Porous silica particle and method for producing the same
Porous silica particles with a tertiary structure address inefficiencies in existing carriers by ensuring uniform size and pore distribution, enhancing the performance of supported substances through improved diffusion and contact with the reaction medium.
Patent Information
- Application Number
- JP2023056237
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing porous silica particles used as carriers for enzymes and catalysts do not effectively exhibit the performance of supported substances due to issues such as non-uniform particle size, inadequate pore distribution, and poor diffusion of reaction liquids, leading to inefficient contact between the supported substance and the reaction medium.
The development of porous silica particles composed of tertiary particles, which are aggregates of porous secondary particles, with specific size and pore volume ranges, and a defined pore distribution, allowing for efficient diffusion and contact between the supported substance and reaction medium.
The tertiary particle structure enhances the performance of supported substances by ensuring uniform particle size, optimal pore volume, and efficient diffusion, thereby improving the effectiveness of carriers like enzyme and catalyst carriers.
Smart Images

Figure 2024143513000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to porous silica particles useful as supports for enzymes, catalysts, etc., and a method for producing the same. [Background technology]
[0002] The technology of producing an aggregate of fine particles (porous particles) by spray-drying fine silica particles has been known for a long time. For example, Patent Document 1 discloses a technology of producing inorganic silica particles having an average particle size of 1 to 20 μm by spray-drying a colloidal liquid containing primary particles having an average particle size of 250 nm or less.
[0003] It has also been proposed to utilize such a technique to produce porous silica particles useful as carrier particles (see Patent Document 2). These porous silica particles have mesopores formed inside the particles with a high degree of uniformity in diameter, and therefore have the characteristic of being able to suppress aggregation of catalytic substances consisting of fine metal particles and effectively exhibit catalytic performance.
[0004] It has also been proposed to produce porous silica having macropores in addition to mesopores (see Patent Documents 3 and 4).
[0005] [Patent Document 1] Japanese Patent Application Publication No. 61-270201 [Patent Document 2] JP 2010-138021 A [Patent Document 3] International Publication No. 2003-2458 [Patent Document 4] JP 2009-73681 A Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, porous silica particles are useful as catalyst supports and the like, and there is a demand for further improvement in their performance as supports.
[0007] An object of the present invention is to provide porous silica particles that can more effectively exert the performance of a support material, and a method for producing the same. [Means for solving the problem]
[0008] The present inventors have found that porous silica particles composed of tertiary particles that satisfy specific requirements are extremely useful as carrier particles, and have thus completed the present invention.
[0009] That is, the present invention relates to porous silica particles which are composed of tertiary particles formed by linking porous secondary particles and which satisfy the following requirements (1) to (6). (1) Average particle size in the range of 50 to 1000 μm (2) Specific surface area is 30 to 250 m 2 / g range (3) Pore volume is in the range of 0.10 to 0.75 ml / g (4) In the pore size distribution (X axis: pore size [Ps], Y axis: value obtained by differentiating pore volume with pore size), the pore size (Pms) ranged from 2 to 50 nm. 1 ) mesopore peak and pore diameters in the range of 50 to 2000 nm (Pms 2 ) macropore peak, and the pore diameter (Pms 1 ) mesopore peak is the pore diameter (Pms 1a ) or the pore size (Pms 1a ) and pore size (Pms 1b ) are the two peaks (5) (Pms 1 )×0.75~(pms 1 ) × 1.25 nm, and the volume of pores having a pore diameter within the range of (Pms 2 )×0.75~(pms 2 ) × 1.25 nm, the total pore volume is 40% or more of the total pore volume. (6) Porosity ranges from 15 to 65%
[0010] The present invention also relates to a method for preparing a dispersion of primary particles, which are spherical silica fine particles, having a particle size variation coefficient (CV value) in the range of 2 to 10% and an average particle size of 10 to 300 nm, a step B of spraying the spray liquid containing the primary particles obtained in the step A into an airflow to prepare secondary particles which are aggregates of spherical silica fine particles, and a method for preparing a dispersion of primary particles, which are spherical silica fine particle aggregates, having a particle size variation coefficient in the range of 2 to 10% and an average particle size of 10 to 300 nm, which are equal to or exceed the primary particles prepared in the step A. The present invention relates to a method for producing porous silica particles, the method comprising the steps of: step C of mixing the secondary particles and binder particles, which are spherical silica fine particles having an average particle diameter of 98:2 to 60:40, at a mass ratio of the secondary particles and the binder particles (secondary particles:binder particles) of 98:2 to 60:40 to prepare a mixed particle dispersion; step D of spraying the spray liquid containing the mixed particles obtained in step C into an air current to prepare tertiary particles, which are an aggregate of secondary particles; and step E of heat-treating the tertiary particles obtained in step D at a temperature in the range of 150 to 600°C. Effect of the Invention
[0011] According to the present invention, it is possible to provide porous silica particles that can more effectively exert the performance of a support substance, and a method for producing the same. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic diagram showing a state in which the porous silica particles carrying a catalyst or the like of the present invention are packed into a column and reacted. [Diagram 2] FIG. 1 is a schematic diagram showing a state in which conventional porous silica particles carrying a catalyst or the like are packed into a column and reacted. [Diagram 3] FIG. 1 is a schematic diagram showing a state in which conventional porous silica particles carrying a catalyst or the like are packed into a column and reacted. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Porous silica particles] The porous silica particles of the present invention are composed of tertiary particles formed by linking porous secondary particles, and satisfy the following requirements (1) to (6).
