Active material and manufacturing method thereof, and electrode mixture, electrode, and battery including the same
A coated active material with specific lithium, phosphorus, and oxygen ratios addresses the issue of storage characteristic changes in solid-state batteries, particularly at high temperatures, by reducing resistance through controlled oxygen and electron transfer.
Patent Information
- Application Number
- JP2023056486
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Solid-state batteries are susceptible to changes in storage characteristics due to environmental conditions, particularly at high temperatures, leading to increased resistance.
An active material with a core particle coated by a compound containing lithium, phosphorus, and oxygen elements, with specific molar ratios, is developed to improve storage characteristics by suppressing oxygen extraction and electron transfer between the solid electrolyte and the active material.
The coated active material effectively reduces resistance increases in solid-state batteries under high-temperature storage conditions, enhancing their storage characteristics.
Smart Images

Figure 2024143696000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an active material and a method for producing the same, and also to an electrode mixture, an electrode, and a battery each containing the active material. [Background technology]
[0002] In recent years, secondary batteries have been attracting attention as an effort to prevent global warming by reducing CO2 emissions. Among them, solid-state batteries are expected to be put to practical use as batteries that combine safety and high energy density. Various techniques are known for forming a coating layer on the surface of an active material in order to improve various performances of solid-state batteries. For example, Patent Document 1 describes coating the surface of an active material with lithium metaphosphate. In this document, the active material is mixed with an aqueous solution of lithium metaphosphate, and then the active material is dried at 400°C to form a coating layer on the surface of the active material.
[0003] Patent Document 2 proposes coating the surface of the active material with lithium niobate, which prevents a resistive layer from being formed between the active material and the solid electrolyte, thereby preventing an increase in the interface resistance and allowing lithium ions to move more smoothly. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2017 / 094416 Brochure [Patent Document 2] International Publication No. 2020 / 175506 Brochure Summary of the Invention [Problem to be solved by the invention]
[0005] A problem with solid-state batteries is that their storage characteristics are easily affected by the storage environment, which is particularly noticeable when the storage environment is high temperature, and which can easily lead to an increase in the resistance of the solid-state battery. Therefore, an object of the present invention is to provide an active material capable of improving the storage characteristics of a solid-state battery, the storage characteristics of which are easily affected by the storage environment. [Means for solving the problem]
[0006] The present invention provides an active material having a core particle and a coating portion disposed on a surface of the core particle, The coating portion includes a compound containing lithium (Li), phosphorus (P), and oxygen (O), The compound has a molar ratio of lithium (Li) element to phosphorus (P) element of 0.5 or more and 2.5 or less, and a molar ratio of oxygen (O) element to phosphorus (P) element of 2.5 or more and 3.5 or less, In the infrared absorption spectrum obtained by Fourier transform infrared spectroscopy (FT-IR), -1 The above-mentioned problems have been solved by providing an active material having a peak in the range of
[0007] The present invention also provides a method for producing an active material, which comprises dry-mixing a mixture containing core particles and a compound containing lithium (Li), phosphorus (P) and oxygen (O) elements while cooling, and disposing a coating portion containing the compound on the surface of the core particles. Effect of the Invention
[0008] According to the present invention, there are provided an active material capable of improving the storage characteristics of a solid-state battery, the storage characteristics of which are easily affected by the storage environment, and a method for producing the same. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a graph showing infrared absorption spectra of the active materials of Examples 1 and 2 and Comparative Example 1, obtained by Fourier transform infrared spectroscopy. [Diagram 2] FIG. 2 is a graph of the P2p spectra obtained by X-ray photoelectron spectroscopy of the active materials of Examples 1 and 2 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will now be described based on its preferred embodiments. The present invention relates to an active material for a battery, for example, an active material for a lithium ion battery, and a manufacturing method thereof. The active material of the present invention has a core particle and a coating portion disposed on the surface of the core particle. The core particle is a portion that occupies the majority of the active material and is composed of an active material base material. The coating portion contains a compound containing phosphorus (P) element (hereinafter referred to as a "phosphorus-containing compound") as described later. The phosphorus-containing compound will be described in detail later. By disposing a coating portion made of a specific compound on the surface of the core particle, the storage characteristics of a solid-state battery, which is a battery whose storage characteristics are easily affected by the storage environment, can be improved. The increase in resistance of the solid-state battery, which is particularly noticeable when the storage environment is high temperature, can be suppressed. The reason why such an effect is obtained is that the coating portion disposed on the surface of the core particle can suppress the extraction of oxygen from the active material to the solid electrolyte and the extraction of electrons from the solid electrolyte to the active material.
[0011] [Phosphorus-containing compound] In the active material of the present invention, the coating portion contains a compound containing lithium (Li), phosphorus (P) and oxygen (O), i.e., a phosphorus-containing compound. It is preferable that the coating portion of the present invention contains a phosphorus-containing compound from the viewpoint of improving the storage characteristics of a solid-state battery, which is a battery whose storage characteristics are easily affected by the storage environment. In addition, since the phosphorus (P) element and the oxygen (O) element have a covalent bond and a high bonding strength, it is difficult for oxygen to be extracted from the coating portion to the solid electrolyte, which is also preferable from the viewpoint of suppressing oxidation of the solid electrolyte.
