Adhesive film and method for manufacturing semiconductor device using adhesive film

The adhesive film with a tetrafluoroethylene and (meth)acrylate polymer layers addresses the issue of solvent-induced swelling and peeling in semiconductor manufacturing, ensuring robust adhesion and improved productivity.

JP2024143519AInactive Publication Date: 2024-10-11AGC INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023056244
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Tetrafluoroethylene polymer films used as adhesive layers in semiconductor manufacturing are susceptible to swelling and cohesive or interfacial failure when exposed to polar solvents, leading to peeling and reduced productivity.

Method used

An adhesive film with a base layer containing a tetrafluoroethylene polymer and an adhesive layer made of a specific (meth)acrylate polymer, designed to have a storage modulus of 400 to 800 MPa at 50°C and less than 1% swelling in polar solvents, ensuring excellent adhesiveness and resistance to polar solvents.

Benefits of technology

The adhesive film maintains adhesion and prevents peeling from the semiconductor wafer or chip during cleaning with polar solvents, enhancing productivity in semiconductor manufacturing by preventing adhesive failure.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide an adhesive film having resistance to a polar solvent and excellent adhesiveness and adhesion between a substrate layer and an adhesive layer.SOLUTION: There is provided an adhesive film which comprises a substrate layer containing a tetrafluoroethylene-based polymer having a storage modulus at 50°C of 400 to 800 MPa and a decreasing rate of a storage modulus in the temperature range from 50°C to 100°C of 20 to 75% and an adhesive layer containing a (meth)acrylate-based polymer in this order, wherein the swelling amount with respect to a polar solvent in the temperature range is less than 1 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive film and a method for manufacturing a semiconductor device using the adhesive film. [Background technology]

[0002] In the processing of semiconductor wafers or semiconductor chips, adhesive films having an adhesive layer on a film substrate of various resins such as tetrafluoroethylene-based polymers are used as dicing sheets for fixing semiconductor wafers and pick-up sheets for picking up semiconductor chips. Patent Document 1 also proposes a component supply sheet that includes a protective cover member made of a protective film and an adhesive layer made of a tetrafluoroethylene polymer, and a base sheet, which is supplied to a device that uses a device that picks up semiconductor elements by pushing them up, in order to place protective cover members for intermediate products in each manufacturing process (solder reflow, dicing, bonding, mounting) of semiconductor elements, circuit boards, microelectromechanical systems (MEMS), etc. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2021 / 141124 Summary of the Invention [Problem to be solved by the invention]

[0004] In the manufacturing process, the semiconductor wafer fixed on the dicing sheet and the semiconductor chips transferred onto the pickup sheet are cleaned by, for example, immersing them in a polar solvent or spraying them with vapor of a polar solvent. During such cleaning, the polar solvent comes into contact with not only the semiconductor wafer or semiconductor chip, but also the adhesive film, which is the dicing sheet or pick-up sheet. Although the film of the tetrafluoroethylene-based polymer as the substrate has excellent solvent resistance, the adhesive layer may swell due to the polar solvent, or the polar solvent may penetrate into the interface between the adhesive layer and the substrate layer or the interface between the adhesive layer and the adherend, causing cohesive failure of the adhesive layer or interfacial failure, and the adherend may fall off from the adhesive film. Furthermore, the peeling angle and peeling speed when peeling the adhesive film from the semiconductor wafer or semiconductor chip are limited, which may affect the productivity of the semiconductor manufacturing process.

[0005] The present inventors have found that an adhesive film having a base layer made of a polymer layer containing a tetrafluoroethylene-based polymer having a specific storage modulus and a pressure-sensitive adhesive layer preferably containing a specific (meth)acrylate-based polymer has excellent physical properties such as heat resistance and electrical insulation based on the tetrafluoroethylene-based polymer, excellent resistance to organic solvents, particularly polar solvents, and excellent adhesion and adhesion between the base layer and the pressure-sensitive adhesive layer. They have also found that such an adhesive film can be effectively applied to a method for manufacturing a semiconductor device, and have arrived at the present invention. An object of the present invention is to provide a pressure-sensitive adhesive film that has resistance to polar solvents, and is excellent in pressure-sensitive adhesive properties and adhesion between a substrate layer and a pressure-sensitive adhesive layer. [Means for solving the problem]

[0006] The present invention has the following aspects. [1] An adhesive film comprising, in this order, a base layer containing a tetrafluoroethylene-based polymer having a storage modulus of 400 to 800 MPa at 50°C and a rate of decrease in storage modulus in the temperature range from 50°C to 100°C of 20 to 75%, and an adhesive layer containing a (meth)acrylate-based polymer, wherein the amount of swelling in polar solvents in the above temperature range is less than 1 mass%. [2] The pressure-sensitive adhesive film of [1], wherein the tetrafluoroethylene-based polymer is a heat-fusible tetrafluoroethylene-based polymer having a melting point of 180 to 320°C. [3] The pressure-sensitive adhesive film of [1] or [2], wherein the base layer is made of a film of the tetrafluoroethylene-based polymer. [4] The pressure-sensitive adhesive film according to any one of [1] to [3], wherein the base layer is a molten sintered body of particles of the tetrafluoroethylene-based polymer, the average particle size of which is less than 10 μm. [5] The pressure-sensitive adhesive film according to any one of [1] to [4], wherein the base layer further contains a (meth)acrylate-based polymer, a polyimide-based polymer, or a polyester-based polymer. [6] The adhesive film of any of [1] to [5], wherein the (meth)acrylate polymer contains 50 mass% or more of units based on alkyl (meth)acrylate, and per 100 mass parts of the alkyl (meth)acrylate, alkyl (meth)acrylate having an alkyl group with 8 to 12 carbon atoms accounts for 95 mass parts or more. [7] The pressure-sensitive adhesive film of any one of [1] to [6], wherein isooctyl (meth)acrylate or lauryl (meth)acrylate accounts for more than 50 parts by mass per 100 parts by mass of the alkyl (meth)acrylate. [8] The pressure-sensitive adhesive film of any one of [1] to [7], wherein the pressure-sensitive adhesive layer further contains a crosslinking agent. [9] The pressure-sensitive adhesive film of any of [1] to [8], wherein the adhesive strength of the pressure-sensitive adhesive layer to a silicon mirror wafer as an adherend is lower than the adhesive strength to the base layer.