[0014] (1) Average particle size in the range of 50 to 1000 μm (2) Specific surface area is 30 to 250 m 2 / g range (3) Pore volume is in the range of 0.10 to 0.75 ml / g (4) In the pore size distribution (X axis: pore size [Ps], Y axis: value obtained by differentiating pore volume with pore size), the pore size (Pms) ranged from 2 to 50 nm. 1 ) mesopore peak and pore diameters in the range of 50 to 2000 nm (Pms 2 ) macropore peak, and the pore diameter (Pms 1 ) mesopore peak is the pore diameter (Pms 1a ) or the pore size (Pms 1a ) and pore size (Pms 1b ) are the two peaks (5) (Pms 1 )×0.75~(pms 1 ) × 1.25 nm, and the volume of pores having a pore diameter within the range of (Pms 2 )×0.75~(pms 2 ) × 1.25 nm, the total pore volume is 40% or more of the total pore volume. (6) Porosity ranges from 15 to 65%
[0015] The porous silica particles of the present invention (FIG. 1) are composed of tertiary particles in which porous secondary particles are connected, and therefore the reaction liquid or reaction gas (hereinafter simply referred to as the reaction liquid) flows smoothly through the macropores in the tertiary particles and quickly diffuses into the mesopores of the particles, so that the reaction liquid efficiently contacts the supported substance supported in the mesopores, and the performance of the supported substance can be effectively exhibited. On the other hand, when secondary particles of the same size as the tertiary particles of the present invention are used (FIG. 2), such particles are difficult to manufacture uniform particles due to defects and cracks that occur during production, and the reaction liquid is difficult to diffuse into the inside of the particles and only contacts the supported substance near the surface of the secondary particles, so that the contact between the reaction liquid and the supported substance is insufficient and the performance of the supported substance cannot be fully exhibited. In addition, when small-diameter secondary particles that constitute the tertiary particles of the present invention are used (FIG. 3), it is difficult to handle them as powder, and the gaps between the particles are small, so the reaction liquid does not flow easily, and the reaction liquid does not efficiently contact the supported substance, and the performance of the supported substance cannot be fully exhibited. Furthermore, it is difficult to separate the particles from the reaction liquid.
[0016] The porous silica particles of the present invention can be used by carrying a functional substance having a specific function. For example, they can be used as an enzyme carrier, a catalyst carrier, an adsorbent carrier, etc., and are preferably used as an enzyme carrier or a catalyst carrier. When the porous silica particles of the present invention are used to carry a functional substance, they can be used in a batch-type container or in a continuous column, but when they are used in a column in a continuous mode, the effects of the present invention are particularly exhibited. In addition, the porous silica particles of the present invention can also be used as an adsorbent without carrying a carrier substance.
[0017] Each requirement is explained below. (1) Average particle size The average particle size of the porous silica particles of the present invention is in the range of 50 to 1000 μm. The particles of the present invention are composed of tertiary particles in which porous secondary particles are linked, and are larger than conventional particles composed of secondary particles as shown in Patent Document 2. With such an average particle size, the particles are easy to handle as a powder, and when the particles are packed in a column or the like, a certain amount of gap can be secured between the particles, allowing the reaction liquid to flow smoothly and allowing the reaction liquid to come into contact with the support material efficiently. The average particle size is preferably in the range of 80 to 800 μm, more preferably in the range of 100 to 500 μm.
[0018] The average particle size in the present invention is measured by a laser diffraction / scattering method.
[0019] (2) Specific surface area The specific surface area of the porous silica particles of the present invention is 30 to 250 m 2 / g. The specific surface area is in the range of 30m 2 If the specific surface area is less than 250 m / g, it is necessary to use a large amount of the carrier, which is economically disadvantageous. 2 If the specific surface area exceeds 40 to 250 m / g, the reaction product is more likely to be re-adsorbed, which may reduce the reaction efficiency, and the particle strength may be insufficient. 2 / g is preferable, and 40 to 200m 2 / g range is more preferred.
[0020] The specific surface area in the present invention is measured by the BET method using nitrogen gas.
[0021] (3) Pore volume The pore volume of the porous silica particles of the present invention is in the range of 0.10 to 0.75 ml / g. If the pore volume is less than 0.10 ml / g, the amount of the supported substance is small when used as a carrier, so that it is necessary to use a large amount, which is economically disadvantageous. If the pore volume exceeds 0.75 ml / g, the strength of the particles becomes insufficient. The pore volume is preferably in the range of 0.20 to 0.60 ml / g, and more preferably in the range of 0.30 to less than 0.50 ml / g.
[0022] The pore volume of the present invention is the total pore volume of mesopores (2 to 50 nm) and macropores (more than 50 to 2000 nm), and the mesopores are measured by the BJH method using nitrogen, and the macropores are measured by mercury intrusion porosimetry. Similarly, the pore distribution and pore diameter (peak value) are also determined by the BJH method and mercury intrusion porosimetry, respectively.
[0023] The pore volume of the macropores in the porous silica particles of the present invention preferably accounts for 10% or more of the pore volume of the entire particle, more preferably 15 to 75%, and even more preferably 20 to 70%.
[0024] (4) Peak in pore size distribution The porous silica particles of the present invention have a pore size distribution (X axis: pore size [Ps], Y axis: value obtained by differentiating pore volume with pore size) of 2 to 50 nm (Pms 1 ) mesopore peak and pore diameters in the range of 50 to 2000 nm (Pms 2 ) macropore peak, and the pore diameter (Pms 1 ) mesopore peak is the pore diameter (Pms 1a ) or the pore size (Pms 1a ) and pore size (Pms 1b ) two peaks (Pms 1a <Pms 1b). That is, the porous silica particles of the present invention include an embodiment having one peak in the mesopore region and one peak in the macropore region, and an embodiment having two peaks in the mesopore region and one peak in the macropore region. Since the porous silica particles of the present invention have a relatively sharp peak in the mesopore region and a peak in the macropore region, when a support material having catalytic function or the like is supported in the mesopores in a state in which aggregation is suppressed and the support material is packed into a column or the like, the reaction liquid flows smoothly through the macropores, and the reaction liquid and the support material come into contact efficiently. Peak pore diameter (Pms 1 The peak pore diameter (Pms) is preferably in the range of 2 to 40 nm, and more preferably in the range of 3 to 30 nm. 2 ) is preferably in the range of 200 to 1500 nm, more preferably in the range of 500 to 1300 nm.
