Method for producing hydrolyzable silyl group-containing organic compound

By employing a specific polar solvent and catalyst, the method efficiently converts hydrolyzable groups in hydrolyzable silyl groups, enhancing curability and reactivity for applications in sealants, adhesives, and coatings.

JP2024143589APending Publication Date: 2024-10-11KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023056347
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods struggle to efficiently convert hydrolyzable groups with larger molecular weights in hydrolyzable silyl groups, leading to slow exchange reactions.

Method used

A method involving a specific amount of a highly polar organic solvent with a dielectric constant of 22 or more, along with an acidic catalyst, is used to exchange hydrolyzable groups in hydrolyzable silyl groups, facilitating the introduction of larger molecular weight groups.

Benefits of technology

This approach enables efficient conversion of hydrolyzable groups, resulting in organic compounds with improved curability and reactivity, suitable for applications in sealants, adhesives, and coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143589000001
    Figure 2024143589000001
  • Figure 2024143589000002
    Figure 2024143589000002
  • Figure 2024143589000003
    Figure 2024143589000003
Patent Text Reader

Abstract

To provide a production method in which an organic compound having a hydrolyzable silyl group containing a hydrolyzable group with a relatively high molecular weight can be efficiently obtained by an exchange reaction of a hydrolyzable group contained in a hydrolyzable silyl group.SOLUTION: A method for producing an organic compound (A) represented by formula (1) includes exchanging substituents by reacting 0.1 pt.wt. or more of a hydroxyl group-containing compound (C) with 100 pts.wt. of an organic compound (B) having a hydrolyzable silyl group such as trimethoxysilyl polyoxypropylene in the presence of 1 pt.wt. or more of an organic solvent (D) having a dielectric constant of 22 or more. (R1 is a group having three or more carbon atoms and a molecular weight of 40 or more; R2 is a substituted / unsubstituted monovalent hydrocarbon group; X is a hydroxyl group or the like; a is 1, 2 or 3; b is 0, 1 or 2; c is 0, 1 or 2; and a+b+c is 3 or less.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an organic compound having a hydrolyzable silyl group. [Background technology]

[0002] Organic polymers that have hydroxyl groups or hydrolyzable groups on silicon atoms and have silicon-containing groups that can form siloxane bonds (hereinafter referred to as "hydrolyzable silyl groups") are known as moisture-reactive polymers. They are used in many industrial products such as sealants, adhesives, coating materials, paints, and pressure-sensitive adhesives because they cure through hydrolysis to form flexible rubber-like cured products.

[0003] It is known that in such hydrolyzable silyl groups, a reaction proceeds in which the hydrolyzable group on the silicon atom is exchanged for another hydrolyzable group. For example, Patent Document 1 discloses a method for producing an organic polymer having a trimethoxysilyl group by reacting an organic polymer having a silicon atom bonded to a hydrolyzable group other than a methoxy group (e.g., a triethoxysilyl group) with methanol in the presence of a catalyst. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-285585 A Summary of the Invention [Problem to be solved by the invention]

[0005] Patent Document 1 merely discloses a reaction for converting a hydrolyzable group, such as an ethoxy group, bonded to a silicon atom in a hydrolyzable silyl group into a methoxy group. In response to this, the inventors attempted to introduce a hydrolyzable group having a larger molecular weight than a methoxy group by a similar exchange reaction, but their investigations revealed that the exchange reaction to a hydrolyzable group having a larger molecular weight may be extremely difficult to proceed.

[0006] In view of the above-mentioned current situation, the present invention aims to provide a production method capable of efficiently obtaining an organic compound having a hydrolyzable silyl group, including a hydrolyzable group having a relatively large molecular weight, by an exchange reaction of the hydrolyzable group contained in the hydrolyzable silyl group. [Means for solving the problem]

[0007] As a result of extensive research, the present inventors have found that a hydrolyzable group having a relatively large molecular weight can be efficiently introduced by carrying out an exchange reaction of a hydrolyzable group contained in a hydrolyzable silyl group using a specific amount of a specific organic solvent, and have arrived at the present invention.

[0008] That is, the present invention provides a method for producing an organic compound (A) having a hydrolyzable silyl group represented by the following general formula (1):

[0009] [ka]

[0010] (In formula (1), R 1 R represents a group having 3 or more carbon atoms and a molecular weight of 40 or more. 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. X represents a hydroxyl group or -OR 1 a is 1, 2, or 3; b is 0, 1, or 2; c is 0, 1, or 2; and a+b+c is 3 or less. Relative to 100 parts by weight of an organic compound (B) having a hydrolyzable silyl group represented by the following general formula (2),

[0011] [ka]

[0012] (In formula (2), R 2 , X, and c are as described above. However, X in formula (2) may be the same as or different from X in formula (1). d is 1, 2, or 3, and c+d is 3 or less. General formula: R 1 OH (in the formula, R 1 is as described above.) reacting in the presence of 1 part by weight or more of an organic solvent (D) having a relative dielectric constant of 22 or more; A part or all of X in the general formula (2) is -OR 1 The present invention relates to a method for producing an organic compound (A), comprising exchanging Effect of the Invention

[0013] According to the present invention, a production method can be provided that can efficiently obtain an organic compound having a hydrolyzable silyl group, including a hydrolyzable group having a relatively large molecular weight, by an exchange reaction of the hydrolyzable group contained in the hydrolyzable silyl group. According to a preferred embodiment of the present invention, a hydrolyzable silyl group-containing organic polymer capable of exhibiting improved curability can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail. [Organic compound (A)] The present embodiment relates to a method for producing an organic compound (A) having a hydrolyzable silyl group represented by the following general formula (1) by utilizing a reaction of exchanging hydrolyzable groups bonded to silicon atoms in the hydrolyzable silyl group. A plurality of hydrolyzable silyl groups represented by general formula (1) that can be contained in the organic compound (A) may have the same structure or different structures.

[0015] [ka]

[0016] R in general formula (1) 1 represents a group having 3 or more carbon atoms and a molecular weight of 40 or more. When introducing a group having a relatively large molecular weight onto a silicon atom through an exchange reaction of a hydrolyzable group, the exchange reaction generally tends to proceed very slowly. However, by using a specific amount of a highly polar organic solvent (D) as described below, the exchange reaction can proceed efficiently. 1 When a plurality of are included, they may be the same or different.

[0017] R 1 The upper limit of the number of carbon atoms in R is not particularly limited, but may be, for example, 30 or less, preferably 20 or less, more preferably 10 or less, even more preferably 6 or less, and particularly preferably 5 or less. 1 The upper limit of the molecular weight is not particularly limited, but may be 400 or less, preferably 200 or less, more preferably 100 or less, and particularly preferably 80 or less.

[0018] R 1 is preferably a substituted or unsubstituted monovalent hydrocarbon group. The hydrocarbon group may be saturated or unsaturated, and may be aliphatic, alicyclic, or aromatic. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include a hydroxyl group, a halogen group such as a chloro group, an alkoxy group such as a methoxy group, and an amino group such as an N,N-diethylamino group. The hydrocarbon group may also have a ketone group (-C(=O)-) or an ester group (-C(=O)-O-).

[0019] R 1 Although the specific structure of is not particularly limited, a suitable example is a group represented by the following general formula (3).

[0020] [ka]

[0021] R in general formula (3) 3 represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. The hydrocarbon group may be either saturated or unsaturated. The number of carbon atoms is preferably 1 to 4, more preferably 1 to 3, further preferably 1 or 2, and most preferably 1. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include halogen groups such as a chloro group, alkoxy groups such as a methoxy group, and amino groups such as an N,N-diethylamino group.

[0022] R 3 Examples of R include unsubstituted alkylene groups such as methylene, ethylene, n-propylene, isopropylene, n-butylene, and tert-butylene; substituted alkylene groups such as chloromethylene, methoxymethylene, and N,N-diethylaminomethylene; and unsaturated hydrocarbon groups such as vinylene, isopropenylene, and allylene. Preferred are substituted or unsubstituted alkylene groups, more preferably methylene, ethylene, and propylene groups, even more preferably methylene and ethylene groups, and most preferably methylene groups. 3 When a plurality of are present, they may be the same or different.

