Toilet roll manufacturing method

The method addresses the hardness and embossment issues in long rolled toilet products by using a three-roll winder with controlled speed variations and fixed positioning, ensuring softness and smoothness throughout the roll.

JP2024143635APending Publication Date: 2024-10-11DAIO PAPER CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023056410
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional long rolled toilet products feel excessively hard when held and exhibit poor sheet softness and smoothness due to embossment crushing near the roll core, particularly in short rolled products used daily.

Method used

A manufacturing method using a surface type winder with three take-up rolls, including a winding process with controlled speed variations and fixed positioning to maintain a set winding diameter, ensuring the embossment is not crushed and the roll feels soft and smooth.

Benefits of technology

The method produces toilet rolls that maintain softness and smoothness even in long products, preventing embossment collapse near the roll core and enhancing user experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143635000001_ABST
    Figure 2024143635000001_ABST
Patent Text Reader

Abstract

To provide a soft toilet roll manufacturing method which is long but seldom crashes embossment.SOLUTION: A toilet roll manufacturing method has a take-up step by a surface type winder that has a first take-up roll, a second take-up roll and a third take-up roll, and performs take-up while supporting an outer peripheral surface with these rolls. In the take-up step, there is provided a wound diameter maintenance period which fixes a position of the third take-up roll and performs take-up while maintaining the set wound diameter after an increased diameter period in which take-up is performed until a set wound diameter is reached while moving the third take-up roll and increasing a wound diameter by the first take-up roll, the second take-up roll and the third take-up roll so that a distance between the third take-up roll on the one hand and the first take-up roll and the second take-up roll on the other becomes long.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a toilet roll. [Background technology]

[0002] In recent years, so-called long toilet rolls have become popular among some consumers of toilet rolls. This is due to the advantages of easy portability after purchase, reduced frequency of purchase and replacement, and convenient storage space. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6726653 [Patent Document 2] Special Publication No. 2013-520379 Summary of the Invention [Problem to be solved by the invention]

[0004] In long-length rolled products, including this type of "conventional long-length rolled product," embossing is applied to ensure softness. Typically, long-length rolled products, including "conventional long-length rolled products," contain recycled paper pulp and are single-embossed.

[0005] However, in the case of conventional long rolled products, the roll tends to feel excessively hard when held in the hand, and consumers may have the impression that the wound sheet is also hard. Furthermore, in the case of this long-length roll product, the sheet is pulled strongly during winding, so the embossing is easily crushed, especially in the area close to the core of the roll, resulting in a poor softness and smoothness of the sheet and a loss of design quality due to the crushed embossing. There is room for improvement, particularly for consumers who use short-length roll products on a daily basis and desire softness.

[0006] Therefore, the main object of the present invention is to provide a new method for producing a long toilet roll product that can improve the above-mentioned disadvantages of long rolled products, makes the roll feel soft, and shows sufficient softness and / or smoothness in the sheet. [Means for solving the problem]

[0007] The method for producing a toilet roll that solves the above problems has the following features. A method for manufacturing a toilet roll, comprising a winding step using a surface-type winder which has a first winding roll, a second winding roll, and a third winding roll and winds the roll while supporting the outer peripheral surface of the roll, In this winding process, After a diameter increasing period in which the third winding roll is moved so that the distance between the third winding roll and the first and second winding rolls is increased, and the winding diameter is increased by the first winding roll, the second winding roll, and the third winding roll until the winding diameter reaches a set diameter, A winding diameter maintaining period is provided during which the position of the third winding roll is fixed and winding is performed while maintaining the set winding diameter. Effect of the Invention

