Manufacturing method for all-solid battery
By laminating electrodes in a controlled dew point environment and press-molding, the method addresses electrode warpage and moisture exposure in all-solid-state batteries, ensuring stable battery characteristics and durability.
Patent Information
- Application Number
- JP2023056376
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
All-solid-state batteries face challenges in maintaining stable battery characteristics and durability due to electrode warpage and moisture exposure during the manufacturing process, despite dew point control measures.
The manufacturing process includes laminating electrodes in a controlled dew point environment of -40°C and 127 ppm water concentration for 20 minutes or more, followed by press-molding to form an electrode laminate, which suppresses warpage and maintains ionic conductivity.
This method results in a high-quality all-solid-state battery with stable electrical properties and durability by preventing moisture-induced conductivity loss and warpage issues.
Smart Images

Figure 2024143611000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an all-solid-state electrolyte. The all-solid-state battery of the present invention includes a lithium ion secondary battery and the like. [Background technology]
[0002] In recent years, with environmental considerations in mind, the development of secondary batteries that can be repeatedly charged and discharged as energy sources for automobiles and homes has been progressing. While the development of secondary batteries that can be expected to have high capacity and high output is expected, at the same time, greater emphasis must be placed on safety.
[0003] Among lithium-ion secondary batteries, which are one of the representative secondary batteries, solid-state batteries using solid electrolytes are known. An all-solid-state battery, which is one of the solid-state batteries, includes a solid electrolyte layer, a positive electrode layer formed on one side of the solid electrolyte layer, a negative electrode layer formed on the other side, a positive electrode plate connected to the positive electrode layer, and a negative electrode plate connected to the negative electrode layer.
[0004] The positive electrode layer can be obtained by coating a positive electrode current collector with a slurry containing positive electrode active material particles, a binder, a solid electrolyte, and a solvent, and then drying the slurry. The positive electrode current collector can be made of aluminum foil or the like. On the other hand, the negative electrode can be obtained by coating a negative electrode current collector with a slurry containing negative electrode active material particles, a binder, a solid electrolyte, and a solvent, and then drying the slurry. The negative electrode current collector can be made of copper foil. Alternatively, a lithium metal layer formed on stainless steel foil can be used as the negative electrode. The positive electrode layer or the negative electrode layer can further contain a conductive assistant.
[0005] The solid electrolyte layer can be formed by dispersing a solid electrolyte powder in a solvent to form a slurry, which is then applied and dried. For example, the solid electrolyte layer can be formed directly on the surface of the negative electrode layer or the positive electrode layer. The solid electrolyte layer can also be obtained by forming the solid electrolyte layer on the surface of a substrate such as a polyethylene terephthalate (PET) film, and then peeling off the PET film.
[0006] The resulting positive and negative electrodes are laminated with a solid electrolyte sandwiched therebetween and pressurized to obtain an electrode laminate. A positive electrode terminal and a negative electrode terminal are attached to this electrode laminate, and the electrode laminate is housed and sealed in an outer container so that one end of each terminal is extended to the outside, to obtain an all-solid-state battery.
[0007] As a solid electrolyte, a sulfide solid electrolyte is known. It is known that the sulfide solid electrolyte is chemically unstable and that its ionic conductivity decreases due to moisture during exposure to the atmosphere. Therefore, when using a sulfide solid electrolyte, the positive electrode or negative electrode active material and the solid electrolyte material itself are sufficiently dried in advance, and the dew point is strictly controlled in the lamination process of the positive electrode, negative electrode, and solid electrolyte layer, so that the assembly can be performed quickly under a low moisture concentration.
[0008] Patent Document 1 discloses that in a slurry drying step for forming an electrode layer of an all-solid-state battery, drying is performed in an atmosphere with a volatile organic compound concentration of 100 ppm or less. Patent Document 2 discloses that a lithium ion conductive solid electrolyte is dried by heating in a temperature range of 80°C to 140°C. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2019-200890 A [Patent Document 2] JP 2008-103145 A Summary of the Invention [Problem to be solved by the invention]
[0010] Even if an all-solid-state battery is assembled under dew point control, it is difficult to completely block exposure to moisture, so it is considered desirable to complete the process up to the stage of sealing the electrode stack in an outer container as quickly as possible. However, no matter how quickly an all-solid-state battery is assembled, the characteristics of the all-solid-state battery may deteriorate.
