Nonaqueous electrolyte secondary battery and manufacturing method of nonaqueous electrolyte secondary battery
The described manufacturing method for non-aqueous electrolyte secondary batteries, with a specific electrode capacity ratio and high-temperature aging, addresses lithium precipitation and durability issues, resulting in improved battery performance.
Patent Information
- Application Number
- JP2023056405
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-30
AI Technical Summary
Existing non-aqueous electrolyte secondary batteries face challenges in lithium precipitation resistance and battery durability, particularly when the positive and negative electrode capacity ratio is adjusted to enhance Li precipitation resistance, leading to decreased durability.
A manufacturing method for non-aqueous electrolyte secondary batteries involving a wound electrode body with a specific capacity ratio of 1.3 to 2.0, where a metal lithium foil is applied to the outermost region of the negative electrode not facing the positive electrode, followed by an initial charging and high-temperature aging process to diffuse Li ions, enhancing both Li precipitation resistance and battery durability.
The method results in a non-aqueous electrolyte secondary battery with improved lithium precipitation resistance and durability, maintaining high capacity retention rates under various conditions.
Smart Images

Figure 2024143631000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a nonaqueous electrolyte secondary battery and a method for manufacturing the nonaqueous electrolyte secondary battery. [Background technology]
[0002] For example, Patent Document 1 listed below discloses a nonaqueous electrolyte secondary battery in which a lithium-containing composite oxide of a transition metal is used for the positive electrode and a carbon material is used for the negative electrode, and the positive and negative electrode plates are spirally wound together with a separator, and a metallic lithium foil is attached to a portion of the negative electrode plate that corresponds to the outermost periphery and does not face the positive electrode plate, and the lithium is diffused into the carbon material by a potential difference or a concentration difference. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-144473 Summary of the Invention [Problem to be solved by the invention]
[0004] Meanwhile, according to the study by the present inventors, it has been found that there is still room for improvement in the above-mentioned nonaqueous electrolyte secondary batteries, for example, from the viewpoint of battery performance (for example, resistance to lithium precipitation and battery durability).
[0005] The present disclosure has been made in view of the above circumstances, and a main object of the present disclosure is to provide a technique for obtaining a nonaqueous electrolyte secondary battery having excellent battery performance. [Means for solving the problem]
[0006] In order to achieve this object, the present disclosure provides a method for producing a nonaqueous electrolyte secondary battery including a wound electrode assembly in which a positive electrode and a negative electrode are superimposed with a separator interposed therebetween and wound, and a nonaqueous electrolyte, the method including the following steps: an assembly preparation step of preparing an assembly in which the wound electrode assembly and the nonaqueous electrolyte are housed in a battery case, in which the ratio of the capacity of the negative electrode to the capacity of the positive electrode in the wound electrode assembly is 1.3 or more and less than 2.0, and a metallic lithium foil is present in at least a part of the outermost periphery of the negative electrode and not facing the positive electrode; an initial charging step of performing an initial charge on the assembly; and a high-temperature aging step of performing an aging treatment on the assembly after the initial charge at a temperature of 60° C. or higher in a charged state in which the potential of the negative electrode is 0.5 V or higher. Although details will be described later, a nonaqueous electrolyte secondary battery having excellent battery performance can be obtained by the method for producing a nonaqueous electrolyte secondary battery having such a configuration.
[0007] From another aspect, the present disclosure provides a nonaqueous electrolyte secondary battery including a wound electrode body in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound, and a nonaqueous electrolyte, wherein a highly integrated lithium element region is present in at least a part of an area in the outermost periphery of the negative electrode that does not face the positive electrode, and the ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.3 or more and less than 2.0. A nonaqueous electrolyte secondary battery having such a configuration is manufactured by, for example, the manufacturing method for a nonaqueous electrolyte secondary battery as described above, and therefore can be said to be a nonaqueous electrolyte secondary battery with excellent battery performance. [Brief description of the drawings]
[0008] [Figure 1] 2 is a flowchart showing each step of a method for manufacturing a nonaqueous electrolyte secondary battery according to one embodiment. [Diagram 2] 4 is a schematic diagram showing the configuration of a wound electrode body prepared in an assembly preparation step according to one embodiment. FIG. [Diagram 3] FIG. 2 is a schematic diagram showing the configuration of a wound electrode body included in a nonaqueous electrolyte secondary battery according to one embodiment. [Figure 4] 1 is a cross-sectional view illustrating a schematic configuration of a nonaqueous electrolyte secondary battery according to one embodiment. [Diagram 5] FIG. 2 is a schematic explanatory diagram for explaining a high lithium element accumulation region in the nonaqueous electrolyte secondary battery according to one embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, some embodiments of the technology disclosed herein will be described with reference to the drawings. In the following drawings, the same reference numerals are used to describe members and parts that perform the same function. In addition, the dimensional relationships (length, width, thickness, etc.) in each drawing do not reflect the actual dimensional relationships. In addition, matters other than those specifically mentioned in this specification and necessary for implementing the technology disclosed herein (for example, the general configuration and manufacturing process of a battery that does not characterize the present invention) can be understood as design matters of a person skilled in the art based on the conventional technology in the field. The technology disclosed here can be implemented based on the contents disclosed in this specification and the technical common sense in the field. In addition, the following description is not intended to limit the present disclosure to the following forms. In addition, the notation "A to B" indicating a range in this specification means "A or more and B or less". In addition, it is intended to include the meaning of "more than A" and "less than B".
