Method for manufacturing three-dimensional molding object
By using recycled materials of thermoplastic resin, elastomer, and talc in the 3D modeling process, the method addresses thermal deterioration issues, enabling the production of three-dimensional structures with maintained mechanical properties.
Patent Information
- Application Number
- JP2023056475
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
The material extrusion-based 3D modeling method using thermoplastic resin faces issues with thermal deterioration during reshaping, leading to a decrease in the mechanical properties of the modeled object.
A method involving the use of recycled materials comprising a thermoplastic resin, a thermoplastic elastomer, and a filler like talc, which are crushed, melted, and extruded to form a three-dimensional object, ensuring the tensile modulus of the injection molded product falls within 50
This approach allows for easy reshaping of three-dimensional structures while effectively suppressing deterioration of mechanical properties, achieving comparable or superior mechanical performance to objects made from virgin materials.
Smart Images

Figure 2024143687000003 
Figure 2024143687000004 
Figure 2024143687000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a three-dimensional object. [Background technology]
[0002] In recent years, a method of forming a three-dimensional object using a manufacturing device for three-dimensional modeling has been attracting attention. To form a three-dimensional object, three-dimensional coordinate data of the three-dimensional object (hereinafter referred to as "3D data") is required. Slicer software slices the 3D data into slices to generate multiple pieces of two-dimensional data. The manufacturing device for three-dimensional modeling sequentially stacks two-dimensional layers based on the multiple pieces of two-dimensional data. In this way, a three-dimensional object is formed (see, for example, Patent Document 1).
[0003] Methods for forming 3D objects include the material extrusion (MEX) method, photolithography, inkjet method, powder adhesion modeling method, powder sintering modeling method, etc. Among these methods, the material extrusion method is attracting particular attention because it allows for a wide range of material selection.
[0004] The material extrusion method is a method of creating three-dimensional objects by extruding thermoplastic resin molten by heat from a nozzle and layering it. As materials used in three-dimensional modeling by the material extrusion method, for example, three-dimensional modeling materials containing thermoplastic resins, thermoplastic elastomers, and fillers have been disclosed (for example, see Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2018-131497 A [Patent Document 2] International Publication No. 2021 / 060278 Summary of the Invention [Problem to be solved by the invention]
[0006] In 3D modeling methods using material extrusion, since thermoplastic resins are used, it is expected that the modeled object can be remodeled in the same way as injection molded products. However, with the material extrusion method, heat is applied again during re-molding, which is expected to result in a decrease in the quality of the molded product due to thermal degradation.
[0007] In view of the above circumstances, an object of the present disclosure is to provide a method for manufacturing a three-dimensional object, which can easily remodel a three-dimensional object while suppressing deterioration of mechanical properties. [Means for solving the problem]
[0008] Specific means for solving the problems include the following aspects.
[0009] <1> A material preparation process for preparing a material for three-dimensional modeling using a recycled material for a three-dimensional model, the recycled material including a thermoplastic resin, a thermoplastic elastomer, and a filler; A melting step of melting the three-dimensional modeling material; a modeling step of extruding the molten three-dimensional modeling material from a nozzle of a three-dimensional model manufacturing apparatus to form a three-dimensional object; A method for manufacturing a three-dimensional object comprising the steps of: <2> The three-dimensional modeling material has a tensile modulus X (MPa) of an injection-molded product obtained by melting the three-dimensional modeling material and injection-molding the material, which satisfies the following formula (I): <1> A method for producing a three-dimensional object according to the above item. Formula (I) 50 <X<4000 <3> The content of the recycled material in the three-dimensional modeling material is 95% by mass or more relative to the total mass of the three-dimensional modeling material. <1> or <2> A method for producing a three-dimensional object according to the above item. Effect of the Invention
[0010] According to the present disclosure, there is provided a method for producing a three-dimensional object, which is capable of easily reshaping a three-dimensional object while suppressing deterioration of mechanical properties. [Brief description of the drawings]
[0011] [Figure 1] 1 is an image of a three-dimensional object produced in Example 1 for evaluating three-dimensional formability. [Diagram 2] FIG. 2 is a schematic diagram showing the punched shapes of samples for evaluating the mechanical properties of the three-dimensional objects produced in Comparative Example 1 and Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following describes embodiments of the present disclosure. The embodiments and examples described below are intended to exemplify the method for producing a three-dimensional object according to the present disclosure, and are not intended to limit the method for producing a three-dimensional object according to the present disclosure.
[0013] In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In the numerical ranges described in stages in this disclosure, the upper limit value described in one numerical range may be replaced by the upper limit value of another numerical range described in stages, and the same applies to the lower limit value. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit of the numerical ranges may be replaced with values shown in the examples.
[0014] In the present disclosure, each component may contain multiple types of corresponding substances. When referring to the amount of each component in a composition in the present disclosure, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In addition, in the present disclosure, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.
[0015] The method for manufacturing a three-dimensional object according to the present disclosure includes a material preparation process for preparing a material for three-dimensional modeling using recycled materials for three-dimensional objects, which include a thermoplastic resin, a thermoplastic elastomer, and a filler; a melting process for melting the material for three-dimensional modeling; and a modeling process for extruding the molten material for three-dimensional modeling from a nozzle of a three-dimensional object manufacturing device to form a three-dimensional object.
