Method for manufacturing transparent conductive film

A solvent-free conductive film formation process using a transparent conductive active energy ray-curable composition, involving heating and curing, addresses the limitations of solvent-free paints by enhancing adhesion and film hardness while maintaining electrical properties and transparency.

JP2024143547APending Publication Date: 2024-10-11MAXELL LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023056282
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Solvent-free conductive paints face challenges in achieving high solid content concentration for improved electrical characteristics while maintaining adhesion and film hardness, with conventional methods leading to poor adhesion and film hardness due to increased non-curing components like fillers and dispersants.

Method used

A method involving the application of a solvent-free transparent conductive active energy ray-curable composition containing inorganic conductive fine particles, followed by heating and irradiation with active energy rays to form a cured film, which includes a coating film forming, heating, and curing process to enhance adhesion and film hardness.

Benefits of technology

The method results in a transparent conductive film with high antistatic performance, excellent adhesion to substrates, and improved film hardness, while maintaining transparency and reducing surface electrical resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143547000001
    Figure 2024143547000001
  • Figure 2024143547000002
    Figure 2024143547000002
  • Figure 2024143547000003
    Figure 2024143547000003
Patent Text Reader

Abstract

To provide a method for manufacturing a transparent conductive film high in adhesion to a base material and film hardness while having high anti-static performance from a solventless transparent conductive active energy ray curable composition.SOLUTION: This method for manufacturing a transparent conductive film containing inorganic conductive fine particles comprises: a step of forming, on a base material, a coated film of a transparent conductive active energy ray curable composition containing inorganic conductive fine particles, an active energy ray curable composition, and a polymerization initiator and having a content of an organic solvent and water of 5 mass% or less; a step of heating the coated film; and a step of irradiating the heated coated film with an active energy ray to form a cured film.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a transparent conductive film containing inorganic conductive fine particles. [Background technology]

[0002] Conventionally, conductive paints containing conductive materials have been widely used to perform antistatic treatment on the surfaces of plastic articles and the like. In recent years, solvent-free paint compositions have been developed as such conductive paints from the viewpoints of environmental consideration, safety, work efficiency, etc. For example, Patent Documents 1 and 2 disclose solvent-free paint compositions containing conductive fine particles and photocurable resins or monomers. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 8-27405 [Patent Document 2] JP 2008-143999 A Summary of the Invention [Problem to be solved by the invention]

[0004] Solvent-free conductive paints are limited in solid content concentration to ensure coating properties, and it is difficult to incorporate a sufficient amount of conductive material. This makes it difficult to improve electrical properties. There are also attempts to increase the solid content concentration by improving the dispersibility of fillers such as inorganic conductive fine particles, but this leads to an increase in non-cured components such as fillers and dispersants in the transparent conductive film, which is a factor that inhibits adhesion and film hardness. In other words, the adhesion and film hardness of the obtained conductive film to the substrate are not necessarily fully satisfactory, and a conductive film that is excellent in all of electrical properties, adhesion and film hardness is desired. In particular, in conductive paints for obtaining transparent conductive films, the demand for improving electrical properties, adhesion and film hardness while ensuring high transparency must be achieved, which is very difficult.

[0005] An object of the present invention is to provide a method for forming a transparent conductive film having high antistatic performance while also exhibiting excellent adhesion to a substrate and film hardness, from a solvent-free transparent conductive active energy ray-curable composition. [Means for solving the problem]

[0006] The present inventors have conducted intensive research to solve the above problems and have completed the present invention. That is, the present invention provides the following preferred embodiments. [1] A method for producing a transparent conductive film containing inorganic conductive fine particles, comprising the steps of: A step of forming a coating film of a transparent conductive active energy ray curable composition on a substrate, the coating film comprising inorganic conductive fine particles, an active energy ray curable compound, and a polymerization initiator, the composition having an organic solvent and water content of 5 mass % or less; heating the coating; and A step of irradiating the heated coating film with active energy rays to form a cured film. A method comprising: [2] The method according to [1] above, wherein the step of heating the coating film is carried out by convection, conduction or radiation. [3] The method according to [1] or [2] above, further comprising the step of forming a cured film in air after the step of heating the coating film. [4] The method according to any one of [1] to [3] above, wherein the content of the monofunctional active energy ray-curable compound in the transparent conductive active energy ray-curable composition is 15 mass% or less based on the total mass of the curable composition. [5] The method according to any one of the above [1] to [4], wherein the inorganic conductive microparticles include at least one selected from the group consisting of tin oxide, antimony-containing tin oxide (ATO), phosphorus-containing tin oxide (PTO), zinc oxide, aluminum-containing zinc oxide (AZO), gallium-containing zinc oxide (GZO), antimony oxide, indium oxide, tin-containing indium oxide (ITO), silver nanoparticles, silver nanowires, copper nanoparticles, and carbon nanotubes. [6] The method according to any one of the above [1] to [5], wherein the active energy ray-curable compound contains an active energy ray-curable compound having a vapor pressure of 1.0 Pa or more and 500 Pa or less at 25°C. [7] The substrate has a surface free energy of 20-40 mJ / m 2 The method according to any one of the above [1] to [6], wherein the substrate is a material selected from the group consisting of fluorine, fluorine- ... [8] The method according to any one of the above [1] to [7], wherein the inorganic conductive fine particles are antimony-containing tin oxide (ATO). [9] The method according to any one of the above [1] to [8], wherein the inorganic conductive fine particles contain aggregated particles, and the average aggregated particle diameter of the aggregated particles is 90 nm or more and 180 nm or less.

[10] The method according to any one of the above [1] to [9], wherein the transparent conductive active energy ray-curable composition further contains a dispersant.

[11] The method according to

[10] above, wherein the dispersant is a polymer having an acid value of 100 KOHmg / g or more.

[12] The method according to

[10] or

[11] , wherein the dispersant is a polymer containing a structural unit having at least one selected from the group consisting of a carboxyl group, a sulfonic acid group, a phosphonic acid group, a phosphoric acid group and a hydroxyl group. Effect of the Invention

[0007] According to the present invention, it is possible to provide a method for forming a transparent conductive film having high antistatic performance while also exhibiting excellent adhesion to a substrate and film hardness, from a solvent-free transparent conductive active energy ray-curable composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.

[0009] The method for producing a transparent conductive film of the present invention is a method for forming a conductive film from a so-called solventless conductive active energy ray-curable composition that does not substantially contain a solvent. The method for producing a transparent conductive film of the present invention includes the following steps: A step of forming a coating film of a transparent conductive active energy ray curable composition containing inorganic conductive fine particles, an active energy ray curable compound, and a polymerization initiator, and having an organic solvent and water content of 5 mass % or less on a substrate (hereinafter also referred to as a "coating film forming step"); A step of heating the coating film (hereinafter also referred to as a "coating film heating step"); and A step of irradiating the heated coating film with active energy rays to form a cured film (hereinafter also referred to as the "cured film forming step"). Includes.

[0010] <Coating film formation process> The coating film forming step is a step of applying a transparent conductive active energy ray curable composition onto a substrate to form a coating film of the conductive composition. The transparent conductive active energy ray curable composition used in the method of the present invention (hereinafter also simply referred to as "conductive composition" or "conductive composition of the present invention") is a solventless composition containing inorganic conductive fine particles, an active energy ray curable compound, and a polymerization initiator, and containing 5 mass% or less of organic solvent and water. The specific composition and preferred embodiments will be described in detail later.

[0011] The substrate for forming the coating film of the conductive composition can be selected from substrates made of various materials known in the art according to the composition of the conductive composition, the characteristics and applications of the conductive film, recycling, environmental regulations, use restrictions due to chemical safety, etc. Substrates that can be used for forming the conductive film include, for example, glass substrates, ceramic substrates, polyester-based resins such as polyethylene terephthalate and polyethylene naphthalate, polyolefins, cellulose-based resins such as cellulose triacetate, amide-based resins such as nylon and aramid, polyether-based resins such as polyphenylene ether and polysulfone ether, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyamideimide-based resins, aromatic polyamide-based resins, cycloolefin polymers, polyvinyl chloride, polyacrylic resins, polystyrene resins, acetal resins such as polyoxymethylene, and the like.

[0012] Conventionally, in the coating film forming process, when a substrate made of a material with low surface free energy is used, the wettability of the coating material is poor, and surface cissing is likely to occur. Furthermore, due to the difference in surface free energy between the composition to be applied and the substrate, uneven distribution of the composition material occurs on the coating film surface, inside the coating film, and at the substrate interface, which may result in poor adhesion and film hardness. In contrast, the coating film heating process in the method of the present invention has the effect of promoting material convection in the wet coating film and preventing uneven distribution of the materials. It is considered that the coating film heating process can prevent unnecessary aggregation of fillers, particularly inorganic conductive fine particles, and can bring about homogenization of the active energy ray curable compound and the polymerization initiator, thereby maximizing the blending effect of each component. Therefore, in the method of the present invention, even when a substrate made of a material with relatively low surface free energy is used, a transparent conductive film that has high antistatic performance and excellent adhesion to the substrate and film hardness can be provided. Therefore, in one embodiment of the present invention, when a substrate made of a material with low surface free energy is used as the substrate, the effect of the present invention can be obtained more significantly.

[0013] In this specification, a "material with low surface free energy" is a material with a surface free energy of 40 mJ / m 2In one embodiment of the present invention, the surface free energy of the substrate is preferably 20 to 40 mJ / m 2 , more preferably 27 to 40 mJ / m 2 , and more preferably 32 to 40 mJ / m 2 When the surface free energy of the substrate is within the above range, the above-mentioned effects of the present invention can be expected to be further enhanced.

[0014] The surface free energy of the substrate can be measured, for example, by a contact angle method or a wetting reagent method. In detail, it can be measured by the method described in the examples below.