[0023] R in general formula (3) 4 represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or -OR 6 Represents R 6 represents a hydrogen atom, or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms.

[0024] R 4 or R 6The hydrocarbon group which can be represented by may be either saturated or unsaturated, and may be either aliphatic, alicyclic, or aromatic. The number of carbon atoms in the hydrocarbon group is preferably 1 to 10, more preferably 1 to 8, further preferably 1 to 6, even more preferably 1 to 3, and particularly preferably 1 or 2. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include a hydroxyl group, a halogen group such as a chloro group, an alkoxy group such as a methoxy group, and an amino group such as an N,N-diethylamino group.

[0025] R 4 Examples of the R include unsubstituted alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; substituted alkyl groups such as chloromethyl, methoxymethyl, N,N-diethylaminomethyl, and methylol; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, toluyl, and 1-naphthyl; and aralkyl groups such as benzyl. R is preferably a substituted or unsubstituted alkyl group or unsaturated hydrocarbon group, more preferably a methyl group, ethyl group, propyl group, vinyl group, methoxymethyl group, or methylol group, even more preferably a methyl group or methylol group, and particularly preferably a methyl group. 4 When a plurality of are present, they may be the same or different.

[0026] R 6 As a concrete example of 4 The specific examples are the same as those of R. 6 is preferably a substituted or unsubstituted alkyl group or an unsaturated hydrocarbon group, more preferably a methyl group, an ethyl group, a propyl group, or a vinyl group, and particularly preferably a methyl group. 6 When a plurality of are present, they may be the same or different.

[0027] R in general formula (3)5 represents an oxygen atom or a nitrogen atom bonded to any group. As shown in general formula (3), R 5 is bonded to the adjacent carbon atom by a double bond. This structure is called a divalent hydrocarbon group R 3 By bonding to an oxygen atom and a silicon atom via R, the curability or reactivity of the hydrolyzable silyl group can be improved. 5 is preferably an oxygen atom.

[0028] R 5 In the above formula, examples of the optional group bonded to the nitrogen atom include a hydrogen atom, or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. The number of carbon atoms in the hydrocarbon group is preferably 1 to 10, more preferably 1 to 6, and even more preferably 1 to 3.

[0029] R represented by the general formula (3) 1 Preferred specific examples of the group include groups represented by the following formulas (4) to (10).

[0030] [ka]

[0031] [ka]

[0032] [ka]

[0033] [ka]

[0034] [ka]

[0035] [ka]

[0036] [ka]

[0037] Also, R 1 Another preferred example of the group is a group represented by the following general formula (11):

[0038] [ka]

[0039] R in general formula (11) 7 represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. The hydrocarbon group may be either saturated or unsaturated. The hydrocarbon group preferably has 1 to 4 carbon atoms, more preferably has 1 to 3 carbon atoms, and even more preferably has 2 or 3 carbon atoms. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include halogen groups such as a chloro group, alkoxy groups such as a methoxy group, and amino groups such as an N,N-diethylamino group.

[0040] R 7 Examples of R include unsubstituted alkylene groups such as methylene, ethylene, n-propylene, isopropylene, n-butylene, and tert-butylene; substituted alkylene groups such as chloromethylene, methoxymethylene, and N,N-diethylaminomethylene; and unsaturated hydrocarbon groups such as vinylene, isopropenylene, and allylene. Preferred are substituted or unsubstituted alkylene groups, more preferably methylene, ethylene, and propylene groups, and even more preferably ethylene and propylene groups. 7 When a plurality of are present, they may be the same or different.

[0041] R in general formula (11) 8represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or a halogen atom. The hydrocarbon group may be saturated or unsaturated, and may be aliphatic, alicyclic, or aromatic. The number of carbon atoms in the hydrocarbon group is preferably 1 to 10, more preferably 1 to 8, even more preferably 1 to 6, even more preferably 1 to 3, and particularly preferably 1 or 2. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include a hydroxyl group, a halogen group such as a chloro group, an alkoxy group such as a methoxy group, and an amino group such as an N,N-diethylamino group.

[0042] R 8 Examples of R include unsubstituted alkyl groups such as hydrogen atom, methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, tert-butyl group, n-hexyl group, 2-ethylhexyl group, and n-dodecyl group; substituted alkyl groups such as chloromethyl group, methoxymethyl group, N,N-diethylaminomethyl group, and methylol group; unsaturated hydrocarbon groups such as vinyl group, isopropenyl group, and allyl group; cycloalkyl groups such as cyclohexyl group; aryl groups such as phenyl group, toluyl group, and 1-naphthyl group; aralkyl groups such as benzyl group, and halogen atoms. R is preferably a hydrogen atom, a substituted or unsubstituted alkyl group or unsaturated hydrocarbon group, or a halogen atom, more preferably a hydrogen atom, a methyl group, an ethyl group, or a halogen atom, even more preferably a hydrogen atom, a methyl group, or an ethyl group, and particularly preferably a hydrogen atom or a methyl group. 8 When a plurality of are present, they may be the same or different.

[0043] R in general formula (1) 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 2When a plurality of are contained, they may be the same or different. The hydrocarbon group may be saturated or unsaturated, and may be aliphatic, alicyclic, or aromatic. The hydrocarbon group preferably has 1 to 10 carbon atoms, more preferably 1 to 8 carbon atoms, even more preferably 1 to 6 carbon atoms, even more preferably 1 to 3 carbon atoms, and particularly preferably 1 or 2 carbon atoms. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include halogen groups such as a chloro group, alkoxy groups such as a methoxy group, and amino groups such as an N,N-diethylamino group.

[0044] R 2 Examples of the R include unsubstituted alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; substituted alkyl groups such as chloromethyl, methoxymethyl, and N,N-diethylaminomethyl; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, toluyl, and 1-naphthyl; and aralkyl groups such as benzyl. R is preferably a substituted or unsubstituted alkyl group, more preferably a methyl group, an ethyl group, a chloromethyl group, or a methoxymethyl group, even more preferably a methyl group or a methoxymethyl group, and particularly preferably a methyl group. 2 When a plurality of are present, they may be the same or different.

[0045] In the general formula (1), X is a hydroxyl group or -OR 1 When a plurality of X's are contained in the general formula (1), they may be the same or different. 1The hydrolyzable group other than is not particularly limited and may be a known hydrolyzable group, for example, a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, an alkenyloxy group, etc. Among these, an alkoxy group, an acyloxy group, a ketoximate group, and an alkenyloxy group are preferred. Since the hydrolysis is mild and easy to handle, an alkoxy group is more preferred, a methoxy group and an ethoxy group are further preferred, and a methoxy group is particularly preferred. When a plurality of Xs are present, they may be the same or different from each other.

[0046] In the general formula (1), a represents any one of 1, 2, and 3, b represents any one of 0, 1, and 2, and c represents any one of 0, 1, and 2. a is not limited to one number, and different numbers may coexist in the organic compound (A). The same applies to b and c. a+b+c is 3 or less, preferably 2 or 3, and particularly preferably 3.

[0047] The organic compound (A) may have only the hydrolyzable silyl group represented by the general formula (1) as the hydrolyzable silyl group, or may have the hydrolyzable silyl group represented by the general formula (1) and another hydrolyzable silyl group not included in the general formula (1). Such another hydrolyzable silyl group is not particularly limited, and an example thereof includes the hydrolyzable silyl group represented by the general formula (2) described later.

[0048] The organic compound (A) may be an organic polymer having a polymer skeleton, or an organic compound having no polymer skeleton. Here, the polymer skeleton refers to a structure in which a plurality of monomer units are formed in succession by bonding a plurality of monomers by addition, condensation, or the like. The monomer species contained in the polymer skeleton may be one type, or a mixture of a plurality of types may be bonded.