[10] The pressure-sensitive adhesive film of any of [1] to [9], wherein one surface of the base layer is surface-treated, and the pressure-sensitive adhesive layer is formed on the surface-treated surface.

[11] The pressure-sensitive adhesive film of any of [1] to

[10] , which has a primer layer between the base layer and the pressure-sensitive adhesive layer.

[12] The pressure-sensitive adhesive film of any one of [1] to

[11] , wherein the polar solvent is ethyl acetate, acetone, methyl ethyl ketone or N-methylpyrrolidone.

[13] An adhesive film according to any one of [1] to

[12] , which is an adhesive sheet for electronic component processing.

[14] A method for manufacturing a semiconductor device, comprising a step of contacting a laminate of an adhesive film and a semiconductor wafer or a semiconductor chip held on the adhesive film of any one of [1] to

[13] with a polar solvent.

[15] The manufacturing method according to

[14] , wherein the polar solvent is ethyl acetate, acetone, methyl ethyl ketone or N-methylpyrrolidone, and the step is a washing step of the semiconductor wafer or the semiconductor chip. Effect of the Invention

[0007] According to the present invention, it is possible to provide an adhesive film that has resistance to polar solvents, and is excellent in adhesiveness and adhesion between a base layer and an adhesive layer. Such an adhesive film can be effectively used as an adhesive sheet for processing electronic components in a method for manufacturing a semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The following terms have the following meanings. The "decrease rate of storage modulus in the temperature range of 50°C to 100°C" of a tetrafluoroethylene-based polymer is a percentage value obtained by dividing the storage modulus at 100°C by the storage modulus at 50°C, when the storage modulus is determined at 1 Hz while heating a tetrafluoroethylene-based polymer layer or film sample (5 mm x 3 cm x 100 μm thick) at a rate of 2 cm between gauge lines and a tensile deformation mode, while heating the sample at 2°C / min between 50°C and 100°C, using a dynamic viscoelasticity measuring device ("DVA-200" manufactured by IT Measurement & Control Co., Ltd.). The swelling amount of the adhesive film is a value calculated using the following formula from the mass (mass A) of a film 1 mm thick and 1 cm square made by laminating multiple sheets of adhesive film, and the mass (mass B) of the film obtained by immersing it in a polar solvent that has been left to stand in an 85°C / 85% RH environment for 1 hour and then drying it. Swelling amount [%] = (mass B - mass A) / mass A × 100 "Average particle size (D50)" is the volume-based cumulative 50% diameter of particles determined by laser diffraction / scattering. In other words, particle size distribution is measured by laser diffraction / scattering, and a cumulative curve is calculated with the total volume of the particle group as 100%, and the particle size is the point on the cumulative curve where the cumulative volume is 50%. The D50 of particles is determined by dispersing the particles in water and analyzing them by the laser diffraction / scattering method using a laser diffraction / scattering type particle size distribution measuring device (LA-920 measuring device, manufactured by Horiba, Ltd.). "Melting point" is the temperature corresponding to the maximum of the melting peak of a polymer as measured by differential scanning calorimetry (DSC). The "glass transition temperature (Tg)" is a value measured by analyzing a polymer using the dynamic mechanical analysis (DMA) method. The "viscosity" is determined by measuring the liquid composition using a Brookfield viscometer at 25° C. and a rotation speed of 30 rpm. The measurement is repeated three times, and the average value of the three measured values ​​is calculated. The term "unit" in a polymer means an atomic group based on a monomer formed by polymerization of the monomer. The unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a part of the unit is converted into a different structure by processing the polymer. Hereinafter, a unit based on monomer a is also referred to simply as a "monomer a unit."

[0009] The adhesive film of the present invention (hereinafter also referred to as "the present adhesive film") comprises, in this order, a base layer containing a tetrafluoroethylene-based polymer (hereinafter also referred to as "F polymer") having a storage modulus of 400 to 800 MPa at 50°C and a rate of decrease in storage modulus in the temperature range of 20 to 75% in the temperature range from 50°C to 100°C, and an adhesive layer containing a (meth)acrylate-based polymer, and has a swelling amount in polar solvents of less than 1 mass% in the above temperature range. The present pressure-sensitive adhesive film has excellent resistance to polar solvents, and is also excellent in adhesiveness and adhesion between the base layer and the pressure-sensitive adhesive layer. The reason for this is not entirely clear, but is thought to be as follows.