[0016] When creating a 3D object using 3D modeling materials that contain thermoplastic resins, etc., it is possible to improve the strength by mixing glass fibers, etc., as a filler. However, when a 3D object created using 3D modeling materials is crushed into flakes and re-pelletized by extrusion (recycled material), the mechanical properties (tensile properties, bending properties) are significantly reduced compared to 3D objects created using virgin materials.
[0017] Therefore, the inventors of the present disclosure conducted repeated experiments and studies, and found that, for example, if a 3D model is made using talc as a filler, the mechanical properties of the 3D model can be equivalent to those of a 3D model made using a virgin material, even if the 3D model is remodeled using a recycled material obtained by crushing a used or defectively molded 3D model into flakes and repelletizing the 3D model. When a 3D model is crushed and repelletized by extrusion, glass fiber is easily broken, but talc is not easily broken. Therefore, if a 3D model uses talc as a filler, it is considered that the deterioration of mechanical properties can be effectively suppressed even if the recycled material obtained by crushing and extruding the talc is used as a 3D modeling material.
[0018] [Material preparation process] In the material preparing step, a material for three-dimensional modeling is prepared using recycled materials for three-dimensional models, which include a thermoplastic resin, a thermoplastic elastomer, and a filler.
[0019] <3D modeling materials> The method for producing a three-dimensional object according to the present disclosure uses, as a three-dimensional modeling material, a recycled material (sometimes referred to as "three-dimensional object recycled material" or simply "recycled material" in this specification) obtained by subjecting a three-dimensional object containing a thermoplastic resin, a thermoplastic elastomer, and a filler to recycling processes such as crushing, melting, and extrusion. Since a filler that does not contain glass fiber, preferably a three-dimensional object containing talc, is used as the raw material for the recycled material, destruction of the filler due to crushing, melting, extrusion, and the like during the recycling process is suppressed. Therefore, even if a three-dimensional object is remodeled using this three-dimensional object recycled material, deterioration of mechanical properties can be suppressed.
[0020] The content of recycled material in the 3D modeling material relative to the total mass of the material for 3D modeling (sometimes referred to as "recycled material content" in this specification) can be set according to the mechanical properties required for the 3D model to be remodeled. From the standpoints of improving the recycled material content and ease of manufacturing, the recycled material content is preferably 95 mass% or more, more preferably 99 mass% or more, and particularly from the standpoint of ease of manufacturing, 100 mass% is particularly preferred.
[0021] Hereinafter, as an example of a three-dimensional printing material, a case where the three-dimensional printing material is composed only of recycled materials for three-dimensional objects (that is, the recycled material content is 100% by mass) will be mainly described.
[0022] (thermoplastic resin) The three-dimensionally molded object recycled material in the present disclosure contains a thermoplastic resin. In this disclosure, the tensile modulus of a thermoplastic resin at 25° C. is 6.0×10 8 Pa or more. The thermoplastic resin is not particularly limited, and any known thermoplastic resin can be used. The thermoplastic resin may be used alone or in combination of two or more kinds. For example, thermoplastic resins include general-purpose plastics, engineering plastics, and super engineering plastics. Examples of general-purpose plastics include high-density polyethylene (HDPE), low-density polyethylene (LDPE), propylene-based polymers (propylene homopolymer (PP)), polyvinyl chloride (PVC), polyvinylidene chloride, polystyrene (PS), polyvinyl acetate (PVAc), polytetrafluoroethylene (PTFE), acrylonitrile butadiene styrene resin (ABS resin), styrene-acrylonitrile copolymer (AS resin), and acrylic resin (PMMA, etc.). Engineering plastics include polyamide (PA), polyacetal (POM), polycarbonate (PC), modified polyphenylene ether (m-PPE, modified PPE, PPO), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), syndiotactic polystyrene (SPS), and cyclic polyolefin (COP). Examples of super engineering plastics include polyphenylene sulfide (PPS), polytetrafluoroethylene (PTFE), polysulfone (PSF), polyethersulfone (PES), amorphous polyarylate (PAR), polyetheretherketone (PEEK), thermoplastic polyimide (PI), and polyamideimide (PAI). Among them, the thermoplastic resin preferably contains one or more selected from the group consisting of high density polyethylene (HDPE), propylene-based polymer, polyamide (PA), polybutylene terephthalate (PBT), syndiotactic polystyrene (SPS), polyphenylene sulfide (PPS) and polyacetal (POM), and more preferably contains a propylene-based polymer.
[0023] The thermoplastic resin may be a crystalline thermoplastic resin or an amorphous thermoplastic resin. For example, from the viewpoint of affinity with the thermoplastic elastomer and the viewpoint of suitably dispersing the filler in the thermoplastic resin, the thermoplastic resin preferably contains a crystalline thermoplastic resin, more preferably contains at least one selected from the group consisting of high density polyethylene (HDPE), propylene-based polymer, polyamide (PA), polybutylene terephthalate (PBT), syndiotactic polystyrene (SPS), polyphenylene sulfide (PPS) and polyacetal (POM), and further preferably contains a crystalline propylene-based polymer. The "crystalline" of a thermoplastic resin refers to having an endothermic peak in differential scanning calorimetry. On the other hand, the "amorphous" of a thermoplastic resin refers to no clear endothermic peak being observed in differential scanning calorimetry.