[0008] According to the present invention, the above-mentioned disadvantages of long rolled products can be improved, and a new manufacturing method for long toilet roll products can be provided in which the roll is easily felt soft and the sheet is sufficiently soft and / or smooth. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a first diagram for explaining a method for manufacturing a toilet roll according to an embodiment. [Diagram 2] FIG. 2 is a second diagram for explaining the manufacturing method of the toilet roll according to the embodiment. [Diagram 3] FIG. 11 is a third diagram for explaining the manufacturing method of the toilet roll according to the embodiment. [Figure 4]FIG. 4 is a fourth diagram for explaining the manufacturing method of the toilet roll according to the embodiment. [Diagram 5] FIG. 6 is a diagram for explaining a speed change of a second winding roll in the embodiment. [Figure 6] 11A and 11B are diagrams for explaining a change in position of a third winding roll in the embodiment. [Figure 7] FIG. 13 is a diagram for explaining a change in position of a third winding roll in a conventional method. [Figure 8] FIG. 1 is a schematic explanatory diagram of a toilet roll. [Figure 9] FIG. 2 is a partial cross-sectional view of a double embossed product. [Figure 10] 1A and 1B are explanatory diagrams of the embossing shape and arrangement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Next, a method for producing a toilet roll according to an embodiment of the present invention will be described in detail below with reference to Figures 1 to 10. However, the present invention is not limited to the shapes shown in the drawings or to this embodiment.

[0011] As shown in FIG. 8, the toilet roll 1 according to this embodiment is a roll of a strip-shaped toilet paper 10 wound around a paper tube (also called a tube core) 20. The manufacturing method of this embodiment is particularly useful for manufacturing toilet rolls having unevenness due to embossing, 2 plies, a winding length of 60 m or more, more preferably 70 m or more, and up to about 80 m in maximum, a diameter L3 of the paper tube 20 of 30 to 45 mm, preferably 34 to 42 mm, and a roll diameter L2 of 110 to 125 mm, more preferably 110 to 120 mm. In such a long product, the roll is likely to feel soft, and the sheet can be a long toilet roll that shows sufficient softness and / or smoothness. The width L1 of the toilet roll is not limited, but is 100 to 130 mm, preferably 105 to 120 mm.

[0012] The manufacturing method of this toilet roll 1, as particularly shown in Figures 1 to 4, includes a winding step using a surface-type winder 60 which has a first winding roll 61, a second winding roll 62, and a third winding roll 63, and which winds up the roll 70 while supporting the outer circumferential surface of the roll.

[0013] One form of this winding process is a process of winding up a wide toilet paper roll, also called a log, with a width several times or more than the product width and the same diameter as the product diameter. In the manufacturing method of the toilet roll, before the winding process for forming the log, a ply-up process of stacking a plurality of sheets to form a plurality of plies, an embossing process of embossing the sheets to give unevenness, and a contact embossing process of applying a contact emboss to the ply-up sheets to laminate and integrate them, etc. are included in an appropriate order. In addition, after the winding process, there is a cutting process of cutting the wound log to the product width to form individual toilet rolls, a packaging process of packaging one or more toilet rolls, etc. In addition to the winding process, there is a paper tube manufacturing process of manufacturing a paper tube for winding the toilet paper. In the present invention, there are no limitations on the processes other than the winding process.

[0014] The first winding roll 61 of the surface-type winder 60 is also called a winder roll, the second winding roll 62 is also called a bed roll, and the third winding roll 63 is also called a nip roll.

[0015] In this surface-type winder 60, as shown in Fig. 1, first, the leading end of the sheet 10 is wound around the supplied paper tube 20 on the first winding roll 61. This is called picking up. One form of adhesion between the paper tube 20 and the leading end of the sheet 10 is performed by an appropriate pick-up glue such as starch glue, adhesive, water, etc.

[0016] 2, the roll to be wound 70 is moved to a winding position X where the roll is wound by the first winding roll 61, the second winding roll 62, and the third winding roll 63 while being sandwiched between the two rolls, the first winding roll 61 and the second winding roll 62. From the time of pick-up until the start of winding by the two rolls, the first winding roll 61 and the second winding roll 62, the sheet is wound around the cardboard tube by about half to several turns, although this is not limited thereto.

[0017] After being moved to the winding position X and winding by the first winding roll 61 and the second winding roll 62 for a predetermined period, as shown in Fig. 3, the third winding roll 63 moves toward and contacts the wound roll 70, and the three winding rolls 61, 62, and 63 support the outer circumferential surface of the wound roll 70 while winding it. At this time, as the winding diameter of the wound roll 70 increases, the third winding roll 63 moves away from the first winding roll 61 and the second winding roll 62. In this embodiment, the period during which the winding diameter of the wound roll 70 is increased by the three winding rolls 61, 62, and 63 is referred to as a diameter increasing period.