[0015] The surface free energy of the substrate can be controlled within a desired range by, for example, appropriately selecting the material constituting the substrate, the processing method of the substrate, and the surface treatment method of the substrate. For example, a substrate with low surface free energy can be obtained by selecting a resin material with low surface energy as described later, or by surface treatment such as physical surface treatment or chemical surface treatment.

[0016] Various resins can be used as materials that can form a substrate with low surface free energy. Examples of such resin materials include those exemplified above as resin materials that form a resin film substrate. In particular, resins having a surface free energy of 20 to 40 mJ / m 2 Examples of resin materials suitable for forming the substrate include polyolefins such as polypropylene and polyethylene, polyether resins such as polyvinyl chloride, polyvinyl fluoride, and polyphenylene ether, polyacrylic resins, polyvinyl alcohol, polystyrene resins, and acetal resins such as polyoxymethylene. These may be used alone or in combination of two or more. Among them, from the viewpoints of versatility, processability, and cost, a substrate formed by containing at least one resin material selected from polyvinyl chloride, polyacrylic resin, and acetal resin is preferred. Such a resin can be formed into a resin film substrate by known means such as a solvent casting method or a melt extrusion method.

[0017] Surface treatments for controlling the surface free energy of the substrate surface within the desired range include physical surface treatments and chemical surface treatments, such as a method of treating the substrate surface with corona or plasma under an atmosphere ranging from vacuum to atmospheric pressure, a method of laser treating the substrate surface, a method of ozone treating the substrate surface, a method of saponifying the substrate surface, a method of flame treating the substrate surface, a method of coating the substrate surface with a coupling agent, a method of primer treating the substrate surface, and a method of cleaning the substrate surface with a chemical solution such as acid or alkali. Among these, the method of treating the substrate surface with corona or plasma is preferred from the viewpoint of processability and ease of control of the surface free energy.

[0018] The method for applying the conductive composition onto the substrate is not particularly limited, and examples thereof include coating methods such as gravure roll method, microgravure roll method, microgravure coater method, slit die coating method, spray method, spin method, reverse roll method, dip method, bar coating method, etc., and printing methods such as gravure printing, screen printing, offset printing, inkjet method, etc. For these coating methods, a known coater corresponding to the coating method to be adopted can be used.

[0019] The thickness of the coating film (wet film thickness) when the conductive composition is applied onto a substrate can be appropriately determined depending on the composition and viscosity of the conductive composition, the properties and use of the conductive film, etc. In one embodiment of the present invention, the thickness of the coating film (wet film thickness) is preferably 1.0 to 30.0 μm, more preferably 1.2 to 25.0 μm, and even more preferably 1.5 to 20.0 μm. When the thickness of the coating film (wet film thickness) is within the above range, the coating film can be efficiently heated in the heating step following the coating film formation step. This can increase the concentration of inorganic conductive fine particles in the resulting coating film (the content of inorganic conductive fine particles per thickness of the conductive film), and can reduce the surface electrical resistance value of the conductive film. The thickness of the coating film can be measured by, for example, a contact type film thickness gauge such as a comb type, rotary type, electromagnetic induction type, eddy current type, electrical resistance type, electrolytic type, ultrasonic type, or stylus type, a non-contact type film thickness gauge such as a reflection spectroscopy type, infrared type, electrostatic capacitance type, or radiation type (fluorescent X-ray, beta ray), or a cross-sectional observation type film thickness gauge such as a transmission electron microscope (TEM) or a scanning electron microscope (SEM). Of these, for measuring the wet film thickness, a contact type film thickness gauge such as a comb type or rotary type, which is easy to use and has good washability, or a non-contact type film thickness gauge such as a reflection spectroscopy type, which can be used online without applying curing energy, is preferred.

[0020] <Coating film heating process> The coating film heating step is a step of heating the coating film of the conductive composition formed in the coating film forming step. The present invention is a method for producing a conductive film from a solvent-free active energy ray curable conductive composition that does not substantially contain a solvent such as an organic solvent or water. Conventionally, in a method for producing a cured film from such a solvent-free active energy ray curable composition, after forming a coating film of the composition, a step of curing the active energy ray curable compound is performed without going through a heating step. This is because the solvent-free active energy ray curable composition does not have a solvent to be removed before curing the active energy ray curable compound, so there is no need for heating. In addition, not requiring a heating step is also advantageous in terms of production efficiency. In contrast, the present inventors have found that the surface electrical resistance value of the obtained conductive film can be greatly reduced by using a solvent-free conductive composition and heating the coating film after forming the coating film of the composition and before curing the active energy ray curable compound. This is thought to be because, although not necessarily limited to, the coating film heating step partially evaporates the active energy ray curable compound constituting the coating film, thereby increasing the content (concentration) of inorganic conductive fine particles per thickness of the coating film obtained. In addition, the method of the present invention in which the concentration of inorganic conductive fine particles in the coating film is increased by heating the coating film is also advantageous in that good coatability based on a moderate viscosity can be ensured during coating. Furthermore, the present inventors have found that heating before curing can also improve film hardness, adhesion to the substrate, and transparency. This is thought to be because the coating film heating step has the effect of promoting material convection in the wet coating film and preventing uneven distribution of materials, and in particular prevents unnecessary aggregation of fillers such as inorganic conductive particles, and maximizes the blending effect of each component by homogenizing the active energy ray curable compound and the polymerization initiator. In other words, it is presumed that preventing uneven distribution of the composition material on the coating film surface, inside the coating film, and at the substrate interface suppresses a decrease in adhesion due to uncured parts of the curable compound at the coating film / substrate interface and non-cured components such as fillers and dispersants, such as inorganic conductive fine particles, and promotes a crosslinked network between the curable compound and the polymerization initiator, thereby improving film hardness.

[0021] The heating method of the coating film in the coating film heating step can be appropriately determined depending on the composition of the conductive composition, the type of substrate, the properties and applications of the conductive film, etc. From the viewpoint of heating efficiency and workability, in the method of the present invention, the heating step is preferably performed by a convection heat transfer method, a conduction heat transfer method, or a radiation heat transfer method. As the heating method, one method may be adopted, or two or more methods may be adopted in combination.

[0022] The convection heat transfer method is a method in which a heating fluid such as heated air (hot air) heated to a high temperature is brought into direct contact with the coating to be treated, and the heat of the heating fluid is supplied to the coating. Heating of the coating by the convection heat transfer method can be carried out using a known dryer capable of heating by the convection heat transfer method, such as a hot air dryer, a hot air oven, a dryer, a box dryer, a band dryer, a spray dryer, a fluidized bed dryer, a flash dryer, or a jet flow dryer (nozzle jet).

[0023] The conductive heat transfer method is a method in which the coating film with the substrate is brought into contact with a high-temperature body such as a heated heating roll, and the coating film is heated by thermal conduction through the contact surface. Heating of the coating film by the conductive heat transfer method can be performed using a known device capable of heating by the conductive heat transfer method, such as a heated roll, a vacuum dryer, a box dryer, an agitator dryer, a cylindrical dryer (drum dryer), or a multi-cylinder dryer (cylinder dryer).

[0024] The radiation heat transfer method, also called axial radiation heat transfer method, is a method that utilizes the radiant energy of infrared rays emitted by a high-temperature body as a heat source, and the infrared rays absorbed by the coating film are converted into heat to heat the coating film. Heating of the coating film by the radiation heat transfer method can be performed using a known device capable of heating by the radiation heat transfer method, such as an infrared heater, a far-infrared heater, or an infrared lamp.

[0025] The heating conditions in the coating heating step can be appropriately determined depending on the composition of the conductive composition, the heating method to be adopted, the type of substrate, the properties and applications of the conductive film, and the like.

[0026] In one embodiment of the present invention, the heating temperature may be, for example, 50 to 150°C, preferably 60 to 120°C, more preferably 70 to 110°C, and even more preferably 80 to 100°C. When the heating temperature in the coating film heating step is within the above range, the coating film can be efficiently heated and a part of the active energy ray curable compound constituting the coating film can be evaporated. This reduces the thickness of the resulting coating film (hereinafter also referred to as "dried coating film"), and the content of inorganic conductive fine particles per thickness of the coating film can be increased. By increasing the content of inorganic conductive fine particles per thickness of the coating film, the surface electrical resistance of the resulting conductive film can be significantly reduced. In addition, excessive evaporation of the active energy ray curable compound can be prevented, and a conductive film with excellent film hardness can be obtained. On the other hand, when the heat resistance temperature or melting point of the substrate is low, if the heating temperature becomes too high, the substrate may be deformed. When a substrate made of a thermoplastic resin is used, the coating film heating step is usually preferably 100°C or less. In this specification, the heating temperature means the temperature of the space or the coating film measured directly at the same position where heating energy is applied to the coating film in various drying methods.

[0027] In one embodiment of the present invention, the heating time may be, for example, 10 seconds to 10 minutes, preferably 10 seconds to 8 minutes, more preferably 10 seconds to 5 minutes, and further preferably 30 seconds to 3 minutes. When the heating time in the coating film heating step is within the above range, the coating film can be efficiently heated and a part of the active energy ray curable compound constituting the coating film can be evaporated. This can increase the content of inorganic conductive fine particles per thickness of the dried coating film. By increasing the content of inorganic conductive fine particles per thickness of the coating film, the surface electrical resistance of the obtained conductive film can be significantly reduced. In addition, excessive evaporation of the active energy ray curable compound can be prevented, and a conductive film with excellent film hardness can be obtained. On the other hand, when the thickness of the substrate is thin, if the heating time is too long, deformation such as curling or shrinkage of the substrate may occur. For example, when a substrate with a thickness of 5 μm to 5000 μm is used, the coating film heating step is usually preferably less than 10 minutes.