[0011] As a result of intensive research by the inventors, it was found that an all-solid-state battery having stable battery characteristics and durability characteristics cannot be obtained unless the manufacturing process of the electrode laminate including the positive electrode, the solid electrolyte membrane, and the negative electrode is further improved. Specifically, there was a problem that the electrodes including the positive electrode and the negative electrode and the solid electrolyte membrane may be warped due to the process of pressing them with high pressure. In order to prevent the solid electrolyte from being exposed to moisture, simply assembling the electrode laminate in a short time may not solve the problem of the electrode laminate warping. [Means for solving the problem]
[0012] The present invention relates to a negative electrode and A positive electrode and A solid electrolyte membrane; to form an electrode stack; exposing the electrode laminate to an environment having a dew point temperature of −40° C. and a moisture concentration of 127 ppm or less for 20 minutes or more; press-molding the electrode stack; The present invention relates to a method for producing an all-solid-state battery, comprising: Effect of the Invention
[0013] According to the manufacturing method of the present invention, a high-quality all-solid-state battery can be obtained in which the solid electrolyte does not suffer from a decrease in ion conductivity due to the influence of moisture, and the decrease in electrical characteristics and durability due to warping of the electrode laminate is also suppressed. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a flow diagram showing an outline of an assembly process for an all-solid-state battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The following describes an embodiment of the present invention with reference to the drawings. Note that the present invention is not limited to the embodiment described below, and can be implemented within the scope of the present invention. The following is an example, and does not limit the present invention in any way.
[0016] <All-solid-state battery> In this specification, the term "all-solid-state battery" refers to a battery in which the electrolyte is made of a solid electrolyte, which will be described later. In addition, in this specification, the term "all-solid-state battery" includes secondary batteries and primary batteries. <Negative electrode> The negative electrode may be any negative electrode used in non-aqueous secondary battery materials, and is not particularly limited. For example, the negative electrode includes a negative electrode collector such as copper foil, and a negative electrode layer containing a negative electrode active material and a solid electrolyte. The negative electrode layer preferably contains a binder. A negative electrode collector made of stainless steel may be used instead of the negative electrode collector such as copper foil, and a lithium metal layer may be formed on the surface of the negative electrode collector by rolling or the like instead of the negative electrode active material. The negative electrode layer containing the negative electrode active material, the solid electrolyte, and the binder may be formed on at least one surface of the negative electrode collector.
[0017] When a negative electrode active material is used for the negative electrode, it is preferable to use a carbon-based active material. As the carbon-based active material, natural graphite, artificial graphite, hard carbon, soft carbon, carbon black, or any mixture thereof can be selected. Natural graphite includes natural graphite with amorphous carbon coated on the particle surface, and similarly, artificial graphite includes artificial graphite with amorphous carbon coated on the particle surface. These natural graphites and artificial graphites can be primary particles or particles in which primary particles are aggregated to form secondary particles, and mixtures thereof. In addition, the negative electrode active material may be a mixture of a carbon-based active material and a silicon-based active material. The negative electrode active material may include metal materials such as aluminum, silver, bismuth, calcium, cerium, indium, magnesium, tin, zinc, and nickel.
[0018] Examples of the binder used in the negative electrode layer include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF), conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles, synthetic rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (NBR), and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin. In addition, examples of the binder include polyacrylic acid, polymethacrylic acid, sodium polyacrylate, potassium polyacrylate, sodium polymethacrylate, potassium polymethacrylate, ethyl polyacrylate, ethyl polyacrylate, butyl polyacrylate, methyl polymethacrylate, ethyl polymethacrylate, butyl polymethacrylate, and any mixture thereof. The content of the binder is preferably 1% by mass or more and less than 10% by mass with respect to the total solid content of the negative electrode layer. If the content of the binder is too high, the surface of the negative electrode active material is covered with the binder in a large area, which may reduce the ionic conductivity and electronic conductivity. If the content of the binder is too low, the electrical contact between the particles of the negative electrode active material may not be properly performed.