[0049] When the organic compound (A) is an organic compound having no polymer skeleton, its specific structure is not particularly limited except that it has a hydrolyzable silyl group represented by the general formula (1). Specific examples include alkoxysilane compounds having alkoxysilyl groups, and silane coupling agents having other functional groups in addition to alkoxysilyl groups (e.g., vinyl groups, epoxy groups, halogen groups, styryl groups, methacryl groups, acrylic groups, amino groups, isocyanurate groups, ureido groups, mercapto groups, isocyanate groups, acid anhydride groups, etc.), in which some or all of the alkoxy groups are replaced with hydrolyzable groups: -OR 1 Examples of compounds that have been exchanged for

[0050] When the organic compound (A) is an organic polymer, its polymer skeleton (also referred to as main chain structure) is not particularly limited, and various main chain structures can be used. Specifically, polyoxyalkylene polymers such as polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymers, and polyoxypropylene-polyoxybutylene copolymers; hydrocarbon polymers such as ethylene-propylene copolymers, polyisobutylene, copolymers of isobutylene and isoprene, and hydrogenated polyolefin polymers obtained by hydrogenating these polyolefin polymers; polyolefins obtained by condensation of dibasic acids such as adipic acid with glycols, or ring-opening polymerization of lactones; Examples of such polymers include ester polymers, (meth)acrylic acid ester polymers obtained by radical polymerization of (meth)acrylic acid ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and stearyl (meth)acrylate, vinyl copolymers obtained by radical polymerization of (meth)acrylic acid ester monomers, vinyl acetate, acrylonitrile, and styrene, polysulfide polymers, polyamide polymers, polycarbonate polymers, and diallyl phthalate polymers. In the above description, (meth)acrylic refers to acrylic and / or methacrylic.

[0051] Among these, saturated hydrocarbon polymers such as polyisobutylene, hydrogenated polyisoprene, and hydrogenated polybutadiene, polyoxyalkylene polymers, and (meth)acrylic acid ester polymers are preferred because they have relatively low glass transition temperatures and the resulting cured products have excellent cold resistance. Only one of these may be used, or two or more may be used in combination.

[0052] Polyoxyalkylene polymers and (meth)acrylic acid ester polymers are particularly preferred because they have high moisture permeability, excellent deep curing properties when made into a one-component curable composition, and excellent adhesive properties. Polyoxyalkylene polymers are more preferred, and polyoxypropylene is even more preferred.

[0053] A (meth)acrylic acid ester-based polymer is useful because, by combining various monomer compositions constituting the polymer, it is possible to obtain effects such as improving adhesiveness, improving heat resistance and weather resistance, and reducing the water absorption of a cured product obtained by curing a curable composition.

[0054] The polyoxyalkylene polymer is preferably a polymer having a repeating unit represented by -RO- (wherein R is a linear or branched alkylene group having 1 to 14 carbon atoms). R is more preferably a linear or branched alkylene group having 2 to 4 carbon atoms. Specific examples of the repeating unit represented by -RO- include -CHO-, -CHCHO-, -CHCH(CH)O-, -CHCH(CH)O-, -CHC(CH)(CH)O-, -CHCHCHCHO-, and the like. The main chain structure of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units.

[0055] In particular, when the organic compound (A) which is a polymer is used as a curable resin contained in a sealant, adhesive, etc., a polyoxypropylene-based polymer having oxypropylene repeating units in an amount of 50% by weight or more, more preferably 80% by weight or more of the polymer skeleton, is preferred because it is amorphous and has a relatively low viscosity.

[0056] The main chain structure of the polyoxyalkylene polymer may be linear or may have a branched chain. When the polymer has a branched chain, the number of the branched chains is preferably 1 to 6 (i.e., the number of terminal hydroxyl groups is 3 to 8), more preferably 1 to 4 (i.e., the number of terminal hydroxyl groups is 3 to 6), and most preferably 1 (i.e., the number of terminal hydroxyl groups is 3). By having a branched chain, it is possible to obtain an effect of improving the restorability of the cured product. In addition, it is also expected to have an effect of reducing the water absorption of the cured product.

[0057] The polyoxyalkylene polymer is preferably one obtained by a ring-opening polymerization reaction of a cyclic ether compound in the presence of an initiator using a polymerization catalyst.

[0058] Examples of the cyclic ether compound include ethylene oxide, propylene oxide, butylene oxide, tetramethylene oxide, and tetrahydrofuran. These cyclic ether compounds may be used alone or in combination of two or more. Among the cyclic ether compounds, it is particularly preferable to use propylene oxide, since it can produce an amorphous polyether polymer having a relatively low viscosity.

[0059] Specific examples of the initiator include alcohols such as butanol, ethylene glycol, propylene glycol, propylene glycol monoalkyl ether, butanediol, hexamethylene glycol, neopentyl glycol, diethylene glycol, dipropylene glycol, triethylene glycol, glycerin, trimethylolmethane, trimethylolpropane, pentaerythritol, and sorbitol; and hydroxyl-terminated polyoxyalkylene polymers having a number average molecular weight of 300 to 4,000, such as polyoxypropylene diol, polyoxypropylene triol, polyoxyethylene diol, and polyoxyethylene triol.

[0060] Examples of the synthesis method of polyoxyalkylene polymers include, but are not limited to, a polymerization method using an alkali catalyst such as KOH, a polymerization method using a transition metal compound-porphyrin complex catalyst such as a complex obtained by reacting an organoaluminum compound with porphyrin as disclosed in JP-A-61-215623, a polymerization method using a composite metal cyanide complex catalyst as disclosed in JP-B-46-27250, JP-B-59-15336, U.S. Pat. No. 3,278,457, U.S. Pat. No. 3,278,458, U.S. Pat. No. 3,278,459, U.S. Pat. No. 3,427,256, U.S. Pat. No. 3,427,334, and U.S. Pat. No. 3,427,335, a polymerization method using a catalyst made of a polyphosphazene salt as exemplified in JP-A-10-273512, and a polymerization method using a catalyst made of a phosphazene compound as exemplified in JP-A-11-060722. A polymerization method using a double metal cyanide complex catalyst is more preferred for reasons of production cost and the fact that a polymer having a narrow molecular weight distribution can be obtained.

[0061] When the organic compound (A) is an organic polymer, it may be a polyoxyalkylene polymer containing other bonds such as urethane bonds and urea bonds in the polymer skeleton, as long as the effect of the invention is not significantly impaired. Specific examples of such polymers include polyurethane prepolymers.

[0062] The polyurethane prepolymer can be obtained by a known method, for example, by reacting a polyol compound with a polyisocyanate compound.

[0063] Specific examples of the polyol compound include polyether polyol, polyester polyol, polycarbonate polyol, and polyether polyester polyol.

[0064] Specific examples of the polyisocyanate compound include diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, methylene-bis(cyclohexyl isocyanate), isophorone diisocyanate, and hexamethylene diisocyanate. The polyurethane prepolymer may be one having either a hydroxyl group or an isocyanate group at the end.

[0065] From the viewpoint of obtaining a curable composition having excellent storage stability and workability, it is particularly preferable that the organic compound (A) is a polyoxyalkylene polymer that does not contain a urethane bond, a urea bond, an ester bond, or an amide bond in the polymer skeleton.

[0066] When the organic compound (A) is an organic polymer, its molecular weight distribution (Mw / Mn) is not particularly limited, but is preferably 1.6 or less, more preferably 1.5 or less, and particularly preferably 1.4 or less. From the viewpoint of improving various mechanical properties such as durability and elongation of the cured product, it is preferably 1.2 or less.

[0067] When the organic compound (A) is an organic polymer, its number average molecular weight, as polystyrene equivalent molecular weight by GPC, is preferably 3,000 to 100,000, more preferably 5,000 to 50,000, and particularly preferably 8,000 to 35,000. When the number average molecular weight is within these ranges, the mechanical properties of the cured product are excellent, and since the amount of hydrolyzable silyl groups introduced is appropriate, it is possible to obtain an organic polymer that exhibits good curability, has an easy-to-handle viscosity, and is excellent in workability while keeping production costs within an appropriate range.