[0010] In the present technology, the term "secondary battery" refers to a general storage device that can be repeatedly charged and discharged, and includes so-called storage batteries such as lithium ion secondary batteries and lithium polymer batteries, as well as storage elements such as electric double layer capacitors. In addition, the term "non-aqueous electrolyte secondary battery" refers to a secondary battery that realizes charging and discharging using a non-aqueous electrolyte as a charge carrier, and the electrolyte may be either a gel electrolyte or a non-aqueous electrolyte. As a configuration that can enjoy the benefits of the present technology, for example, a non-aqueous electrolyte solution that is liquid at room temperature (e.g., 25°C) and in which a supporting salt (electrolyte salt) that serves as a charge carrier is dissolved in a non-aqueous solvent may be used. In addition, the term "active material" refers to a substance that can reversibly absorb and release a chemical species that serves as a charge carrier in a secondary battery. In addition, in the present technology, "SOC" means a state of charge, and indicates a state of charge when the state of charge at which the upper limit voltage is obtained is 100% and the state of charge at which the lower limit voltage is obtained is 0% within the range of operating voltages that can be reversibly charged and discharged.
[0011] Hereinafter, as an example, an embodiment in which the nonaqueous electrolyte secondary battery is a flat prismatic lithium ion secondary battery will be described. Here, FIG. 1 is a flowchart showing each step of the manufacturing method of the nonaqueous electrolyte secondary battery according to one embodiment. FIG. 2 is a schematic diagram showing the configuration of the wound electrode body prepared in the assembly preparation step according to one embodiment. FIG. 3 is a schematic diagram showing the configuration of the wound electrode body included in the nonaqueous electrolyte secondary battery according to one embodiment. FIG. 4 is a cross-sectional view showing the configuration of the nonaqueous electrolyte secondary battery according to one embodiment. FIG. 2 is a corresponding view of the wound electrode body prepared in the assembly preparation step according to FIG. 5. Here, in FIG. 2, the separator is omitted for ease of viewing. Note that the manufacturing method of the nonaqueous electrolyte secondary battery disclosed herein may further include other steps at any stage, and if the steps are not described as essential, they can be appropriately deleted. In addition, the order of the steps can be changed as long as the effect of the technology disclosed herein is exerted.
[0012] First, the method for producing a nonaqueous electrolyte secondary battery according to the present embodiment is a method for producing a nonaqueous electrolyte secondary battery including a wound electrode body in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound, and a nonaqueous electrolyte. As shown in Fig. 1, the method for producing such a nonaqueous electrolyte secondary battery includes an assembly preparation step of preparing an assembly in which a wound electrode body and a nonaqueous electrolyte are housed in a battery case; an initial charging step of performing an initial charge on the assembly; and a high-temperature aging step of performing an aging treatment on the assembly after the initial charge at a temperature of 60°C or higher in a charged state in which the potential of the negative electrode is 0.5V or higher. Here, the assembly preparation process is characterized in that the wound electrode body used has a ratio of the capacity of the negative electrode to the capacity of the positive electrode (hereinafter also simply referred to as the "positive / negative electrode capacity ratio") of 1.3 or more and less than 2.0, and a metallic lithium foil is present in at least a part of the outermost periphery of the negative electrode and in an area not facing the positive electrode (hereinafter also simply referred to as the "non-positive electrode facing area of the negative electrode").
[0013] For example, an example of a method for improving Li (lithium) precipitation resistance is to increase the value of the positive and negative electrode capacity ratio. However, in such a case, it is known that the durability of the battery (which can also be called the capacity maintenance rate of the battery) tends to decrease due to excessive formation of the SEI film, etc. Therefore, further development of a technology that can achieve both Li precipitation resistance and battery durability has been required. Then, as a result of intensive research by the present inventor, it was found that excellent Li precipitation resistance can be realized by increasing the positive and negative electrode capacity ratio to 1.3 or more and less than 2.0 in a wound electrode body. Furthermore, it was found that by providing a metallic lithium foil to at least a part of the region that is the outermost periphery of the negative electrode and does not face the positive electrode, Li ions can be diffused in the negative electrode during high-temperature aging as described above to replenish Li ions, thereby achieving excellent battery durability. That is, according to the manufacturing method of a nonaqueous electrolyte secondary battery including the above-mentioned assembly preparation step (step S1), initial charging step (step S2), and high-temperature aging step (step S3), a nonaqueous electrolyte secondary battery in which excellent Li precipitation resistance and excellent battery durability are both achieved can be obtained. Each step will be described below. Note that the structure of the assembly is similar to that of the nonaqueous electrolyte secondary battery 100, except that the wound electrode body has a metallic lithium foil, and therefore FIG. 4 can be appropriately referred to in the description of the assembly.
[0014] (Assembly preparation process: step S1) As described above, in this step, an assembly (battery assembly) is prepared in which the wound electrode body 20 and the non-aqueous electrolyte 80 are housed in the battery case 30. Here, the ratio of the capacity of the negative electrode 60 to the capacity of the positive electrode 50 in the wound electrode body 20 is 1.3 or more and less than 2.0. In addition, the metallic lithium foil 10 is present in at least a part of the region of the wound electrode body 20 that is the outermost periphery of the negative electrode 60 and does not face the positive electrode 50 (this can also be referred to as the outermost periphery of the negative electrode 60 and where one side of the negative electrode 60 does not face the positive electrode 50. This corresponds to the region between P1 and P2 of the negative electrode 60 in FIG. 2).