[0019] In addition to the above compounds, the binder component may further include carboxymethylcellulose (referred to as "CMC"), which is a cellulose derivative, or a metal salt of carboxymethylcellulose (e.g., sodium carboxymethylcellulose, potassium carboxymethylcellulose). When CMC or a metal salt of CMC is further added as a binder component, the content of CMC or the CMC metal salt is preferably 0.05% by mass or more and 1.5% by mass or less with respect to the total solid content of the negative electrode layer.
[0020] The negative electrode layer may further contain a conductive assistant. The conductive assistant is a material for reducing the resistance of the electrode. Examples of the conductive assistant include carbon black such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, carbon nanotubes, carbon nanofibers, carbon brushes, and other carbon fibers.
[0021] When carbon nanotubes or carbon nanofibers are used as the conductive assistant, the content of the conductive assistant is 0.01% by mass to 3% by mass, preferably 0.03% by mass to 1% by mass, based on the total solid content of the negative electrode layer.
[0022] In addition to the above-mentioned materials, the negative electrode layer may appropriately contain electrode additives that are generally used for forming electrodes, such as thickeners, dispersants, and stabilizers.
[0023] <Solid electrolyte membrane> The negative electrode, solid electrolyte film, and positive electrode used in the manufacturing method of the embodiment include a solid electrolyte. Examples of the solid electrolyte used here include an oxide-based solid electrolyte and a sulfide-based solid electrolyte. As the oxide-based solid electrolyte, for example, a garnet-type, NASICON-type, or perovskite-type oxide-based material can be used. As the sulfide-based solid electrolyte, any known sulfide-based material can be used, for example, LiPO 4 -Li 2 S-SiS, 75%Li 2 S-25%P 2 S 5 mixture, Li 2 S-SiS 2 , Li 2 SP 2 S 5 , Li 3 P.S. 4 , Li 3 PO 4 -Li 2 S-Si 2 S., Li 3 PO 4 -Li 2 S-SiS 2 , LiI-Li2 S.B. 2 S 3 , LiI-Li 2 S-SiS 2 , LiI-Li 2 SP 2 S 5 , LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 Li 2 SP 2 S 5 -LiCl, Li 6 P.S. 5 Cl, Li 10 GeP 2 S 12 , Li 3.25 Ge 0.25 P 0.75 S 4 In the embodiment, it is preferable to use a sulfide-based solid electrolyte. The solid electrolyte membrane used in the embodiment refers to a thin flat surface having a predetermined area and made of a solid electrolyte. The solid electrolyte membrane may be a single layer (a solid electrolyte membrane made of one type of solid electrolyte) or a multi-layer (a solid electrolyte membrane made of two or more types of solid electrolyte membranes stacked together).
[0024] In the present invention, the solid electrolyte membrane is preferably formed to have a thickness of 15 to 150 μm. If the thickness is smaller than this, a short circuit is likely to occur when the solid electrolyte is press-formed under high pressure. On the other hand, if the thickness is larger than this, the cell volume will be excessively increased, and the energy density per unit volume of the all-solid-state battery will not increase.
[0025] <Positive electrode> The positive electrode can be a positive electrode used in a non-aqueous secondary battery material, and is not particularly limited. For example, the positive electrode includes a positive electrode current collector and a positive electrode layer containing a positive electrode active material and a solid electrolyte. The positive electrode layer preferably contains a binder. The positive electrode layer containing the positive electrode active material, the solid electrolyte, and the binder can be formed on at least one surface of the positive electrode current collector.
[0026] The positive electrode current collector can be made of stainless steel, aluminum, nickel, titanium, or a positive electrode current collector in which the surface of aluminum or stainless steel is surface-treated with carbon, nickel, titanium, or silver.