[0028] In the method of the present invention, the coating film is preferably heated so that the thickness of the dried coating film obtained after heating (dry film thickness) is thinner than the thickness of the coating film before heating (wet film thickness). The thinner film thickness of the dried coating film increases the content of inorganic conductive fine particles per thickness of the coating film. This can reduce the surface electrical resistance of the obtained conductive film. In one embodiment of the present invention, the dry film thickness of the coating film after the coating film heating step is preferably 98% or less, more preferably 90% or less, even more preferably 80% or less, particularly preferably 70% or less of the wet film thickness of the coating film before drying, and in some cases may be, for example, 60% or less, or 55% or less. The film thickness before and after the heating step can be controlled by appropriately selecting the drying temperature and drying time depending on the composition of the conductive composition, the heating method used, and the like. The thickness of the coating film can be measured using, for example, a contact type film thickness gauge such as an electromagnetic induction type, an eddy current type, an electrical resistance type, an electrolysis type, an ultrasonic type, or a stylus type; a non-contact type film thickness gauge such as a reflection spectroscopy type, an infrared type, an electrostatic capacitance type, or a radiation type (fluorescent X-ray, beta ray); or a cross-sectional observation type film thickness gauge such as a transmission electron microscope (TEM) or a scanning electron microscope (SEM).

[0029] The thickness of the dry coating film (dry film thickness) can be appropriately determined depending on the composition of the conductive composition, the properties and use of the conductive film, the heating method, etc. In one embodiment of the present invention, the thickness of the dry coating film (dry film thickness) is preferably 0.3 to 25 μm, more preferably 0.4 to 20 μm, and even more preferably 0.5 to 15 μm. When the thickness of the dry coating film (dry film thickness) is within the above range, the content of inorganic conductive fine particles per thickness of the conductive film is likely to be increased, and the surface electrical resistance value of the conductive film is likely to be significantly reduced. In addition, the film hardness and adhesion are likely to be improved.

[0030] In a preferred embodiment of the present invention, the coating film heating step is carried out by a method including a convection heat transfer method, specifically, a convection heat transfer method using a hot air dryer, a hot air oven, or a dryer is preferred.

[0031] <Cured film formation process> The cured film forming step is a step of forming a cured film by irradiating the heated coating film with active energy rays. The heated coating film is irradiated with active energy rays to polymerize and cure the active energy ray curable compound in the coating film, thereby forming a conductive film as a cured film of the conductive composition. In the method of the present invention, the heated coating film can be used in the cured film forming step without cooling. The advantages of curing a wet coating film of a solventless conductive composition while heating it include the fact that the convection of the curable compound (hereinafter also referred to as the "solvent monomer") that also functions as a solvent promotes the dispersion and homogenization of various materials, and that the diffusion rate (mobility) of the initiator radicals and monomer radicals can be increased by reducing the viscosity of the solvent monomer, thereby improving transparency, adhesion, and / or film hardness. On the other hand, the process of cooling the heated wet coating film may cause supersaturated precipitation of materials that have low solubility in the solvent monomer, or unnecessary aggregation of inorganic conductive fine particles. By curing the wet coating film without cooling it, the decrease in conductivity and transparency caused by the cooling process can be suppressed. In addition, the work process and time are shortened, which is also advantageous in improving production efficiency.

[0032] The light to be irradiated to the dried coating film is appropriately selected according to the type of active energy ray curable compound contained in the dried coating film (particularly, the type of polymerizable group that the curable compound has), the type of polymerization initiator and the amount thereof.Specifically, for example, one or more active energy rays selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays and γ rays and active electron rays can be mentioned.Among them, ultraviolet light is preferred because it is easy to control the progress of polymerization reaction and can use equipment that is widely used in the field.

[0033] Examples of the light source of the active energy rays include a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 265 to 440 nm, a chemical lamp, a black light lamp, a microwave excited mercury lamp, and a metal halide lamp.

[0034] The conditions for irradiation with active energy rays are appropriately determined depending on the composition of the conductive composition, and are not particularly limited. For example, the cumulative light amount is preferably 10 to 3,000 mJ / cm. 2 , more preferably 50 to 2,000 mJ / cm 2 , and more preferably 100 to 1,000 mJ / cm 2 The irradiation intensity, number of irradiations, and irradiation time can be appropriately determined so as to achieve the above.

[0035] In one embodiment of the present invention, the cured film forming step is preferably carried out under air. Carrying out the cured film forming step under air means that the coating film of the conductive composition irradiated with the active energy rays is irradiated with the active energy rays in a state where the coating film is exposed to air. An example of a state where the coating film is not exposed to air is when, for example, the conductive composition is applied to a substrate to form a coating film, and then the coating film is covered with an appropriate resin film for the purpose of preventing polymerization inhibition caused by oxygen, and the film is used in the coating film heating step or the cured film forming step. By carrying out the cured film forming step under air, the evaporation of the active energy ray curable compound contained in the conductive composition is easily carried out appropriately. This makes it possible to increase the content of inorganic conductive fine particles per thickness of the conductive film, and the surface electrical resistance of the conductive film is easily reduced significantly. In addition, due to the synergistic effects of active material convection, reduction in film thickness, and increase in the content of inorganic conductive fine particles caused by heating and evaporation of the wet coating film, the film hardness and adhesion can be further improved. Furthermore, when the cured film formation step is carried out under air, there is no need to provide a layer on the coating film to isolate the coating film from air as described above, and there is also no need to remove this layer after the coating film is cured, which is advantageous in terms of production efficiency and cost of the conductive film.

[0036] <Conductive composition> In the method of the present invention, a conductive film is formed from a so-called solventless conductive composition that contains inorganic conductive fine particles, an active energy ray-curable compound, and a polymerization initiator, and has an organic solvent and water content of 5 mass% or less.

[0037] (Inorganic conductive fine particles) The conductive composition used in the method of the present invention contains inorganic conductive fine particles. By containing inorganic conductive fine particles, the desired electrical properties can be imparted to the cured film obtained from the conductive composition. In general, inorganic conductive fine particles and dispersants are non-curable components, and when present at the substrate interface, they tend to be inhibitors and reduce the adhesion of the resulting cured film. However, in the present invention, even if a relatively large content of inorganic conductive fine particles is mixed, the dispersion and homogenization of various materials due to the solvent monomer convection in the coating film heating process can suppress the decrease in adhesion, so that high adhesion to the substrate can be ensured. As a result, the conductive film obtained by the method of the present invention can ensure high adhesion to the substrate while exhibiting low surface electrical resistance.

[0038] In the present invention, the inorganic conductive fine particles are not particularly limited in terms of their components (materials) as long as they are particles having electrical conductivity, and components known as conductive particles can be used. Specifically, for example, conductive metal oxide particles such as tin oxide and zinc oxide; conductive nitride particles; conductive metal oxide particles containing one or more metal oxides selected from the group consisting of antimony oxide, indium oxide, tin oxide, zinc oxide, and cadmium oxide as the main component, and further containing tin, antimony, phosphorus, aluminum, and gallium, such as antimony-containing tin oxide (ATO), tin-containing indium oxide (ITO), phosphorus-containing tin oxide (PTO), aluminum-containing zinc oxide (AZO), and gallium-containing zinc oxide (GZO); silver nanoparticles; silver nanowires; and copper nanoparticles; carbon nanotubes; conductive carbon; core-shell particles coated with a conductive material, such as particles in which the surface of titanium oxide is coated with a conductive material such as ATO; and the like. The inorganic conductive fine particles may be used alone or in combination of two or more kinds. In particular, because of their excellent conductivity, transparency, thermal stability, light stability, etc., the inorganic conductive microparticles preferably contain at least one type selected from the group consisting of tin oxide, antimony-containing tin oxide (ATO), phosphorus-containing tin oxide (PTO), zinc oxide, aluminum-containing zinc oxide (AZO), gallium-containing zinc oxide (GZO), antimony oxide, indium oxide, tin-containing indium oxide (ITO), silver nanoparticles, silver nanowires, copper nanoparticles, and carbon nanotubes, more preferably at least one type selected from tin oxide and antimony-containing tin oxide (ATO), and even more preferably antimony-containing tin oxide (ATO).

[0039] In the conductive composition, the inorganic conductive fine particles include aggregated particles, and it is preferable that the inorganic conductive fine particles are mainly present as aggregated particles. In this specification, aggregated particles refer to secondary particles formed by a plurality of primary particles of the inorganic conductive fine particles contacting each other. When the inorganic conductive fine particles are present as aggregated particles, the surface electrical resistance value of the cured film obtained can be equal to or less than that of the case where the inorganic conductive fine particles are present as primary particles with a smaller blending amount, so that it is easy to adjust the surface electrical resistance value to a desired value while ensuring good coatability of the conductive composition. The shape of the aggregated particles may be any shape formed by aggregation of the primary particles of the inorganic conductive fine particles, such as spherical, ellipsoidal, or flat, but is preferably spherical. In this specification, "mainly present as aggregated particles" means that more than 50 mass% of the inorganic conductive fine particles are present as aggregated particles based on the total mass of the inorganic conductive fine particles. In one embodiment of the present invention, preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and particularly preferably 95 mass% or more of the inorganic conductive fine particles are present as aggregated particles based on the total mass of the inorganic conductive fine particles.