[0015] The positive electrode 50 used in the assembly preparation step S1 may be a known positive electrode used in a lithium ion secondary battery. The positive electrode 50 typically includes a positive electrode collector 52 and a positive electrode active material layer 54 supported by the positive electrode collector 52, as shown in FIG. 3, for example. The positive electrode active material layer 54 may be provided on one side or both sides of the positive electrode collector 52, but is preferably provided on both sides. The positive electrode 50 typically includes a positive electrode active material layer non-formed portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode collector 52 is exposed) as shown in FIG. 3.
[0016] In this embodiment, the outermost periphery of the wound electrode body 20 is the negative electrode 60. Therefore, as shown in Fig. 3, in the wound electrode body 20, the positive electrode 50 is located on the inner periphery side (in other words, on the winding axis WL side).
[0017] A known positive electrode current collector used in lithium ion secondary batteries may be used as the positive electrode current collector 52, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., aluminum, nickel, titanium, stainless steel, etc.). As the positive electrode current collector 52, aluminum foil is preferred.
[0018] The dimensions of the positive electrode current collector 52 are not particularly limited and may be appropriately determined depending on the battery design. When an aluminum foil is used as the positive electrode current collector 52, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.
[0019] The positive electrode active material layer 54 contains a positive electrode active material. As the positive electrode active material, a known positive electrode active material used in a lithium ion secondary battery may be used. Specifically, for example, as the positive electrode active material, a lithium composite oxide, a lithium transition metal phosphate compound, or the like may be used. The crystal structure of the positive electrode active material is not particularly limited, and may be a layered structure, a spinel structure, an olivine structure, or the like.
[0020] Examples of the lithium composite oxide include lithium nickel composite oxide, lithium cobalt composite oxide, lithium manganese composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.
[0021] In this specification, the term "lithium nickel cobalt manganese composite oxide" includes oxides containing Li, Ni, Co, Mn, and O as constituent elements, as well as oxides containing one or more additional elements other than those. Examples of such additional elements include transition metal elements and typical metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn. The additional element may be a semimetal element such as B, C, Si, or P, or a nonmetal element such as S, F, Cl, Br, or I. This also applies to the above-mentioned lithium nickel composite oxide, lithium cobalt composite oxide, lithium manganese composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.
[0022] Examples of the lithium transition metal phosphate compound include lithium iron phosphate (LiFePO 4 ), lithium manganese phosphate (LiMnPO 4 ), lithium manganese iron phosphate, etc.
[0023] These positive electrode active materials may be used alone or in combination of two or more. The positive electrode active material is preferably a lithium nickel cobalt manganese based composite oxide.
[0024] The average particle diameter (median diameter: D50) of the positive electrode active material is not particularly limited, but is, for example, 0.05 μm to 25 μm, preferably 1 μm to 20 μm, and more preferably 3 μm to 15 μm. The average particle diameter (D50) of the positive electrode active material can be determined, for example, by a laser diffraction scattering method.
[0025] The positive electrode active material layer 54 may contain components other than the positive electrode active material, such as trilithium phosphate, a conductive material, a binder, etc. As the conductive material, for example, carbon black such as acetylene black (AB) or other carbon materials (e.g., graphite, etc.) can be suitably used. As the binder, for example, polyvinylidene fluoride (PVDF) can be used.
[0026] The content of the positive electrode active material in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is preferably 70 mass% or more, more preferably 80 mass% to 97 mass% or less, and even more preferably 85 mass% to 96 mass% or less. The content of the trilithium phosphate in the positive electrode active material layer 54 is not particularly limited, but is preferably 1 mass% to 15 mass% or less, and more preferably 2 mass% to 12 mass% or less. The content of the conductive material in the positive electrode active material layer 54 is not particularly limited, but is preferably 1 mass% to 15 mass% or less, and more preferably 3 mass% to 13 mass% or less. The content of the binder in the positive electrode active material layer 54 is not particularly limited, but is preferably 1 mass% to 15 mass% or less, and more preferably 1.5 mass% to 10 mass% or less.
[0027] The thickness of the positive electrode active material layer 54 is not particularly limited, but is, for example, from 10 μm to 300 μm, and preferably from 20 μm to 200 μm.
[0028] The positive electrode 50 can be prepared by a known method. For example, a positive electrode paste containing a positive electrode active material and optional components is prepared, and the positive electrode paste is applied to the positive electrode current collector 52, dried, and pressed as necessary to prepare the positive electrode 50. In this specification, the term "paste" is used to include forms called "slurry" and "ink."
[0029] The negative electrode 60 used in the assembly preparation step S1 may be a known negative electrode used in a lithium ion secondary battery. The negative electrode 60 typically includes a negative electrode current collector 62 and a negative electrode active material layer 64 supported by the negative electrode current collector 62, for example, as shown in FIG. 3. The negative electrode active material layer 64 may be provided on one side or both sides of the negative electrode current collector 62, but is preferably provided on both sides. The negative electrode 60 typically includes a negative electrode active material layer non-formed portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) as shown in FIG. 3.
[0030] A known negative electrode current collector used in lithium ion secondary batteries may be used as the negative electrode current collector 62, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., copper, nickel, titanium, stainless steel, etc.). Copper foil is preferable as the negative electrode current collector 62.