[0018] In this surface type winder 60, the first winding roll 61 and the second winding roll 62 have different rotation speeds. In the present invention, the speed of each roll means the circumferential speed. By slightly differentiating the rotation speed of the second winding roll 62 based on the rotation speed of the first winding roll 61, the sheet 10 is wound tightly or loosely around the cardboard tube 20. In this embodiment, the ratio of the speed of the second winding roll 62 to the speed of the first winding roll 61 is called the follow-up value. In addition, the specific speed of the first winding roll 61 is not necessarily limited. It can be the speed during production in the production of a known toilet roll having 1 to 4 plies, a winding length of 25 to 100 mm, and a winding diameter of 110 to 125 mm. In one embodiment, it is 100 to 800 m / min. In particular, in long products with a winding length of 60 m or more, the winding speed during production tends to be fast, and the recesses due to embossing tend to be easily crushed. From the viewpoint of the effects of the present invention, the speed of the first winding roll is more preferably 250 to 750 m / min, and particularly preferably 550 to 650 m / min. The speed of the first winding roll is constant while winding at least one roll.

[0019] FIG. 5 is a graph showing the change in speed of the second winding roll 62 in this embodiment. The manufacturing method of the toilet roll of this embodiment is preferably and characteristically provided with a first speed change period (period B in FIG. 5) in which the speed of the second winding roll 62 is increased stepwise until it reaches the reference value P, immediately after picking up the sheet 10 wound around the cardboard tube 20, during the above-mentioned diameter increasing period (period A in FIG. 5) in which the third winding roll 63 comes into contact with the wound roll 70 and increases the winding diameter while being supported by the three rolls of the first winding roll 61, the second winding roll 62, and the third winding roll 63. The speed of the second winding roll 62 is increased stepwise until it reaches the reference value P, as shown by the reference value P. In this embodiment, the speed of the second winding roll is increased by changing the speed in two stages. The picking up is performed at C in FIG. 5.

[0020] The reference value P in this embodiment, i.e., the follow-up value during the diameter increasing period A during which the roll diameter is increased while being supported by the three rolls, the first winding roll 61, the second winding roll 62, and the third winding roll 63, is not necessarily limited, but is 99.0 to 99.9%, more preferably 99.4 to 99.9%, when manufacturing the long product, particularly a two-ply double embossed product, in which the sheet is prone to stretching. At this reference value P, the sheet is wound with a slight difference between the feed of the roll side by the second winding roll 62 and the new winding of the sheet by the first winding roll.

[0021] The speed of the second winding roll 62 in the first speed change period B is lower than the speed before it is increased to the reference value P, that is, the reference value P. In other words, the speed difference between the first winding roll 61 and the second winding roll 62 is larger than the reference value P. Then, the speed of the second winding roll 62 increases stepwise after the second winding roll 62 comes into contact with the wound roll 70. In such a first speed change period B, the speed difference is the largest when the wound roll 70 comes into contact with the second winding roll 62 immediately after picking up, and as a result, the wound roll 70 is moved extremely quickly to the predetermined winding position X where winding is performed by the first winding roll 61, the second winding roll 62, and the third winding roll 63. Therefore, the sheet 10 is moved to the winding position X while the length of the sheet 10 to be wound around the cardboard tube 20 while being sandwiched between the first winding roll 61 and the second winding roll 62 is still short. Therefore, the sheet near the paper tube, i.e., the portion close to the edge of the roll core, is pulled or clamped, and the length of the sheet that is pulled becomes extremely short, and the unevenness caused by the embossing process in the portion close to the edge of the roll core is less likely to be crushed. On the other hand, since the speed of the second winding roll 62 is increased in stages up to the reference value P, the edge of the roll core does not become too loose, and winding can be performed at an appropriate reference value P. The number of stages for changing the speed of the second winding roll is not limited, but one to three stages are preferable, and two stages are particularly preferable.