[0025] Here, the pore diameter (Pms 2 The macropores based on the peak of the pore diameter (Pms 1a ) and pore size (Pms 1b ) are two peaks (Pms 1a <Pms 1b ) pore size (Pms 1b Mesopores based on the peak of the pore diameter (Pms 1a ) are pores within the secondary particles, and the pore diameter (Pms 1a The mesopore volume 1a based on the peak of 1a decreases, and the pore diameter (Pms 1b ) the mesopore volume 1b based on the peak increases.
[0026] (5) Pore volume ratio The porous silica particles of the present invention are 1 )×0.75~(pms 1 ) × 1.25 nm, and the volume of pores having a pore diameter within the range of (Pms 2 )×0.75~(pms 2The total pore volume of the pores having a pore diameter in the range of Pms × 1.25 nm is 40% or more of the total pore volume. 1a and Pms 1b If the two peaks are 1 The pore volume based on Pms 1a Pore volume and Pms based on 1b is the sum of the volumes based on
[0027] If it is less than 40% of the total pore volume, the pore size distribution is non-uniform, stress is concentrated in relatively large pores, and problems such as weakened strength in practical use are likely to occur. The total pore volume is preferably 50% or more of the total pore volume, more preferably 55 to 80%.
[0028] Also, (pms 1 )×0.75~(pms 1 The total pore volume of pores having a pore diameter within the range of (Pms)×1.25 nm is preferably in the range of 20 to 70% of the total pore volume, and more preferably in the range of 30 to 50%. 2 )×0.75~(pms 2 The total pore volume of pores having pore diameters within the range of 10 to 50%, and more preferably 20 to 40%, of the total pore volume.
[0029] Also, (pms 1 )×0.75~(pms 1 The total pore volume of pores having a pore diameter within the range of (Pms)×1.25 nm is preferably in the range of 50 to 80% of the total pore volume in the mesopore region (2 to 50 nm), and more preferably in the range of 60 to 80%. 2 )×0.75~(pms 2 )×1.25 nm is preferably in the range of 20 to 80%, more preferably 30 to 70%, of the total pore volume in the macropore region (more than 50 to 2000 nm).
[0030] Here, when the mesopore peak is one peak, the porous silica particles of the present invention preferably satisfy the following requirement (5A).
[0031] (5A)(Pms 1a )×0.75~(pms 1a The total pore volume of pores having a pore diameter within the range of (Pms) × 1.25 nm is in the range of 20 to 70% of the total pore volume, and 2 )×0.75~(pms 2 The total pore volume of pores having a pore diameter within the range of 10 to 50% of the total pore volume.
[0032] (P.M. 1a )×0.75~(pms 1a The total pore volume of pores having a pore diameter within the range of (Pms) × 1.25 nm is more preferably in the range of 20 to 50% of the total pore volume. 2 )×0.75~(pms 2 The total pore volume of pores having a pore diameter within the range of 10 to 30% of the total pore volume.
[0033] Furthermore, when the mesopore peak is a two-peak structure, the porous silica particles of the present invention preferably satisfy the following requirement (5B).
[0034] (5B)(Pms 1a )×0.75~(pms 1a The total pore volume of pores having a pore diameter within the range of (Pms) × 1.25 nm is in the range of 1 to 50% of the total pore volume, and 1b )×0.75~(pms 1b The total pore volume of pores having a pore diameter within the range of (Pms) × 1.25 nm is in the range of 1 to 50% of the total pore volume, and 2 )×0.75~(pms 2 The total pore volume of pores having a pore diameter within the range of 10 to 50% of the total pore volume.
[0035] (P.M. 1a )×0.75~(pms 1a The total pore volume of pores having a pore diameter within the range of (Pms) × 1.25 nm is more preferably in the range of 10 to 40% of the total pore volume.1b )×0.75~(pms 1b The total pore volume of pores having a pore diameter within the range of (Pms)×1.25 nm is more preferably in the range of 10 to 40% of the total pore volume. 2 )×0.75~(pms 2 The total pore volume of pores having pore diameters within the range of 1.25 nm×1.35 nm is more preferably within the range of 20 to 40% of the total pore volume.
[0036] In the porous silica particles of the present invention, pores having a pore diameter of less than 5 nm preferably account for 5% or more of the total pore volume.
[0037] (6) Porosity The porous silica particles of the present invention have a porosity in the range of 15 to 65%. If the porosity is less than 15%, the amount of material that can be supported is small when used as a carrier, which is not practical. If the porosity is more than 65%, the strength of the particles may not be maintained. The porosity is preferably in the range of 30 to 60%, and more preferably in the range of 40 to 55%.
[0038] The porosity of the present invention is calculated from the pore volume determined by the BJH method and the mercury injection method using the following formula (1).
[0039] Porosity (%) = Pore volume / (Pore volume + 0.4545) * 100 Equation (1) 0.4545(cm 3 / g) = volume of 1g of silica (density of silica = 2.2g / cm 3 (Calculated from
[0040] The porous silica particles of the present invention may be surface-treated as desired. The strength of the particles can be improved by surface treatment. When used as a carrier, it has the effect of increasing affinity with the supporting material and increasing the supporting power. When used as an adsorbent, it is expected to have the effect of increasing selectivity and increasing the adsorption efficiency of the target adsorbate.
[0041] For example, by adding an organosilicon compound represented by the following general formula and / or a partial hydrolyzate thereof together with an acid or alkali, a silica-based coating layer having organic functional groups can be formed on the surface of the particles.
[0042] General formula: R n Si(OR′) 4-n (wherein R and R' are hydrocarbon groups selected from an alkyl group having 1 to 18 carbon atoms, an aryl group having 1 to 18 carbon atoms, a vinyl group, or an acryl group, and n is an integer of 0, 1, 2, or 3.)
[0043] The porous silica particles of the present invention may have various shapes depending on the application, and examples of such shapes include spherical shapes such as elliptical and circular shapes, as well as cylindrical and rod-like shapes.