[0031] The dimensions of the negative electrode current collector 62 are not particularly limited and may be appropriately determined depending on the battery design. When a copper foil is used as the negative electrode current collector 62, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.
[0032] The negative electrode active material layer 64 contains a negative electrode active material. As the negative electrode active material, for example, a carbon material such as graphite, hard carbon, soft carbon, etc. The graphite may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material.
[0033] The average particle diameter (median diameter: D50) of the negative electrode active material is not particularly limited, but is, for example, 0.1 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 5 μm to 20 μm. The average particle diameter (D50) of the negative electrode active material can be determined, for example, by a laser diffraction scattering method.
[0034] The negative electrode active material layer 64 may contain components other than the active material, such as a binder, a thickener, etc. As the binder, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), etc. may be used. As the thickener, for example, carboxymethyl cellulose (CMC), etc. may be used.
[0035] The content of the negative electrode active material in the negative electrode active material layer is preferably 90% by mass or more, more preferably 95% by mass or more and 99% by mass or less. The content of the binder in the negative electrode active material layer is preferably 0.1% by mass or more and 8% by mass or less, more preferably 0.5% by mass or more and 3% by mass or less. The content of the thickener in the negative electrode active material layer is preferably 0.3% by mass or more and 3% by mass or less, more preferably 0.5% by mass or more and 2% by mass or less.
[0036] The thickness of the negative electrode active material layer 64 is not particularly limited, but is, for example, not less than 10 μm and not more than 300 μm, and preferably not less than 20 μm and not more than 200 μm.
[0037] The negative electrode 60 can be prepared by making according to a known method. For example, the negative electrode 60 can be prepared by making a negative electrode paste containing a negative electrode active material and optional components, applying the negative electrode paste to a negative electrode current collector 62, drying, and pressing as necessary.
[0038] The positive electrode 50 and the negative electrode 60 are typically used as a wound electrode body 20 in which the positive electrode 50 and the negative electrode 60 are stacked with a separator 70 interposed therebetween.
[0039] The separator 70 may be a porous sheet (film) made of a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, or polyamide. Such a porous sheet may have a single-layer structure or a laminated structure of two or more layers (for example, a three-layer structure in which a PP layer is laminated on both sides of a PE layer). A heat-resistant layer (HRL) may be provided on the surface of the separator 70.
[0040] The thickness of the separator 70 is not particularly limited, but is, for example, from 5 μm to 50 μm, and preferably from 10 μm to 30 μm.
[0041] The wound electrode body 20 can be produced according to a known method. In this embodiment, the outermost surface of the wound electrode body 20 is the negative electrode 60. Specifically, first, the positive electrode 50 and the negative electrode 60 are stacked with the separator 70 interposed therebetween. At this time, as shown in FIG. 3, the positive electrode 50 is stacked with the negative electrode 60 so that the positive electrode active material layer non-forming portion 52a and the negative electrode 60 is stacked with the negative electrode active material layer non-forming portion 62a protruding in opposite directions from the widthwise ends of the two separators 70. In this embodiment, the negative electrode 60 is provided with a metallic lithium foil 10 in advance at a predetermined position of the portion that is the outermost periphery of the negative electrode 60 when the wound electrode body 20 is formed and that is not opposed to the positive electrode 50.
[0042] Next, the obtained laminate is wound. The winding of the laminate can be performed according to a known method. For example, the laminate can be wound on the outer peripheral surface of a winding core using a winding machine equipped with a known winding core. The winding conditions can be the same as known conditions.
[0043] Here, the number of windings of the wound electrode body 20 is not particularly limited as long as the effect of the technology disclosed herein is exhibited. On the other hand, the more the number of windings of the wound electrode body 20, the more likely it is that the uniform diffusion of Li ions into the inside of the negative electrode 60 becomes insufficient, and the Li precipitation resistance tends to decrease. That is, from this viewpoint, a wound electrode body with a large number of windings is suitable as a target to which the technology disclosed herein is applied. From this viewpoint, the number of windings of the wound electrode body 20 is preferably 4 times (in other words, 4 turns) or more, more preferably 10 times or more, even more preferably 20 times or more, even more preferably 25 times or more, and particularly preferably 30 times or more. The number of windings of the wound electrode body 20 may be, for example, 100 times or less, 70 times or less, or 50 times or less.
[0044] Next, in this embodiment, the wound laminate is pressed to produce a flat wound electrode body. As shown in FIG. 2, the wound electrode body 20 after the pressing process has a pair of curved portions (R portions) 20r and a flat portion 20f connecting the pair of curved portions 20r. The pressing process can be performed by pressing the laminate wound in the above-mentioned winding step using a known pressing device used in the manufacture of a general flat wound electrode body. The pressing conditions may be the same as known conditions. However, in other embodiments, the pressing process may not be performed, and the wound electrode body may be cylindrical or the like.
[0045] 2, a metallic lithium foil 10 is applied (attached) to at least a part of the region of the negative electrode 60 at the outermost periphery of the wound electrode body 20 that does not face the positive electrode. For example, an adhesive can be used to apply the metallic lithium foil 10. One example of such an adhesive is a resin adhesive composed of polypropylene (PP), polyethylene (PE), acrylic resin, or the like.