[0068] The molecular weight of the organic polymer can also be expressed as an end-group-converted molecular weight obtained by directly measuring the end group concentration of the polymer precursor before the introduction of hydrolyzable silyl groups by titration analysis based on the principles of the hydroxyl value measurement method of JIS K 1557-1 and the iodine value measurement method specified in JIS K 0070, and taking into consideration the structure of the organic polymer (the degree of branching determined by the polymerization initiator used). The end-group-converted molecular weight of the organic polymer can also be obtained by preparing a calibration curve of the number average molecular weight obtained by general GPC measurement of the polymer precursor and the above-mentioned end-group-converted molecular weight, and converting the number average molecular weight obtained by GPC of the organic polymer into the end-group-converted molecular weight.

[0069] In order to obtain a good rubber-like cured product, it is preferable that the hydrolyzable silyl groups (including both hydrolyzable silyl groups represented by general formula (1) and hydrolyzable silyl groups not included in general formula (1); the same applies below) contained in the organic polymer are present at the polymer chain end. Since this shows good curability and is likely to exhibit rubber elastic behavior, the number of hydrolyzable silyl groups per polymer chain end of the organic polymer is preferably 0.5 or more on average, more preferably 0.6 or more, even more preferably 0.7 or more, and particularly preferably 0.8 or more.

[0070] The number of polymer chains per molecule of the organic polymer is preferably 2 to 8, more preferably 2 to 4, and particularly preferably 2 or 3. The number of hydrolyzable silyl groups in one molecule of the organic polymer is preferably from 1 to 7 on average, more preferably from 1 to 3.4, and particularly preferably from 1 to 2.6.

[0071] When the organic polymer is branched, the hydrolyzable silyl group may be at the end of the main chain of the organic polymer, at the end of a side chain (branched chain), or at both. In particular, when the hydrolyzable silyl group is at the end of the main chain, the molecular weight between crosslinking points becomes long, which is preferable since it is easy to obtain a rubber-like cured product that has high strength, high elongation, and low elastic modulus.

[0072] [Method for producing organic compound (A)] The method for producing the organic compound (A) according to the present embodiment involves reacting an organic compound (B) having a hydrolyzable silyl group represented by the following general formula (2) with a compound represented by the general formula: R 1 OH (in the formula, R 1 The process includes a step of reacting a hydroxyl-containing compound (C) represented by the general formula (2) in the organic compound (B) in the presence of an organic solvent (D) having a relative dielectric constant of 22 or more. Through this reaction, a part or all of the hydrolyzable groups X in the hydrolyzable silyl group of the general formula (2) in the organic compound (B) is converted to hydrolyzable groups -OR 1 Hereinafter, this reaction may be referred to as an exchange reaction of a hydrolyzable group.

[0073] [Organic compound (B)] The organic compound (B) has a hydrolyzable silyl group represented by the following general formula (2): The structure of the organic compound (B) may be the same as the structure of the organic compound (A) except for the hydrolyzable silyl group.

[0074] [ka]

[0075] In general formula (2), R 2 , X, and c are as defined above for general formula (1). 2 and c is R in formula (1). 2and c may be the same as

[0076] X in formula (2) may be the same as X in formula (1). However, depending on the type of organic solvent (D) used, X may also be substituted during the exchange reaction of the hydrolyzable group, so X in formula (2) may be different from X in formula (1). For example, when X in formula (2) is an ethoxy group and methanol is used as the organic solvent (D) to carry out the exchange reaction of the hydrolyzable group, X in formula (1) may be a methoxy group.

[0077] In the general formula (2), d is any one of 1, 2, and 3. d is not limited to one number, and different numbers may coexist in the organic compound (B). c+d is 3 or less, preferably 2 or 3, and particularly preferably 3.

[0078] The method for producing the organic compound (B) is not particularly limited, but when the organic compound (B) is an organic polymer, the following production methods (a) to (d) can be mentioned. (a) After converting the terminal hydroxyl groups of a hydroxyl-terminated organic polymer to carbon-carbon unsaturated groups, HSiX d R 2 c (In the formula, R 2 , X, c, and d are as defined above).

[0079] (b) OCN-W-SiX d R 2 c (In the formula, R 2 , W, X, c, and d are as defined above),

[0080] (c) After converting the terminal hydroxyl groups of the hydroxyl-terminated organic polymer to carbon-carbon unsaturated groups, HS-W-SiX d R 2 c (In the formula, R 2, W, X, c, and d are as defined above),

[0081] (d) A hydroxyl-terminated organic polymer is reacted with a polyisocyanate compound to synthesize an NCO-terminated organic polymer, and then the resulting polymer is subjected to reaction with HNR-W-SiX d R 2 c (Wherein, R is hydrogen or an alkyl group. R 2 , W, X, c, and d are as described above) or HS-W-SiX d R 2 c (In the formula, R 2 , W, X, c, and d are as defined above.

[0082] In the above methods (a) and (c), examples of the carbon-carbon unsaturated group include a vinyl group, an allyl group, a methallyl group, an allenyl group, and a propargyl group.

[0083] In each of the above-mentioned methods, the organic compound (A), which is an organic polymer obtained by using a silane compound in which W is represented by a methylene group, is preferred in that it exhibits extremely high curability.

[0084] Method (a) is preferred since it tends to give an organic compound (A) having good storage stability, while methods (b), (c) and (d) are preferred since they give a high conversion in a relatively short reaction time.

[0085] The introduction of hydrolyzable silyl groups by the method (a) has been proposed in JP-B-45-36319, JP-B-46-12154, JP-A-50-156599, JP-A-54-6096, JP-A-55-13767, JP-A-55-13468, JP-A-57-164123, JP-B-3-2450, U.S. Pat. No. 3,632,557, U.S. Pat. No. 4,345,053, U.S. Pat. No. 4,366,307, U.S. Pat. No. 4,960,844, and other publications. Examples of such polymers include those proposed in JP-A-61-197631, JP-A-61-215622, JP-A-61-215623, and JP-A-61-218632, in which a hydrolyzable silyl group is introduced by hydrosilylation or the like into a polyoxypropylene polymer having a high molecular weight and narrow molecular weight distribution, with a number average molecular weight of 6,000 or more and Mw / Mn of 1.6 or less, and a polymer proposed in JP-A-3-72527.

[0086] As described in WO 2013 / 180203, an organic polymer having two or more carbon-carbon unsaturated bonds at one polymer chain end is used to produce an organic polymer (B) by the above-mentioned methods (a) and (c), which has two or more hydrolyzable silyl groups at one polymer chain end. Organic compound (A), which is an organic polymer produced from such organic compound (B), exhibits high curability, and the resulting cured product is expected to have high strength and high recovery.

[0087] In addition, when the organic compound (B) is an organic compound that does not have a polymer skeleton, a known silane coupling agent having an alkoxysilyl group and other functional groups as described above can be used as the organic compound (B).

[0088] [Hydroxyl group-containing compound (C)] The hydroxyl-containing compound (C) is represented by the general formula: 1 It is a compound represented by OH. 1 is as already defined for general formula (1) and represents a group having 3 or more carbon atoms and a molecular weight of 40 or more. Therefore, methanol, ethanol, propargyl alcohol (R 1The molecular weight of 39) is not included in the hydroxyl-containing compound (C). When using a low-molecular-weight hydroxyl-containing compound that is not included in the hydroxyl-containing compound (C), the exchange reaction of the hydrolyzable group can proceed even without using the organic solvent (D).

[0089] The hydroxyl group-containing compound (C) includes organic compounds having a structure containing a hydroxyl group in the usual sense, as well as 1,3-diketones (e.g., acetylacetone) that coexist with an enol form due to keto-enol tautomerism.