[0024] The propylene polymer is a polymer having at least propylene as a constituent unit. The propylene-based polymer may be a homopolymer of propylene or a copolymer of propylene and another monomer. When the propylene-based polymer is a copolymer, for example, a copolymer of propylene and an α-olefin having 2 to 20 carbon atoms (excluding propylene) can be mentioned. For example, the copolymer of propylene and an α-olefin having 2 to 20 carbon atoms can be propylene-ethylene copolymer, propylene-1-butene copolymer, propylene-ethylene-1-butene copolymer, propylene-4-methyl-1-pentene copolymer, mixtures thereof, etc.
[0025] When the propylene-based polymer is a copolymer, the propylene-based polymer may be any one of a random copolymer, an alternating copolymer, a block copolymer, and a graft copolymer.
[0026] When the propylene-based polymer is a copolymer, the ratio of the structural units derived from propylene in the propylene-based polymer may be appropriately designed according to the desired properties of the three-dimensional object. For example, the ratio of the structural units derived from propylene in the propylene-based polymer is preferably 50 mol% or more, more preferably 70 mol% to 99.5 mol%, and even more preferably 80 mol% to 98 mol%, relative to 100 mol% of all structural units in the propylene-based polymer.
[0027] The stereoregularity of the propylene polymer may be any of isotactic, syndiotactic and a mixture thereof.
[0028] The content of the propylene-based polymer is preferably 95.0% by mass or more, more preferably 98.0% by mass or more, and even more preferably 99.9% by mass or more, based on 100% by mass of the total amount of the thermoplastic resin.
[0029] The crystallization temperature (Tc) of the thermoplastic resin is preferably from 90°C to 140°C, and more preferably from 110°C to 130°C. The crystallization temperature of a thermoplastic resin is measured by a differential scanning calorimeter (DSC) at a temperature drop rate of 10° C. / min.
[0030] The crystallinity of the thermoplastic resin is preferably from 2% to 80%, and more preferably from 5% to 75%. The degree of crystallinity of a thermoplastic resin is calculated from the heat of fusion resulting from the melting of the main component in the heat flow curve obtained using a differential scanning calorimeter (DSC). The heat flow curve is obtained by holding the thermoplastic resin at -40°C for 5 minutes under a nitrogen atmosphere, and then raising the temperature at 10°C / min. Specifically, a differential scanning calorimeter (Perkin-Elmer, DSC-7) is used to obtain a heat flow curve by holding 5 mg of a sample at -40°C for 5 minutes under a nitrogen atmosphere, and then raising the temperature at 10°C / min. The heat of fusion is calculated from the heat of fusion resulting from the melting of the main component in the obtained heat flow curve using the following formula. Crystallinity = (ΔH / ΔH0)×100(%) In the formula, ΔH is the heat of fusion (J / g) calculated from the heat of fusion curve derived from the melting of the main component of the thermoplastic resin, and ΔH0 is the heat of fusion (J / g) of perfect crystallization of the main component. For example, when the main component is ethylene, ΔH0 is 293 J / g, and when the main component is propylene, ΔH0 is 210 J / g.
[0031] The melting point of the thermoplastic resin is preferably 90°C or higher, more preferably 110°C or higher and 200°C or lower, and even more preferably 110°C or higher and 180°C or lower.
[0032] The melting point can be measured in the same manner as in the measurement of the melting point of a thermoplastic elastomer described below.
[0033] From the viewpoint of suppressing deterioration of the mechanical properties of the remodeled 3D object, the content of the thermoplastic resin can be in the range of 0.1 mass % or more and less than 100 mass %, more preferably in the range of 10 mass % to 70 mass %, and even more preferably in the range of 20 mass % to 60 mass %, relative to the total mass of the 3D object recycled material.
[0034] (Thermoplastic elastomer) The three-dimensionally shaped recycled material in the present disclosure contains a thermoplastic elastomer. When the three-dimensional object recycling material contains a thermoplastic elastomer, deformation of the three-dimensional object being remodeled is effectively suppressed.
[0035] Thermoplastic elastomers have rubber-like elasticity. Rubber-like elasticity refers to the property that when a load is applied to a resin, the shape of the resin changes, and when the load is removed, the shape of the resin returns to its original shape. Specifically, a thermoplastic elastomer has a tensile modulus of elasticity of 6.0×10 at 25°C. 8 It refers to a thermoplastic resin having a modulus of elasticity of less than Pa. In this respect, a thermoplastic elastomer is distinguished from a thermoplastic resin.
[0036] The thermoplastic elastomer is preferably a copolymer containing structural units derived from an α-olefin and structural units derived from an olefin different from the α-olefin.
[0037] The α-olefin may generally contain one kind of α-olefin having 2 to 20 carbon atoms alone or two or more kinds of α-olefins in combination. Among them, the α-olefin is preferably an α-olefin having 3 or more carbon atoms, and more preferably an α-olefin having 3 to 8 carbon atoms.
[0038] Examples of the α-olefin include 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3,3-dimethyl-1-butene, 4-methyl-1-pentene, 1-octene, etc. One or more of the α-olefins are used. Among these, from the viewpoint of availability, 1-butene, 1-pentene, 1-hexene, and 4-methyl-1-pentene are preferred as the α-olefin.
[0039] The olefin other than the α-olefin is preferably an olefin having 2 to 4 carbon atoms, and examples of the olefin include ethylene, propylene, butene, etc. Among them, the olefin other than the α-olefin is more preferably an olefin having 2 to 3 carbon atoms.
[0040] Examples of copolymers that are thermoplastic elastomers include ethylene-α-olefin copolymers, propylene-α-olefin copolymers, and butene-α-olefin copolymers.