[0046] As the metal lithium foil 10, for example, commercially available ones can be used without any particular restrictions as long as the effect of the technology disclosed herein can be obtained. In the metal lithium foil 10, when the entire metal lithium foil is 100 mass%, the content of metal lithium is, for example, 97 mass% or more, preferably 98 mass% or more, 99 mass% or more, or 99.5 mass% or more (for example, 100 mass%). Here, components other than metal lithium may be, for example, unavoidably contained in small amounts due to raw materials, manufacturing processes, etc. In this embodiment, the shape of the metal lithium foil 10 is rectangular, but in other embodiments, it may be circular, elliptical, polygonal, or various other shapes. The size of the metal lithium foil 10 is preferably appropriately determined depending on the dimensions of the wound electrode body 20, etc. For example, the area where the metallic lithium foil 10 is applied (when the metallic lithium foil is applied in multiple places, the total area of the multiple places) may be an area equivalent to 1% to 20% or 5% to 15% of the area of the negative electrode 60 not facing the positive electrode, which is 100%. The thickness of the metallic lithium foil 10 can be within a range of, for example, 0.01 mm to 5 mm (or 0.05 mm to 1 mm). An example of the dimensions of the metallic lithium foil 10 is length: 10 mm to 30 mm, width: 10 mm to 30 mm, and thickness: 0.01 mm to 5 mm.
[0047] The portion to which the metal lithium foil 10 is applied is not particularly limited as long as it is a region of the negative electrode 60 that does not face the positive electrode. The metal lithium foil 10 may be disposed in the curved portion 20r of the wound electrode body 20, may be disposed in the flat portion 20f, or may be disposed in the curved portion 20r and the flat portion 20f. In addition, when the metal lithium foil 10 is disposed in the flat portion 20f of the wound electrode body 20 as in the present embodiment, the metal lithium foil 10 is more firmly fixed to the wound electrode body 20, which is preferable. In the present embodiment, the metal lithium foil 10 is disposed in only one place in the region of the negative electrode 60 that does not face the positive electrode, but is not limited thereto. In other embodiments, the metal lithium foil 10 may be disposed in a plurality of separate places in the region of the negative electrode 60 that does not face the positive electrode.
[0048] In addition, in this embodiment, in the wound electrode body 20, the ratio of the capacity of the negative electrode 60 to the capacity of the positive electrode 50 is 1.3 or more and less than 2.0. Here, if the weight of the negative electrode is increased to increase the positive / negative electrode capacity ratio, the energy density may decrease. Therefore, the positive / negative electrode capacity ratio is set to less than 2.0. Furthermore, if the positive / negative electrode capacity ratio is less than 1.3, Li deposition is likely to occur, and the capacity maintenance rate of the battery may decrease. Therefore, the positive / negative electrode capacity ratio is set to 1.3 or more. From the viewpoint of improving the Li deposition resistance, the positive / negative electrode capacity ratio is preferably 1.5 or more, more preferably 1.8 or more.
[0049] The "positive and negative electrode capacity ratio" can be calculated by separately calculating the capacity of the positive electrode and the capacity of the negative electrode, and using the following formula: capacity of the negative electrode ÷ capacity of the positive electrode. Here, the positive and negative electrode capacity ratio can be easily adjusted, for example, by changing the basis weight of the positive and negative electrodes or by changing the type of the positive and negative electrode active material. The "basis weight" refers to the value obtained by dividing the mass of the electrode active material layer by the area of the formation region (mass of the electrode active material layer / area of the formation region). The capacity of the positive electrode can be calculated as the capacity (i.e., the initial positive electrode charge capacity) when a half cell is prepared with Li metal as the counter electrode and initially charged in a voltage range corresponding to the full cell (for example, about 2 to 4.2 V). The capacity of the negative electrode can be calculated, for example, by adding up the initial negative electrode discharge capacity and the operating voltage range of the negative electrode.
[0050] Next, the battery case 30 is prepared. Specifically, as shown in FIG. 3, a body of the battery case 30 having an opening and a lid of the battery case 30 are prepared. The opening has a dimension that allows the wound electrode body 20 to be inserted. The lid has a dimension that closes the opening of the body of the battery case 30. The lid is provided with a thin-walled safety valve 36 that is set to release the internal pressure when the internal pressure of the battery case 30 rises to a predetermined level or higher, and an injection port (not shown) for injecting a non-aqueous electrolyte. The battery case 30 is made of a lightweight metal material with good thermal conductivity, such as aluminum.
[0051] In addition, a nonaqueous electrolyte 80 (here, a nonaqueous electrolyte) is prepared. The nonaqueous electrolyte may be the same as that of a conventional electrolyte, and is not particularly limited. The nonaqueous electrolyte typically contains a nonaqueous solvent and a supporting salt (electrolyte salt). As the nonaqueous solvent, various organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones that are used in electrolytes of general lithium ion secondary batteries can be used without any particular limitation. Specific examples include ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), and trifluorodimethyl carbonate (TFDMC). Such nonaqueous solvents can be used alone or in appropriate combination of two or more.
[0052] The supporting salt is, for example, LiPF 6 , LiBF 4 , lithium salts such as lithium bis(fluorosulfonyl)imide (LiFSI) (preferably LiPF 6 The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.
[0053] In addition, the nonaqueous electrolyte 80 may contain various additives other than the above-mentioned components, such as film-forming agents such as vinylene carbonate (VC) and oxalate complexes; gas generating agents such as biphenyl (BP) and cyclohexylbenzene (CHB); and thickeners, so long as the effects of the present invention are not significantly impaired.