[0027] The positive electrode active material preferably contains a lithium nickel-based composite oxide as the positive electrode active material. The lithium nickel-based composite oxide is represented by the general formula Li x Ni y Me (1-y) O 2 (wherein Me is at least one metal selected from the group consisting of Al, Mn, Na, Fe, Co, Cr, Cu, Zn, Ca, K, Mg, and Pb). The lithium manganese-based composite oxide that can include the lithium manganese-based composite oxide is, for example, lithium manganate (LiMnO 2 ), lithium manganese spinel oxide (LiMn 2 O 4 The positive electrode active material is particularly a material represented by the general formula Li x Ni y Co z Mn (1-y-z) O 2It is preferable that the positive electrode active material contains a lithium nickel manganese cobalt composite oxide having a layered crystal structure represented by the formula: Here, in the general formula, x is 1≦x≦1.2, y and z are positive numbers satisfying y+z<1, and the value of y is 0.5 or more. In order to obtain a high-capacity battery, it is particularly preferable that y>1-yz and y>z. The lithium nickel composite oxide having this general formula is, in other words, a lithium nickel cobalt manganese composite oxide. The lithium nickel cobalt manganese composite oxide is a lithium nickel composite oxide that is preferably used to increase the capacity of a battery. In addition, the positive electrode active material is a lithium nickel composite oxide having the general formula LiMPO 4 (M is at least one selected from the group consisting of Mn, Fe, Co and Ni). The surface of the positive electrode layer may contain LiNbO 3 The buffer layer may be formed by coating the positive electrode layer with a material such as . The buffer layer can be formed with a thickness of 10 nm or less to suppress the interface resistance between the positive electrode layer and the solid electrolyte membrane. The buffer layer can be formed on the surface of the positive electrode layer by a sol-gel method or the like.
[0028] Examples of binders that form the positive electrode layer together with the positive electrode active material include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF); conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles; styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (ACRB). Examples of the rubber include synthetic rubber such as NBR (Nylon Brass) and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin.
[0029] The positive electrode layer may also contain a conductive assistant. Examples of the conductive assistant include carbon black such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, carbon nanofibers, carbon nanotubes, carbon nanobrushes, and other carbon fibers. In addition, the positive electrode layer may appropriately contain electrode additives that are generally used for forming electrodes, such as thickeners, dispersants, and stabilizers.
[0030] <Cell Creation> First, we will explain how to prepare the negative electrode. There are several methods for preparing the negative electrode. Regardless of the method used, it is preferable to prepare the negative electrode in a low moisture environment under dew point control in order to suppress the adsorption of moisture into the solid electrolyte.
[0031] <Preparation of negative electrode> When using a negative electrode in which a negative electrode active material is formed on a negative electrode current collector, a slurry in which a negative electrode active material, a solid electrolyte, and a binder are dispersed in a dehydrated organic solvent is applied to a part or all of the surface of a negative electrode current collector such as a copper foil, and dried to obtain a negative electrode precursor sheet. The obtained negative electrode precursor sheet is compressed by a press molding method such as a roll press, a uniaxial press, a rubber press, or an isostatic press (cold isostatic press method [CIP], hot isostatic press method [WIP], and especially cold isostatic press method is preferable), to obtain a negative electrode sheet. Examples of organic solvents include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, N-methylpyrrolidone, as well as ether solvents, thiol solvents, butyl butyrate, etc., and it is preferable that all of them are dehydrated.
[0032] Alternatively, a granulated negative electrode active material containing at least a negative electrode active material, a solid electrolyte, and a binder can be transferred to a negative electrode current collector to obtain a negative electrode precursor sheet. In this case, a surface layer containing a polymer component such as a binder that enhances adhesion to the granulated negative electrode active material may be formed in advance on the surface of the negative electrode current collector. The negative electrode layer may also contain a conductive assistant. The obtained negative electrode precursor sheet is compressed by a press molding method such as a roll press, a uniaxial press, a rubber press, or a cold isostatic press (CIP, WIP) to obtain a negative electrode sheet.
[0033] Alternatively, a metallic lithium layer such as lithium foil is disposed on all or part of a stainless steel negative electrode current collector, and these are then bonded together by rolling or other treatment to obtain a negative electrode sheet.