[0022] The speed of the second winding roll 62 in the first speed-changing period B is not necessarily limited, but in terms of tensile strength, etc., the basis weight of one ply is set to 11.0 to 14.0 g / m 2When the sheet is laminated in two plies and an embossment is formed on the two-ply sheet to produce the long product, the speed change rate D1 of the second winding roll 62 immediately after picking up is preferably 4.8 to 5.5%. The speed change rate is the rate of change with respect to the reference value P (the speed change rates are shown as D1 and D2 in FIG. 5). That is, in the first speed change period B, the speed is increased from a speed 4.8 to 5.5% slower than the speed of the reference value P to the reference value P. This speed change rate D1 is more appropriate for a two-ply paper thickness of 130 to 210 μm and a sheet that is easily stretched, such as a double embossed product. The winding performed only by the first winding roll 61 and the second winding roll 62 in this first speed change period B is, although not limited to, 1.8 to 9.0% of the winding length.

[0023] Regarding the change in the speed of the second winding roll 62 in the first speed change period B, in particular, the speed is increased stepwise until the second winding roll 62 reaches the reference value P. In particular, it is desirable to provide at least a first increase period B1 in which the speed is increased rapidly immediately after pick-up, and a second increase period B2 in which the speed is increased gradually to the reference value P. By providing a first rising period B1 in which the speed is rapidly increased, the roll 70 is moved very quickly to a predetermined winding position X where the roll 70 is wound by the first winding roll 61, the second winding roll 62, and the third winding roll 63. Since the number of windings is small and the winding length is short, the impact on the sheet due to tension during winding and contact with the winding rollers is small. Furthermore, by providing a second rising period B2 in which the speed is gradually increased to a reference value P where the roll 70 is wound by the three rolls together with the third winding roll 63, the difference in the degree of tightness of the sheet when wound by the first winding roll 61 and the second winding roll 62 becomes small compared to the diameter increasing period A, and the winding property of the part of the sheet near the edge of the roll core is improved. For example, in toilet rolls, spiral wrinkles may occur at the edge of the roll core, but the occurrence of such spiral wrinkles is preferably prevented.

[0024] Although the specific time of the first speed change period B is not limited, in one embodiment of the production of a long product having the unevenness due to the above-mentioned embossing, a two-ply winding length of 60 m or more, and a roll diameter of 110 to 125 mm, it is desirable that the first speed change period B is more than 0% and 12% or less of the winding length. Theoretically, it is sufficient if the first speed change period is even a little, but more specifically, the lower limit is 3% or more of the winding length.

[0025] As described above, in the diameter increasing period A, the first winding roll 61, the second winding roll 62, and the third winding roll 63 come into contact with the wound roll 70 that has been moved to the winding position X, and the three winding rolls 61, 62, and 63 support the outer circumferential surface of the wound roll 70 while winding it. At this time, as the winding diameter of the wound roll 70 increases, the position of the third winding roll 63 moves away from the first winding roll 61 and the second winding roll 62. In one embodiment of the diameter increasing period A, the speed difference between the first winding roll 61 and the third winding roll 63 is the same, or the third winding roll is made slightly faster in consideration of the movement of the third winding roll. The third winding roll 63 supports the outer circumferential surface to suppress the occurrence of wrinkles, and also affects the speed of diameter increase and the formation of gaps between the sheets, i.e., the winding density. In particular, the speed of the second winding roll 62 is set as a follow-up value, and is set slightly slower than the first winding roll 61, so that the sheet is wound tightly, but this affects the softness and tightness of the roll in combination with the position of the third winding roll 63. The speed of the third winding roll is not limited, but is 100 to 100.2% of the speed of the first winding roll.

[0026] This manufacturing method is further characterized in that, after the diameter increasing period A, a winding diameter maintaining period Q is provided in which the position of the third winding roll 63 is fixed and winding is performed while maintaining the set winding diameter. Furthermore, during this winding diameter maintaining period Q, it is preferable to provide a second speed changing period G of the second winding roll 62 in which the speed of the second winding roll 62 is increased to a reference value P or higher and wound.

[0027] The winding diameter can be maintained by fixing the position of the third winding roll 63 after the diameter increasing period A. That is, since the outer circumferential surface of the wound roll 70 is supported by the first winding roll 61, the second winding roll 62, and the third winding roll 63, the winding diameter is determined by the distance between the first winding roll 61, the second winding roll 62, and the third winding roll 63. Since the positions of the first winding roll 61 and the second winding roll 62 are fixed in the surface-type winder 60 at the winding position X, if the movement of the third winding roll 63 is stopped and its position is fixed, the increase in the winding diameter of the wound roll 70 stops and the winding diameter is maintained.