[0040] In the present invention, the average agglomerated particle diameter of the inorganic conductive fine particles is preferably 90 nm or more and 180 nm or less. When the average agglomerated particle diameter of the inorganic conductive fine particles is 90 nm or more, a conductive path is easily formed in the agglomerated particles. This reduces the electrical resistance between the particles, so that high electrical properties can be obtained by blending a relatively small amount of inorganic conductive fine particles. Therefore, it is possible to achieve both excellent coating properties and good antistatic performance. In addition, when the average agglomerated particle diameter is 180 nm or less, the inorganic conductive fine particles do not become in a state of being aggregated more than necessary, and dispersibility and uniformity can be improved. This makes it difficult for scattering and diffraction of visible light to occur, and a conductive film with a low haze value and excellent transparency can be obtained. From the viewpoint of more easily obtaining the above-mentioned effect by controlling the average agglomerated particle diameter to a specific range, the average agglomerated particle diameter of the inorganic conductive fine particles is preferably 92 nm or more, more preferably 100 nm or more, even more preferably 105 nm or more, particularly preferably 110 nm or more, and also preferably 175 nm or less, more preferably 165 nm or less, even more preferably 155 nm or less, particularly preferably 150 nm or less.

[0041] In the present invention, the average agglomerated particle size of the inorganic conductive fine particles is the average particle size of the agglomerated particles that can be measured by a dynamic light scattering method, and is the median particle size (D 50 ) means. For measuring the average aggregate particle size of inorganic conductive fine particles, a general measuring device capable of measuring the average particle size by dynamic light scattering can be used, but the measuring device for aggregate particles in a solventless conductive composition must be capable of measuring the particle size of inorganic conductive fine particles dispersed as aggregate particles regardless of whether the sample is diluted or not. Examples of such measuring devices include a concentrated particle size analyzer manufactured by Otsuka Electronics Co., Ltd., a multi-analyte nanoparticle size measuring system, a particle size distribution measuring device manufactured by Microtrac, a laser diffraction type particle size distribution measuring device manufactured by Shimadzu Corporation, and a laser diffraction / scattering type particle size distribution measuring device manufactured by Horiba, Ltd. In addition, when diluting, it is necessary to select a solvent that does not change the aggregate state of the inorganic conductive fine particles. More specifically, the average aggregate particle size of inorganic conductive fine particles can be measured, for example, according to the method described in the examples described later.

[0042] The average agglomerated particle size of the inorganic conductive microparticles can be controlled within a desired range by adjusting, for example, the type of active energy ray-curable compound constituting the conductive composition, the type and amount of the dispersant, and the dispersion treatment conditions of the inorganic conductive microparticles (for example, the inorganic conductive microparticle concentration, treatment time, treatment temperature, bead material, bead diameter, speed, filling rate, etc.).

[0043] In the present invention, the average primary particle size of the inorganic conductive fine particles is usually 10 nm or more and 50 nm or less, and preferably 10 nm or more and 30 nm or less. When the average primary particle size of the inorganic conductive fine particles is within the above range, the average aggregate particle size of the inorganic conductive fine particles can be easily controlled within a specific range. In this specification, the average primary particle diameter of the inorganic conductive fine particles refers to the average particle diameter obtained by observing and measuring the particle diameters of individual primary particles separated by grain boundaries using nanoparticles of the inorganic conductive fine particles themselves as a sample, and then averaging the particle diameters of at least 100 particles using a transmission electron microscope (TEM).

[0044] In the present invention, the amount of inorganic conductive fine particles present as primary particles is preferably 30 mass % or less, more preferably 20 mass % or less, even more preferably 10 mass % or less, and particularly preferably 5 mass % or less, relative to the total mass of the inorganic conductive fine particles.

[0045] The content of the inorganic conductive fine particles in the conductive composition is preferably 40% by mass or more and 60% by mass or less based on the total mass of the conductive composition. When the content of the inorganic conductive fine particles is equal to or more than the lower limit, sufficient antistatic performance can be imparted to the obtained cured film. When the content is equal to or less than the upper limit, the increase in viscosity of the composition, the decrease in coatability, and the decrease in adhesion caused by the inclusion of the inorganic conductive fine particles can be suppressed. From the viewpoint of imparting good antistatic performance to the obtained cured film while ensuring excellent coatability, the content of the inorganic conductive fine particles is preferably 42% by mass or more, more preferably 45% by mass or more, and is preferably 58% by mass or less, more preferably 55% by mass or less based on the total mass of the conductive composition.

[0046] (Active energy ray curable compound) In the present invention, the conductive composition contains an active energy ray-curable compound. The active energy ray-curable compound functions as a dispersion medium for inorganic conductive fine particles and is a component that forms a matrix resin that disperses and fixes the inorganic conductive fine particles in the obtained cured film.

[0047] The active energy ray curable compound is a component having the property of being polymerized and cured by irradiation with active energy rays such as ultraviolet rays, and examples thereof include polymerizable compounds having at least one reactive group in the molecule. Examples of the reactive group include groups that can be involved in a polymerization reaction by active radicals or acids generated from a polymerization initiator, and specifically include vinyl groups, (meth)acryloyl groups, oxiranyl groups, oxetanyl groups, and the like. Among them, radical polymerizable groups are preferred, vinyl groups and (meth)acryloyl groups are more preferred, and (meth)acryloyl groups are even more preferred. In this specification, "(meth)acryloyl" represents both or either of acryloyl and methacryloyl, and the same applies to "(meth)acrylate" and the like below. The active energy ray curable compound may be any of a monomer, a prepolymer, and an oligomer. The active energy ray curable compound may be used alone or in combination of two or more kinds.

[0048] In the present invention, the active energy ray curable compound is preferably a compound that can function as a dispersion medium for inorganic conductive fine particles and can be cured by active energy rays. As such an active energy ray curable compound, a polymerizable compound conventionally used in the field can be widely adopted. Since it has excellent reactivity and tends to easily impart appropriate strength and hardness to the obtained cured film, in one embodiment of the present invention, it is preferable that the conductive composition contains an active energy ray curable compound having at least two reactive groups (hereinafter, also referred to as a "polyfunctional active energy ray curable compound"). The polyfunctional active energy ray curable compound may be any of a monomer, an oligomer, and a polymer. For example, a polyfunctional ethylenically unsaturated monomer (monomer) having two or more ethylenic double bonds in the molecule can be mentioned.

[0049] Examples of the active energy ray-curable compound having at least two reactive groups include Linear or branched alkylene glycol di(meth)acrylate having 10 to 25 carbon atoms, or 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 2-n-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, Meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, propoxylated neopentyl glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glycerin propoxy tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, alkoxylated hexanediol di(meth)acrylate, dodecane di(meth)acrylate, etc.; Examples of the cyclic structure-containing di(meth)acrylate or tri(meth)acrylate having 10 to 30 carbon atoms include cyclohexanedimethanol di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A propylene oxide adduct di(meth)acrylate, and the like; vinyl ether group-containing (meth)acrylic acid esters such as 2-(2-vinyloxyethoxy)ethyl (meth)acrylate; allyl group-containing (meth)acrylic acid esters such as 2-(allyloxymethyl)methyl (meth)acrylate; Examples of the amino acrylate include difunctional or higher functional amino acrylates such as amino (meth) acrylate, amine modified polyether (meth) acrylate, amine modified polyester (meth) acrylate, amine modified epoxy (meth) acrylate, and amine modified urethane (meth) acrylate.

[0050] From the viewpoint of improving the curability of the conductive composition, it is preferable to contain a polyfunctional (meth)acrylate compound having at least two (meth)acryloyl groups (hereinafter also referred to as a "polyfunctional (meth)acrylate compound"). In addition, it is more preferable to contain a bifunctional (meth)acrylate compound having two (meth)acryloyl groups in the molecule (hereinafter also referred to as a "bifunctional (meth)acrylate compound"), since this can improve the curability of the conductive composition and is appropriately easy to remove in the coating film heating step. Particularly suitable bifunctional (meth)acrylate compounds in the present invention include 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 2-(2-vinyloxyethoxy)ethyl (meth)acrylate, and 2-(allyloxymethyl)methyl (meth)acrylate. In one embodiment of the present invention, the conductive composition preferably contains at least one selected from the group consisting of these bifunctional (meth)acrylate compounds, and particularly preferably contains 1,6-hexanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 2-(2-vinyloxyethoxy)ethyl (meth)acrylate, and 2-(allyloxymethyl)methyl (meth)acrylate as the bifunctional (meth)acrylate compound. These compounds perform an excellent function as a dispersion medium for the inorganic conductive fine particles, and are also advantageous in that the average aggregate particle size and viscosity of the inorganic conductive fine particles can be easily controlled within a desired range.

[0051] In one embodiment of the present invention, it is preferable that the active energy ray curable compound contains a trifunctional or higher functional (meth)acrylate compound together with a bifunctional (meth)acrylate compound. By containing a plurality of compounds as a polyfunctional active energy ray curable compound, the hardness and adhesion of the obtained cured film can be further increased. The trifunctional or higher functional (meth)acrylate compound is more preferably a trifunctional (meth)acrylate compound, for example, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glycerin propoxy tri(meth)acrylate, etc. In one embodiment of the present invention, it is particularly preferable that the trifunctional or higher functional (meth)acrylate compound contains pentaerythritol tri(meth)acrylate.

[0052] The conductive composition may contain an active energy ray curable compound having one reactive group in the molecule as the active energy ray curable compound (hereinafter also referred to as "monofunctional active energy ray curable compound"). Examples of the monofunctional active energy ray curable compound include monofunctional ethylenically unsaturated monomers having one ethylenic double bond in the molecule, specifically, for example, alkyl (meth)acrylates having a linear or branched alkyl group, (meth)acrylates having a cyclic structure such as an alicyclic structure, an aromatic ring structure, or a heterocyclic structure in the molecule, and monofunctional ethylenically unsaturated monomers containing nitrogen atoms such as (meth)acrylamide and N-vinyl lactams.