[0034] <Preparation of solid electrolyte membrane> Next, a solid electrolyte membrane is formed on the surface of the negative electrode. Regardless of the method used to form the solid electrolyte membrane, it is preferable to form it in a low moisture environment under dew point control in order to prevent moisture from being adsorbed by the solid electrolyte.
[0035] A slurry in which a solid electrolyte is dispersed in an organic solvent is applied to the surface of the negative electrode layer formed on a copper foil or the surface of metallic lithium formed on a stainless steel foil, and then dried to form a solid electrolyte film on the surface of the negative electrode. Examples of the organic solvent include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, and it is preferable that all of them are dehydrated.
[0036] Alternatively, a slurry in which a solid electrolyte is dispersed in an organic solvent is applied to the surface of a polyester film mainly composed of polyester, followed by drying to form a solid electrolyte film, and then laminating the polyester film together with the surface of the negative electrode layer or the surface of metallic lithium so that the solid electrolyte film is in contact with the surface of the negative electrode layer or the surface of metallic lithium, thereby forming a solid electrolyte film on the surface of the negative electrode.
[0037] The laminated negative electrode and solid electrolyte membrane are compressed by a press molding method such as roll press, uniaxial press, rubber press, or isostatic press (CIP, WIP), to obtain a negative electrode-solid electrolyte membrane laminate. When the solid electrolyte is laminated together with a polyester sheet and pressurized, the polyester film is peeled off from the solid electrolyte membrane. In this case, it is also preferable to use a polyester film whose surface is coated with a release agent such as silicone so that the polyester film can be easily peeled off from the solid electrolyte membrane.
[0038] <Preparation of positive electrode> Next, the preparation of the positive electrode will be described. Regardless of the method used to prepare the positive electrode, it is preferable to prepare the positive electrode in a low moisture environment under dew point control in order to suppress adsorption of moisture.
[0039] A slurry in which a positive electrode active material, a solid electrolyte, and a binder are dispersed in a dehydrated organic solvent is applied to a part or the whole surface of a positive electrode current collector such as aluminum, and then dried to obtain a positive electrode sheet. Examples of organic solvents include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, and it is preferable that all of them are dehydrated.
[0040] <Formation of Electrode Laminate> The positive electrode sheet is laminated on the negative electrode-solid electrolyte membrane laminate to obtain an electrode laminate precursor. When a sulfide solid electrolyte is used as the solid electrolyte, the ionic conductivity of the solid electrolyte decreases due to exposure to moisture. Therefore, after obtaining the electrode laminate precursor, it is desirable to compress the electrode laminate precursor by a method such as roll press, uniaxial press, rubber press, or isostatic press (CIP, WIP) within a predetermined time to obtain an electrode laminate. The predetermined time is, for example, within 2 days in an environment with a dew point of -40°C and a moisture concentration of 127 ppm or less. If the time passes beyond this, there is a risk of performance deterioration due to water absorption by the solid electrolyte, which is not preferable from the viewpoint of decreasing productivity of all-solid-state batteries.
[0041] The positive electrode can be first roll-pressed in the form of a thin sheet consisting of only a positive electrode layer formed on a positive electrode current collector, and then laminated onto the negative electrode-solid electrolyte membrane laminate, or, from the viewpoint of production efficiency, can be placed on the negative electrode-solid electrolyte membrane laminate without applying pressure to the positive electrode sheet alone, or with only enough pressure to hold down the positive electrode sheet with the conveying arm of the lamination machine. This step is the step immediately before the isostatic pressing to form the electrode laminate.
[0042] When the positive electrode sheet is roll-pressed, the voids in the positive electrode active material and solid electrolyte are crushed at first, but the positive electrode is distorted by springback when the pressure applied to the compact is released. Because the positive electrode is extremely thin, it tends to warp immediately after pressing. However, if the positive electrode sheet is placed on the negative electrode-solid electrolyte membrane laminate in this state and isostatically pressed immediately, the effect of springback becomes significant after the electrode laminate is formed, and fine peeling occurs at the interface between the positive electrode sheet and the solid electrolyte membrane, which may affect the battery characteristics.