[0010] The base layer constituting this adhesive film has a certain rigidity in the so-called normal temperature range below 50°C, but in the temperature range of 50 to 100°C where this adhesive film is used, for example, when contacting with a polar solvent in a semiconductor manufacturing process, the storage modulus of the F polymer contained in the base layer is a predetermined decrease rate, which increases the flexibility of the base layer and is thought to suppress peeling from the adhesive layer. In addition, the adhesive layer, which is preferably based on a specific (meth)acrylate polymer described below and has a predetermined range of alkyl (meth)acrylate content, has low wettability to polar solvents, so that together with the base layer having solvent resistance based on the F polymer, swelling of the adhesive film due to polar solvents is suppressed, and it is thought to improve resistance to polar solvents in a concerted manner. As a result, even when the pressure-sensitive adhesive film comes into contact with a polar solvent, the pressure-sensitive adhesive layer is prevented from swelling or dissolving, and further from peeling off from the base layer, and the adhesive strength is maintained. Therefore, when the pressure-sensitive adhesive film is applied to a manufacturing method of a semiconductor device as a pressure-sensitive adhesive sheet for processing electronic components, it is possible to prevent the semiconductor wafer or semiconductor chip (adherend) from falling off or being damaged during the cleaning process of semiconductor manufacturing, and this can contribute to improving the production efficiency.

[0011] The (meth)acrylate polymer contained in the adhesive layer of this adhesive film preferably contains 50% by mass or more of units based on alkyl (meth)acrylate, and among 100 parts by mass of the alkyl (meth)acrylate, alkyl (meth)acrylates having an alkyl group with 8 to 12 carbon atoms account for 95 parts by mass or more. The content of units based on alkyl (meth)acrylate is preferably 65% ​​by mass or more, more preferably 75% by mass or more, and preferably 90% by mass or less. Further, the amount of alkyl (meth)acrylate having an alkyl group with 8 to 12 carbon atoms in 100 parts by mass of the alkyl (meth)acrylate is more preferably 97 parts by mass or more.

[0012] Examples of alkyl (meth)acrylates having an alkyl group with 8 to 12 carbon atoms include 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, etc. When the content of units based on these alkyl (meth)acrylates is within the above-mentioned range, the pressure-sensitive adhesive layer tends to have excellent both resistance to polar solvents and adhesiveness. Furthermore, from the viewpoint that longer-chain alkyl groups are present in the adhesive layer at a high density and resistance to polar solvents is easily improved, it is preferable that isooctyl (meth)acrylate or lauryl (meth)acrylate accounts for more than 50 parts by mass, more preferably 65 parts by mass or more, and even more preferably 80 parts by mass or more, per 100 parts by mass of alkyl (meth)acrylate. Examples of alkyl (meth)acrylates other than those mentioned above include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate.

[0013] The (meth)acrylate polymer may further contain units based on polymerizable monomers other than alkyl (meth)acrylates. Other polymerizable monomers include vinyl esters such as vinyl acetate, α-olefins such as ethylene, propylene, butene, unsaturated aromatic hydrocarbons such as styrene, dialkyl(meth)acrylamides, and functional group-containing monomers having a polymerizable double bond and a functional group such as a hydroxyl group, a carboxyl group, an amino group, a substituted amino group, an epoxy group, etc. Among these, functional group-containing monomers are preferred, and functional group-containing monomers having a hydroxyl group or a carboxyl group in the molecule are more preferred. Examples of such functional group-containing monomers include hydroxyl group-containing (meth)acrylates such as 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate; and carboxyl group-containing monomers such as acrylic acid, methacrylic acid, and itaconic acid. These may be used alone or in combination of two or more. The (meth)acrylate polymer preferably contains units based on a functional group-containing monomer in a proportion of 15 to 50% by mass, and more preferably 15 to 35% by mass. The method for producing the (meth)acrylate polymer is not particularly limited, and known methods such as solution polymerization and emulsion polymerization can be applied.

[0014] In addition, by reacting a functional group of a unit based on a functional group-containing monomer in the above-mentioned (meth)acrylate polymer with a polymerizable group-containing compound having a substituent reactive with the functional group and an active energy ray-polymerizable group such as a (meth)acryloyl group, an active energy ray-polymerizable group can be introduced into the side chain of the (meth)acrylate polymer, and an active energy ray-curable polymer that can be cured by active energy rays such as ultraviolet rays and electron beams can be obtained. In the case of a pressure-sensitive adhesive layer containing such an active energy ray-curable polymer, the pressure-sensitive adhesive layer can be cured by irradiation with active energy rays, thereby controlling the adhesiveness according to the application. The substituent of the polymerizable group-containing compound is preferably an isocyanate group, an epoxy group, etc. Examples of the polymerizable group-containing compound include (meth)acryloyloxyethyl isocyanate, 3-isopropenyl-α,α-dimethylbenzyl isocyanate, (meth)acryloyl isocyanate, allyl isocyanate, glycidyl (meth)acrylate; (meth)acrylic acid; a (meth)acryloyl monoisocyanate compound obtained by reacting a diisocyanate compound or a polyisocyanate compound with hydroxyethyl (meth)acrylate; and an acryloyl monoisocyanate compound obtained by reacting a diisocyanate compound or a polyisocyanate compound with a polyol compound and hydroxyethyl (meth)acrylate.