[0028] FIG. 6 is a graph showing the change in position of the third winding roll with respect to the maintenance of the winding diameter. In FIG. 6, the vertical axis indicates the position of the third winding roll 63, and the horizontal axis indicates time. In the manufacturing method of this embodiment, as shown in FIG. 6, after the third winding roll 63 comes into contact with the wound roll 70 (Y indicates the contact position in FIG. 6), the position of the third winding roll 63 changes as the diameter of the wound roll 70 increases. In FIG. 6, A corresponds to the diameter increase period. Then, at a predetermined position K just before O, which is the winding end position, the position of the third winding roll 63 is fixed and winding is performed. The period between points K and O in the figure is the winding diameter maintenance period Q. For comparison, FIG. 7 is a graph showing the change in position of the third winding roll in a conventional manufacturing method. In the conventional method, the position of the third winding roll is changed to the winding end position O, and no period for maintaining the winding diameter is provided.

[0029] In addition, when the second speed change period G is provided, it is not necessary to make the entire winding diameter maintaining period Q the second speed change period G. The second speed change period G is not limited, but in the case of manufacturing the long product of the 2-ply sheet in which the embossment is formed, it is the period during which 8.0 to 12.0% of the set winding length is wound from the end of the set winding length. This specific period is more appropriate for the 2-ply paper thickness of 130 to 210 μm and for the sheet that is easily stretched such as the double embossed product. In the period other than the second speed change period G in the winding diameter maintaining period Q, the speed of the second winding roll may be the reference value P.

[0030] The winding diameter maintaining period Q is a period longer than the second speed change period G, and is not limited to a specific period, but in the case of manufacturing the long product with the embossment formed on the two-ply sheet, it is the period from 88% to 90% of the set winding length to the end of winding. During this period, the position of the third winding roll 63 can be fixed. This specific period is more appropriate for the two-ply paper thickness of 130 to 210 μm and for the sheet that is easily stretched, such as the double embossed product.

[0031] The speed change rate D2 of the second winding roll 62 during the second speed change period G is not limited, but is about 0.5 to 4.0%, and is preferably 1.0 to 3.5% when manufacturing the long product in which the embossment is formed on the two-ply sheet. In other words, the speed of the second winding roll 62 is made 1.0 to 3.5% faster than the follow-up value of the reference value P. This speed change rate D2 is more appropriate for a two-ply paper thickness of 130 to 210 μm and a sheet that is prone to stretching, such as a double embossed product.

[0032] During the winding diameter maintenance period Q, the wound roll 70 is wound so that the preceding roll portion is pushed into the sheet to be wound. The winding diameter maintenance period Q is performed at or near the outer circumferential surface of the toilet roll, since it is performed after the diameter increasing period A, i.e., after a predetermined winding diameter is reached. At this position, the outer circumferential length of the roll is long, so the sheet is easily stretched and the roll layer is easily deformed, and therefore such a winding diameter maintenance period Q can be set.

[0033] During the roll diameter maintenance period Q, the sheet is wound tightly while being taut, and the preceding roll presses in on the sheet, so the sheet is taut and tightly wound with a slight slack between the sheet being wound and the preceding roll around which it is wound. This is thought to mean that when the roll is held in the hand, although there is no slack in the winding, the layer of a certain thickness (depth) from the outer periphery or the inner layer feels soft, and the roll as a whole tends to feel soft.

[0034] In particular, when the second speed change period G is provided, the sheet is wound tightly while being taut and the preceding roll is pushing the sheet, so that the sheet is taut and tightly wound while there is a slight slack between the sheet being wound and the preceding roll around which it is wound. Therefore, when the roll is held in the hand, although there is no slack in the winding, the layer of a certain thickness (depth) from the outer circumferential surface or the inner layer feels softer, and it is thought that the roll as a whole tends to feel softer.