[0090] Specific examples of the hydroxyl group-containing compound (C) include, but are not limited to, R 1 Examples of the hydroxyl group-containing compound (C) represented by the general formula (3) include hydroxyacetone, 4-hydroxy-2-butanone, acetoin, 3-hydroxy-3-methyl-2-butanone, propioin, 5-hydroxy-2-pentanone, diacetone alcohol, acetylacetone, methyl glycolate, methyl lactate, and dihydroxyacetone. Also, R 1 Examples of the hydroxyl group-containing compound (C) represented by the general formula (11) include 3-butyn-2-ol, 2-methyl-3-butyn-2-ol, 3-butyn-1-ol, 3-pentyn-2-ol, 2-methyl-3-pentyn-2-ol, 3-pentyn-1-ol, 4-pentyn-2-ol, 2-methyl-4-pentyn-2-ol, and 4-pentyn-1-ol. These hydroxyl group-containing compounds (C) may be used alone or in combination of two or more.

[0091] The amount of the hydroxyl group-containing compound (C) used is 0.1 parts by weight or more based on 100 parts by weight of the organic compound (B). By using the hydroxyl group-containing compound (C) in such an amount, a hydrolyzable group: -OR 1 When the amount of the hydroxyl group-containing compound (C) used is less than 0.1 parts by weight, the exchange reaction of the hydrolyzable groups does not proceed easily.

[0092] The amount of the hydroxyl group-containing compound (C) used is preferably 0.2 parts by weight or more, more preferably 0.5 parts by weight or more, and even more preferably 1 part by weight or more. The upper limit is not particularly limited and may be appropriately set in consideration of the desired reaction rate, but may be, for example, 100 parts by weight or less. It is preferably 50 parts by weight or less, more preferably 30 parts by weight or less, and even more preferably 20 parts by weight or less. It may be 10 parts by weight or less.

[0093] [Organic solvent (D)] In this embodiment, the exchange reaction of the hydrolyzable group is carried out in the presence of a highly polar organic solvent (D), which allows the exchange reaction of the hydrolyzable group with the hydroxyl-containing compound (C) having a relatively large molecular weight to be carried out efficiently.

[0094] The organic solvent (D) is a highly polar organic solvent. Specifically, the organic solvent (D) is an organic solvent having a relative dielectric constant of 22 or more. Even if an organic solvent having a relative dielectric constant of less than 22 (e.g., acetone, THF (tetrahydrofuran), 1-propanol) is used, it is difficult to proceed with the exchange reaction of the hydrolyzable group by the hydroxyl group-containing compound (C). The relative dielectric constant of the organic solvent (D) may be 24 or more. There is no particular upper limit, but it may be 200 or less. It may be 100 or less, or 50 or less. Here, the relative dielectric constant is a value at 25°C.

[0095] Specific examples of organic solvents (D) having a relative dielectric constant of 22 or more include alcohols such as methanol (32.7), ethanol (24.6), and ethylene glycol (37.7); amides such as dimethylformamide (36.7) and N-methylpyrrolidone (32); sulfur compounds such as dimethylsulfoxide (46.7); nitriles such as acetonitrile (37.5), and nitromethane (36.7). The numbers in parentheses are the values ​​of the relative dielectric constant. Among them, methanol or ethanol is preferable because the viscosity of the resulting organic compound (A) can be suppressed, making it easy to handle. Only one type of organic solvent (D) may be used, or two or more types may be used in combination.

[0096] The amount of organic solvent (D) used is 1 part by weight or more per 100 parts by weight of organic compound (B). By using the organic solvent (D) in such an amount, the exchange reaction of the hydrolyzable group by the hydroxyl group-containing compound (C) can be efficiently promoted. If the amount of organic solvent (D) used is less than 1 part by weight, the exchange reaction of the hydrolyzable group does not easily proceed.

[0097] The amount of the organic solvent (D) used is preferably 2 parts by weight or more, more preferably 5 parts by weight or more, from the viewpoint of promoting the exchange reaction of the hydrolyzable group. The upper limit is not particularly limited, but if it is too much, it takes a long time to remove it after the reaction, so it is preferably 100 parts by weight or less. It is more preferably 50 parts by weight or less, even more preferably 30 parts by weight or less, and particularly preferably 20 parts by weight or less.

[0098] The exchange reaction of the hydrolyzable group is preferably carried out in the presence of a catalyst in order to promote the reaction. As the catalyst, an acid, a base, a metal alkoxide, etc. can be used, but it is preferable to use an acid catalyst (E) because the exchange reaction of the hydrolyzable group can proceed in a short time even with a small amount of use. Among them, Bronsted acids are particularly preferable.

[0099] Specific examples of the acid catalyst (E) include hydrogen halide compounds such as hydrogen chloride and hydrogen bromide, sulfuric acid, nitric acid, trihaloacetic acids such as trifluoromethanesulfonic acid and trifluoroacetic acid, perchloric acid, solid acid catalysts, etc. Hydrogen halide compounds are preferred, and hydrogen chloride is particularly preferred.

[0100] The amount of the acid catalyst (E) used is not particularly limited, but may be, for example, about 0.01 to 1 part by weight, or about 0.1 to 1 part by weight, per 100 parts by weight of the organic compound (B).

[0101] The reaction temperature for the exchange reaction of the hydrolyzable groups is not particularly limited, but may be about 0 to 120° C., or may be about 20 to 100° C. The reaction time is also not particularly limited, but may be about 10 minutes to 12 hours, or may be about 30 minutes to 5 hours.

[0102] After the exchange reaction of the hydrolyzable groups is completed, the acid catalyst (E) is preferably removed by volatilization under reduced pressure, or captured by an epoxy compound, or deactivated by neutralization with a basic compound. In particular, it is preferable to capture the acid catalyst (E) with an epoxy compound. In addition, when the acid catalyst (E) is a solid acid catalyst, it can be easily removed by filtration or the like.

[0103] Specific examples of epoxy compounds that can be used to capture the acid catalyst (E) include aliphatic epoxy compounds such as propylene oxide, ethylene oxide, 2,3-butylene oxide, and isobutylene oxide; glycidyl ethers such as methyl glycidyl ether, allyl glycidyl ether, butyl glycidyl ether, phenyl glycidyl ether, 2-ethylhexyl glycidyl ether, and polypropylene glycol diglycidyl ether; Baycolox 10, Baycolox 12, Baycolox 14, Baycolox 16, and Baycolox. Examples of the epoxy compounds include epoxidized α-olefins having 4 to 30 carbon atoms, such as α-pinene oxide, limonene monoxide, and limonene dioxide; epoxidized vegetable oils, such as epoxidized soybean oil and epoxidized linseed oil; epoxidized fatty acid esters, such as Sanso Cizer E-6000 and Sanso Cizer E-4030 (all manufactured by New Japan Chemical Co., Ltd.); and alicyclic epoxy compounds, such as Sanso Cizer E-PS, Sanso Cizer E-PO, and Sanso Cizer nE-PS (all manufactured by New Japan Chemical Co., Ltd.). Only one type of epoxy compound may be used, or two or more types may be used in combination. Among these, epoxidized α-olefins, epoxidized vegetable oils, epoxidized fatty acid esters, and alicyclic epoxy compounds are preferred, and epoxidized vegetable oils are particularly preferred.

[0104] The amount of the epoxy compound used is not particularly limited and may be appropriately set taking into consideration the remaining amount of the acid catalyst (E). However, the amount is preferably 1 molar equivalent or more, more preferably 10 molar equivalents or more, relative to the remaining amount of the acid catalyst (E).

[0105] After the exchange reaction of the hydrolyzable groups, or, in the case where an epoxy compound is added, after deactivating the acidic catalyst (E) by adding the epoxy compound, the organic compound (A) can be obtained by removing volatile components including the unreacted hydroxyl group-containing compound (C) and the organic solvent (D) from the reaction system, as necessary.