[0054] Next, the positive terminal 42 and the positive current collector 42a, and the negative terminal 44 and the negative current collector 44a are attached to the lid of the battery case 30. The positive current collector 42a and the negative current collector 44a are welded by ultrasonic welding, resistance welding, or the like to the positive active material layer non-forming portion 52a and the negative active material layer non-forming portion 62a exposed at the ends of the wound electrode body 20, respectively. Then, the wound electrode body 20 is housed inside the battery case 30 body through its opening.
[0055] Next, a non-aqueous electrolyte is injected through the injection port of the lid of the battery case 30. After the non-aqueous electrolyte is injected, the injection port is sealed to obtain an assembly. The injection port can be sealed according to a known method. In this manner, an assembly can be obtained.
[0056] (Initial charging process: step S2) As described above, in this step, the assembly is initially charged. In the initial charging, it is preferable to charge the constructed assembly to a predetermined voltage value in a room temperature range. For example, an external power source is connected between the positive electrode (positive electrode terminal) and the negative electrode (negative electrode terminal) of the assembly, and charging (for example, constant current constant voltage charging) is performed to a predetermined voltage. Here, the room temperature range in the initial charging step refers to a temperature range that is, for example, room temperature, and can be 20°C ± 15°C. The temperature to which the assembly is exposed in the initial charging process can be selected from a temperature range of, for example, 5°C to 35°C, and is preferably 20°C to 30°C. In addition, the voltage between the positive and negative electrode terminals in the initial charging process (for example, the maximum voltage) may vary depending on the type of active material and non-aqueous solvent used, but it may be set to a voltage range that can be shown when the SOC of the assembly is in the range of approximately 80% or more (for example, 90 to 105%) of the fully charged state (for example, the rated capacity of the battery). The charge rate in the initial charging process may be the same as a conventionally known charge rate that can be generally adopted when initially charging a conventional assembly, for example, about 0.1 to 10 C. Such a charging process may be performed once, but may also be repeated two or more times, for example, with a discharging process between them.
[0057] (High temperature aging process: step S3) As described above, in this step, the assembly after the initial charge is aged for a predetermined time at a temperature of 60° C. or higher in a charged state where the potential of the negative electrode 60 is 0.5 V or higher. In this way, by aging (holding, placing) the assembly and the negative electrode 60 in a charged state where the potential of the negative electrode 60 is 0.5 V or higher in a high temperature range of 60° C. or higher, the Li ions eluted from the metallic lithium foil 10 can be suitably diffused to the inside of the negative electrode 60. This allows the capacity retention rate of the battery 100 to be suitably maintained. In the high-temperature aging step, from the viewpoint of more suitably obtaining the effects as described above, the potential of the negative electrode 60 is more preferably 1 V or higher, and may be 2 V or higher or 3 V or higher. The potential of the negative electrode 60 can be, for example, 5 V or lower, 4 V or lower. In the high-temperature aging step, from the viewpoint of more suitably obtaining the effects as described above, the temperature at which the aging is performed is more preferably 70° C. or higher. The temperature at which the aging is performed can be, for example, 90° C. or lower, 80° C. or lower. The time for such high-temperature aging treatment may be, for example, a total time from the start of temperature rise of 5 to 100 hours, preferably 10 to 50 hours. As a means for heating the above-mentioned assembly, for example, a thermostatic bath, an infrared heater, or the like may be appropriately used.
[0058] As described above, according to the method for producing a nonaqueous electrolyte secondary battery including the assembly preparation step (step S1), the initial charging step (step S2), and the high-temperature aging step (step S3), a nonaqueous electrolyte secondary battery can be obtained in which both lithium precipitation resistance and battery durability are suitably achieved. In addition, the nonaqueous electrolyte secondary battery obtained by the method for producing a nonaqueous electrolyte secondary battery according to the present embodiment has, for example, the following characteristics. Here, FIG. 5 is a cross-sectional view taken along line VV in FIG. 4, and is a schematic explanatory view for explaining a high lithium element accumulation region in a nonaqueous electrolyte secondary battery according to one embodiment. Note that in FIG. 5, the separator is omitted for ease of viewing.
[0059] That is, the nonaqueous electrolyte secondary battery 100 obtained by the manufacturing method of the nonaqueous electrolyte secondary battery according to this embodiment is a nonaqueous electrolyte secondary battery including a wound electrode body 20 in which a positive electrode 50 and a negative electrode 60 are stacked and wound with a separator 70 interposed therebetween, and a nonaqueous electrolyte 80. In addition, a high lithium element accumulation region 110 is present in at least a part of the outermost periphery of the negative electrode 60 and in the region not facing the positive electrode 50. The ratio of the capacity of the negative electrode 60 to the capacity of the positive electrode 50 is 1.3 or more and less than 2.0.
[0060] Here, the "highly integrated lithium element region" can be said to be a region showing a trace of the metallic lithium foil 10 after the Li ions are dissolved in the high-temperature aging process. The trace of the metallic lithium foil 10 may be a scrap of the metallic lithium foil 10, or the metallic lithium foil 10 may be scattered. Alternatively, the metallic lithium foil 10 itself may disappear, and the Li element may be present in a high concentration. In this specification, the "highly integrated lithium element region" refers to a region containing a high concentration of Li element present in the outermost negative electrode 60. In such a region, the ratio of Li atoms to all atoms may be 5 atomic % or more, or 10 atomic % or more. This ratio of Li atoms can be measured by a known method (for example, ICP emission spectroscopy, etc.).