[0041] Examples of thermoplastic elastomers include ethylene-propylene copolymers (EPR), ethylene-1-butene copolymers (EBR), ethylene-1-pentene copolymers, ethylene-1-octene copolymers (EOR), propylene-1-butene copolymers (PBR), propylene-1-pentene copolymers, and propylene-1-octene copolymers (POR).
[0042] Among these, the thermoplastic elastomer is preferably a copolymer containing a constitutional unit derived from an α-olefin having 2 to 8 carbon atoms and a constitutional unit derived from an olefin having 2 to 3 carbon atoms. Propylene-based elastomers are preferred because they have excellent compatibility with thermoplastic resins (particularly propylene-based polymers) and further suppress deformation of the three-dimensional object to be remodeled.
[0043] Furthermore, the α-olefins may form random copolymers or block copolymers.
[0044] The melting point of the thermoplastic elastomer is preferably from 30°C to 120°C. When the melting point is between 30°C and 120°C, the thermoplastic elastomer acts as an adhesive between the modeling layers of a three-dimensional object modeled by the material extrusion method. This improves the adhesive strength between the modeling layers of a three-dimensional object modeled by the material extrusion method. In the material extrusion method, the modeling layers are made of recycled material from three-dimensional objects extruded from a nozzle.
[0045] The melting point is a value determined as the temperature Tm at the melting peak position appearing on an endothermic curve by differential scanning calorimetry (DSC). The melting point is determined from the endothermic curve obtained by placing a sample in an aluminum pan, heating it to 230°C at 100°C / min, holding it at 230°C for 5 minutes, lowering it to -70°C at -10°C / min, and then heating it again at 10°C / min.
[0046] The lower limit of the melt flow rate (MFR; 230° C., 2.16 kg load) of the thermoplastic elastomer is preferably 0.5 g / 10 min or more, more preferably 1 g / 10 min or more, further preferably 2 g / 10 min or more, and particularly preferably 5 g / 10 min. The upper limit of the melt flow rate (MFR; 230° C., 2.16 kg load) of the thermoplastic elastomer is preferably 70 g / 10 min or less, more preferably 35 g / 10 min or less, and further preferably 30 g / 10 min or less. When the upper and lower limits of the MFR of the thermoplastic elastomer are within the above ranges, deformation of the three-dimensional object to be remodeled can be more effectively suppressed.
[0047] The melt flow rate (MFR) is a value measured in accordance with ASTM D1238-65T under conditions of 230° C. and a load of 2.16 kg.
[0048] The thermoplastic elastomer is preferably a thermoplastic elastomer having a Shore A hardness of 50-99, or a thermoplastic elastomer having a Shore D hardness of 30-60. When the hardness of the thermoplastic elastomer is 50 or more in Shore A hardness or 30 or more in Shore D hardness, the thermoplastic elastomer is less likely to deform. In other words, the shape of the thermoplastic elastomer is more likely to be maintained. Therefore, when a three-dimensional object is formed using a three-dimensional object manufacturing device described later, the thermoplastic elastomer is more likely to enter the screw of the cylinder. As a result, the discharge efficiency of the molten three-dimensional object material is improved. This makes it easier to obtain a three-dimensional object with a smooth surface and excellent appearance. For the same reasons as above, the lower limit of the hardness is preferably a Shore A hardness of 55 or more or a Shore D hardness of 40 or more, and more preferably a Shore A hardness of 60 or more or a Shore D hardness of 50 or more. There is no particular restriction on the upper limit of the hardness, and it is preferably a Shore A hardness of 96 or less or a Shore D hardness of 60 or less. Among the above, for the same reasons as above, the lower limit of the hardness is more preferably a Shore D hardness of 40 or more, and even more preferably a Shore D hardness of 50 or more.
[0049] The Shore A hardness and Shore D hardness are values measured in accordance with the method described in ASTM D2240.
[0050] Specific examples of thermoplastic elastomers include the TAFMER (registered trademark) series manufactured by Mitsui Chemicals, Inc. (e.g., TAFMER DF605, TAFMER DF610, TAFMER DF640, TAFMER DF710, TAFMER DF740, TAFMER DF7350, TAFMER DF810, TAFMER DF840, TAFMER DF8200, TAFMER DF940, TAFMER DF9200, TAFMER DF110, TAFMER H-0530S ... Examples of such polyimide resins include TAFMER H-1030S, TAFMER H-5030S, TAFMER XM-7070, TAFMER XM-7080, TAFMER XM-7090, TAFMER BL2491M, TAFMER BL2481M, TAFMER BL3110M, TAFMER BL3450M, TAFMER MA8510, TAFMER MH7010, TAFMER MH7020, TAFMER MH5020, TAFMER PN-2070, and TAFMER PN-3560. Among the above, the Toughmer XM series, which is a propylene-based elastomer, is preferred because it has excellent compatibility with thermoplastic resins (particularly propylene-based polymers) and further suppresses deformation of the three-dimensional object to be remodeled. The Toughmer XM series has excellent compatibility with thermoplastic resins (especially propylene-based polymers) and can maintain the breaking stress α required for 3D objects. This improves the adhesive strength between the layers of 3D objects created by the material extrusion method.
[0051] The thermoplastic elastomer is preferably a propylene-based elastomer. The propylene-based elastomer is a thermoplastic elastomer having at least propylene as a constituent unit. The thermoplastic elastomer is preferably a propylene-based elastomer having a melting point of 80° C. to 120° C., a Shore D hardness of 40 to 60, and an MFR of 2 g / 10 min to 20 g / 10 min, so that the three-dimensional object has smaller stress distortion and is less prone to warping. An example of a propylene-based elastomer having a melting point of 80° C. to 120° C., a Shore D hardness of 40 to 60, and an MFR of 2 g / 10 min to 20 g / 10 min is Toughmer XM-7090.