[0035] Here, the winding diameter maintaining period Q, the first speed change period B, and the second speed change period G in this manufacturing method affect the softness of the roll and the softness of the sheet. There is an effect at least on long products. This has been discovered by the present inventors. That is, long products have a longer winding length than normal products, and the layers of the sheet in the roll are denser. For this reason, it is possible to set the winding settings of the sheet in one layer differently from the other layers, and the different settings also affect the feeling of softness of the entire roll.

[0036] In particular, in this manufacturing method, although the degree of influence varies depending on the physical properties of the sheet, the quality of the winding of the layer at a predetermined thickness (depth) from the outer circumferential surface is different from that before during the winding diameter maintenance period Q and further during the second speed change period G, so that the roll as a whole tends to feel softer. Furthermore, during the first speed change period B, the crushing of the unevenness due to the embossing at the edge of the roll core and the occurrence of spiral wrinkles are prevented.

[0037] Such improvements in roll quality are observed during the winding diameter maintenance period Q, the first speed change period B, and the second speed change period G. In one form of the sheet, the basis weight of one ply is 11.0 to 14.0 g / m 2 The sheet is laminated in two plies, and the two-ply sheet is embossed. In particular, the thickness of the two-ply sheet is 130 to 210 μm, the roll length is 60 m or more, and the roll diameter is 110 to 120 mm.

[0038] This manufacturing method is also suitable for toilet paper rolls made from 100% pulp or close to pure pulp (less than 30% recycled paper pulp). This is because the paper is soft and has few stiff fibers, so the toilet paper surface is smooth and silky, with excellent surface properties. Toilet paper rolls are made up of multiple layers of rolled toilet paper, so it is thought that the surface properties have an effect on the toilet paper.

[0039] This manufacturing method is suitable for double embossed toilet paper toilet rolls. As shown in the schematic diagram of FIG. 9, double embossed (designated by symbol E2) has recesses formed on both sides, and there is no or little difference between the front and back of the laminated sheet. However, double embossed is not limited to a form in which the recesses on the front and back face each other as in the illustrated example. In addition, when both sides of the laminated sheet are recessed, the user touches the gently angled dome parts between the recesses with his / her fingertips, and moreover, touches the front and back with multiple fingers, so that the user feels that the dome parts are formed on the front and back, so that the fingertips feel soft, and the smooth surface is strongly felt through the fingertips due to the formation of the flexible pulp raw material and the formation of the gently angled dome parts. And the sheet is easy to stretch. This characteristic of double embossing is also a reason why it is suitable for this manufacturing method.

[0040] Here, the depth of the recesses formed by the embossing process according to the present invention is not limited. It can be as deep as the recesses formed by known embossing processes. It can also be adjusted as appropriate. Here, the embossing pattern of the embodiment is not necessarily limited. The embossing can be an appropriate embossing pattern such as micro embossing, dot embossing, design embossing, etc. However, in long products with a winding length of 60 m or more, the paper tends to have a low basis weight and thickness, so the recesses formed by the embossing process are easily crushed during production. Therefore, the manufacturing method according to the present invention is particularly effective for the depth of the recesses formed by the embossing process in long products.

[0041] In one form of toilet roll manufactured by this manufacturing method, in a long product with a winding length of 60 m or more and a winding diameter of 125 m or less, when the toilet roll is unwound, there is a small difference in appearance between the recesses at a position close to the outer circumferential surface of the roll that corresponds to 8 to 12% of the winding length from the winding end and the recesses at a position close to the edge of the roll core that corresponds to 8 to 12% of the winding length from the winding end. In other words, the recesses at a position close to the edge of the roll core are not crushed, or the crushing of the recesses is difficult to feel even when they are close to the edge of the roll core.

[0042] Here, the embossing pattern of the embodiment is not necessarily limited, and the embossing may be any suitable embossing pattern such as micro embossing, dot embossing, design embossing, or the like.