[0053] Examples of the monofunctional active energy ray-curable compound include 2-phenoxyethyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, diethylene glycol methyl ether (meth)acrylate, 2-(2-ethoxyethoxy)ethyl (meth)acrylate, stearyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, lauryl (meth)acrylate, isodecyl (meth)acrylate, Examples of such acrylates include 3,3,5-trimethylcyclohexyl (meth)acrylate, isooctyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, tridecyl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, alkoxylated tetrahydrofurfuryl (meth)acrylate, 2-tert-butylcyclohexanol (meth)acrylate, and 4-tert-butylcyclohexyl (meth)acrylate.

[0054] In one embodiment of the present invention, the ratio of the polyfunctional active energy ray curable compound to the total amount of the active energy ray curable compounds contained in the conductive composition (total amount when two or more kinds are included) is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, particularly preferably 95 mass% or more, and all the active energy ray curable compounds contained in the conductive composition may be polyfunctional active energy ray curable compounds. In addition, the ratio of the polyfunctional (meth)acrylate compound to the total amount of the polyfunctional active energy ray curable compounds contained in the conductive composition (total amount when two or more kinds are included) is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and all the polyfunctional active energy ray curable compounds may be polyfunctional (meth)acrylate compounds. Furthermore, the proportion of the bifunctional (meth)acrylate compound in the total amount of the polyfunctional active energy ray curable compounds contained in the conductive composition (the total amount when two or more types are contained) is preferably 60 mass% or more, more preferably 70 mass% or more, even more preferably 75 mass% or more, particularly preferably 80 mass% or more, and particularly preferably 85 mass% or more. When the proportion of the polyfunctional active energy ray curable composition in the conductive composition and the proportion of the polyfunctional or bifunctional (meth)acrylate compound in the polyfunctional active energy ray curable compound are above the lower limit, the hardness and electrical properties of the resulting cured film can be improved while maintaining good dispersibility of the inorganic conductive fine particles and good coatability due to the incorporation of the active energy ray curable compound.

[0055] In one embodiment of the present invention, the content of the polyfunctional active energy ray curable compound in the conductive composition (the total amount when two or more types are included) is preferably 20 to 55 mass%, more preferably 25 to 50 mass%, and even more preferably 30 to 45 mass%, based on the total mass of the conductive composition. When the content of the polyfunctional active energy ray curable compound in the conductive composition is within the above range, the hardness and electrical properties of the obtained cured film can be improved while maintaining good dispersibility and coatability of the inorganic conductive fine particles.

[0056] In one embodiment of the present invention, the proportion of the monofunctional active energy ray curable compound in the total amount of the active energy ray curable compounds contained in the conductive composition (the total amount when two or more types are contained) is preferably 30 mass% or less, more preferably 20 mass% or less, even more preferably 15 mass% or less, particularly preferably 10 mass% or less, and particularly preferably 5 mass% or less, and the conductive composition may not contain a monofunctional active energy ray curable compound. When the proportion of the monofunctional active energy ray curable composition in the conductive composition is within the above range, the strength and hardness of the obtained cured film can be improved while ensuring the coatability by blending the monofunctional active energy ray curable compound.

[0057] In one embodiment of the present invention, the content of the monofunctional active energy ray curable compound in the conductive composition (the total amount when two or more types are included) is preferably 15 mass% or less, more preferably 10 mass% or less, and even more preferably 5 mass% or less, based on the total mass of the conductive composition, and the conductive composition may not contain a monofunctional active energy ray curable compound. When the content of the monofunctional active energy ray curable compound in the conductive composition is within the above range, the strength and hardness of the obtained cured film can be improved while ensuring the coatability by blending the monofunctional active energy ray curable compound.

[0058] In the present invention, the conductive composition preferably contains an active energy ray curable compound having a vapor pressure of 1.0 Pa or more and 500 Pa or less at 25°C. In the conductive composition containing a curable compound having such a vapor pressure, the active energy ray curable compound having a low vapor pressure remains in the coating film appropriately even after the coating film heating step. Therefore, the concentration of the inorganic conductive fine particles can be increased in the coating film heating step, and the polymerization of the active energy ray curable compound can be sufficiently advanced in the cured film forming step. This makes it possible to obtain a conductive film having low surface electrical resistance and excellent film hardness. From the viewpoint of further enhancing the above-mentioned effect, the conductive composition contains an active energy ray curable compound having a vapor pressure of preferably 1.0 to 500 Pa, more preferably 1.0 to 300 Pa, and even more preferably 1.0 to 100 Pa at 25°C. The vapor pressure of the active energy ray-curable compound can be measured at 25°C using an appropriate method, for example, a gas flow method, an isoteniscope method, a DSC method, a boiling point method, or a static method, depending on the properties of the sample to be measured, the amount of the sample, and the magnitude of the vapor pressure.

[0059] In one embodiment of the present invention, the content of active energy ray curable compounds in the conductive composition having a vapor pressure of 1.0 Pa or more and 500 Pa or less at 25°C, preferably having a vapor pressure within the above-mentioned preferred range (total amount when two or more types are included), relative to the total mass of the active energy ray curable compounds, is preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 85 mass% or more. When the content of the active energy ray curable compounds having the specific vapor pressure is within the above range, it becomes easier to balance the volatility of the active energy ray curable compounds in the coating film heating step and the reactivity of the active energy ray curable compounds in the cured film forming step. This makes it possible to obtain a conductive film with low surface electrical resistance and excellent film hardness.

[0060] From the viewpoint of easily ensuring good coatability of the composition while excellent dispersibility of the inorganic conductive fine particles, it is preferable that the active energy ray curable compound contains an active energy ray curable compound having a standalone viscosity of 150 mPa·s or less at 25°C (hereinafter also referred to as "active energy ray curable low viscosity compound"). In one embodiment of the present invention, the standalone viscosity of the active energy ray curable low viscosity compound at 25°C is more preferably 60 mPa·s or less, and further preferably 30 mPa·s or less. The standalone viscosity of the active energy ray curable low viscosity compound at 25°C is usually 1 mPa·s or more. The viscosity of the active energy ray-curable compound is the viscosity of a monomer alone, and can be measured, for example, by an E-type viscometer TVE-22 manufactured by Toki Sangyo Co., Ltd.

[0061] In one embodiment of the present invention, the proportion of active energy ray-curable compounds having a simple viscosity of 150 mPa s or less at 25°C (active energy ray-curable low-viscosity compounds) in the total amount of active energy ray-curable compounds contained in the conductive composition is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 85 mass% or more, and is preferably 98 mass% or less, more preferably 95 mass% or less.

[0062] The content of the active energy ray curable compound in the conductive composition is preferably 25% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, based on the total mass of the conductive composition, and is preferably 60% by mass or less, more preferably 55% by mass or less, and even more preferably 50% by mass or less. When the content of the active energy ray curable compound is within the above range, a conductive composition having excellent dispersibility of inorganic conductive fine particles and good coatability can be obtained.

[0063] <Polymerization initiator> In the present invention, the conductive composition contains a polymerization initiator. The polymerization initiator is a compound capable of initiating a polymerization reaction of an active energy ray-curable compound. As the polymerization initiator, a photopolymerization initiator that generates active radicals or acids by the action of light is preferred, since it can initiate a polymerization reaction under lower temperature conditions, and a photopolymerization initiator that generates radicals by the action of light is more preferred. As the polymerization initiator, only one type may be used, or two or more types may be used in combination.

[0064] As the polymerization initiator, a known polymerization initiator can be used. For example, an acylphosphine oxide compound, an α-aminoalkylphenone compound, an α-hydroxyquinone compound, a thioxanthone compound, a benzoin compound, an anthraquinone compound, a ketal compound, etc. are listed. Among them, it is preferable to include an α-aminoalkylphenone compound as the polymerization initiator.

[0065] Specific examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,3,5,6-tetramethylbenzoyldiphenylphosphine oxide, 2,6-dimethylbenzoyldiphenylphosphine oxide, 4-methylbenzoyldiphenylphosphine oxide, 4-ethylbenzoyldiphenylphosphine oxide, and the like. Examples of the acylphosphine oxide include sphingoyl, 4-isopropylbenzoyldiphenylphosphine oxide, 1-methylcyclohexanoylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2,4,6-trimethylbenzoylphenylphosphinic acid isopropyl ester, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide. These may be used alone or in combination. Examples of commercially available acylphosphine oxide compounds include "DAROCURE TPO" manufactured by BASF.

[0066] Specific examples of the α-aminoalkylphenone compounds include 2-methyl-1[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1, and 2-methyl-1-[4-(methoxythio)phenyl]-2-morpholinopropan-2-one. These may be used alone or in combination. Commercially available α-aminoalkylphenone compounds include, for example, "Omnirad 369" and "Omnirad 907" manufactured by IGM Resins.

[0067] Specific examples of the α-hydroxyquinone compounds include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-phenylpropan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one, and 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one. These may be used alone or in combination. Commercially available α-hydroxyquinone compounds include "Omnirad 184", "DAROCURE 1173", "Omnirad 2959", and "Omnirad 127".

[0068] Specific examples of the thioxanthone compounds include thioxanthone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, and 1-chloro-4-propoxythioxanthone. These compounds may be used alone or in combination. Commercially available thioxanthone compounds include "MKAYACURE DETX-S" manufactured by Nippon Kayaku Co., Ltd. and "Chivacure ITX" manufactured by Double Bond Chemical Co., Ltd.

[0069] Specific examples of the benzoin compound include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, and benzoin isobutyl ether.

[0070] Specific examples of the anthraquinone compound include 2-ethylanthraquinone, 2-t-butylanthraquinone, 2-chloroanthraquinone, and 2-amylanthraquinone.

[0071] Specific examples of the ketal compounds include acetophenone dimethyl ketal, benzyl dimethyl ketal, and the like, and benzophenone compounds having 13 to 21 carbon atoms, such as benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, and 4,4'-bismethylaminobenzophenone.