[0052] The content of the thermoplastic elastomer is preferably in the range of more than 0.1 mass% and less than 100 mass%, more preferably in the range of 10 mass% or more and less than 100 mass%, even more preferably in the range of 10 mass% to 70 mass%, and particularly preferably in the range of 20 mass% to 50 mass%, relative to the total mass of the three-dimensional molded recycled material.
[0053] It is preferable that the three-dimensionally shaped recycled material satisfies the following (a1), (b1), and (c1). (a1) The content of thermoplastic elastomer is 10% by mass or more and less than 70% by mass of the total mass of the three-dimensional model recycled material. (b1) The content of filler is 10% by mass or more and less than 50% by mass of the total mass of the recycled 3D model. (c1) The total content of the thermoplastic elastomer and the filler is 20% by mass or more and less than 90% by mass of the total mass of the three-dimensional model recycled material.
[0054] It is more preferable that the three-dimensionally molded recycled material satisfies any one of the following (a2), (b2), and (c2). A three-dimensional object made using recycled materials for three-dimensional objects that satisfy any one of the following (a2), (b2), and (c2) has smaller stress distortion, is less likely to break, and is less likely to warp. (a2) The content of thermoplastic elastomer is 15% by mass or more and 25% by mass or less, and the content of filler is 35% by mass or more and 45% by mass or less, based on the total mass of the three-dimensional model recycled material. (b2) The content of thermoplastic elastomer is 25% by mass or more and 35% by mass or less, and the content of filler is 15% by mass or more and 45% by mass or less, based on the total mass of the three-dimensional model recycled material. (c2) The content of thermoplastic elastomer is 35% by mass or more and 45% by mass or less, and the content of filler is 15% by mass or more and 35% by mass or less, based on the total mass of the three-dimensional model recycled material.
[0055] Of the above (a2), (b2), and (c2), it is more preferable that the three-dimensionally molded recycled material satisfies any one of the following (a3) and (b3). A 3D object made from recycled materials that satisfy either one of the following (a3) and (b3) has even smaller stress distortion and can more faithfully materialize the 3D data. (a3) The content of thermoplastic elastomer is 25% by mass or more and 35% by mass or less, and the content of filler is 25% by mass or more and 35% by mass or less, based on the total mass of the three-dimensional model recycled material. (b3) The content of thermoplastic elastomer is 35% by mass or more and 45% by mass or less, and the content of filler is 15% by mass or more and 35% by mass or less, based on the total mass of the three-dimensional model recycled material.
[0056] (filling material) The three-dimensionally shaped recycled material in the present disclosure contains a filler other than glass fiber, and one preferred filler is talc. Talc is not easily destroyed by the crushing, melting, etc. that occurs when producing recycled materials from 3D objects. Therefore, when a 3D object is remodeled using recycled materials produced by recycling processes such as crushing and extrusion of a 3D object containing talc as a filler, the deterioration of mechanical properties is suppressed compared to the original 3D object that was the raw material for the recycled material.
[0057] Talc is also known as talc. Talc is hydrated magnesium silicate. Hydrated magnesium silicate is a type of layered clay mineral, and is composed of magnesium (Mg) and silicon (Si) combined with oxygen and hydroxyl groups. The chemical structure of talc is generally: [Mg3Si4O 10 (OH)2] or [3MgO 4SiO2 H2O].
[0058] The shape of the talc is not particularly limited, and is preferably, for example, scaly, elliptical, or the like.
[0059] The upper limit of the volume average particle diameter of the talc is preferably 30 μm or less, more preferably 10 μm or less.The lower limit of the volume average particle diameter of the talc is preferably 1 μm or more, more preferably 5 μm or more.
[0060] The volume average particle size of talc is defined as the particle size value at which the cumulative volume of each particle, measured while talc is dispersed in water using a particle size distribution measuring device such as a laser diffraction / scattering type particle size distribution measuring device, is 50% of the total volume when the volume of each particle is cumulatively calculated from the smallest particle size side based on the particle size of each particle.
[0061] The talc content in the three-dimensional object recycled material may be set depending on the mechanical properties required for the three-dimensional object to be remodeled; from the viewpoint of suppressing deterioration in the mechanical properties and deformation (particularly warping) of the three-dimensional object to be remodeled, the talc content is from 5% to 70% by mass, preferably more than 5% to 55% by mass, and more preferably more than 5% to 45% by mass, relative to the total mass of the three-dimensional object recycled material. If the talc content is 5% by mass or more and 70% by mass or less, the deterioration of the mechanical properties and deformation (particularly warpage) of the three-dimensional object to be remodeled are suppressed.
[0062] For example, the filler is not limited to talc, and may include inorganic fillers other than talc (excluding glass fiber), organic fillers, glittering powders, pigment powders, composite fillers thereof, etc. The fillers other than talc may be used alone or in combination of two or more kinds.