[0106] The volatile components may be left without being removed. In this case, the organic compound (A) may contain any amount of the hydroxyl group-containing compound (C) and the organic solvent (D).

[0107] (Application) The organic compound (A) has a hydrolyzable silyl group with good curability or reactivity, and can be used, for example, as a dehydrating agent or a curable material. In particular, when the organic compound (A) is an organic polymer, it is suitable as a curable material. Therefore, the organic compound (A) can constitute a curable composition containing it.

[0108] The curable composition preferably contains a curing catalyst for the purpose of promoting the reaction of hydrolyzing and condensing the hydrolyzable silyl group, i.e., the curing reaction. As the curing catalyst, a conventionally known catalyst can be used, specifically, an organic tin compound, a metal carboxylate, an amine compound, a carboxylic acid, an alkoxy metal, an inorganic acid, a mixture thereof, etc. can be used.

[0109] The curable composition may contain other additives such as silicon compounds, adhesion promoters, plasticizers, solvents, diluents, silicates, fillers, sagging inhibitors, antioxidants, light stabilizers, ultraviolet absorbers, physical property adjusters, tackifier resins, compounds containing epoxy groups, photocurable substances, oxygen curable substances, surface property improvers, epoxy resins, other resins, flame retardants, and foaming agents. In addition, the curable composition may contain various additives as necessary for the purpose of adjusting the physical properties of the composition or the cured product. Examples of such additives include, for example, curability adjusters, radical inhibitors, metal deactivators, antiozonants, phosphorus-based peroxide decomposers, lubricants, pigments, and fungicides.

[0110] The curable composition can be used as an adhesive, a sealing material for buildings, ships, automobiles, roads, etc., an adhesive, a waterproofing material, a coating waterproofing material, a mold release agent, an anti-vibration material, a vibration-damping material, a sound-proofing material, a foaming material, a paint, a spraying material, etc. The cured product obtained by curing the curable composition according to this embodiment has excellent flexibility and adhesiveness, and can therefore be suitably used as a sealing material or an adhesive.

[0111] When the organic compound (A) is an organic compound having no polymer skeleton, the organic compound (A) can also be used as a silane coupling agent or the like.

[0112] The following items enumerate preferred aspects of the present disclosure, but the present invention is not limited to the following items. [Item 1] A method for producing an organic compound (A) having a hydrolyzable silyl group represented by the general formula (1), comprising the steps of: (In formula (1), R 1 R represents a group having 3 or more carbon atoms and a molecular weight of 40 or more. 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. X represents a hydroxyl group or -OR 1 a is 1, 2, or 3; b is 0, 1, or 2; c is 0, 1, or 2; and a+b+c is 3 or less. Relative to 100 parts by weight of the organic compound (B) having a hydrolyzable silyl group represented by the general formula (2), (In formula (2), R 2 , X, and c are as described above. However, X in formula (2) may be the same as X in formula (1) or may be different. d is 1, 2, or 3, and c+d is 3 or less. General formula: R 1 OH (in the formula, R 1 is as described above.) reacting in the presence of 1 part by weight or more of an organic solvent (D) having a relative dielectric constant of 22 or more; A part or all of X in the general formula (2) is -OR 1 4. A method for producing an organic compound (A), comprising exchanging [Item 2] 2. The method according to item 1, wherein the organic solvent (D) comprises at least one selected from the group consisting of methanol, ethanol, acetonitrile, dimethylformamide, dimethylsulfoxide, and N-methylpyrrolidone. [Item 3] 2. The process according to item 1, wherein the organic solvent (D) comprises methanol and / or ethanol. [Item 4] R 1 The method according to any one of items 1 to 3, wherein the compound is represented by the general formula (3). (In formula (3), R 3 R represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. 4 represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or -OR 6 R 6 R represents a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 5 represents an oxygen atom or a nitrogen atom bonded to any group. [Item 5] R 5 is an oxygen atom. [Item 6] R 1 is represented by any one of the formulas (4) to (10), 6. The method according to item 5, wherein the hydroxyl group-containing compound (C) is hydroxyacetone, 4-hydroxy-2-butanone, acetylacetone, dihydroxyacetone, methyl glycolate, acetoin, or 3-hydroxy-3-methyl-2-butanone. [Item 7] R 1 The method according to any one of items 1 to 3, wherein the compound is represented by the general formula (11). (In formula (11), R 7 R represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. 8represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or a halogen atom. [Item 8] R 8 8. The method according to item 7, wherein represents a hydrogen atom or a methyl group. [Item 9] 9. The process according to any one of items 1 to 8, wherein the organic compound (A) is an organic polymer. [Item 10] 10. The method according to item 9, wherein the polymer backbone of the organic polymer is a polyoxyalkylene polymer. [Item 11] 11. The method according to item 9 or 10, wherein X in general formula (2) is a methoxy group, and the organic solvent (D) contains at least one selected from methanol, ethanol, acetonitrile, dimethylformamide, dimethylsulfoxide, and N-methylpyrrolidone. [Item 12] 12. The method according to any one of items 9 to 11, wherein the organic solvent (D) comprises methanol. [Item 13] 13. The method according to any one of items 9 to 12, wherein the reaction between the organic compound (B) and the hydroxyl group-containing compound (C) is carried out in the presence of an acid catalyst (E). [Item 14] Item 14. The process according to item 13, wherein the acid catalyst (E) comprises hydrogen chloride. EXAMPLES

[0113] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The number average molecular weight in the examples is a GPC molecular weight measured under the following conditions. Liquid delivery system: Tosoh HLC-8420GPC Column: Tosoh TSKgel SuperH series Solvent: THF (tetrahydrofuran) Molecular weight: Polystyrene equivalent Measurement temperature: 40℃

[0114] The identification of compounds and the calculation of reaction rates were carried out using the following nuclear magnetic resonance (NMR) spectrometer: 1 This was measured by 1 H NMR. Equipment: AVANCE III HD500 digital equipment (BRUKER) The reaction rate is calculated by dividing all hydrolyzable groups (-OR 1 and X) -OR 1 The ratio (x) of hydrolyzable groups was calculated as follows:

[0115] The viscosity of the polymer was measured at 23° C. using a viscometer RE85U (manufactured by Toki Sangyo Co., Ltd.).

[0116] (Synthesis Example 1) Using polyoxypropylene glycol having a number average molecular weight of about 4,500 as an initiator, propylene oxide was polymerized with zinc hexacyanocobaltate glyme complex catalyst to obtain polyoxypropylene (F-1) having a number average molecular weight of 27,900 and hydroxyl groups at both ends. Sodium methoxide was added in an amount of 1.1 molar equivalents relative to the hydroxyl groups of the hydroxyl-terminated polyoxypropylene (F-1) as a 28% methanol solution. After removing the methanol by vacuum distillation, 1.3 molar equivalents of allyl chloride was added relative to the hydroxyl groups of the polymer (F-1) and reacted at 130°C for 1 hour, after which the allyl chloride was distilled off. The resulting unpurified allyl-terminated polyoxypropylene was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation, and the metal salts in the polymer were removed by distilling the hexane from the resulting hexane solution under reduced pressure. As a result of the above, polyoxypropylene (G-1) having carbon-carbon unsaturated bonds (allyl groups) was obtained. Next, 50 ppm of platinum divinyldisiloxane complex (3 wt% isopropanol solution in terms of platinum) and 0.89 wt. parts of trimethoxysilane were added to 100 wt. parts of polymer (G-1) at 90°C to carry out a hydrosilylation reaction of the allyl group of polymer (G-1). The reaction was carried out at 90°C until trimethoxysilane was completely consumed, and then the volatile components were distilled off. As a result, polyoxypropylene (B-1) having a trimethoxysilyl group was obtained.

[0117] Example 1 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 10 parts by weight of methanol and 2 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 1 hour. After that, 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-1). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1 It was confirmed that the reaction rate x was generated (expressed by formula (4)). The reaction rate x was calculated by the above-mentioned method, and the results are shown in Table 1. The same applies below.