[0061] In one embodiment, the ratio of the capacity of the negative electrode 60 to the capacity of the positive electrode 50 is 1.5 or more, and may be 1.8 or more.
[0062] In one embodiment, the number of windings of the wound electrode body 20 is, for example, 4 times (in other words, 4 turns) or more, and may be 10 times or more, 20 times or more, 25 times or more, or 30 times or more. The number of windings of the wound electrode body 20 may be 100 times or less, 70 times or less, or 50 times or less.
[0063] <Battery uses> Battery 100 can be used for various purposes, but can be suitably used, for example, as a power source (driving power source) for a motor mounted on a vehicle such as a passenger car or truck. The type of vehicle is not particularly limited, but examples include a plug-in hybrid electric vehicle (PHEV), a hybrid electric vehicle (HEV), and a battery electric vehicle (BEV). Battery 100 has reduced variation in battery reaction, and can therefore be suitably used to construct a battery pack.
[0064] Although one embodiment of the present disclosure has been described above, the above embodiment is merely an example. The present disclosure can be implemented in various other forms. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes to the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modified form, and it is also possible to add another modified form to the above-mentioned embodiment. In addition, if the technical feature is not described as essential, it is also possible to delete it as appropriate.
[0065] For example, in the above embodiment, the case where the lithium ion secondary battery is a flat rectangular type has been described, but the present invention is not limited to this. In other embodiments, the lithium ion secondary battery may be configured as a cylindrical lithium ion secondary battery, etc.
[0066] The nonaqueous electrolyte secondary battery disclosed herein can be constructed according to known methods as a nonaqueous electrolyte secondary battery other than a lithium ion secondary battery.
[0067] Test examples relating to the present invention will be described below, but it is not intended that the present invention be limited to those shown in these test examples.
[0068] <Preparation of Sample 1> LiNi as a positive electrode active material1 / 3 Co 1 / 3 Mn 1 / 3 O 2 A slurry for forming a positive electrode active material layer was prepared by mixing LNCM, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder with N-methylpyrrolidone (NMP) in a mass ratio of LNCM:AB:PVDF=90:5:5. This slurry was applied to both sides of a long aluminum foil with a basis weight of 10 mg / cm. 2 After coating and drying, the density of the positive electrode active material layer was 2.5 g / cm 3 The mixture was rolled and pressed until it reached a thickness of 100 mm to prepare a positive electrode.
[0069] A natural graphite-based carbon material was prepared as the negative electrode active material. This natural graphite-based carbon material (C), styrene butadiene rubber (SBR), and carboxymethyl cellulose (CMC) were mixed with ion-exchanged water in a mass ratio of C:SBR:CMC=97:2:1 to prepare a slurry for forming a negative electrode active material layer. This slurry was applied to both sides of a long copper foil with a basis weight of 9 mg / cm. 2 After coating and drying, the density of the negative electrode active material layer was 1.2 g / cm 3 The mixture was rolled and pressed until it reached a thickness of 100 mm to prepare a negative electrode.
[0070] Two separators (porous polyolefin sheets with a three-layer structure of PP / PE / PP) were prepared. The prepared positive and negative electrodes were stacked facing each other with the separator interposed therebetween, and wound to prepare a wound electrode body. Here, the number of windings of the wound electrode body was 30 turns. The outermost periphery of the wound electrode body was the negative electrode, and a rectangular metallic lithium foil was provided in a part of the area of the outermost negative electrode that did not face the positive electrode. The metallic lithium foil was provided at the position shown in FIG. 2. The dimensions of the metallic lithium foil were 15 mm long, 15 mm wide, and 5 mm thick, relative to the area (40 mm long, 48 mm wide) of the outermost negative electrode that did not face the positive electrode. Then, an electrode current collector was welded to the wound electrode body, and the wound electrode body was housed in a rectangular aluminum battery case, and a nonaqueous electrolyte was poured into it. The non-aqueous electrolyte was a mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of EC:EMC:DMC=3:4:3, and LiPF 6 was dissolved at a concentration of 1.1 mol / L. The battery case was then sealed to prepare an assembly.
[0071] Next, in a temperature environment of 25°C, the assembly was charged at a constant current of 0.1C to 4.15V using a commercially available charger, with the positive terminal as the anode and the negative terminal as the cathode, and then discharged at a constant current of 3V. This charge and discharge was performed twice as an initial charge. The capacity at the second discharge was measured and used as the initial capacity.
[0072] The obtained lithium ion secondary battery was discharged to 2 V, and then aged for 12 hours in a thermostatic chamber at 60° C. In this manner, a lithium ion secondary battery for evaluation according to Sample 1 was produced.
[0073] <Preparation of Samples 2 to 4> Lithium ion secondary batteries for evaluation according to Samples 2 to 4 were produced in the same manner as Sample 1, except that the positive and negative electrode capacity ratios were as shown in Table 1. Here, the positive and negative electrode capacity ratios were adjusted by changing the basis weight of the negative electrode.
[0074] <Preparation of Samples 5 to 8> Evaluation lithium-ion secondary batteries according to Samples 5 to 8 were fabricated in the same manner as Samples 1 to 4, except that a lithium metal foil was not provided to a part of the region not facing the positive electrode of the outermost negative electrode.