[0043] In addition, a suitable example of the embossed pattern is a pattern in which the area of ​​the recesses is 1.0 to 2.5 mm 2 and density is 5.0-50 pieces / cm 2 and the embossing depth is 0.100 to 0.500 mm. This improves the softness of the toilet paper, and also increases the softness of the paper in a rolled state like a toilet roll, making it easier for consumers to feel that it is soft when they hold it in their hands. In particular, as shown in Fig. 10, the recesses 31 (Fig. 10A) whose bottom surface is a square with diagonal L4 x diagonal L4 = 1.0-1.5 x 1.0-1.5 mm, or the recesses 32 whose four corners of the square are extended diagonally outward (Fig. 10B) are arranged in a diagonal lattice pattern with a center distance L5 of 4.5-5.5 mm and an arrangement angle of 45° with respect to the width direction, and have valley lines 33 extending from the four corners of the recesses between the recesses 31 (32). It is preferable that the valley lines 33 are arranged in a gradually gradual arch shape in cross section so that the four corners of the recesses 31 (32) are the deepest and the middle between the recesses is the shallowest. This embossed pattern distributes tension during winding by the valley lines at 45° in the width direction, making it easy to adjust the winding hardness, and the embossing is unlikely to become unclear even when wound into a long length. In addition, the toilet paper itself is excellent in terms of softness and excrement wiping properties.

[0044] The pulp fibers in the toilet roll toilet paper produced by this manufacturing method are not particularly limited, but are preferably 70 to 100% by mass of virgin pulp and 0 to 30% by mass of recycled paper pulp. When recycled paper pulp is blended, it can be produced more cheaply than one consisting of 100% by mass of virgin pulp. In addition, recycled paper pulp tends to have finer fibers than the pulp fibers before recycling in the process of recycling pulp from recycled paper, and due to the nature of such fibers, the fibers become dense without increasing the paper thickness, but the fibers become finer, making it difficult to achieve paper strength. If excessively blended, the texture such as flexibility and smoothness decreases. Therefore, in consideration of the characteristics of recycled paper pulp, its blending ratio may be determined to be in the range of 0 to 30% by mass. The type of recycled paper pulp is not necessarily limited, but recycled paper pulp made from milk carton recycled paper and high-quality recycled paper is particularly preferable. These materials contain a large amount of softwood kraft pulp (NBKP) or hardwood kraft pulp (LBKP) derived from the raw materials, making them easy to develop paper strength.

[0045] On the other hand, it is particularly preferable that the virgin pulp is 100%, and in particular, the virgin pulp is preferably softwood kraft pulp (NBKP) and hardwood kraft pulp (LBKP).The blend ratio of these NBKP:LBKP is preferably 20:80 to 50:50.

[0046] In the toilet roll toilet paper manufactured in the embodiment, 75 to 90% by mass of the fibers constituting the toilet roll are desirably pulp derived from hardwood. Hardwood-derived pulp has short fiber length and is easy to improve the texture of the paper surface. By making the hardwood-derived pulp 75% by mass or more, the smoothness is increased and the paper tends to be hard to feel when used. In addition, LBKP, LUKP, LOKP, etc. are known as hardwood-derived pulp, but bleached LBKP is preferable. In addition, the fiber other than hardwood-derived pulp is desirably pulp derived from softwood. In this case, bleached NBKP is preferable.

[0047] The "basis weight", "paper thickness", "roll diameter", and "paper tube diameter" in the embodiment can be measured as follows.

[0048] [Basic weight] The measurements were made as basis weight per sheet in accordance with JIS P 8124 (2011).

[0049] [Paper thickness] A 2-ply test piece cut to 10 cm x 10 cm was thoroughly conditioned under the conditions of JIS P 8111 (1998), and the thickness was measured under the same conditions using a dial thickness gauge (thickness measuring device) "PEACOCK G type" (manufactured by Ozaki Manufacturing Co., Ltd.). Specifically, after making sure that there is no dirt or dust between the plunger and the measurement table, the plunger is lowered onto the measurement table, the dial thickness gauge's scale is moved to set the zero point, the plunger is then raised and the test piece is placed on the measurement table, and the plunger is slowly lowered at a speed of 1 mm / sec or less to read the gauge at that time. During the measurement, care should be taken to ensure that the metal plunger terminal (a circular flat surface with a diameter of 10 mm) is perpendicular to the paper plane. The measured paper thickness is the average value obtained by performing 10 measurements.

[0050] [Roll diameter] The roll diameter was calculated by measuring the circumference of the roll at three points in the width direction using a diameter rule (Muratec KDS Co., Ltd.) and calculating the average value of the three points. The unit is mm and is expressed to one decimal place.

