally aligned optically absorptive anisotropic film A are different from the absorption axis direction and maximum absorption wavelength in the horizontally aligned optically absorptive anisotropic film B. [2] The laminate according to [1], wherein the dichroic dye compound A and the dichroic dye compound B are each selected from different hues selected from the group consisting of cyan, magenta, and yellow, or the group consisting of red, green, and blue. [3] The laminate according to [1] or [2], wherein the dichroic dye compound A and the dichroic dye compound B are each two kinds selected from different hues in the group of cyan, magenta, and yellow or the group of red, green, and blue. [4] The laminate according to any one of [1] to [3], wherein the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B are both cured products of optically absorptive anisotropic film-forming compositions having a polymerizable liquid crystal compound. [5] The laminate according to any one of [1] to [4], wherein in at least one of the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B, the polymerizable liquid crystal compound is a liquid crystal compound that forms a smectic phase. [6] The laminate according to any one of [1] to [5], wherein in both the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B, the polymerizable liquid crystal compound is a liquid crystal compound that forms a smectic phase. [7] The laminate according to any one of [1] to [6], further comprising a retardation plate having a phase difference of π / 2 and a slow axis in an orientation of 45°±5° with respect to each of the absorption axes of the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B. [8] The laminate according to [7], wherein a front retardation value Re(λ) of the retardation plate satisfies the following formula (1): Re(450) <Re(550)<Re(650)…(1) [9] The laminate according to either [7] or [8], wherein the horizontally aligned optically absorptive anisotropic film A, the horizontally aligned optically absorptive anisotropic film B, and the retardation plate are laminated in this order.

[10] The laminate according to [7] or [8], wherein the retardation plate, the horizontally aligned optically absorptive anisotropic film A, and the horizontally aligned optically absorptive anisotropic film B are laminated in this order.

[11] A display device comprising the laminate according to any one of [1] to

[10] and a light source that outputs light toward the laminate. [Explanation of symbols]

[0179] 1A, 1B... display device, 2... light source, 3... laminate, 11A, 11B... laminate plate, 12... retardation plate.

Claims

1. The present invention includes a horizontally aligned optically absorptive anisotropic film A having a dichroic dye compound A, and a horizontally aligned optically absorptive anisotropic film B having a dichroic dye compound B, A laminate, wherein the absorption axis direction and the maximum absorption wavelength in the horizontally aligned optically absorptive anisotropic film A are different from the absorption axis direction and the maximum absorption wavelength in the horizontally aligned optically absorptive anisotropic film B.

2. 2. The laminate according to claim 1, wherein the dichroic dye compound A and the dichroic dye compound B are each selected from different hues selected from the group of cyan, magenta, and yellow or the group of red, green, and blue.

3. 2. The laminate according to claim 1, wherein the dichroic dye compound A and the dichroic dye compound B are each two kinds selected from different hues in the group of cyan, magenta, and yellow or the group of red, green, and blue.

4. 2. The laminate according to claim 1, wherein the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B are both cured products of optically absorptive anisotropic film-forming compositions containing a polymerizable liquid crystal compound.

5. 5. The laminate according to claim 4, wherein in at least one of the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B, the polymerizable liquid crystal compound is a liquid crystal compound that forms a smectic phase.

6. 5. The laminate according to claim 4, wherein in both the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B, the polymerizable liquid crystal compound is a liquid crystal compound that forms a smectic phase.

7. The laminate according to claim 1, further comprising a retardation plate having a phase difference of π / 2 and a slow axis in an orientation of 45°±5° with respect to each of the absorption axes of the horizontally aligned optically absorptive anisotropic film A and the horizontally aligned optically absorptive anisotropic film B.

8. The laminate according to claim 7 , wherein the front retardation value Re(λ) of the retardation plate satisfies the following formula (1): Re(450)<Re(550)<Re(650)…(1)

9. 8. The laminate according to claim 7, wherein the horizontally aligned optically absorptive anisotropic film A, the horizontally aligned optically absorptive anisotropic film B, and the retardation plate are laminated in this order.

10. 8. The laminate according to claim 7, wherein the retardation plate, the horizontally aligned optically absorptive anisotropic film A, and the horizontally aligned optically absorptive anisotropic film B are laminated in this order.

11. The laminate according to any one of claims 1 to 10, A display device comprising: a light source that outputs light toward the laminate.

Citation Information

Patent Citations

  • Reflection type liquid crystal display device

    JP2000089208A

  • Stereoscopic image print and method for producing the same

    JP2012003121A

  • Polarizing film, circularly polarizing plate, and organic el image display device using these

    JP2013109090A

  • Polarizing plate

    JP2017083843A

  • Color polarizing film, antireflection film and display device

    JP2017156746A