[0063] Examples of inorganic fillers other than talc include inorganic powders other than talc (hereinafter simply referred to as "inorganic powders"), glittering inorganic powders, composite inorganic powders, and inorganic fibers. Examples of inorganic powders include titanium oxide, black titanium oxide, konjou, ultramarine, red iron oxide, yellow iron oxide, black iron oxide, zinc oxide, aluminum oxide, silica, magnesium oxide, zirconium oxide, magnesium carbonate, calcium carbonate, chromium oxide, chromium hydroxide, carbon black, aluminum silicate, magnesium silicate, aluminum magnesium silicate, mica, synthetic mica iron, sericite, moss-hige (magnesium sulfate whiskers), kaolin, silicon carbide, barium sulfate, bentonite, smectite, and boron nitride. Examples of the shiny inorganic powder include bismuth oxychloride, titanium oxide-coated mica, iron oxide-coated mica, iron oxide-coated mica titanium, iron oxide-titanium oxide sintered body, and aluminum powder. Examples of the composite inorganic powder include fine particle titanium oxide-coated mica titanium, fine particle zinc oxide-coated mica titanium, barium sulfate-coated mica titanium, titanium oxide-containing silica, and zinc oxide-containing silica. Examples of inorganic fibers include carbon fibers, etc. Although glass fibers are sometimes used as a filler for three-dimensional objects, the method for producing a three-dimensional object according to the present disclosure does not include glass fibers as a filler.
[0064] The organic filler may include resin particles, pulp, and the like. Examples of the resin particles include carbon fiber, polyethylene, polypropylene, polystyrene, tetrafluoroethylene, silicone powder, and polyphenylene ether. Examples of pulp include cellulose and cellulose derivatives.
[0065] (Other Ingredients) The material for 3D modeling using the recycled 3D model material in the present disclosure may contain, in addition to the above-mentioned thermoplastic elastomer, thermoplastic resin, and filler, other components within a range that suppresses the deterioration of mechanical properties when remodeled. Examples of the additives include ultraviolet absorbers, stabilizers, antioxidants, plasticizers, colorants, tinting agents, flame retardants, antistatic agents, fluorescent brighteners, matting agents, and impact strength improvers. From the viewpoint of recycling, biomass-derived raw materials may also be included.
[0066] The other components described above may be contained in the three-dimensional object that is the raw material for the three-dimensional object recycled material, or may be added as part of the material for the three-dimensional object separately from the three-dimensional object recycled material.
[0067] In addition to the thermoplastic resin, thermoplastic elastomer, and talc contained in the 3D model, which is the raw material of the 3D model recycled material, one or more of virgin thermoplastic resin, thermoplastic elastomer, and talc (i.e., not recycled material) may be added as part of the 3D modeling material. In particular, since the resin components (thermoplastic resin, thermoplastic elastomer) contained in the recycled material tend to deteriorate due to heat during re-pelletization, it is preferable to add a virgin material as part of the 3D modeling material (for example, within 5% by mass of the total mass of the 3D modeling material). In addition, recycled materials different from three-dimensional object recycled materials, for example, recycled materials made from three-dimensional objects that contain thermoplastic resin but do not contain thermoplastic elastomers, and recycled materials that are not derived from three-dimensional objects, may be blended.
[0068] In addition, when using a material for 3D modeling that is a mixture of recycled 3D model materials and other materials, such as the above-mentioned virgin materials or other recycled materials, it is preferable that the content of each of the thermoplastic resins, thermoplastic elastomers, and talc mentioned above is within the respective ranges mentioned above relative to the total mass of the material for 3D modeling including other materials.
[0069] The method for producing a recycled material using a three-dimensional object containing a thermoplastic resin, a thermoplastic elastomer, and talc is not particularly limited, and a known method can be applied. For example, a method in which a three-dimensional object (used product, defective product, etc.) containing a thermoplastic resin, a thermoplastic elastomer, and talc is collected, crushed into flakes using a crusher, and then re-pelletized by extrusion can be used. Furthermore, the shape and size of the three-dimensional object recycled material are not particularly limited, and for example, any shape and size that can be used in a material extrusion type three-dimensional object manufacturing device can be adopted.
[0070] The material for three-dimensional modeling using the three-dimensional model recycled material according to the present disclosure preferably has a tensile modulus of elasticity X (MPa) that satisfies the following formula (I) when made into an injection molded product. Formula (I) 50 <X<4000
[0071] If the tensile modulus X of the injection molded product of the material for 3D modeling exceeds 50 MPa, additive manufacturing can be performed stably. On the other hand, if the tensile modulus X of the injection molded product of the material for 3D modeling is less than 4000 MPa, a 3D model that maintains the same modeling properties as when virgin material is used can be manufactured. From this viewpoint, 300≦X≦4000 is preferable, and 1000≦X≦2500 is more preferable. The tensile modulus X of the injection molded product can be adjusted by the composition of the recycled material of the three-dimensional model, or by other recycled or virgin materials that are added as part of the three-dimensional modeling material as needed.
[0072] The tensile modulus X of the injection molded product is measured in accordance with JIS K7161-2:2014. The test speed is 1 mm / min.
[0073] The injection molded product used to measure the tensile modulus X is a 1A type test piece specified in JIS K7161-2:2014 obtained by injection molding a 3D model recycled material. The total length of the injection molded product is 170 mm. The thickness of the injection molded product is 2.5 mm. The heating temperature for injection molding is 200° C. The injection pressure (holding pressure) for injection molding is 45 MPa. The injection molded product may be a machined product obtained by injection molding a material for three-dimensional modeling using recycled materials and then machining the injection molded product.
[0074] [Melting process] In the melting process, the material for three-dimensional modeling using the above-mentioned three-dimensional model recycled material is melted.