[0044] [Method of manufacturing porous silica particles] The above-mentioned porous silica particles can be produced, for example, by the following method. That is, the method for producing porous silica particles of the present invention includes the steps of: step A of preparing a dispersion of primary particles that are spherical silica fine particles having a particle size variation coefficient in the range of 2 to 10% and an average particle size of 10 to 300 nm; step B of spraying the spray liquid containing the primary particles obtained in step A into an air stream to prepare secondary particles that are spherical silica fine particle aggregates; step C of mixing the secondary particles obtained in step B with binder particles that are spherical silica fine particles having a particle size variation coefficient in the range of 2 to 10%, an average particle size of 10 to 300 nm, and an average particle size equivalent to or greater than that of the primary particles prepared in step A at a mass ratio of the secondary particles and the binder particles (secondary particles:binder particles) of 98:2 to 60:40 to prepare a mixed particle dispersion; step D of spraying the spray liquid containing the mixed particles obtained in step C into an air stream to prepare tertiary particles that are secondary particle aggregates; and step E of heat-treating the tertiary particles obtained in step D at a temperature in the range of 150 to 600°C.
[0045] Each step will be described below. (Process A) In step A, a dispersion liquid of primary particles, which are spherical silica fine particles having a particle size variation coefficient in the range of 2 to 10% and an average particle size of 10 to 300 nm, is prepared.
[0046] Specifically, for example, a dispersion of spherical silica microparticles having an average particle diameter of 10 to 300 nm, preferably 10 to 100 nm, is prepared, and then centrifugal separation is performed to separate coarse particles. The particle diameter variation coefficient is adjusted to within the range of 2 to 10%, thereby preparing a desired dispersion of spherical silica microparticles whose particle diameter distribution exhibits a monodisperse phase.
[0047] As for the conditions for the centrifugation treatment, it is usually recommended that the concentration of the spherical silica microparticle dispersion be 1 to 50% by mass, and that the centrifugal force be in the range of 500 to 20,000×g.
[0048] The above-mentioned predetermined spherical silica fine particle dispersion may be purchased and used.
[0049] The average particle size and the coefficient of variation (CV value) of particle size of the primary particles of the present invention are measured by an image analysis method.
[0050] (B process) In step B, the spray liquid containing the primary particles obtained in step A is sprayed into an air current to prepare secondary particles which are spherical aggregates of silica fine particles.
[0051] The solvent for the spray liquid may be water or an organic solvent, such as monohydric alcohols such as ethanol, propanol, and butanol, or polyhydric alcohols such as ethylene glycol.
[0052] The particle concentration in the spray liquid is preferably in the range of 2 to 60% by mass, more preferably in the range of 4 to 50% by mass. By performing spray drying within this concentration range, desired secondary particles can be stably obtained.
[0053] As the spray drying method, a conventionally known method such as a rotating disk method, a pressure nozzle method, a two-fluid nozzle method, etc. can be adopted. In particular, the two-fluid nozzle method disclosed in JP-B-2-61406 is preferred because it can obtain secondary particles with a uniform particle size distribution and it is easy to control the average particle size.
[0054] The drying temperature at this time varies depending on the concentration of the primary particle dispersion, the processing speed, etc., but for example, the inlet temperature of the spray dryer is preferably in the range of 100 to 300° C., and the outlet temperature is preferably in the range of 40 to 100° C. More preferably, the inlet temperature is in the range of 210 to 250° C., and the outlet temperature is in the range of 50 to 55° C. The spray speed depends on the shape of the spray dryer, etc., but is preferably in the range of, for example, 0.1 to 3 L / hour.
[0055] The secondary particles that have undergone step B (and step F, which will be described later) satisfy, for example, the following requirements. a) The average particle size is preferably 0.5 to 50 μm, and more preferably 5 to 30 μm. b) The specific surface area is preferably 30 to 250 m 2 / g c) The pore volume is preferably 0.10 to 0.25 ml / g, more preferably 0.12 to 0.20 ml / g. d) The pore diameter (D1) of the peak value in the pore diameter distribution (X axis: pore diameter, Y axis: value obtained by differentiating the pore volume with the pore diameter) is preferably 2 to 50 nm, more preferably 3 to 45 nm. e) The total pore volume of pores having a pore diameter within the range of (D1)×0.75 to (D1)×1.25 nm is preferably 70% or more, more preferably 80% or more of the total pore volume (i.e., the total mesopore volume). f) The porosity is preferably 5 to 50%, more preferably 10 to 30%. g) Sphericity is preferably 0.90 to 1.00
[0056] (C process) In step C, the secondary particles obtained in step B are mixed with binder particles, which are spherical silica microparticles having a particle size variation coefficient in the range of 2 to 10%, an average particle size of 10 to 300 nm, and an average particle size equivalent to or larger than that of the primary particles prepared in step A, in a mass ratio of the secondary particles to the binder particles (secondary particles:binder particles) of 98:2 to 60:40 to prepare a mixed particle dispersion.
[0057] If the binder particles are smaller than the average particle size of the primary particles prepared in step A, the binder particles may penetrate into the pores (mesopores) of the secondary particles and block the pores of the secondary particles. If the binder particles are less than the above ratio, the binding force between the secondary particles is weak and the desired structure cannot be produced. On the other hand, if the binder particles are more than the above ratio, sufficient macropores cannot be formed and the effect of promoting diffusion inside the particles cannot be obtained.
[0058] As the binder particles, the primary particles prepared in the step A may be used, or primary particles prepared separately may be used. When prepared separately, primary particles having an average particle size equal to or larger than that of the primary particles prepared in the step A are used. The average particle size of the binder particles is preferably 200 nm or less, more preferably 150 nm or less. The method for preparing the binder particles is the same as the method for the step A.
[0059] The mass ratio of the secondary particles to the binder particles (secondary particles:binder particles) is preferably from 95:5 to 75:25, and more preferably from 90:10 to 70:30.