[0015] When the (meth)acrylate polymer is reacted with the polymerizable group-containing compound, the amount of the compound is preferably 50 to 100 mol %, more preferably 65 to 95 mol %, based on the content of the functional group-containing monomer in the (meth)acrylate polymer. If a part of the functional groups in the (meth)acrylate polymer is left unreacted, a crosslinked structure can be formed with a crosslinking agent described later, and the adhesiveness of the adhesive layer can be controlled. The weight average molecular weight of the active energy ray-curable polymer is preferably 100,000 or more and 1,500,000 or less. In this specification, "(meth)acrylate" is a term that collectively refers to acrylate, methacrylate, and both of them. "(meth)acryloyl" is a term that collectively refers to acryloyl, methacryloyl, and both of them.

[0016] The pressure-sensitive adhesive layer in the pressure-sensitive adhesive film may further contain a crosslinking agent. When the pressure-sensitive adhesive layer has a crosslinked structure due to the action of the crosslinking agent, the adhesiveness of the pressure-sensitive adhesive film does not decrease excessively, and the resistance of the pressure-sensitive adhesive layer to polar solvents is likely to be maintained. Examples of the crosslinking agent include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an imine-based crosslinking agent, etc. Among these, an isocyanate-based crosslinking agent is preferred. When a crosslinking agent is further contained, the amount thereof is preferably 0.8 parts by mass or less per 100 parts by mass of the (meth)acrylate polymer, more preferably in the range of 0.005 to 0.3 parts by mass, from the viewpoint of ensuring the resistance to polar solvents and adhesiveness of the adhesive layer of the present adhesive film.

[0017] The (meth)acrylate polymer or active energy ray curable polymer itself has adhesiveness. The adhesive layer is preferably formed from an adhesive composition containing a (meth)acrylate polymer or active energy ray curable polymer and, if necessary, a photopolymerization initiator. Here, the adhesive composition may contain other polymers, active energy ray polymerizable compounds, dyes, pigments, deterioration inhibitors, antistatic agents, flame retardants, silicone compounds, chain transfer agents, etc., within the range in which the adhesive layer can maintain resistance to polar solvents.

[0018] Examples of the photopolymerization initiator include a benzoin compound, an acetophenone compound, an acylphosphine oxide compound, a titanocene compound, a thioxanthone compound, a peroxide compound, etc. When a photopolymerization initiator is contained, the amount thereof is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the active energy ray-curable polymer.

[0019] The F polymer constituting the base layer of the present pressure-sensitive adhesive film is a polymer containing units (hereinafter also referred to as "TFE units") based on tetrafluoroethylene (hereinafter also referred to as "TFE"), which has a melting point of 180°C or higher. The melting point of the F polymer is more preferably 260°C or higher, and even more preferably 280°C or higher. The melting point of the F polymer is preferably 320°C or lower. In this case, the base layer of the present pressure-sensitive adhesive film is likely to have excellent heat resistance. The glass transition point of the F polymer is preferably 50° C. or higher, more preferably 75° C. or higher. The glass transition point of the F polymer is preferably 150° C. or lower, more preferably 125° C. or lower. The fluorine content of the F polymer is preferably 60% by mass or more, more preferably 70% by mass or more. The fluorine content of the F polymer is preferably 76% by mass or less.

[0020] The storage modulus of the F polymer at 50° C. is 400 to 800 MPa. Such a storage modulus is more preferably 450 MPa or more. Also, such a storage modulus is more preferably 700 MPa or less. Furthermore, the storage modulus of the F polymer at 50° C. is within the above range, and the rate of decrease in the storage modulus in the temperature range from 50° C. to 100° C. is within the range of 20 to 75%. The rate of decrease is more preferably 40% or more. Also, the rate of decrease is more preferably 65% ​​or less. When the storage modulus of the F polymer falls within the above range, the above-mentioned mechanism of action is more easily manifested, and the adhesion of the base layer to the pressure-sensitive adhesive layer of the present pressure-sensitive adhesive film and the resistance to polar solvents are improved.

[0021] The F polymer is preferably polytetrafluoroethylene (PTFE), a polymer containing TFE units and units based on ethylene (ETFE), a polymer containing TFE units and units based on propylene, a polymer containing TFE units and units based on perfluoro(alkyl vinyl ether) (PAVE) (PAVE units) (PFA), or a polymer containing TFE units and units based on hexafluoropropylene (FEP). These polymers may further contain units based on other comonomers. Examples of PTFE include low molecular weight PTFE and modified PTFE. PAVE is preferably CF2=CFOCF3, CF2=CFOCF2CF3 or CF2=CFOCF2CF2CF3 (hereinafter also referred to as "PPVE"), and more preferably PPVE.

[0022] The F polymer preferably has an oxygen-containing polar group, more preferably has a hydroxyl- or carbonyl-containing group, and even more preferably has a carbonyl-containing group. In this case, the adhesiveness between the base layer and the adhesive layer in the present pressure-sensitive adhesive film tends to be excellent. The hydroxyl-containing group is preferably a group containing an alcoholic hydroxyl group, more preferably -CF2CH2OH or -C(CF3)2OH. The carbonyl group-containing group is preferably a carboxyl group, an alkoxycarbonyl group, an amide group, an isocyanate group, a carbamate group (-OC(O)NH2), an acid anhydride residue (-C(O)OC(O)-), an imide residue (-C(O)NHC(O)-, etc.) or a carbonate group (-OC(O)O-), and more preferably an acid anhydride residue. When the F polymer has an oxygen-containing polar group, the number of oxygen-containing polar groups in the F polymer is 1×10 6 The number of oxygen-containing polar groups per unit is preferably 10 to 5000, more preferably 100 to 3000. The number of oxygen-containing polar groups in the F polymer can be quantified by the composition of the polymer or the method described in WO 2020 / 145133.