[0043] On the other hand, if an attempt is made to laminate a positive electrode sheet on a negative electrode-solid electrolyte membrane laminate without applying substantial pressure to the positive electrode sheet and then perform isostatic pressing, the positive electrode sheet will tend to warp due to the influence of gas present in the voids in the positive electrode layer when the laminate is vacuum-sealed in the pretreatment for isostatic pressing. In this case as well, the warping of the positive electrode may affect the electrode laminate and may affect the electrode laminate and battery characteristics.
[0044] Therefore, it is preferable to leave a predetermined time or more between laminating the positive electrode sheet and the negative electrode-solid electrolyte membrane laminate and performing press molding. In this way, the influence of the warping of the positive electrode is mitigated, and distortion after isostatic pressing can be reduced. The predetermined time is, for example, 20 minutes or more in an environment with a dew point of -40°C and a moisture concentration of 127 ppm or less. This makes it possible to mitigate the warping of the electrode laminate to a degree that does not cause an influence of press molding. When a plurality of negative electrodes, solid electrolyte membranes, and positive electrodes are laminated, it is preferable to finally laminate the positive electrode sheet and the negative electrode-solid electrolyte membrane laminate, and then perform press molding after a predetermined time has elapsed.
[0045] <Sealing of electrode laminate> The obtained electrode laminate is desirably sealed in an exterior case immediately. One end of a rectangular metal plate serving as a negative terminal is attached to the negative current collector, and one end of a rectangular metal terminal serving as a positive terminal is attached to the positive current collector, and then the electrode laminate is housed in an aluminum exterior case. Of the inner surfaces of the exterior case, at least the surface facing the electrode laminate is preferably formed with a resin layer such as polyolefin. The resin layer is heated to melt the resin, and then solidified again to seal the electrode laminate in the aluminum exterior case. At this time, the other end of the positive terminal and the other end of the negative terminal are arranged so as to be drawn out of the exterior case. At the portion where the positive terminal and the negative terminal contact the resin layer on the inner surface of the exterior case, a layer of the same or different type of resin as the resin used in the resin layer on the inner surface of the exterior case can be provided to strengthen the adhesion of the exterior case at that portion. EXAMPLES
[0046] A battery was fabricated according to the flow shown in the embodiment of the invention. Figure 1 is a flow diagram summarizing the embodiment of the invention.
[0047] [I] Formation of negative electrode-solid electrolyte membrane laminate (1) A foil (manufactured by Honjo Metals Co., Ltd.) was prepared as a negative electrode, in which a 20 μm thick metallic lithium layer was formed on the surface of a 10 μm thick stainless steel negative electrode current collector. (2) Li as a solid electrolyte in xylene as an organic solvent 6 P.S. 5 The slurry containing Cl (D50: 8 μm) was applied to the surface of a polyester film mainly composed of polyester and dried to obtain a solid electrolyte membrane. The obtained solid electrolyte membrane was laminated with a polyester film so as to be in contact with the surface of metallic lithium. (3) The negative electrode-solid electrolyte membrane laminate of (2) above was laminated and vacuum sealed in a nylon vacuum pack and held at room temperature (25°C) under a pressure of 400 MPa for 1 minute. Thereafter, while still laminated and sealed, the negative electrode-solid electrolyte membrane laminate was compressed by an isostatic pressure pressing method to obtain a negative electrode-solid electrolyte membrane laminate with a porosity of 7% in the negative electrode layer. The size of the negative electrode and solid electrolyte laminate was 50 mm x 70 mm. (4) The polyester film was peeled off from the solid electrolyte membrane to obtain a negative electrode-solid electrolyte membrane laminate.
[0048] [II] Lamination of the positive electrode sheet and the negative electrode-solid electrolyte membrane laminate (1) LiNi as the positive electrode active material 0.8 Co 0.1 Mn 0.1 O 2 (D50:8μm) 70 mass% and Li as a solid electrolyte 6 P.S. 5 A slurry of 25 mass% Cl (average particle size 1 μm), 2 mass% acetylene black (manufactured by Timcal Japan Co., Ltd.), and 3 mass% styrene-butadiene rubber (SBR) as a binder dispersed in xylene, an organic solvent, was applied to an aluminum foil (manufactured by UACJ Corporation) with a thickness of 10 μm and dried to form a positive electrode layer, thereby obtaining a positive electrode. (2) The positive electrode obtained in (1) above was cut to 45 mm × 65 mm, and laminated so that the positive electrode layer was in contact with the solid electrolyte membrane of the negative electrode-solid electrolyte membrane laminate prepared in [I] to obtain an electrode laminate precursor. The number of layers of the positive electrode and negative electrode-solid electrolyte membrane laminate was one each.