[0075] The heating means for melting the three-dimensionally shaped recycled material is not particularly limited, and any known heating means can be used.
[0076] In the melting step, it is preferable to use a three-dimensional object manufacturing device equipped with a heating means such as an electric heater.
[0077] The temperature at which the three-dimensionally shaped recycled material is melted is not particularly limited and may be set appropriately depending on the properties of the thermoplastic resin. The temperature at which the three-dimensionally shaped recycled material is melted may be, for example, a temperature of +10°C to +150°C based on the higher of the melting point or the glass transition temperature (Tg) of the thermoplastic resin.
[0078] In the melting step, for example, the material for three-dimensional printing may be melted and kneaded. By melting and kneading the material for three-dimensional printing, the material for three-dimensional printing tends to be mixed more uniformly. Therefore, the occurrence of unevenness in the material of the obtained three-dimensional object is easily suppressed. As a result, the variation and deformation of the mechanical properties of the remodeled three-dimensional object tends to be suppressed.
[0079] [Modeling process] In the modeling process, molten material for 3D modeling is extruded from the nozzle of a 3D object manufacturing device to create a 3D object.
[0080] For example, a 3D object can be created by extruding molten 3D modeling material from the nozzle of a 3D object manufacturing device and stacking 2D layers on a substrate in sequence based on multiple 2D data. The multiple 2D data are generated by slicer software, which slices the 3D coordinate data of the 3D object to be created.
[0081] The three-dimensional object manufacturing device may be a material extrusion type three-dimensional object manufacturing device. There are no particular limitations on the material extrusion type three-dimensional object manufacturing device, and any known device or known device configuration may be used.
[0082] The three-dimensional object manufacturing device may be, for example, a device including a cylinder, a nozzle, and a heating means. The three-dimensional modeling material is supplied to the cylinder. The nozzle is provided at a location downstream of the cylinder in the discharge direction of the three-dimensional modeling material. The nozzle discharges the three-dimensional modeling material. The heating means is provided on the cylinder. The heating means heats and melts the three-dimensional modeling material. The 3D modeling device extrudes heated and melted 3D modeling material from a nozzle, and layer-by-layer models the 3D modeling material extruded from the nozzle, thereby creating a 3D model.
[0083] The cylinder may have a screw therein. The screw kneads the three-dimensional modeling material. The three-dimensional object manufacturing apparatus may further include a table device that is disposed opposite the nozzle. The molten three-dimensional object material extruded from the nozzle is stacked on the table device. The three-dimensional object manufacturing apparatus may further include a control means for controlling the spatial coordinates of the substrate and the nozzle, and the amount of the three-dimensional object material extruded from the nozzle. It is preferable that the control means controls the discharge of the molten three-dimensional object material extruded from the nozzle, and controls the movement of the nozzle and / or the table device in the X-axis, Y-axis, and Z-axis directions relative to a reference plane.
[0084] There are no particular limitations on the three-dimensional object to be remodeled using the recycled three-dimensional object material, and the three-dimensional object may have a different shape or purpose from the original three-dimensional object that is the raw material of the recycled material.
[0085] [Other processes] The method for manufacturing a three-dimensional object according to the present disclosure may further include, for example, a processing step in which the three-dimensional object manufactured in the modeling step is processed.
[0086] As described above, according to the method for producing a three-dimensional object disclosed herein, a three-dimensional object containing a thermoplastic resin, a thermoplastic elastomer, and talc is crushed and re-pelletized by extrusion to obtain a three-dimensional object recycled material, which can be used as a material for three-dimensional modeling to easily re-produce a three-dimensional object with reduced deterioration in mechanical properties.
[0087] When reproducing a 3D object with the same shape as the original 3D object (recycled original product) used as the raw material for the recycled material, it is possible to produce a 3D object with the same mechanical properties (for example, strength reduction of 10% or less) and appearance as the original recycled product by using the same 3D object production equipment and conditions as the original recycled product. Furthermore, the original three-dimensional object that is the raw material of the recycled material is not limited to one made from virgin material, but may be a three-dimensional object made from recycled material. According to the method of manufacturing a three-dimensional object of the present disclosure, a three-dimensional object can be manufactured with a high recycled material content, which reduces manufacturing costs and contributes greatly to the reuse of resources. EXAMPLES
[0088] Hereinafter, the present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to the following examples as long as it does not deviate from the gist of the disclosure. In addition, unless otherwise specified, "parts" are based on mass.
[0089] [Comparative Example 1] <Preparing materials for 3D modeling> The following materials were mixed, melted, and extruded to prepare virgin pellets (size: φ2.5 × 3 mm) for use in 3D modeling.
[0090] (Thermoplastic elastomer) 43% by mass XM7090: Toughmer XM-7090 (Mitsui Chemicals, Inc.)
[0091] (Thermoplastic resin) 17% by mass J105G: Prime Polypro J-105G (propylene homopolymer, Prime Polymer Co., Ltd.)
[0092] (Filler) 40% by weight Talc (volume average particle size 5μm~10μm)
[0093] <Manufacturing of 3D objects> Using the above virgin pellets, a three-dimensional object V1 (height H: 4 mm, width W: 200 × 240 mm) having a shape with straight sections, curved sections, and bent sections was manufactured using a material extrusion type three-dimensional object manufacturing device (GEM444, manufactured by Eslab). - Build speed: 600mm / min Nozzle temperature: 200℃ Layer pitch: 1.5mm
[0094] [Example 1] <3D modeling materials> As a recycled material for three-dimensional modeling, the five three-dimensional models produced in Comparative Example 1 were crushed, melted, and extruded again to produce recycled pellets (size: φ2.5×3 mm).