[0023] The oxygen-containing polar group may be contained in a unit based on a monomer in the F polymer, or may be contained in a terminal group of the main chain of the F polymer, the former being preferred. The latter embodiment includes an F polymer having an oxygen-containing polar group as a terminal group derived from a polymerization initiator, a chain transfer agent, etc., and an F polymer obtained by subjecting an F polymer to plasma treatment or ionizing radiation treatment.

[0024] The F polymer is preferably a polymer having a carbonyl group-containing group containing TFE units and PAVE units, more preferably a polymer containing TFE units, PAVE units, and units based on a monomer having a carbonyl group-containing group, and containing these units in this order, 90 to 99 mol%, 0.99 to 9.97 mol%, and 0.01 to 3 mol%, based on all units. Specific examples of such F polymers include the polymers described in WO 2018 / 16644. The monomer having a carbonyl group-containing group is preferably itaconic anhydride, citraconic anhydride, or 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also referred to as "NAH"), and more preferably NAH.

[0025] The content of the F polymer in the base layer is preferably 80% by mass or more, more preferably 90% by mass or more. The content may be 100% by mass or less than 100% by mass.

[0026] The substrate layer may further contain, in addition to the F polymer, another polymer selected from a (meth)acrylate-based polymer, a polyimide-based polymer, or a polyester-based polymer. Examples of the (meth)acrylate polymer include the same polymers as the (meth)acrylate polymers mentioned above in the explanation of the pressure-sensitive adhesive layer. Examples of the polyimide-based polymer include polyimide resins and polyamideimide resins. Among them, at least one aromatic imide polymer selected from the group consisting of aromatic polyimides, aromatic polyamic acids, aromatic polyamideimides, and aromatic polyamideimide precursors is preferred. Examples of polyester-based polymers include semi-aromatic polyesters such as polyethylene terephthalate, and liquid crystalline aromatic polyesters. These other polymers may be contained in one or more kinds. When the base layer further contains these other polymers, the affinity between the pressure-sensitive adhesive layer and the base layer is enhanced, and the adhesive strength between the layers is likely to be improved. When the other polymer is further contained, the content thereof is preferably 1 to 20% by mass relative to the F polymer.

[0027] In the present pressure-sensitive adhesive film, one surface of the base layer may be surface-treated, and the pressure-sensitive adhesive layer may be formed on the surface-treated surface. Surface treatment methods include corona discharge treatment, plasma treatment, UV ozone treatment, excimer treatment, chemical etching, silane coupling treatment, etc. By such surface treatment, oxygen-containing polar groups are introduced into the surface of the base layer that contacts the pressure-sensitive adhesive layer, increasing adhesion and improving the adhesive strength between the base layer and the pressure-sensitive adhesive layer. The pressure-sensitive adhesive film may have a primer layer between the substrate layer and the pressure-sensitive adhesive layer. The primer layer can be formed by applying a silane coupling agent or the like to the surface of the substrate.

[0028] The substrate layer in the present pressure-sensitive adhesive film is preferably formed from a resin film containing an F polymer. The substrate layer is preferably a molten sintered body of F polymer particles (hereinafter also referred to as "F particles") having an average particle size of less than 10 μm. Specifically, the substrate layer of the present pressure-sensitive adhesive film can be produced by a method in which a liquid composition containing F particles and a dispersion medium (hereinafter also referred to as "the present liquid composition") is applied to the surface of a base film and heated to form a molten sintered body.

[0029] The F particles preferably have an average particle size (D50) of 0.3 μm or more and less than 10 μm. The D50 of the F particles is preferably 0.5 μm or more, more preferably 1.0 μm or more. The D50 of the F particles is preferably less than 10 μm, more preferably 8 μm or less. In this case, the liquid composition is likely to have excellent dispersibility and processability, and excellent surface appearance. The F particles are particles containing an F polymer, and preferably consist of an F polymer. One type of F particle may be used, or two or more types of F particles may be used.

[0030] The dispersion medium contained in the present liquid composition is preferably at least one selected from the group consisting of water, amides, ketones and esters. Examples of amides include N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylpropanamide, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N,N-diethylformamide, hexamethylphosphoric triamide, and 1,3-dimethyl-2-imidazolidinone. Examples of the ketone include acetone, methyl ethyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl n-pentyl ketone, methyl isopentyl ketone, 2-heptanone, cyclopentanone, cyclohexanone, and cycloheptanone. Examples of the ester include methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, methyl pyruvate, ethyl pyruvate, methyl methoxypropionate, ethyl ethoxypropionate, ethyl 3-ethoxypropionate, γ-butyrolactone, and γ-valerolactone.

[0031] The liquid composition may further contain a surfactant. The surfactant is preferably a nonionic surfactant. Examples of the nonionic surfactant include glycol-based surfactants, acetylene-based surfactants, silicone-based surfactants, and fluorine-based surfactants.