[0118] Example 2 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 10 parts by weight of methanol and 6 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove the hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-2). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1 It was confirmed that the kinetic energy of the saturation current (expressed as equation (4)) was generated.

[0119] Example 3 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, and then 10 parts by weight of dimethylformamide and 2 parts by weight of hydroxyacetone were added and reacted at 70°C for 1 hour. After that, 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-3). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1 It was confirmed that the kinetic energy of the saturation current (expressed as equation (4)) was generated.

[0120] Example 4 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, and then 10 parts by weight of dimethyl sulfoxide and 2 parts by weight of hydroxyacetone were added and reacted at 70°C for 1 hour. After that, 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-4). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1 It was confirmed that the kinetic energy of the saturation current (expressed as equation (4)) was generated.

[0121] Example 5 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 10 parts by weight of N-methylpyrrolidone and 3.8 parts by weight of hydroxyacetone were added and reacted at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-5).1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1 It was confirmed that the kinetic energy of the saturation current (expressed as equation (4)) was generated.

[0122] Example 6 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 20 parts by weight of acetonitrile and 4 parts by weight of hydroxyacetone were added and reacted at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-6). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1 It was confirmed that the kinetic energy of the saturation current (expressed as equation (4)) was generated.

[0123] Example 7 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 2700 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 10 parts by weight of methanol and 3.7 parts by weight of 4-hydroxy-2-butanone, and the reaction was carried out at 70°C for 1 hour. After that, 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-7). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from 4-hydroxy-2-butanone: -OR 1 (R 1 It was confirmed that the saturation current (expressed as equation (5)) occurs.

[0124] Example 8 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, followed by 10 parts by weight of methanol and 4.3 parts by weight of 3-hydroxy-3-methyl-2-butanone, and the mixture was reacted at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-8). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from 3-hydroxy-3-methyl-2-butanone: -OR 1 (R 1 It was confirmed that the saturation current (expressed as in equation (10)) occurs.

[0125] Example 9 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 15 parts by weight of methanol and 1.9 parts by weight of acetylacetone, and the reaction was carried out at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-9). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from acetylacetone: -OR 1 (R 1 It was confirmed that the saturation current (expressed as equation (6)) occurs.

[0126] Example 10 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 10 parts by weight of methanol and 2.3 parts by weight of methyl glycolate, and the reaction was carried out at 70°C for 1 hour. After that, 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-10). 1 H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from methyl glycolate: -OR 1 (R 1 It was confirmed that the sigma-induced ...

[0127] Example 11 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 15 parts by weight of methanol and 1.2 parts by weight of dihydroxyacetone, and the reaction was carried out at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-11). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from dihydroxyacetone: -OR 1 (R 1 It was confirmed that the sigma-induced ...

[0128] Example 12 To 100 parts by weight of polyoxypropylene (G-1) having carbon-carbon unsaturated bonds (allyl groups) obtained in Synthesis Example 1, 50 ppm of platinum divinyldisiloxane complex (3 wt% isopropanol solution in terms of platinum) and 1.33 parts by weight of triethoxysilane were added to carry out a hydrosilylation reaction of the allyl groups of the polymer (G-1). The reaction was carried out at 90°C until the triethoxysilane was completely consumed, and then the volatile components were distilled off. As a result, polyoxypropylene (B-2) having triethoxysilyl groups was obtained. To 100 parts by weight of polyoxypropylene (B-2) having triethoxysilyl groups, 2700 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 14 parts by weight of ethanol and 3.2 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 1 hour. After that, 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-12). 1 Analysis by H NMR spectroscopy revealed that the ethoxy groups in the triethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1 It was confirmed that the kinetic energy of the saturation current (expressed as equation (4)) was generated.

[0129] (Example 13) To 100 parts by weight of polyoxypropylene (B-2) having triethoxysilyl groups, 2700 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 10 parts by weight of ethanol and 6 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 1 hour. After that, 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-13). 1 Analysis by H NMR spectroscopy revealed that the ethoxy groups in the triethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1 It was confirmed that the kinetic energy of the saturation current (expressed as equation (4)) was generated.

[0130] (Synthesis Example 2) To 100 parts by weight of the hydroxyl-terminated polyoxypropylene (F-1), 30 ppm of a bismuth (III) 2-ethylhexanoate solution (Bi: 25%) and 0.95 molar equivalents of (3-isocyanatepropyl)trimethoxysilane relative to the hydroxyl groups of the polymer were added, and a urethanization reaction was carried out on the hydroxyl groups of the polymer to obtain polyoxypropylene (B-3) having trimethoxysilyl groups.

[0131] Example 14 To 100 parts by weight of polyoxypropylene (B-3) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 10 parts by weight of methanol and 1.8 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 3 hours. After that, 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-14). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1 It was confirmed that the reaction was caused by the reaction of 1,2-dihydrolyzable groups (represented by formula (4)). However, since the peaks corresponding to the hydrolyzable groups before and after the reaction overlapped, it was not possible to calculate the reaction rate.

[0132] Example 15 To 0.43 g of 3-chloropropyltrimethoxysilane, 5.0 g of THF and 18 mg of 1% hydrogen chloride (methanol solution) were added, and further 1.0 g of methanol and 1.3 g of hydroxyacetone were added, and the reaction was carried out at 70° C. for 2 hours. 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from hydroxyacetone: -OR 1 (R 1It was confirmed that the reaction was caused by the reaction of 1,2-dihydrolyzable groups (represented by formula (4)). However, since the peaks corresponding to the hydrolyzable groups before and after the reaction overlapped, it was not possible to calculate the reaction rate.

[0133] (Example 16) To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 15 parts by weight of methanol and 17 parts by weight of 3-butyn-2-ol were added and reacted at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-15). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from 3-butyn-2-ol: -OR 1 It was confirmed that this was occurring.

[0134] (Example 17) To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 15 parts by weight of methanol and 20 parts by weight of 2-methyl-3-butyn-2-ol were added and reacted at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-16). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from 2-methyl-3-butyn-2-ol: -OR 1 It was confirmed that this was occurring.

[0135] (Example 18) To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 15 parts by weight of methanol and 17 parts by weight of 3-butyn-1-ol were added and reacted at 70°C for 1 hour, after which 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-17). 1 Analysis by H NMR spectroscopy revealed that the methoxy groups in the trimethoxysilyl groups contained in the raw material were reduced, and the hydrolyzable groups derived from 3-butyn-1-ol: -OR 1 However, since the peaks corresponding to the hydrolyzable groups before and after the reaction overlapped, it was not possible to calculate the reaction rate.