[0072] The content of the polymerization initiator is preferably 8 parts by mass or more and 27 parts by mass or less, more preferably 8.5 parts by mass or more, even more preferably 9 parts by mass or more, and more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, relative to 100 parts by mass of the active energy ray curable compound. When the content of the polymerization initiator is equal to or more than the lower limit, the curability of the conductive composition can be sufficiently increased, and when it is equal to or less than the upper limit, the amount of the active energy ray curable compound remaining uncured can be reduced. On the other hand, when the content of the polymerization initiator is too small, the surface electrical resistance value of the obtained cured film becomes too high, and antistatic performance may not be obtained. In addition, when the amount of the polymerization initiator is too large, the polymerization initiator is difficult to dissolve sufficiently in the conductive composition.

[0073] <Dispersant> The conductive composition preferably further contains a dispersant. The dispersant here means a dispersant for dispersing the inorganic conductive fine particles described above. In the present invention, the conductive composition preferably contains at least one dispersant for dispersing the inorganic conductive fine particles contained in the conductive composition. As long as the inorganic conductive fine particles can be dispersed as aggregated particles having a desired average aggregated particle size in the active energy ray curable compound serving as the dispersion medium, various dispersants used for the purpose of improving particle dispersibility and preventing sedimentation can be adopted. Examples of such dispersants include modified acrylic (co)polymers, acrylic (co)polymers, salts of polymer (co)polymers having acid groups, hydroxyl group-containing carboxylic acid esters, alkylol aminoamides, unsaturated polycarboxylic acid polyaminoamides, alkyl ammonium salts or phosphate ester salts of polymer copolymers, etc. The dispersants may be used alone or in combination of two or more.

[0074] In one embodiment of the present invention, the conductive composition preferably contains a polymer having an acid value of 100 mgKOH / g or more as a dispersant. When a polymer having an acid value of 100 mgKOH / g or more is used, inorganic conductive fine particles are easily present in the composition as aggregated particles having an average aggregated particle diameter within a range specified in the present invention, and the viscosity of the conductive composition is easily controlled to a range suitable for good coating properties. The reason for this is not clear, but it is speculated that hydroxyl groups are often present on the surface of inorganic conductive fine particles, and when the acid value increases, the apparent pH decreases, and the hydroxyl groups present on the surface of the inorganic conductive fine particles are positively charged, so that the acid groups of the dispersant are easily adsorbed, leading to improved dispersibility. The upper limit of the acid value of the dispersant is not particularly limited, but is usually 200 mgKOH / g or less, preferably 150 mgKOH / g or less, from the viewpoint of the length of the molecular chain per acid group. The acid value means the number of mg of KOH required to neutralize 1 g of the dispersant solid content, and can be determined, for example, by potentiometric titration in accordance with JIS K 0070.

[0075] The amine value of the dispersant is preferably 90 mgKOH / g or less, more preferably 80 mgKOH / g or less, and may be 0 mgKOH / g. When the amine value is equal to or less than the upper limit, the dispersibility and coatability of the inorganic conductive fine particles are more likely to be improved. The amine value means the number of mg of KOH equivalent to the amount of HCl required to neutralize 1 g of the dispersant solid content, and can be measured, for example, by potentiometric titration in accordance with JIS K 7237.

[0076] As the structure that easily has the desired acid value, the dispersant is preferably a polymer that includes a structural unit having at least one kind of acid group. Examples of the acid group in the structural unit having an acid group include a carboxyl group, a sulfonic acid group, a phosphonic acid group, a phosphoric acid group, a hydroxyl group, and a thiol group. Among them, it is preferable to have at least one selected from the group consisting of a carboxyl group, a sulfonic acid group, a phosphonic acid group, a phosphoric acid group, and a hydroxyl group, more preferably to have at least one selected from the group consisting of a carboxyl group, a sulfonic acid group, and a phosphoric acid group, and even more preferably to have a phosphoric acid group.

[0077] The weight average molecular weight of the dispersant is preferably at least 800, more preferably at least 1000, and is preferably at most 30000, more preferably at most 10000. When the weight average molecular weight of the dispersant is at least the above lower limit, good dispersion stability is easily obtained by the dispersant, and when it is at most the above upper limit, an excessive increase in viscosity is suppressed, and the coatability of the conductive composition can be improved. The weight average molecular weight can be determined as a styrene-equivalent molecular weight by general gel permeation chromatography (GPC).

[0078] As the dispersant, a commercially available product may be used. Examples of such commercially available dispersants include DISPERBYK-102, DISPERBYK-106, DISPERBYK-145, DISPERBYK-111, DISPERBYK-180, BYK-P105, and TEGO Disper655 manufactured by BYK-Chemie.

[0079] The content of the dispersant in the conductive composition is preferably 8 parts by mass or more and 25 parts by mass or less with respect to 100 parts by mass of the inorganic conductive fine particles. When the amount of the dispersant is equal to or more than the lower limit, the viscosity of the conductive composition can be easily controlled to a viscosity range suitable for good coating properties. When the amount of the dispersant is equal to or less than the upper limit, the average aggregate particle size of the inorganic conductive fine particles can be easily controlled to a desired range. From the viewpoint of dispersibility and coating properties, the content of the dispersant is more preferably 9 parts by mass or more, even more preferably 10 parts by mass or more, and more preferably 20 parts by mass or less, even more preferably 18 parts by mass or less, and particularly preferably 15 parts by mass or less with respect to 100 parts by mass of the inorganic conductive fine particles.

[0080] The conductive composition used in the method of the present invention is a so-called solventless composition. In this specification, the term "solventless" means that the content of organic solvent and water in the conductive composition (when the conductive composition contains organic solvent and water, or when the conductive composition contains multiple organic solvents, the total amount of the organic solvents) is 5 mass% or less with respect to the total mass of the conductive composition. In the present invention, the content of organic solvent and water in the conductive composition is preferably 3 mass% or less, more preferably 1 mass% or less, and in one embodiment of the present invention, the conductive composition does not contain organic solvent and water.

[0081] In the present invention, the conductive composition is a transparent conductive composition. In this specification, the transparent conductive composition means a conductive composition capable of forming a conductive film having translucency capable of transmitting light, particularly visible light, and specifically means a property of having a total light transmittance of 60 or more. The total light transmittance can be measured, for example, according to JIS K 7361.

[0082] In the present invention, the conductive composition may contain, as necessary, additives that can be generally incorporated into transparent conductive compositions, in addition to inorganic conductive fine particles, active energy ray curable compounds, polymerization initiators, and dispersants, within a range that does not impair the effects of the present invention when used in the method of the present invention. Examples of such additives include storage stabilizers, surface conditioners, antioxidants, light stabilizers, polymerization inhibitors, chain transfer agents, and photosensitizers. These may be used alone or in combination of two or more.

[0083] For example, by including a surface conditioner, it becomes easier to control the surface tension of the conductive composition within an appropriate range, and the coatability becomes easier to improve. Examples of the surface conditioner include silicone compounds having a polydimethylsiloxane structure such as polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, and polyaralkyl-modified polydimethylsiloxane, and fluorine-based surface conditioners.

[0084] When the conductive composition contains a surface conditioner, the content thereof is preferably 0.005 mass % or more, more preferably 0.01 mass % or more, and is preferably 3 mass % or less, more preferably 2 mass % or less, and even more preferably 1.5 mass % or less, relative to the total mass of the conductive composition.

[0085] Examples of the polymerization inhibitor include nitroso-based polymerization inhibitors, hydroquinone, methoxyhydroquinone, benzoquinone, p-methoxyphenol, TEMPO, TEMPOL (HO-TEMPO), Al cupferron, and hindered amines.

[0086] When the conductive composition contains a polymerization inhibitor, the content thereof is preferably 0.001 to 1 mass %, more preferably 0.005 mass % or more, even more preferably 0.01 mass % or more, and is preferably 0.5 mass % or less, more preferably 0.3 mass % or less, relative to the total mass of the conductive composition.

[0087] The conductive composition for forming a transparent conductive film usually does not contain a colorant, but may be colored by including a small amount of a pigment and / or dye, such as a bluing agent, as long as it is transparent. Therefore, the content of the colorant in the conductive composition is usually 0.3 mass % or less, preferably 0.1 mass % or less, more preferably 0.05 mass % or less, based on the total mass of the conductive composition, and the lower limit is 0 mass %.

[0088] In the present invention, the conductive composition preferably has a viscosity of 20 mPa·s to 150 mPa·s at 25°C. From the viewpoint of ensuring better coatability, the viscosity at 25°C is preferably 20 to 100 mPa·s, more preferably 20 to 60 mPa·s. The viscosity can be measured in accordance with JIS K5600-2-3, for example, using an E-type viscometer. The viscosity of the conductive composition can be controlled by adjusting the type and amount of the active energy ray-curable compound, the amount of the inorganic conductive fine particles, the type and amount of the dispersant, etc.

[0089] <Method of manufacturing conductive composition> In the present invention, the conductive composition can be produced, for example, by a method including a step of mixing inorganic conductive fine particles, an active energy ray-curable compound, and a dispersant to obtain a mixture (hereinafter also referred to as a "mixing step"), and a step of subjecting the mixture to a dispersion treatment in order to control the average agglomerated particle size of the agglomerated particles contained in the inorganic conductive fine particles (hereinafter also referred to as a "dispersion treatment step").