[0032] The liquid composition may further contain another polymer different from the F polymer, selected from a (meth)acrylate-based polymer, a polyimide-based polymer, or a polyester-based polymer. Such another polymer may be contained in the liquid composition as non-hollow particles, or may be dissolved or dispersed in the dispersion medium constituting the liquid composition. By using a liquid composition containing such another polymer, a base layer containing the F polymer and the other polymer can be produced. The details of the other polymer selected from the (meth)acrylate-based polymer, the polyimide-based polymer, and the polyester-based polymer are the same as those of the other polymer that may be contained in the base layer. Among them, the aromatic imide polymer is preferably contained in the liquid composition as a varnish dissolved in a dispersion medium. When the present liquid composition further contains another polymer, the content of the other polymer relative to the F particles is preferably 1 to 20% by mass.

[0033] The present liquid composition may further contain additives such as a thixotropic agent, a viscosity modifier, an antifoaming agent, a dehydrating agent, a plasticizer, a weather resistance agent, an antioxidant, a heat stabilizer, a lubricant, an antistatic agent, a whitening agent, a colorant, a conductive agent, a release agent, and a flame retardant.

[0034] The content of F particles in the liquid composition is preferably 25% by mass or more, more preferably 30% by mass or more, and is preferably 75% by mass or less, more preferably 60% by mass or less. The viscosity of the liquid composition is preferably 10 mPa·s or more, more preferably 100 mPa·s or more. The viscosity of the liquid composition is preferably 10,000 mPa·s or less, more preferably 3,000 mPa·s or less. In this case, the liquid composition has excellent coatability and is easy to form a substrate layer having a desired thickness. In addition, the liquid composition having a viscosity in this range is easy to highly express the physical properties of the F polymer in the substrate layer formed therefrom.

[0035] This liquid composition can be subjected to a molding method such as extrusion into a sheet to form a molded product such as a sheet containing the F polymer. The sheet obtained by extrusion may be further cast by press molding, calendar molding, etc. The sheet is preferably further heated to remove the dispersion medium and bake the F polymer.

[0036] In addition, if the liquid composition is applied to the surface of a base film and heated to form a polymer layer containing the F polymer, i.e., a substrate layer, a laminate having the base film and the substrate layer in this order can be obtained. Examples of the base film include films of heat-resistant resins such as polyimide, polyamide, polyetheramide, polyphenylene sulfide, polyaryletherketone, polyamideimide, liquid crystal polyester, and tetrafluoroethylene polymer. The substrate layer is preferably formed by applying the liquid composition to the surface of a base film, heating to remove the dispersion medium, and further heating to sinter the F polymer. The substrate layer is separated from the resulting laminate to obtain a substrate layer containing the F polymer, which is a molten sintered body of the F particles.

[0037] Examples of methods for applying the present liquid composition include a coating method, a droplet discharging method, and a dipping method, and preferably a roll coating method, a knife coating method, a bar coating method, a die coating method, or a spray method. The heating for removing the dispersion medium is preferably performed at 100 to 200°C for 0.1 to 30 minutes. In this heating, the dispersion medium does not need to be completely removed, but only needs to be removed to the extent that the layer formed by the packing of the F particles can maintain a self-supporting film. In addition, when heating, air may be blown onto the surface to promote removal of the dispersion medium by air drying.

[0038] The heating for baking the F polymer is preferably carried out at a temperature equal to or higher than the melting point of the F polymer, more specifically, at 340 to 400° C. for 0.1 to 30 minutes. The heating device for each heating may be an oven or a ventilation drying furnace. The heat source in the device may be a contact type heat source (hot air, hot plate, etc.) or a non-contact type heat source (infrared rays, etc.). The heating may be carried out under normal pressure or under reduced pressure. The atmosphere during each heating may be either an air atmosphere or an inert gas atmosphere (helium gas, neon gas, argon gas, nitrogen gas, etc.).

[0039] The thickness of the base layer of the present pressure-sensitive adhesive film is preferably 20 μm or more and 200 μm or less. The thickness of the base layer is more preferably 25 μm or more, and even more preferably 50 μm or more. The thickness of the base layer is more preferably 110 μm or less, and even more preferably 90 μm or less. In this case, the above-mentioned effects are more effectively exhibited, and the adhesion between the base layer and the pressure-sensitive adhesive layer is more easily improved. In addition, the force resisting bending of the base material can be easily controlled within an appropriate range, making it easier to ensure pick-up properties in, for example, semiconductor manufacturing processes. The thickness of the pressure-sensitive adhesive layer is preferably in the range of 8 to 30 μm, more preferably 8 to 25 μm, from the viewpoint of ensuring resistance of the pressure-sensitive adhesive layer to polar solvents and adhesion to the adherend and the base layer.

[0040] The adhesive strength between the base layer and the adhesive layer is preferably 5 N / cm or more, more preferably 10 N / cm or more, in terms of peel strength. The upper limit of the peel strength is 100 N / cm. In this case, the adhesive film can be suitably used as an adhesive sheet for processing electronic parts. In the present pressure-sensitive adhesive film, it is preferable that the adhesive strength of the pressure-sensitive adhesive layer to the silicon mirror wafer as an adherend is lower than the adhesive strength to the base layer. Specifically, the adhesive strength of the adhesive layer when the adherend is a silicon mirror wafer is more preferably 0.1 to 2 N / cm in terms of peel strength. When the adhesive strength when the adherend is a silicon mirror wafer, is within the above range, the adhesive strength at the interface between the adhesive layer and the adherend surface is high, and the adhesive film can be effectively used as an adhesive sheet for electronic component processing that has higher resistance to polar solvents.