[0075] <Evaluation of Capacity Retention Rate after Li Deposition Cycle Test> Each of the fabricated evaluation lithium-ion secondary batteries was adjusted to SOC 50% in a temperature environment of 25°C. Thereafter, it was placed in a temperature environment of -10°C, and charge and discharge were repeated 200 cycles with a charge of 20C for 10 seconds and a discharge of 2C for 100 seconds per cycle for each evaluation lithium-ion secondary battery. Thereafter, it was placed in a temperature environment of 25°C, and the discharge capacity was measured in the same manner as the initial capacity. The capacity retention rate (%) was determined from the formula: (discharge capacity after charge and discharge cycles / initial capacity) × 100. The results are shown in the corresponding columns of Table 1. Here, when such a capacity retention rate is 65% or more, it is evaluated that the capacity retention rate after the Li deposition cycle test is excellent.
[0076] <Evaluation of Capacity Retention Rate after 60°C Storage Test> Each of the fabricated evaluation lithium-ion secondary batteries was adjusted to SOC 80% in a temperature environment of 25°C. Each of these evaluation lithium-ion secondary batteries was placed in a thermostat at 60°C and stored for 60 days. Thereafter, the discharge capacity after storage was measured in the same manner as the initial capacity. The capacity retention rate (%) was determined from the formula: (discharge capacity after high-temperature storage / initial capacity) × 100. The results are shown in Table 1. Here, when such a capacity retention rate is 95% or more, it is evaluated that the capacity retention rate after the 60°C storage test is excellent.
[0077]
Table 1
[0078] As shown in Table 1, the lithium ion secondary batteries for evaluation according to Samples 1 to 3 obtained by the manufacturing method for a non-aqueous electrolyte secondary battery disclosed herein were confirmed to have excellent capacity retention rates after Li precipitation cycles and capacity retention rates after a storage test at 60°C, compared with Sample 4, in which the positive and negative electrode capacity ratio is outside the range of 1.3 or more and less than 2.0, Samples 5 to 7, in which the positive and negative electrode capacity ratio is within the range of 1.3 or more and less than 2.0 but a metallic lithium foil was not applied to a part of the region of the outermost negative electrode that does not face the positive electrode, and Sample 8, in which the positive and negative electrode capacity ratio is outside the range of 1.3 or more and less than 2.0 and a metallic lithium foil was not applied to the region of the outermost negative electrode that does not face the positive electrode. That is, it can be seen that the batteries obtained by the manufacturing method for a non-aqueous electrolyte secondary battery disclosed herein have excellent lithium precipitation resistance and battery durability.
[0079] In addition, when comparing the evaluation lithium ion secondary batteries according to Samples 1 to 3, it was confirmed that when the positive and negative electrode capacity ratio was 1.5 or more (more preferably 1.8 or more), the capacity retention rate after Li deposition cycles was particularly excellent.
[0080] Although the embodiment of the present invention has been described above, the above embodiment is merely an example. The present invention can be implemented in various other forms. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in the relevant field. The technology described in the claims includes various modifications and changes of the above-exemplified embodiment. [Explanation of symbols]
[0081] 10 Lithium metal foil 20 Wound electrode body 30 Battery case 36 Safety valve 42 Positive terminal 42a Positive current collector 44 Negative terminal 44a Negative current collector plate 50 Positive electrode (positive electrode sheet) 52 Positive electrode current collector 52a Portion where positive electrode active material layer is not formed 54 Cathode active material layer 60 Negative electrode (negative electrode sheet) 62 Negative electrode current collector 62a Part where negative electrode active material layer is not formed 64 Negative electrode active material layer 70 Separator 100 Nonaqueous electrolyte secondary battery 110 High concentration of lithium element
Claims
1. a wound electrode body in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound; A non-aqueous electrolyte; A method for producing a non-aqueous electrolyte secondary battery comprising the following steps: an assembly preparation step of preparing an assembly in which the wound electrode body and the nonaqueous electrolyte are housed in a battery case, wherein in the wound electrode body, a ratio of a capacity of the negative electrode to a capacity of the positive electrode is 1.3 or more and less than 2.0, and a metallic lithium foil is present in at least a part of a region of the outermost periphery of the negative electrode that does not face the positive electrode; an initial charging step of charging the assembly; and a high-temperature aging step of subjecting the assembly after the initial charge to an aging treatment at a temperature of 60° C. or higher in a charged state in which the potential of the negative electrode is 0.5 V or higher; The method for producing a non-aqueous electrolyte secondary battery includes the steps of:
2. 2. The method for producing a nonaqueous electrolyte secondary battery according to claim 1, wherein a ratio of a capacity of said negative electrode to a capacity of said positive electrode is 1.5 or more.
3. 3. The method for producing a nonaqueous electrolyte secondary battery according to claim 1, wherein the wound electrode body is wound four or more times.
4. a wound electrode body in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween and wound; A non-aqueous electrolyte; A non-aqueous electrolyte secondary battery comprising: a high lithium element accumulation region is present in at least a part of the outermost periphery of the negative electrode and in a region not facing the positive electrode, a ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.3 or more and less than 2.
0.
5. 5. The nonaqueous electrolyte secondary battery according to claim 4, wherein a ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.5 or more.
6. 6. The nonaqueous electrolyte secondary battery according to claim 4, wherein the wound electrode body is wound four or more times.
Citation Information
Patent Citations
Nonaqueous secondary battery and its manufacture
JP1999288712A
Nonaqueous electrolyte secondary battery
JP2014165050A
Lithium ion battery
JP2016072226A
Secondary battery with nonaqueous electrolyte
JP1993144473A