[0051] [Paper tube diameter] The diameter of the paper tube was calculated by measuring the circumference of the paper tube at three points in the width direction using a diameter rule (Muratec KDS Co., Ltd.) and calculating the average value of the three points. The unit is mm and is expressed to one decimal place.

[0052] [Test example] The conventional manufacturing method and the manufacturing method according to the embodiment of the present invention were used to produce a sheet having an embossed pattern shown in FIG. 10(B) and a basis weight of 12.3 g / m 2Toilet paper was produced by winding it up to a length of 60 m under the conditions of a paper thickness of 140 μm and double embossing, and a test was conducted to visually check for crushed embossing at a position close to the outer circumference of the roll, which corresponds to 8 to 12% of the roll length, and for crushed embossing at a position close to the core of the roll, which corresponds to 8 to 12% of the roll length from the winding end.

[0053] The evaluation was made on a 5-point scale as follows: "1" the embossing was crushed, "2" the embossing mark was visible but the embossing was crushed, "3" the embossing was not crushed, "4" the embossing mark was clear and the embossing was clearly visible, and "5" the embossing was clearly visible.

[0054] As a result of evaluation by 10 subjects, the toilet roll manufactured by the method according to the present invention was rated by all subjects as 4 to 5 both in positions close to the outer periphery and in positions close to the edge of the roll core, whereas the toilet roll manufactured by the conventional method was rated as 1 to 2 in positions close to the edge of the roll core. From these results, it can be seen that according to the manufacturing method of the present invention, even if the sheet is pulled strongly during winding as in the case of a long roll product, the embossing near the edge of the roll core is less likely to be crushed, and crushing of the embossing is improved. [Industrial Applicability]

[0055] The toilet roll of the present invention can be used not only for home use but also for commercial use (for example, in airport toilets used by an unspecified number of people, in hospitals, etc.). [Explanation of symbols]

[0056] 1...toilet roll, 10...toilet paper, 20...paper tube (tube core), L1...toilet roll roll diameter, L2...toilet roll tube core diameter, L3...toilet roll width, 31, 32...recess, E, E2...embossment, M...ridge. 60...surface type winder, 61...first winding roll, 62...second winding roll, 63...third winding roll, 70...wound roll, X...winding position, A...diameter increase period, B...first speed change period, P...reference value (speed of the second winding roll at the follow-up value), G...second speed change period, C...pickup position, Y...contact position of the third winding roll with the wound roll, O...winding end position, Q...winding diameter maintenance period, D1, D2...speed change rate.

Claims

1. A method for manufacturing a toilet roll, comprising a winding step using a surface-type winder which has a first winding roll, a second winding roll, and a third winding roll and winds the roll while supporting the outer peripheral surface of the roll, In this winding process, After a diameter increasing period in which the third winding roll is moved so that the distance between the third winding roll and the first and second winding rolls is increased, and the winding diameter is increased by the first winding roll, the second winding roll, and the third winding roll until the winding diameter reaches a set diameter, A winding diameter maintaining period is provided during which the position of the third winding roll is fixed and winding is performed while maintaining the set winding diameter. A method for producing a toilet roll comprising the steps of:

2. A follow-up value, which is a difference between the speed of the first winding roll and the speed of the second winding roll during the diameter increasing period, is set as a reference value, The method for manufacturing a toilet roll according to claim 1, wherein the speed of the second winding roll is increased to a reference value or higher during the period in which the winding diameter is maintained.

3. A follow-up value, which is a difference between the speed of the first winding roll and the speed of the second winding roll during the diameter increasing period, is set as a reference value, Immediately after picking up the sheet by winding it around the paper tube, a first speed change period for the second winding roll is provided in which the speed of the second winding roll is increased until the speed of the second winding roll reaches the reference value. A method for producing the toilet roll according to claim 1 or 2.

4. 4. The method for producing a toilet roll according to claim 3, wherein the first speed change period is a stepwise speed change period, and includes at least a first speed increase period immediately after picking up, in which the speed is rapidly increased, and a second speed increase period in which the speed is gradually increased to the reference value.

Citation Information

Patent Citations

  • Rewinding machine and winding method

    JP2013520379A

  • Sanitary tissue paper roll and its manufacturing method

    JP6726653B2