[0090] When preparing the conductive composition, all the components constituting the conductive composition can be mixed and stirred at the same time, but in order to easily control the average aggregate particle size of the inorganic conductive fine particles to a desired range, it is preferable to mix the three components of the inorganic conductive fine particles, the active energy ray curable compound, and the dispersant in advance. Such a mixing process is, for example, a process in which the inorganic conductive fine particles (hereinafter also referred to as "raw inorganic conductive fine particles") that are raw materials and exist as particles or aggregates having a particle size larger than the average aggregate particle size of the inorganic conductive fine particles finally desired are mixed with a dispersant for dispersing the raw inorganic conductive fine particles and an active energy ray curable compound that is a dispersion medium to obtain a mixture of these.

[0091] The average (aggregated) particle size of the raw inorganic conductive fine particles used to obtain aggregated particles of inorganic conductive fine particles constituting the conductive composition is not particularly limited, and may be, for example, about 10 to 50 times larger than the average aggregated particle size of the finally desired inorganic conductive fine particles. By using inorganic conductive fine particles that exist as particles or aggregates having a particle size that is moderately larger than the average aggregated particle size of the finally desired inorganic conductive fine particles as the raw material, aggregated particles of inorganic conductive fine particles having an average aggregated particle size in a desired specific range can be efficiently obtained.

[0092] In the mixing step, the amount of the raw inorganic conductive fine particles to be added can be appropriately determined depending on the composition of the desired conductive composition, the type of inorganic conductive fine particles, the type of dispersant, the type of active energy ray curable compound, and the like. Considering the amount of reduction of the inorganic conductive fine particles after the dispersion treatment process described below, the amount of the raw inorganic conductive fine particles mixed in the mixing step is preferably larger than the amount of the inorganic conductive fine particles to be included in the final conductive composition, specifically, for example, about 5 to 10% by mass. Therefore, in one embodiment of the present invention, in the method for producing a conductive composition, the amount of the raw inorganic conductive fine particles mixed in the mixing step is preferably 43% by mass or more and 65% by mass or less, more preferably 45% by mass or more, even more preferably 47% by mass or more, and even more preferably 63% by mass or less, and even more preferably 60% by mass or less, based on the total mass of the mixture obtained by mixing the raw inorganic conductive fine particles, the active energy ray curable compound, the dispersant, and other components (for example, polymerization initiator, etc.) as necessary. When the ratio (concentration) of the raw inorganic conductive fine particles in the mixture is within the above range, the conditions for dispersing the raw inorganic conductive fine particles are efficient.

[0093] The mixing conditions of the raw inorganic conductive fine particles, the active energy ray curable compound, and the dispersant are not particularly limited, and may be appropriately determined so as to obtain a uniform mixture depending on the (aggregated) particle size and concentration of the raw inorganic conductive fine particles, the type of the active energy ray curable compound, the equipment and facilities used for mixing, etc. For example, a dissolver, a butterfly mixer, etc. may be used as the agitator.

[0094] The dispersion treatment step is a step of dispersing the raw inorganic conductive fine particles into aggregated particles having a desired average aggregate particle diameter, preferably 90 nm to 180 nm. In this step, it is preferable that more than 50 mass % of the inorganic conductive fine particles, preferably 70 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and particularly preferably 95 mass % or more of the inorganic conductive fine particles are dispersed into aggregated particles having an average aggregate particle diameter of 90 nm to 180 nm, based on the total mass of the obtained inorganic conductive fine particles.

[0095] The dispersion of the raw inorganic conductive fine particles can be carried out using known dispersion processing equipment such as a ball mill, a bead mill, a sand mill, a pico mill, a paint conditioner, a roll mill, a jet mill, an ultrasonic disperser, a homogenizer, a disperser, etc. Among them, from the viewpoint of easily obtaining aggregated particles having a desired particle size efficiently in a short time, a mechanical dispersion processing equipment using a media is preferred, and a bead mill is more preferred. These equipments may be used in combination as necessary.

[0096] When a ball mill or a bead mill is used in the dispersion treatment, the material of the media (balls or beads) is not particularly limited, and for example, glass, alumina, ceramics, titania, zirconia, steel, etc. can be used. From the viewpoint of easily shortening the dispersion treatment time and more efficiently dispersing into the desired aggregated particles, the bead diameter (diameter) is preferably 0.2 to 1 mm, more preferably 0.2 to 0.5 mm. The filling rate of the media in the dispersion treatment machine is not particularly limited, but from the viewpoint of easily suppressing atypical shape during dispersion, it is preferably 50 to 95%, more preferably 70 to 90%. The dispersion treatment time may be appropriately determined according to the particle diameter of the raw inorganic conductive fine particles and the type of dispersion treatment equipment used so as to obtain the desired average aggregated particle diameter, and is usually 1 to 120 minutes, preferably 10 to 60 minutes.

[0097] The dispersion treatment time is not particularly limited, and may be appropriately determined depending on the (aggregated) particle size and concentration of the raw inorganic conductive fine particles, the type of the active energy ray curable compound, the equipment and facilities used for mixing, etc. Usually, the longer the dispersion treatment time, the smaller the average aggregate particle size of the inorganic conductive fine particles becomes.

[0098] By controlling the viscosity of the dispersion of inorganic conductive fine particles obtained through the dispersion treatment step to be within the range of, for example, 20 to 400 mPa·s, it becomes easier to control the viscosity of the final conductive composition to a range suitable for obtaining good coatability without affecting the aggregation state of the inorganic conductive fine particles. The viscosity can be measured in accordance with JIS K5600-2-3, for example, using an E-type viscometer.

[0099] The conductive composition of the present invention can be obtained by adding the remaining components constituting the conductive composition, such as a polymerization initiator, to the mixture of inorganic conductive fine particles, active energy ray curable compound, and dispersant obtained by the dispersion treatment process and mixing them.

[0100] <Conductive film> For example, after the above-mentioned conductive composition is applied onto a substrate to form a coating film, a coating film heating step is carried out according to the method of the present invention described above, and the resulting dried coating film is irradiated with active energy rays, thereby obtaining a conductive film as a cured film of the conductive composition.

[0101] The conductive film obtained according to the method of the present invention has a surface electrical resistance of 5×10 5 Ω / □ or more 1×10 9 It is preferably Ω / □ or less, and more preferably 1×10 6 Ω / □ or more, more preferably 5×10 6 Ω / □ or more, and more preferably 5×10 8 Ω / □ or less, more preferably 1×10 8 The surface electrical resistivity can be controlled by adjusting the type, amount and average aggregate particle size of the inorganic conductive fine particles in the conductive composition, the type and amount of the active energy ray-curable compound, and the like, and then carrying out the coating film heating step in the method of the present invention. The surface electrical resistance value can be measured using a surface electrical resistance measuring device. In detail, it can be measured by, for example, the method described in the examples below.

[0102] The conductive film obtained according to the method of the present invention has a total light transmittance of preferably 60% or more, more preferably 65% ​​or more, even more preferably 70% or more, and particularly preferably 80% or more. The upper limit of the total light transmittance is 100%. The cured film made of the conductive composition of the present invention has a haze of preferably 4% or less, more preferably 3% or less, and even more preferably 2.5% or less. When the total light transmittance and haze are within the above ranges, the conductive film has better transparency. The total light transmittance and haze of the cured film can be measured, for example, according to JIS K 7361.

[0103] From the viewpoint of ensuring high film hardness, the conductive film obtained according to the method of the present invention preferably has a pencil hardness on its surface of H or more, more preferably 2H or more, and in some cases may be, for example, 3H or more. The pencil hardness can be measured, for example, in accordance with JIS K 5400.

[0104] The conductive film obtained according to the method of the present invention has excellent antistatic performance, film hardness, and adhesion to substrates, and also has high transparency, and is therefore suitable for use as a laminate having a conductive film on a substrate, for example, as an antistatic film for plastic products, an antistatic film for window glass, a packaging film for semiconductor products, a plastic antistatic sheet for equipment covers, antistatic properties for displays, touch panel electrodes, wiring electrodes, light control film electrodes, solar cell electrodes, and the like. EXAMPLES

[0105] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.

[0106] 1. Preparation of Conductive Composition and Conductive Film <Example 1> (1) Preparation of conductive composition (i) Preparation of a dispersion of inorganic conductive particles In a 250 ml plastic container containing zirconia beads (250 g) with a diameter of 0.3 mm, an active energy ray curable compound, inorganic conductive fine particles, a dispersant, and a polymerization inhibitor were added according to the composition shown in "Dispersion Liquid" in Table 1, and the mixture was dispersed for 20 minutes using a paint shaker (manufactured by Toyo Seiki Seisakusho). After the dispersion process, the beads were removed to obtain a dispersion liquid of inorganic conductive fine particles.

[0107] (ii) Preparation of conductive composition (dispersion blend composition) To the dispersion of inorganic conductive fine particles obtained in (i) above, an active energy ray curable compound, a polymerization initiator, a polymerization inhibitor, and a surface conditioner were added according to the composition shown in "Dispersion Blended Composition" in Table 1, and the mixture was stirred for 30 minutes using a stirrer to prepare a dispersion blended composition (conductive composition). The blending amounts of all components contained in the dispersion blended composition are shown in Table 1 as the composition of the conductive composition.

[0108] (2) Properties of active energy ray-curable compounds (i) Single unit viscosity The viscosity of each active energy ray-curable compound was measured at a measurement temperature of 25° C. using an E-type viscometer, TV22 cone type (manufactured by Toki Sangyo Co., Ltd.). (i) Vapor pressure The vapor pressure of each active energy ray-curable compound was measured at a measurement temperature of 25° C. using a gas flow method.

[0109] (3) Physical properties of conductive compositions (i) Viscosity of the conductive composition The viscosity of the conductive composition was measured using an E-type viscometer, TV22 cone type (manufactured by Toki Sangyo Co., Ltd.) at a measurement temperature of 25° C. The results are shown in Table 1.

[0110] (ii) Surface tension The surface tension of the conductive composition was measured at 25° C., 20 seconds after the start of measurement, using a fully automatic balanced electrosurface tensiometer ESB-V (manufactured by Kyowa Interface Science Co., Ltd.) The results are shown in Table 1.