[0136] Comparative Example 1 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups obtained in Synthesis Example 1, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, and 2 parts by weight of hydroxyacetone was added and reacted at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-1). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0137] Comparative Example 2 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, and then 10 parts by weight of 1-propanol and 2 parts by weight of hydroxyacetone were added and reacted at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-2). 1Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0138] Comparative Example 3 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, and then 10 parts by weight of acetone and 2 parts by weight of hydroxyacetone were added and reacted at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-3). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0139] Comparative Example 4 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, and then 10 parts by weight of THF and 2 parts by weight of hydroxyacetone were added and reacted at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-4). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0140] Comparative Example 5 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 2700 ppm of 1% hydrogen chloride (methanol solution) was added, and then 3.7 parts by weight of 4-hydroxy-2-butanone was added and reacted at 70°C for 1 hour, after which 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-5). 1Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0141] Comparative Example 6 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 4.3 parts by weight of 3-hydroxy-3-methyl-2-butanone was added and reacted at 70°C for 1 hour, after which 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-6). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0142] Comparative Example 7 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 1.9 parts by weight of acetylacetone was added and reacted at 70°C for 1 hour, after which 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-7). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0143] Comparative Example 8 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, and then 2.3 parts by weight of methyl glycolate was added and reacted at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-8). 1Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0144] Comparative Example 9 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 1.2 parts by weight of dihydroxyacetone was added and reacted at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-9). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0145] Comparative Example 10 To 100 parts by weight of polyoxypropylene (B-2) having triethoxysilyl groups, 2700 ppm of 1% hydrogen chloride (methanol solution) was added, and 3.2 parts by weight of hydroxyacetone was added and reacted at 70°C for 1 hour. After that, 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-10). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in ethoxy groups in the triethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0146] Comparative Example 11 To 0.43 g of 3-chloropropyltrimethoxysilane, 5.0 g of THF and 18 mg of 1% hydrogen chloride (methanol solution) were added, and 1.3 g of hydroxyacetone was added, followed by reaction at 70° C. for 2 hours. 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0147] Comparative Example 12 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and 17 parts by weight of 3-butyn-2-ol was added and reacted at 70°C for 1 hour, after which 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-11). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0148] Comparative Example 13 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 20 parts by weight of 2-methyl-3-butyn-2-ol was added and reacted at 70°C for 1 hour, after which 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-12). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0149] Comparative Example 14 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride (methanol solution) was added, and then 17 parts by weight of 3-butyn-1-ol was added and reacted at 70°C for 1 hour, after which 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-13). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0150] Comparative Example 15 To 100 parts by weight of the polyoxypropylene (B-1) having trimethoxysilyl groups obtained in Synthesis Example 1, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, and then 10 parts by weight of methanol and 0.05 parts by weight of hydroxyacetone were added and reacted at 70°C for 1 hour. After that, 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-14). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0151] Comparative Example 16 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride (methanol solution) was added, followed by the addition of 0.1 parts by weight of methanol and 2 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-15). 1 Analysis by 1 H NMR spectroscopy revealed that no reduction in methoxy groups in the trimethoxysilyl groups contained in the raw material, i.e., no progress of an exchange reaction, could be confirmed.

[0152] (Examples 19 to 35, Comparative Examples 17 to 31) Under an atmosphere of 23°C and relative humidity of 50%, 0.5 parts by weight of DBU (1,8-diazabicyclo[5,4,0]undecene-7, manufactured by Tokyo Chemical Industry Co., Ltd.) was added to 100 parts by weight of the polymer shown in Table 1 filled in a plastic container, and the mixture was stirred with a spatula for 1 minute to mix.

[0153] (Skinning time) The time when mixing was completed was defined as the start time of measurement, and the time when the surface was touched with a spatula and the composition to be evaluated no longer adhered to the spatula was defined as the skinning time. The results are shown in Table 1.

[0154] (viscosity ratio) The viscosity of the raw material polymer and the viscosity of the polymer obtained by the exchange reaction were measured, and the viscosity ratio was calculated by the following formula. A smaller viscosity ratio is better in that the viscosity of the polymer obtained after the reaction is low and easy to handle. Viscosity ratio = (viscosity of polymer obtained after reaction (polymer A or A')) ÷ (viscosity of raw material polymer (polymer B)) In Table 1, those with a viscosity ratio of less than 150% are indicated as ◯, and those with a viscosity ratio of 150% or more are indicated as △.

[0155] [Table 1]

[0156] (result) As is clear from the results of Examples 1 to 18 and Comparative Examples 1 to 16, when a hydroxyl-containing compound (C) is reacted with polyoxypropylene having a trimethoxysilyl group or a triethoxysilyl group, or a low molecular weight compound having a trimethoxysilyl group, to carry out an exchange reaction with the methoxy group of the trimethoxysilyl group or the ethoxy group of the triethoxysilyl group, the exchange reaction proceeds efficiently by using a specific amount or more of an organic solvent (D) having a dielectric constant of 22 or more.

[0157] As is clear from the "Viscosity ratio" in Table 1, when methanol or ethanol is used as the organic solvent (D), the increase in viscosity of the polymer tends to be small, and the polymer obtained after the reaction has a low viscosity and is easy to handle.

[0158] From the results of Examples 19 and 20 and Comparative Example 30 in Table 1, it can be seen that when the amount of hydroxyl-containing compound (C) used is small, the exchange reaction does not proceed easily, and as the amount of hydroxyl-containing compound (C) used increases, the exchange reaction proceeds more smoothly and the reaction rate improves. From the results of Example 19 and Comparative Example 31 in Table 1, it is understood that when the amount of the organic solvent (D) used is small, the exchange reaction does not easily proceed.

[0159] Furthermore, as is clear from the results of Examples 19 to 35 and Comparative Examples 17 to 31, the polymers obtained in each Example had a shorter skinning time when mixed with a curing catalyst compared to the polymers of each Comparative Example, indicating that the polymers had improved curability.

Claims

1. A method for producing an organic compound (A) having a hydrolyzable silyl group represented by the following general formula (1), comprising the steps of: 【Chemistry 1】 (In formula (1), R 1 R represents a group having 3 or more carbon atoms and a molecular weight of 40 or more. 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. X represents a hydroxyl group or -OR 1 a is 1, 2, or 3; b is 0, 1, or 2; c is 0, 1, or 2; and a+b+c is 3 or less. Relative to 100 parts by weight of an organic compound (B) having a hydrolyzable silyl group represented by the following general formula (2), 【Chemistry 2】 (In formula (2), R 2 , X, and c are as described above. However, X in formula (2) may be the same as or different from X in formula (1). d is 1, 2, or 3, and c+d is 3 or less. General formula: R 1 OH (in the formula, R 1 is as described above.) reacting in the presence of 1 part by weight or more of an organic solvent (D) having a relative dielectric constant of 22 or more; A part or all of X in the general formula (2) is -OR 1 A method for producing an organic compound (A), comprising exchanging

2. The method according to claim 1, wherein the organic solvent (D) comprises at least one selected from the group consisting of methanol, ethanol, acetonitrile, dimethylformamide, dimethylsulfoxide, and N-methylpyrrolidone.

3. The method according to claim 1 , wherein the organic solvent (D) comprises methanol and / or ethanol.

4. R 1 The method according to any one of claims 1 to 3, wherein the compound is represented by the following general formula (3): 【Chemistry 3】 (In formula (3), R 3 R represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. 4 represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or -OR 6 represents R 6 R represents a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 5 represents an oxygen atom or a nitrogen atom bonded to any group.

5. R 5 The method according to claim 4 , wherein is an oxygen atom.

6. R 1 is represented by any one of the following formulas (4) to (10): 【Chemistry 4】 【Chemistry 5】 【Chemistry 6】 【Chemistry 7】 【Chemistry 8】 【Chemistry 9】 【Chemistry 10】 The method according to claim 5, wherein the hydroxyl group-containing compound (C) is hydroxyacetone, 4-hydroxy-2-butanone, acetylacetone, dihydroxyacetone, methyl glycolate, acetoin, or 3-hydroxy-3-methyl-2-butanone.

7. R 1 The method according to any one of claims 1 to 3, wherein the compound is represented by the following general formula (11): 【Chemistry 11】 (In formula (11), R 7 R represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. 8 represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or a halogen atom.

8. R 8 The method according to claim 7 , wherein represents a hydrogen atom or a methyl group.

9. The method according to any one of claims 1 to 3, wherein the organic compound (A) is an organic polymer.

10. The method according to claim 9 , wherein the polymer backbone of the organic polymer is a polyoxyalkylene polymer.

11. The method according to claim 9, wherein X in the general formula (2) is a methoxy group, and the organic solvent (D) includes at least one selected from methanol, ethanol, acetonitrile, dimethylformamide, dimethylsulfoxide, and N-methylpyrrolidone.

12. The process according to claim 9, wherein the organic solvent (D) comprises methanol.

13. The method according to claim 9, wherein the reaction between the organic compound (B) and the hydroxyl group-containing compound (C) is carried out in the presence of an acid catalyst (E).

14. The process according to claim 13, wherein the acidic catalyst (E) comprises hydrogen chloride.

Citation Information

Patent Citations

  • Production method of organic polymer having trimethoxysilyl group at terminal end

    JP2008285585A