[0060] (D process) In step D, the spray liquid containing the mixed particles obtained in step C is sprayed into an air current to prepare tertiary particles, which are an aggregate of secondary particles.
[0061] The treatment in step D is basically the same as that in step B. However, in step D, in order to obtain large diameter particles, it is preferable to spray large droplets using a rotary disk (atomizer) or a one-fluid nozzle, and then dry them. It is also preferable to supply the slurry while stirring it so that the secondary particles in the slurry do not settle.
[0062] (E process) In step E, the secondary particles obtained in step D are heat-treated at a temperature in the range of 150 to 600°C. The heat treatment can increase the bonding strength between the secondary particles. If the heat treatment temperature is less than 150°C, the effect of improving the bonding strength may not be observed. On the other hand, if the heat treatment temperature exceeds 600°C, the particles may shrink, and the gaps between the finally obtained secondary particles may become smaller.
[0063] The method for producing porous silica particles of the present invention may include a step F of heat-treating the secondary particles obtained in the step B. (F process) Step F is a step that is provided after step B and before step C, and in step F, the secondary particles obtained in step B are heat-treated at a temperature in the range of 150 to 600°C. The heat treatment can increase the bonding strength between the primary particles. If the heat treatment temperature is less than 150°C, the effect of improving the bonding strength may not be observed. On the other hand, if the heat treatment temperature exceeds 600°C, the secondary particles may shrink, and the voids in the finally obtained porous secondary particles may become smaller.
[0064] In the method for producing porous silica particles of the present invention, the following steps G to I may be carried out, if desired, following the step E.
[0065] (G process) In step G, a dispersion of the heat-treated tertiary particles obtained in step E is prepared. Specifically, the heat-treated tertiary particles are allowed to cool or cooled to room temperature to 40°C, and dispersed in water and / or an organic solvent to prepare a dispersion. As the organic solvent, monohydric alcohols such as ethanol, propanol, butanol, and polyhydric alcohols such as ethylene glycol can be used. The particle concentration of the dispersion is preferably in the range of 0.1 to 40% by mass, and more preferably in the range of 0.5 to 20% by mass.
[0066] (H process) In step H, the following i) or ii) is added to the dispersion liquid obtained in step G to perform surface treatment of the outer surfaces of the tertiary particles. i) Acid or alkali ii) An acid or alkali and an organosilicon compound represented by the following general formula and / or its partial hydrolyzate: General formula: R n Si(OR′) 4-n (wherein R and R' are hydrocarbon groups selected from an alkyl group having 1 to 18 carbon atoms, an aryl group having 1 to 18 carbon atoms, a vinyl group, and an acrylic group, and n is an integer of 0, 1, 2, or 3.)
[0067] In the case of i) above, an aqueous solution of an acid or alkali is usually used. The type of acid or alkali is not particularly limited, but examples include an aqueous solution of hydrochloric acid, an aqueous solution of boric acid, and an aqueous solution of ammonium.
[0068] The acid or alkali in the case of ii) above is defined in the same manner as in the case of i). Specific examples of the organosilicon compound represented by the general formula include tetramethoxysilane, tetraethoxysilane, tetraisopropoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, diphenyldiethoxysilane, isobutyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(βmethoxyethoxy)silane, 3,3,3-trifluoropropyltrimethoxysilane, methyl-3,3,3-trifluoropropyldimethoxysilane, β-(3,4 epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxytripropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropyltriethoxysilane, γ -methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-methacryloxypropyltriethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, trimethylsilanol, methyltrichlorosilane, methyldichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, phenyltrichlorosilane, diphenyldichlorosilane, vinyltrichlorosilane, trimethylbromosilane, diethylsilane, and the like.
[0069] The acid or alkali added together with the organosilicon compound and / or its partial hydrolysate also functions as a catalyst for hydrolysis, but a catalyst for hydrolysis may be added if desired. When a basic catalyst such as an alkali metal hydroxide, aqueous ammonia, or amine is used as the hydrolysis catalyst, the basic catalyst can be removed after hydrolysis and the solution can be used as an acid solution. When an acid catalyst such as an organic acid or inorganic acid is used to prepare the hydrolysate, it is preferable to remove the acid catalyst by ion exchange or the like after hydrolysis. The obtained hydrolysate of the organosilicon compound is preferably used in the form of an aqueous solution. Here, the aqueous solution means that the hydrolysate is not in a gel-like opaque state but is transparent.
[0070] (I process) In step I, the silica particles are separated from the dispersion liquid obtained in step H, dried, and then heat-treated at 100 to 300° C. This gives surface-treated porous silica particles. EXAMPLES
[0071] Examples of the present invention will be described in detail below, but the technical scope of the present invention is not limited to these examples.
[0072] [Example 1-1] (Preparation of primary particles) 1667 g of silica sol (JGC Catalysts and Chemicals: Cataloid SI-30, average particle size 12 nm, concentration 30% by mass) was continuously poured into the rotor (model: QNS, capacity: 1 L) of a centrifuge (Kokusan Co., Ltd., continuous high-speed centrifuge H-660), and the liquid was passed through at 7000 G at a speed of 400 g / min, and the liquid was continuously collected to perform a centrifugation process for coarse particles. The coarse particles settled in the rotor.
[0073] 2000 g of the recovered water-diluted silica sol (silica concentration 15% by mass) was subjected to cation exchange and adjusted to pH = 2.0, after which silicic acid liquid (silica concentration 4.8% by mass) was added so that the ratio of [silica in silica sol] / [silica in silicic acid liquid] was 9 / 1, and further diluted with pure water to a slurry concentration of 5%, and stirred to prepare a slurry.
[0074] (Preparation of secondary particles) The obtained slurry was subjected to a spray dryer, and spray-dried by supplying air to one of two-fluid nozzles at a flow rate of 2 L / hr and to the other nozzle at a flow rate of 0.75 MPa in a dry air stream adjusted to an inlet temperature of 240°C and an outlet temperature of 50 to 55°C, to obtain a powder consisting of an aggregate of spherical silica fine particles. This powder was calcined at 450°C for 3 hours to obtain porous silica particles A1 (secondary particles).