[0041] The adhesive film may further have a release sheet laminated on the surface of the adhesive layer in order to protect the adhesive layer before use. Examples of the release sheet include films made of resins such as polyethylene terephthalate, polypropylene, and polyethylene, or foamed films thereof; and papers such as glassine paper, coated paper, and laminated paper coated with a release agent such as silicone, fluorine, or carbamate containing a long-chain alkyl group. Furthermore, the surface of the base layer opposite to the surface having the pressure-sensitive adhesive layer may be coated with various coating films, or another film having high resistance to polar solvents may be laminated thereon.

[0042] The pressure-sensitive adhesive film can be produced by diluting the above-mentioned pressure-sensitive adhesive composition with a solvent as necessary, applying the composition to one surface of a base layer to a predetermined dry thickness, and drying the composition to form a pressure-sensitive adhesive layer. Alternatively, the pressure-sensitive adhesive composition can be diluted with a solvent as necessary, applying the composition to a release sheet to a predetermined dry thickness, and drying the composition to form a pressure-sensitive adhesive layer, which can then be transferred to the surface of the base layer.

[0043] The pressure-sensitive adhesive film has a swelling amount of less than 1% by mass in a polar solvent in the temperature range of 50° C. to 100° C. The swelling amount is preferably 0.1% by mass or less. The lower limit of the swelling amount is 0% by mass. Here, polar solvents include ethyl acetate, acetone, methyl ethyl ketone or N-methylpyrrolidone.When the swelling amount of these polar solvents is within the above-mentioned range, the deformation of the base layer and the adhesive layer is small, so that the peeling of the base layer and the adhesive layer is suppressed.In addition, the adhesion is easily maintained, and the adherend such as semiconductor wafer or semiconductor chip is not easily dropped off.

[0044] This adhesive film can be effectively used as an adhesive sheet for processing electronic components in a method for manufacturing a semiconductor device, which includes a step of contacting a laminate of this adhesive film and a semiconductor wafer (hereinafter also referred to simply as "wafer") or a semiconductor chip (hereinafter also referred to simply as "chip") held on the adhesive film with a polar solvent. Examples of sheets for processing electronic components include dicing sheets used to hold a wafer and the resulting chips when the wafer is diced, and pick-up sheets onto which a group of diced chips is transferred and then used to pick up the chips.

[0045] The adhesive film is particularly preferably applied to a semiconductor device manufacturing process including a step in which a semiconductor wafer or semiconductor chip (adherend) held on the adhesive film is contacted with a polar solvent, which specifically means a cleaning step in which adhesive or the like remaining on the adherend is removed. In detail, the wafer is transferred onto the dicing sheet, which is the adhesive film, and cut into individual circuits to form chips, and then the chips are picked up from the dicing sheet. When transferring the wafer onto the dicing sheet, the laminate of the dicing sheet and the wafer is brought into contact with a polar solvent. That is, the process includes a step of washing the wafer with a polar solvent while the wafer is held on the adhesive film. In addition, the wafer is held on a hard support such as glass, and the wafer is cut into individual chips through back grinding and processing, and the chips are picked up by transferring them to the pick-up sheet, which is the adhesive film. This process also includes a step of contacting the laminate of the pick-up sheet and the chips with a polar solvent, i.e., washing with a polar solvent while the chips are held on the adhesive film. The present pressure-sensitive adhesive film can be preferably used in the semiconductor device manufacturing process including these steps. Examples of polar solvents used for washing include ethyl acetate, acetone, methyl ethyl ketone, N-methylpyrrolidone, etc. Among them, it is preferable to use methyl ethyl ketone and N-methylpyrrolidone. After being peeled off from the dicing sheet or pick-up sheet, the chip is mounted on a circuit board or the like in a conventional manner, and then subjected to resin sealing or the like to obtain a semiconductor device.

[0046] The present adhesive film is preferably used as an adhesive sheet for processing electronic components in a method for manufacturing a semiconductor device, which includes a step of holding a semiconductor wafer or semiconductor chip having protruding electrodes such as cylindrical electrodes or spherical electrodes on its surface, or a semiconductor wafer or semiconductor chip having so-called through-hole vias (TSVs), and washing the held semiconductor wafer or chip with a polar solvent.

[0047] Although the present adhesive film and the manufacturing method of the semiconductor device have been described above, the present invention is not limited to the configuration of the above-mentioned embodiment. For example, the present adhesive film and the manufacturing method of the semiconductor device may have any other configuration in addition to the configuration of the above-mentioned embodiment, or may be replaced with any configuration that produces a similar effect. EXAMPLES

[0048] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. Details of the film used as the substrate of the pressure-sensitive adhesive film and the (meth)acrylate polymer contained in the pressure-sensitive adhesive layer are shown below. Base material 1: A polymer containing 97.9 mol% of TFE units, 0.1 mol% of NAH units, and 2.0 mol% of PPVE units, in that order, and having a carbonyl group-containing group with a main chain carbon number of 1×10 6 A 25 μm thick film containing a tetrafluoroethylene polymer (melting point: 300°C, storage modulus at 50°C: 500 MPa, reduction in storage modulus at 50°C to 100°C: 60%) having 1000 molecules per unit. Substrate 2: A 25 μm thick film containing a tetrafluoroethylene polymer containing 45 mol % and 55 mol % of TFE units and ethylene units, in that order (storage modulus at 50° C.: 710 MPa, reduction rate of storage modulus at 50° C. to 100° C.: 22%) Substrate 3: A 25 μm thick film containing a tetrafluoroethylene polymer containing TFE units and vinylidene fluoride-based units (storage modulus at 50° C.: 800 MPa, reduction rate of storage modulus at 50° C. to 100° C.: 18%) (Meth)acrylate polymer 1: A UV-curable polymer having a number average molecular weight of 600,000, obtained by reacting a (meth)acrylate polymer containing 80% by mass of units based on lauryl acrylate and 20% by mass of units based on 2-hydroxyethyl acrylate with methacryloyloxyethyl isocyanate.