[0095] <Manufacturing of 3D objects> A three-dimensional model R1 was produced in the same manner as in Comparative Example 1, except that the recycled pellets were used as the three-dimensional modeling material.
[0096] [evaluation] (3D formability) To evaluate the three-dimensional formability, the appearances of the three-dimensional object V1 and the three-dimensional object R1 were each visually evaluated. Fig. 1 is an image showing the appearance of the three-dimensional object R1 produced in Example 1. The appearance of the three-dimensional object R1 was equivalent to that of the three-dimensional object V1, and no superiority or inferiority in appearance was observed.
[0097] (Mechanical properties of 3D objects) Using a material extrusion type 3D modeling manufacturing device (GEM444, manufactured by Eslab), 3D modeling material (virgin pellets or recycled pellets) was placed into the hopper and supplied into the cylinder. Next, the material for 3D modeling was heated to a temperature of 180° C. to 240° C. by a heater provided on the cylinder, and melted (melting process).
[0098] Next, the 3D data model below was sliced to generate multiple 2D data. Based on the multiple 2D data, the setting parameters were set as shown below, and a measurement object before machining was created using the material extrusion method (MEX) (modeling process). <3D data> · 205mm x 205mm x 100mm high rectangular column Thickness: 2.0mm in tension, 4.0mm in bending <Setting parameters> -Modeling speed: Tensile 1500mm / min, bending 750mm / min Nozzle temperature: 240℃ Layer pitch: Tensile 1.0mm, Bending 2.0mm
[0099] As shown in Figure 2, a sample perpendicular to the lamination direction (Figure 2(A)) and a sample parallel to the lamination direction (Figure 2(B)) were punched out from the flat sidewall portion 10 of the obtained 3D model in the shape of a 1BA test piece (white areas S1 and S2). Using each sample, the tensile modulus of elasticity and tensile stress at break were measured in accordance with JIS K7161-2:2014, and the flexural modulus of elasticity and flexural strength were measured in accordance with JIS K7171:2016. The measurement results are shown in Table 1.
[0100] [Table 1]
[0101] As seen in Table 1, even though the 3D model of Example 1 was produced using recycled pellets that were made by crushing, extruding, and re-pelletizing the 3D model of Comparative Example 1, which was produced using virgin pellets, the tensile properties and bending properties were 95% or more compared to 100% of the 3D model of Comparative Example 1, and mechanical properties at the same or higher levels were obtained. In particular, the tensile modulus exceeded 110% in both the directions perpendicular and parallel to the lamination direction.
[0102] (Mechanical properties of injection molded products) Using the virgin pellets used in Comparative Example 1 or the recycled pellets used in Example 1, injection molding was performed under the following conditions to produce injection molded products (size: tensile JIS K7161-2: 1A type defined in 2014, bending JIS K7161). <Setting parameters> ·Heating temperature: 200℃ Injection pressure (holding pressure): 45MPa
[0103] The tensile modulus and tensile breaking stress of each of the injection molded articles produced were measured in accordance with JIS K7161-2: 2014, and the flexural modulus was measured in accordance with JIS K7171: 2016. The results are shown in Table 2.
[0104] [Table 2]
[0105] As seen in Table 2, the injection molded products using recycled pellets had the same levels of tensile modulus, tensile stress at break, and flexural modulus as the injection molded products using virgin pellets. These results also show that molding using recycled material obtained from three-dimensional objects containing thermoplastic resin, thermoplastic elastomer, and talc can effectively suppress deterioration of mechanical properties compared to virgin materials, and can be suitably used for manufacturing three-dimensional objects. [Explanation of symbols]
[0106] 10 Part of a 3D model (for measuring mechanical properties) S1 Punched shape of sample perpendicular to stacking direction S2 Punched shape of sample parallel to stacking direction
Claims
1. A material preparation process for preparing a material for three-dimensional modeling using a recycled material for a three-dimensional model, the recycled material including a thermoplastic resin, a thermoplastic elastomer, and a filler; A melting step of melting the three-dimensional modeling material; a modeling step of extruding the molten three-dimensional modeling material from a nozzle of a three-dimensional object manufacturing apparatus to form a three-dimensional object; A method for manufacturing a three-dimensional object comprising the steps of:
2. 2. The method for producing a three-dimensional object according to claim 1, wherein the three-dimensional modeling material is injection molded at a heating temperature of 200° C. and an injection pressure of 45 MPa, and the tensile modulus X (MPa) of the injection molded product satisfies the following formula (I): Formula (I) 50<X<4000
3. The method for manufacturing a three-dimensional object according to claim 1 or 2, wherein a content of the recycled material in the material for three-dimensional printing is 95 mass % or more with respect to a total mass of the material for three-dimensional printing.
Citation Information
Patent Citations
Three-dimensional (3D) printer capable of recycling printing base material
CN203449610U
Waterproof sheet
JP1993222214A
Expanded sheet of recovered thermoplastic polyester resin, its molded object and method for manufacturing this molded object
JP2005313557A
Resin molding material for three-dimensional molding devices and filament for three-dimensional molding devices
JP2018131497A
Fused deposition modeling-based resin composition for three-dimensional molding, and filament molding containing the same, and molded body
JP2020029089A