[0111] (iii) Average agglomerated particle size of inorganic conductive fine particles The average aggregate particle size of the inorganic conductive fine particles in the conductive composition was measured using a concentrated particle size analyzer FPAR-1000 (manufactured by Otsuka Electronics Co., Ltd.). The measurement was performed at a measurement temperature of 25°C using a measurement composition prepared by diluting the dispersion of the inorganic conductive fine particles or the conductive composition to be measured with dipropylene glycol monomethyl ether acetate (DPMA) so that the light intensity was 10,000 to 50,000 cps. The results are shown in Table 1.

[0112] (4) Preparation of cured film (conductive film) (i) Procedure for preparing conductive film (Coating film formation process) The substrate was a transparent acrylic resin sheet (Kuraray Co., Ltd., extrusion method, surface free energy 38 mJ / m 2 The conductive composition prepared above was applied onto the substrate using a bar coater PI-1210 (manufactured by Tester Sangyo Co., Ltd.) to form a coating film having a wet thickness of 3 μm. (Coating film heating process) The wet coating was then dried at 90° C. for 1 minute using an explosion-proof dryer. (cured film formation process) Immediately after drying with hot air in the coating film heating process, a UV lamp ECS-1511S (high pressure mercury lamp manufactured by iGraphics Co., Ltd.) was used to apply 200 mW / cm illuminance. 2 , cumulative light intensity 500mJ / cm 2 The coating was irradiated with ultraviolet light of 1000 nm in an air atmosphere to obtain a cured film.

[0113] (ii) Measurement of the surface free energy of the substrate The surface free energy of the substrate was determined by measuring the contact angles of water, diiodomethane, and n-hexadecane solutions on the substrate surface using a contact angle meter (PG-X, manufactured by Matsubo Corporation), and calculating the surface free energy from the contact angles obtained based on a theoretical formula (extended Fowkes equation) for determining surface free energy.

[0114] (iii) Wet film thickness measurement The wet film thickness was measured by a reflectance spectroscopic interference film thickness meter.

[0115] <Example 2> A conductive film was prepared in the same manner as in the preparation of the cured film (conductive film) of Example 1, except that the same conductive composition as in Example 1 was used and the conditions of the coating film heating step were set to 70°C for 1 minute.

[0116] <Example 3> A conductive film was produced in the same manner as in the production method of the cured film (conductive film) of Example 1, except that a 50 μm thick PET film (manufactured by Toray Industries, Inc.) was laminated on the wet coating film in the coating film formation process and the coating film heating process was performed at 70° C. for 1 minute, using the same conductive composition as in Example 1. The lamination process is intended to prevent the evaporation of the active energy ray-curable compound from the wet coating film surface and to suppress oxygen inhibition during UV lamp irradiation.

[0117] <Example 4> A conductive composition and a conductive film were prepared in the same manner as in Example 1, except that the type and amount of the active energy ray-curable compound were changed according to the description in Table 1.

[0118] <Comparative Example 1> A conductive film was produced in the same manner as in the production method of the cured film (conductive film) of Example 1, except that the same conductive composition as in Example 1 was used and the coating film heating step was not performed.

[0119] <Comparative Example 2> A conductive composition was prepared in the same manner as in Example 1, except that no inorganic conductive fine particles were added, and the amount of the active energy ray-curable compound added was changed according to the description in Table 1. A conductive film was prepared in the same manner as in the preparation of the cured film (conductive film) in Example 1, using the obtained conductive composition, except that a 50 μm-thick PET film (manufactured by Toray Industries, Inc.) was laminated on the wet coating film in the coating film formation step, and the coating film heating step was performed under conditions of 70° C. for 1 minute.

[0120] <Comparative Example 3> Conductive compositions and conductive films were prepared in the same manner as in Example 1, except that the type and amount of active energy ray-curable compound were changed according to the description in Table 1 and an organic solvent was added.

[0121] [Table 1]

[0122] Details of each component listed in Table 1 are as follows. Inorganic conductive particles: ATO particles, SN-100P (manufactured by Ishihara Sangyo Kaisha, Ltd., average primary particle size: 10-30 nm) Dispersant: BYK-106 (manufactured by BYK Japan), salt of polymer with phosphate group, acid value: 132 mg KOH / g, amine value: 74 mg KOH / g Active energy ray curable compound-1: 1,6-hexanediol diacrylate (Viscoat #230: manufactured by Osaka Organic Chemical Industry Co., Ltd.), bifunctional, vapor pressure at 25°C: 2.0 Pa, simple viscosity at 25°C: 7.0 mPa s Active energy ray curable compound-2: Tetrahydrofurfuryl acrylate (Sartomer SR285: manufactured by Arkema), monofunctional, vapor pressure at 25°C: 199.0 Pa, simple viscosity at 25°C: 2.8 mPa s Active energy ray curable compound-3: Pentaerythritol triacrylate (Light Acrylate PE-3A: Kyoeisha Chemical), trifunctional, vapor pressure at 25°C: not measurable, viscosity at 25°C: 525.0 mPa s Polymerization inhibitor: 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl (H-TEMPO: manufactured by Evonik Degussa Japan) Polymerization initiator: 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone (Omnirad 907, IGM Resins BV) Surface conditioner: Acrylic group-containing polyether modified polydimethylsiloxane (BYK-UV3500, manufactured by BYK Japan) Organic solvent: Cyclohexanone (UBE)

[0123] [Table 2]

[0124] 2. Characterization of Conductive Films The properties of the conductive films produced in the examples and comparative examples were evaluated by the following methods. The results are shown in Table 3. (1) Film thickness The thickness of the conductive film was measured by cutting the acrylic sheet of the substrate and observing the cross section with a scanning electron microscope (SEM, Hitachi "S-4500").

[0125] (2) Appearance The appearance of the conductive film was evaluated visually. [Appearance evaluation criteria] A: No coating streaks, no particle agglomerations, transparent and clear B: Slight coating streaks, slight particle agglomerations, slightly opaque C: Coating unevenness, particle agglomeration, opaque and cloudy

[0126] (3) Surface electrical resistance The surface electrical resistance value of the conductive film was measured using a Hiresta (manufactured by Mitsubishi Chemical Corporation) and a URS probe at the maximum voltage at which the applied voltage could be measured.

[0127] (4) Total light transmittance and haze The total light transmittance and haze of the conductive film were measured using a haze meter NDH-2000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in the "HouHou 3" mode.

[0128] (5) Pencil hardness The pencil hardness of the conductive film was measured using a surface property tester "HEIDON-14DR" manufactured by Shinto Scientific Co., Ltd.

[0129] (6) Adhesion The adhesion of the conductive film was evaluated by cross-cutting the conductive film, attaching an adhesive sheet [Cellotape (registered trademark) (manufactured by Nichiban Co., Ltd.)] to the adhesive layer side, and then peeling it off. [Adhesion evaluation criteria] A: No peeling at all B: Slightly peeled off C: Partially peeled off D: The entire area where the adhesive sheet was attached peeled off.

[0130] [Table 3]

Claims

1. A method for producing a transparent conductive film containing inorganic conductive fine particles, comprising the steps of: A step of forming a coating film of a transparent conductive active energy ray-curable composition on a substrate, the coating film comprising an inorganic conductive fine particle, an active energy ray-curable compound, and a polymerization initiator, the organic solvent and water content of which is 5 mass % or less; heating the coating; and A step of irradiating the heated coating film with active energy rays to form a cured film. A method comprising:

2. 10. The method of claim 1, wherein the step of heating the coating is performed by convection, conduction, or radiation.

3. The method of claim 1 , further comprising the step of forming a cured film under air after the step of heating the coating.

4. The method according to claim 1 , wherein the content of the monofunctional active energy ray-curable compound in the transparent conductive active energy ray-curable composition is 15 mass % or less based on the total mass of the curable composition.

5. 2. The method according to claim 1, wherein the inorganic conductive microparticles include at least one selected from the group consisting of tin oxide, antimony-containing tin oxide (ATO), phosphorus-containing tin oxide (PTO), zinc oxide, aluminum-containing zinc oxide (AZO), gallium-containing zinc oxide (GZO), antimony oxide, indium oxide, tin-containing indium oxide (ITO), silver nanoparticles, silver nanowires, copper nanoparticles, and carbon nanotubes.

6. The method according to claim 1 , wherein the active energy ray-curable compound comprises an active energy ray-curable compound having a vapor pressure of 1.0 Pa or more and 500 Pa or less at 25° C.

7. The substrate has a surface free energy of 20 to 40 mJ / m 2 The method according to claim 1 , wherein the substrate is

8. The method of claim 1 , wherein the inorganic conductive particulate is antimony-containing tin oxide (ATO).

9. The method according to claim 1 , wherein the inorganic conductive fine particles include aggregated particles, and the average aggregated particle size of the aggregated particles is 90 nm or more and 180 nm or less.

10. The method of claim 1 , wherein the transparent conductive active energy ray curable composition further comprises a dispersant.

11. The method of claim 10, wherein the dispersant is a polymer having an acid number of 100 KOHmg / g or greater.

12. The method of claim 10, wherein the dispersant is a polymer comprising structural units having at least one selected from the group consisting of a carboxyl group, a sulfonic acid group, a phosphonic acid group, a phosphoric acid group, and a hydroxyl group.

Citation Information

Patent Citations

  • Solventless active energy ray-curable coating composition and method for producing the same and substrate with functional thin film

    JP2010053242A

  • Clear and electrically conductive coating

    JP1996027405A

  • Photocurable hard coating agent and resin molding fitted with hard coat film comprising the photocurable hard coating agent

    JP2008143999A