[0075] (Preparation of binder particles) 1667 g of silica sol (JGC Catalysts and Chemicals: Cataloid SI-30, average particle size 12 nm, concentration 30% by mass) was continuously poured into the rotor (model: QNS, capacity: 1 L) of a centrifuge (Kokusan Co., Ltd., continuous high-speed centrifuge H-660), and the liquid was passed through at 7000 G at a speed of 400 g / min, and the liquid was continuously collected to perform a centrifugation process for coarse particles. The coarse particles settled in the rotor. The recovered silica sol was diluted with water to prepare 2000 g of a slurry having a silica concentration of 15 mass %.
[0076] (Tertiary particle granulation) The secondary particles were dispersed in pure water, and the binder particles were added to the dispersion while stirring to prepare a slurry having a solids ratio of secondary particles to binder particles of 90:10 and a silica concentration of 30 mass %. The obtained slurry was subjected to a spray dryer and spray-dried by supplying it with an atomizer into a dry air stream adjusted to an inlet temperature of 240°C and an outlet temperature of 100°C, to obtain a powder consisting of porous silica particles A (secondary particles) and spherical silica fine particles (binder particles). This powder was calcined at 450°C for 3 hours to obtain porous silica particles B1-1 (tertiary particles).
[0077] [Example 1-2] Porous silica particles B1-2 (tertiary particles) were obtained in the same manner as in Example 1-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was 80:20.
[0078] [Examples 1-3] Porous silica particles B1-3 (tertiary particles) were obtained in the same manner as in Example 1-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was set to 70:30.
[0079] [Examples 1-4] Porous silica particles B1-4 (tertiary particles) were obtained in the same manner as in Example 1-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was set to 60:40.
[0080] [Example 2-1] In the granulation of the tertiary particles, porous silica particles B2-1 (tertiary particles) were obtained in the same manner as in Example 1-1, except that silica sol (manufactured by JGC Catalysts and Chemicals Co., Ltd.: Cataloid SI-80P, average particle size 80 nm, concentration 40 mass%) was prepared as follows and used as the binder particles.
[0081] (Preparation of binder particles) 1000 g of silica sol (JGC Catalysts and Chemicals: Cataloid SI-80P, average particle size 80 nm, concentration 40% by mass) was continuously poured into the rotor (model: QNS, capacity: 1 L) of a centrifuge (Kokusan Co., Ltd., continuous high-speed centrifuge H-660), and the liquid was passed through at a speed of 400 g / min at 2120 G, and the liquid was continuously collected to perform a centrifugation process for coarse particles. The coarse particles settled in the rotor. The recovered silica sol was diluted with water to prepare 2000 g of a slurry having a silica concentration of 15 mass %.
[0082] [Example 2-2] Porous silica particles B2-2 (tertiary particles) were obtained in the same manner as in Example 2-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was 80:20.
[0083] [Example 2-3] Porous silica particles B2-3 (tertiary particles) were obtained in the same manner as in Example 2-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was set to 70:30.
[0084] [Example 2-4] Porous silica particles B2-4 (tertiary particles) were obtained in the same manner as in Example 2-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was set to 60:40.
[0085] [Example 3-1] (Preparation of primary particles and secondary particles) Porous silica particles A3 (secondary particles) were obtained in the same manner as in Example 1-1, except that a water-diluted product (silica concentration 30% by mass) of Cataloid SI-45P (average particle diameter 45 nm, concentration 40% by mass) manufactured by JGC Catalysts and Chemicals Co., Ltd. was used as the silica sol.
[0086] (Preparation of binder particles) 1000 g of silica sol (JGC Catalysts and Chemicals: Cataloid SI-80P, average particle size 80 nm, concentration 40% by mass) was continuously poured into the rotor (model: QNS, capacity: 1 L) of a centrifuge (Kokusan Co., Ltd., continuous high-speed centrifuge H-660), and the liquid was passed through at a speed of 400 g / min at 2120 G, and the liquid was continuously collected to perform a centrifugation process for coarse particles. The coarse particles settled in the rotor. The recovered silica sol was diluted with water to prepare 2000 g of a slurry having a silica concentration of 15 mass %.
[0087] (Tertiary particle granulation) The secondary particles were dispersed in pure water, and the binder particles were added to the dispersion while stirring to prepare a slurry having a solid content ratio of secondary particles to binder particles of 90:10 and a concentration of 30%. The obtained slurry was subjected to a spray dryer and spray-dried by supplying it with an atomizer into a dry air stream adjusted to an inlet temperature of 240°C and an outlet temperature of 100°C, to obtain a powder consisting of porous silica particles A (secondary particles) and spherical silica fine particles (binder particles). This powder was calcined at 450°C for 3 hours to obtain porous silica particles B3-1 (tertiary particles).
[0088] [Example 3-2] Porous silica particles B3-2 (tertiary particles) were obtained in the same manner as in Example 3-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was 80:20.
[0089] [Example 3-3] Porous silica particles B3-3 (tertiary particles) were obtained in the same manner as in Example 3-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was set to 70:30.
[0090] [Example 3-4] Porous silica particles B3-4 (tertiary particles) were obtained in the same manner as in Example 3-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was set to 60:40.
[0091] [Example 4-1] (Preparation of primary particles and secondary particles) Porous silica particles A4 (secondary particles) were obtained in the same manner as in Example 1-1, except that a silica sol was used that was a water-diluted product (silica concentration 30% by mass) of Cataloid SI-80P manufactured by JGC Catalysts and Chemicals Co., Ltd., with an average particle diameter of 80 nm and a concentration of 40% by mass (Cataloid SI-80P manufactured by JGC Catalysts and Chemicals Co., Ltd.).