[0049] [Examples 1-3] A liquid adhesive composition containing a (meth)acrylate polymer 1 was applied to a release film ("SP-PET3811" manufactured by Lintec Corporation) and dried at 100°C for 1 minute to obtain an adhesive layer having a thickness of 10 μm. The adhesive layer and substrate 1 were then bonded together, and the release film was removed to obtain adhesive film 1. Further, adhesive film 2 and adhesive film 3 were obtained in the same manner, except that substrate 1 was replaced with substrate 2 and substrate 3, respectively. Each adhesive film was attached to the mirror surface of a silicon mirror wafer and then fixed by irradiation with ultraviolet light, and then immersed in N-methylpyrrolidone at 75° C. for 15 minutes. Next, the adhesive films were attempted to be peeled off from the silicon wafer at a tensile speed of 300 mm / min and a peeling angle of 180°. As a result, Adhesive Film 1 and Adhesive Film 2 could be peeled off without leaving any adhesive layer on the silicon mirror wafer, but this was not possible with Adhesive Film 3. Furthermore, when the polar solvent was N-methylpyrrolidone, the swelling amounts of Adhesive Film 1 and Adhesive Film 2 were each less than 1 mass%. [Industrial Applicability]

[0050] The adhesive film of the present invention has resistance to polar solvents, and has excellent adhesion and adhesion between the substrate layer and the adhesive layer.Therefore, it can be suitably used in the manufacture of semiconductor devices, for example, as an adhesive sheet for electronic component processing.The adhesive film of the present invention can also be used as a release film used in the resin sealing process of semiconductors, a component protection tape used in the reflow process, a masking tape used in high-temperature painting, a masking tape used in the sputtering process, a masking tape used in the deposition process, and an electrical insulating film.

Claims

1. The adhesive film comprises, in this order, a base layer containing a tetrafluoroethylene-based polymer having a storage modulus of 400 to 800 MPa at 50°C and a rate of decrease in storage modulus in the temperature range of 20 to 75% in the temperature range from 50°C to 100°C, and an adhesive layer containing a (meth)acrylate-based polymer, and the adhesive film has an amount of swelling in polar solvents of less than 1 mass% in the above temperature range.

2. The pressure-sensitive adhesive film according to claim 1, wherein the tetrafluoroethylene-based polymer is a heat-meltable tetrafluoroethylene-based polymer having a melting point of 180 to 320°C.

3. The pressure-sensitive adhesive film according to claim 1 , wherein the base layer is made of a film of the tetrafluoroethylene-based polymer.

4. The pressure-sensitive adhesive film according to claim 1 , wherein the base layer is a molten sintered body of the tetrafluoroethylene polymer particles having an average particle size of less than 10 μm.

5. The pressure-sensitive adhesive film according to claim 1 , wherein the base layer further contains a (meth)acrylate-based polymer, a polyimide-based polymer, or a polyester-based polymer.

6. The (meth)acrylate-based polymer contains 50% by mass or more of units based on alkyl (meth)acrylate, and in 100 parts by mass of the alkyl (meth)acrylate, the alkyl group has 8 to 12 carbon atoms. The adhesive film according to claim 1.

7. The pressure-sensitive adhesive film according to claim 1 , further comprising more than 50 parts by mass of isooctyl (meth)acrylate or lauryl (meth)acrylate per 100 parts by mass of the alkyl (meth)acrylate.

8. The pressure-sensitive adhesive film according to claim 1 , wherein the pressure-sensitive adhesive layer further contains a crosslinking agent.

9. The adhesive film according to claim 1 , wherein the adhesive strength of the adhesive layer to a silicon mirror wafer as an adherend is lower than the adhesive strength to the base layer.

10. The pressure-sensitive adhesive film according to claim 1 , wherein one surface of the base layer is surface-treated, and the pressure-sensitive adhesive layer is formed on the surface-treated surface.

11. The pressure-sensitive adhesive film according to claim 1 , further comprising a primer layer between the base layer and the pressure-sensitive adhesive layer.

12. The pressure-sensitive adhesive film according to claim 1, wherein the polar solvent is ethyl acetate, acetone, methyl ethyl ketone or N-methylpyrrolidone.

13. The pressure-sensitive adhesive film according to any one of claims 1 to 12, which is an adhesive sheet for processing electronic parts.

14. A method for manufacturing a semiconductor device comprising a step of contacting a laminate of the adhesive film and the semiconductor wafer or the semiconductor chip with a polar solvent while holding a semiconductor wafer or a semiconductor chip on the adhesive film according to any one of claims 1 to 13.

15. 15. The method according to claim 14, wherein the polar solvent is ethyl acetate, acetone, methyl ethyl ketone or N-methylpyrrolidone, and the step is a cleaning step of the semiconductor wafer or the semiconductor chip.