[0049] [III] Mitigating the warping of the positive electrode sheet The electrode laminate precursor obtained in [II] above was stored in a space where the atmosphere was controlled to a dew point temperature of -40°C and a moisture concentration of 127 ppm or less until press molding. The time from laminating the last positive electrode sheet to press molding was set to the time shown in Table 1 (Examples 1 to 3 and Comparative Examples 1 to 2).
[0050] [IV] Pressurizing the electrode stack (1) The electrode laminate precursor obtained in each Example was laminated and vacuum sealed in a nylon vacuum pack and held at room temperature (25° C.) under a pressure of 400 MPa for 1 minute. Next, while still laminated and sealed, the electrode laminate precursor was compressed by an isostatic pressing method to obtain an electrode laminate with a positive electrode layer porosity of 5%.
[0051] [V] Encapsulation in outer case (1) The electrode laminate obtained in [IV] above was enclosed in an outer case by the method described in the embodiment, and a battery was obtained in which the positive and negative terminals were extended outside the aluminum outer case (manufactured by Dai Nippon Printing Co., Ltd.).
[0052] The obtained battery was charged at a constant current of 0.05C up to 4.25V, then switched to constant voltage charging, and cut off at 0.005C. The average discharge operating voltage was then obtained when the battery was discharged at a constant current of 0.05C up to 2.5V. Table 1 shows the average discharge operating voltages of other examples and comparative examples when the average discharge operating voltage of Example 1 is taken as 1. In addition, the "wrinkles after pressing" in Table 1 is evaluated as "present" when wrinkles were observed by visually observing the electrode laminate obtained after compressing the electrode laminate precursor by an isostatic pressing method, and "absent" when wrinkles were observed. [Table 1]
[0053] From Table 1, it can be said that it is preferable to leave a time of 20 minutes or more between the final lamination of the positive electrode sheet and the negative electrode-solid electrolyte membrane laminate and the press molding.
[0054] The embodiment of the present invention is merely an example and is not limited thereto. For example, an aluminum laminate film is used for the exterior case, but a strong aluminum can case or a cylindrical case may also be used. 6 P.S. 5 Although Cl is used, the present invention can be applied to any sulfide-based solid electrolyte that has low chemical stability with water. Although the positive and negative electrodes are adjusted to a predetermined size in advance, they may be laminated and then quickly cut into a predetermined shape. Needless to say, other design changes are possible within the scope of the present invention.
Claims
1. A negative electrode; A positive electrode and A solid electrolyte membrane; to form an electrode stack; exposing the electrode laminate to an environment having a dew point temperature of −40° C. and a moisture concentration of 127 ppm or less for 20 minutes or more; press-molding the electrode stack; A method for producing an all-solid-state battery, comprising:
2. The method for producing an all-solid-state battery according to claim 1, wherein the electrode laminate is exposed to an environment having a dew point temperature of −40° C. and a moisture concentration of 127 ppm or less for 2 days or less.
3. The method for producing an all-solid-state battery according to claim 1 or 2, wherein the electrode laminate is press-molded by an isostatic pressing method.
4. The method for producing an all-solid-state battery according to claim 3 , wherein the isostatic pressing method is cold isostatic pressing method.
5. The method for producing an all-solid-state battery according to claim 3 , wherein the solid electrolyte is a sulfide-based solid electrolyte.
6. The method for producing an all-solid-state battery according to claim 4 , wherein the solid electrolyte is a sulfide-based solid electrolyte.
Citation Information
Patent Citations
Battery material manufacturing method and all-solid battery
JP2008103145A
Method for manufacturing electrode layer
JP2019200890A