[0092] (Preparation of binder particles) 1000 g of silica sol (JGC Catalysts and Chemicals: Cataloid SI-80P, average particle size 80 nm, concentration 40% by mass) was continuously poured into the rotor (model: QNS, capacity: 1 L) of a centrifuge (Kokusan Co., Ltd., continuous high-speed centrifuge H-660), and the liquid was passed through at a speed of 400 g / min at 2120 G, and the liquid was continuously collected to perform a centrifugation process for coarse particles. The coarse particles settled in the rotor. The recovered silica sol was diluted with water to prepare 2000 g of a slurry having a silica concentration of 15 mass %.
[0093] (Tertiary particle granulation) The secondary particles were dispersed in pure water, and the binder particles were added thereto while stirring, to prepare a slurry having a solids ratio of secondary particles to binder particles of 90:10 and a silica concentration of 30 mass %. The obtained slurry was subjected to a spray dryer and spray-dried by supplying it with an atomizer into a dry air stream adjusted to an inlet temperature of 240°C and an outlet temperature of 100°C, to obtain a powder consisting of porous silica particles A (secondary particles) and spherical silica fine particles (binder particles). This powder was calcined at 450°C for 3 hours to obtain porous silica particles B4-1 (tertiary particles).
[0094] [Example 4-2] Porous silica particles B4-2 (tertiary particles) were obtained in the same manner as in Example 4-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was 80:20.
[0095] [Example 4-3] Porous silica particles B4-3 (tertiary particles) were obtained in the same manner as in Example 4-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was set to 70:30.
[0096] [Example 4-4] Porous silica particles B4-4 (tertiary particles) were obtained in the same manner as in Example 4-1, except that in the granulation of the tertiary particles, the solid content ratio of the secondary particles to the binder particles was set to 60:40.
[0097] [Comparative Example 1] The porous silica particles A1 (secondary particles) produced in Example 1-1 were used as porous silica particles B'1 according to Comparative Example 1.
[0098] [Comparative Example 2] The porous silica particles A3 (secondary particles) produced in Example 3-1 were used as porous silica particles B'2 according to Comparative Example 2.
[0099] [Comparative Example 3] In the granulation of the tertiary particles, porous silica particles B'3 (tertiary particles) were obtained in the same manner as in Example 1-1, except that silica sol (manufactured by JGC Catalysts and Chemicals Co., Ltd.: Cataloid SI-30, average particle size 12 nm, concentration 30 mass%) was prepared as follows and used as the binder particles. 1a ) peak is due to the formation of mesopores by binder particles, and the larger pore diameter (Pms 1b ) peaks are mesopores within the secondary particles.
[0100] (Preparation of binder particles) 1667 g of silica sol (JGC Catalysts and Chemicals: Cataloid SI-30, average particle size 12 nm, concentration 30% by mass) was continuously poured into the rotor (model: QNS, capacity: 1 L) of a centrifuge (Kokusan Co., Ltd., continuous high-speed centrifuge H-660), and the liquid was passed through at 7000 G at a speed of 400 g / min, and the liquid was continuously collected to perform a centrifugation process for coarse particles. The coarse particles settled in the rotor. The recovered silica sol was diluted with water to prepare 2000 g of a slurry having a silica concentration of 15 mass %.
[0101] [Comparative Example 4] The porous silica particles A4 (secondary particles) produced in Example 4-1 were used as porous silica particles B'4 according to Comparative Example 4.
[0102] The porous silica particles B of the example and the porous silica particles B' of the comparative example produced above were used for evaluation (water flow test and enzyme reaction efficiency test).
[0103] <Water flow test> (Test Method) Each porous silica particle 50cm 3 The above was packed into a glass column (inner diameter 20 mm, length 400 mm) and the space velocity (SV) was measured when pure water was passed through the column at a pressure of 0.1 mPa.
[0104] Space velocity (SV) = (amount of water passing per hour) / (amount of porous silica particles packed) (1 / Hr)
[0105] (evaluation) 〇:SV:3 or more △:SV:1 or more, less than 3 ×:SV:less than 1
[0106] <Enzyme reaction efficiency test> (Specific activity test of immobilized enzyme (racemase) (measurement of specific activity based on the rate of change in circular dichroism of L-Ala over time)) The porous silica particles B3-1, B3-2, B3-3, and B3-4 according to the examples, and the porous silica particles B'2 and B'3 according to the comparative examples were surface-treated using a silane coupling agent ("KBM-903" (3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd.), and then racemase was immobilized using the method described in JP 2012-16351 A. The porous silica particles used had mesopores (secondary particle pores) of 20 nm suitable for supporting the enzyme (racemase) to be supported.
[0107] The immobilized enzyme (equivalent to 2 μg of racemase adsorbed on the enzyme immobilization carrier) was mixed with 2.5 ml of substrate solution (10 mM L-alanine, 10 mM potassium phosphate, pH 7.5) in a test tube and reacted at 30° C. to obtain a suspension. This suspension was used as the sample.
[0108] The sample consisting of the suspension was placed in a 1 cm square quartz cell and set in a circular dichroism spectrometer ("J-820" manufactured by JASCO Corporation). The suspension in the cell was stirred with a magnetic stirrer, and the cell was kept at 30° C. with a Peltier temperature control device.
[0109] Next, the ellipticity of L-alanine at a wavelength of 204 nm was measured at 1-second intervals for 5 minutes using a circular dichroism spectrometer. The molar ellipticity of L-alanine was set to 23 mdeg / mM to measure the L-alanine concentration in the suspension, and the activity was calculated from the amount of alanine converted per unit time. The specific activity was calculated using the following formula.
[0110] Specific activity = [Activity of enzyme immobilized on porous silica] / [Activity of enzyme before immobilization]
[0111] (evaluation) 〇: Specific activity = 0.8 or more △: Specific activity = 0.6 or more to less than 0.8 ×: specific activity = less than 0.6
[0112] Table 1 shows a summary of the production conditions, properties, and evaluation results of the produced porous silica particles in the above-mentioned Examples and Comparative Examples.
[0113] [Table 1]
[0114] The methods for measuring various parameters are as follows. [Average particle size of porous silica particles (secondary and tertiary particles) (laser diffraction / scattering method)] The particle size distribution was measured in a dry state using a particle size analyzer (Seishin Enterprise Co., Ltd., Laser Micronsizer LMS-3000), and the average particle size of the porous silica particles was calculated.
[0115] [Average particle size of primary particles and coefficient of variation of particle size (CV value)] The particles were photographed (magnification 250,000 times) using a scanning electron microscope (JSM-5300, manufactured by JEOL Ltd.), and the average particle size of 250 particles in this image was measured using an image analyzer (IP-1000, manufactured by Asahi Kasei Corporation), and the coefficient of variation (CV value) for particle size distribution was calculated. Specifically, the particle size of each of the 250 particles was measured, and the average particle size and standard deviation of the particle size were calculated from the values, and calculated from the following formula. Coefficient of variation (CV value) = (Standard deviation of particle size (σ) / Average particle size (Dn)) x 100 (%)
[0116] [Specific surface area of porous silica particles (secondary and tertiary particles), pore volume and pore diameter of mesopores] 10 g of sample was placed in a crucible, dried at 300°C for 1 hour, and then cooled to room temperature in a desiccator. 0.15 g was placed in a glass cell, and nitrogen gas was adsorbed onto the sample while vacuum degassing using a Belsorp mini II (manufactured by Japan Bell Co., Ltd.), and the specific surface area was calculated. In addition, the pore volume and pore diameter (peak value) in the range of 2 to 50 nm were calculated from the data during desorption.
[0117] [Pore volume and pore diameter of macropores in porous silica particles (tertiary particles)] 10 g of sample was placed in a crucible, dried at 300°C for 1 hour, then cooled to room temperature in a desiccator and measured by mercury intrusion porosimetry using PM-33 (manufactured by QuantaCrome). Mercury was injecting at 3.5 kPa to 231 MPa (0.5 to 33,000 psi), and the pore distribution was calculated from the relationship between pressure, pore diameter, and intrusion amount. Based on the measurement results for pores with diameters of 50 to 2,000 nm, the pore volume and pore diameter (peak value) of macropores were calculated. [Industrial Applicability]
[0118] INDUSTRIAL APPLICABILITY The porous silica particles of the present invention can be used as a carrier for enzymes and the like and are therefore industrially useful.
Claims
1. A porous silica particle comprising tertiary particles formed by connecting porous secondary particles, and satisfying the following requirements (1) to (6): (1) Average particle size in the range of 50 to 1000 μm (2) Specific surface area is 30 to 250 m 2 / g range (3) Pore volume in the range of 0.10 to 0.75 ml / g (4) In the pore size distribution (X axis: pore size [Ps], Y axis: value obtained by differentiating pore volume by pore size), pore sizes in the range of 2 to 50 nm (Pms 1 ) mesopore peak and pore diameters in the range of 50 to 2000 nm (Pms 2 ) macropore peak, and the pore diameter (Pms 1 ) mesopore peak is the pore diameter (Pms 1a ) or the pore diameter (Pms 1a ) and pore diameter (Pms 1b ) are the two peaks (5) (PMs 1 )×0.75~(Pms 1 ) × 1.25 nm, and the volume of pores having a pore diameter in the range of (Pms 2 )×0.75~(Pms 2 ) × 1.25 nm, and the total pore volume of the pores having a pore diameter in the range of 40% or more of the total pore volume (6) Porosity ranges from 15 to 65%
2. 2. The porous silica particle according to claim 1, characterized in that the mesopore peak is one peak and satisfies the following requirement (5A). (5A) (Pms 1a )×0.75~(Pms 1a The total pore volume of pores having a pore diameter within the range of (Pms) × 1.25 nm is in the range of 20 to 70% of the total pore volume, and 2 )×0.75~(Pms 2 ) × 1.25 nm, the total pore volume of pores having a pore diameter in the range of 10 to 50% of the total pore volume
3. 2. The porous silica particle according to claim 1, characterized in that the mesopore peak is two peaks and satisfies the following requirement (5B). (5B) (Pms 1a )×0.75~(Pms 1a The total pore volume of pores having a pore diameter within the range of 1 to 50% of the total pore volume, and (Pms 1b )×0.75~(Pms 1b The total pore volume of pores having a pore diameter within the range of 1 to 50% of the total pore volume, and (Pms 2 )×0.75~(Pms 2 ) × 1.25 nm, the total pore volume of pores having a pore diameter in the range of 10 to 50% of the total pore volume
4. A step A of preparing a dispersion of primary particles which are spherical silica fine particles having a particle size variation coefficient in the range of 2 to 10% and an average particle size of 10 to 300 nm; A step B of spraying the spray liquid containing the primary particles obtained in the step A into an air flow to prepare secondary particles which are spherical silica fine particle aggregates; a step C of mixing the secondary particles obtained in the step B with binder particles which are spherical silica fine particles having a particle size variation coefficient in the range of 2 to 10%, an average particle size of 10 to 300 nm, and an average particle size equivalent to or exceeding that of the primary particles prepared in the step A, in a mass ratio of the secondary particles to the binder particles (secondary particles:binder particles) of 98:2 to 60:40 to prepare a mixed particle dispersion; A step D of spraying the spray liquid containing the mixed particles obtained in the step C into an air flow to prepare tertiary particles which are an aggregate of secondary particles; A step E of heat-treating the tertiary particles obtained in the step D at a temperature in the range of 150 to 600° C.; 2. A method for producing porous silica particles, comprising the steps of:
5. 5. The method for producing porous silica particles according to claim 4, wherein the average particle size of the binder particles is 150 nm or less.
6. 5. The method for producing porous silica particles according to claim 4, wherein the mass ratio of the secondary particles to the binder particles (secondary particles:binder particles) in the step C is 95:5 to 75:
25.
7. 5. The method for producing porous silica particles according to claim 4, further comprising a step F of heat-treating the secondary particles obtained in the step B at a temperature in the range of 150 to 600°C.