[0012] The phosphorus-containing compound preferably has a molar ratio of lithium (Li) element to phosphorus (P) element of, for example, 0.5 or more, more preferably 0.8 or more, and even more preferably 0.9 or more. Furthermore, the molar ratio of lithium (Li) element to phosphorus (P) element is, for example, preferably 2.5 or less, more preferably 1.5 or less, even more preferably 1.2 or less, and even more preferably 1.1 or less. When the molar ratio of lithium (Li) to phosphorus (P) is within the above range, the withstand voltage of the coating is improved, which makes it difficult for oxygen to be extracted from the coating to the solid electrolyte, thereby suppressing oxidation of the solid electrolyte. Considering the above, it is preferable that the molar ratio of lithium (Li) element to phosphorus (P) element is in the above range from the viewpoint of improving the storage characteristics of a solid-state battery, whose storage characteristics are easily affected by the storage environment.
[0013] Furthermore, the phosphorus-containing compound preferably has a molar ratio of oxygen (O) element to phosphorus (P) element of, for example, 2.5 or more, more preferably 2.7 or more, and even more preferably 2.9 or more. Furthermore, the molar ratio of oxygen (O) element to phosphorus (P) element is, for example, preferably 3.5 or less, more preferably 3.3 or less, and even more preferably 3.1 or less. When the molar ratio of oxygen (O) to phosphorus (P) is within the above range, the withstand voltage of the coating is improved, which makes it difficult for oxygen to be extracted from the coating to the solid electrolyte, thereby suppressing oxidation of the solid electrolyte. Considering the above, it is preferable that the molar ratio of oxygen (O) element to phosphorus (P) element is in the above range from the viewpoint of improving the storage characteristics of a solid-state battery, whose storage characteristics are easily affected by the storage environment.
[0014] Examples of the phosphorus-containing compound include lithium salts of phosphoric acid, phosphoric acid, phosphine, phosphorane, sodium phosphate, and potassium phosphate. Examples of the lithium salts of phosphoric acid include lithium orthophosphate, and its condensates such as lithium pyrophosphate, lithium metaphosphate, and lithium polyphosphate. It is particularly preferable to use lithium metaphosphate as the phosphorus-containing compound. This is because it can effectively improve the storage characteristics of a solid-state battery, which is a battery whose storage characteristics are easily affected by the storage environment. The phosphorus-containing compound can be used alone or in combination of two or more types.
[0015] The phosphorus-containing compound forming the coating portion may contain other elements in addition to the above-mentioned lithium (Li), phosphorus (P) and oxygen (O). Examples of other elements include carbon (C) element, nitrogen (N) element, etc. These may be used alone or in combination of two or more.
[0016] The phosphorus-containing compound is preferably contained in an amount of, for example, 0.1 mass % or more relative to the active material, more preferably 0.5 mass % or more, even more preferably 1.0 mass % or more, and even more preferably 3.0 mass % or more. The phosphorus-containing compound is preferably contained in an amount of, for example, 10.0% by mass or less, more preferably 8.0% by mass or less, and even more preferably 7.0% by mass or less, relative to the active material. The amount of the phosphorus-containing compound contained in the active material is preferably within the above range from the viewpoint of effectively improving the storage characteristics of a solid-state battery, which is a battery whose storage characteristics are easily affected by the storage environment, and is particularly preferable from the viewpoint of effectively suppressing an increase in the resistance of the solid-state battery, which becomes significant when the storage environment is high temperature.
[0017] [Covering part] The phosphorus-containing compound is present on the surface of the core particle as (I) particles, (II) aggregated particles, or (III) a layer. The term "layer" refers to a state in which the compound is present with a certain thickness. In this specification, any of the above embodiments (I) to (III) is included in the "coating portion containing a phosphorus-containing compound is formed."
[0018] The proportion of the phosphorus-containing compound contained in the coating portion is, for example, preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more. When the proportion of the phosphorus-containing compound contained in the coating portion is within this range, the storage characteristics of the solid-state battery, which is a battery whose storage characteristics are easily affected by the storage environment, can be effectively improved. In particular, the increase in resistance of the solid-state battery, which becomes significant when the storage environment is high temperature, can be effectively suppressed. The closer the proportion of the phosphorus-containing compound contained in the coating portion is to 100% by mass, the more it contributes to suppressing the generation of a high-resistance layer.
[0019] The coating portion may further contain other compounds in addition to the above-mentioned phosphorus-containing compound. The other compounds are compounds different from the above-mentioned phosphorus-containing compound. The state of existence of these compounds in the coating portion depends on the method of forming the coating portion. Depending on the method of forming the coating portion, the phosphorus-containing compound and the other compounds may be present in the coating portion in a mixed state. Alternatively, depending on the method for forming the coating part, a layer mainly containing a phosphorus-containing compound and a layer mainly containing other compounds may be laminated to form the coating part. In this case, a layer mainly containing a phosphorus-containing compound may be present on the surface of the core particle, and a layer mainly containing other compounds may be present thereon. Conversely, a layer mainly containing other compounds may be present on the surface of the core particle, and a layer mainly containing a phosphorus-containing compound may be present thereon. The other compound is preferably an oxide. The oxide preferably contains lithium (Li). By containing Li in the oxide, the storage characteristics of a solid-state battery, which is a battery whose storage characteristics are easily affected by the storage environment, can be effectively improved. From the viewpoint of making this advantage more prominent, the oxide preferably contains, in addition to Li, an A element (A represents at least one element selected from niobium (Nb), tantalum (Ta), sulfur (S), and zirconium (Zr). Hereinafter, an oxide containing Li and A is also referred to as "LiA oxide" for convenience.
[0020] An example of LiA oxide is Li2SO4, where the A element is S. In addition, an example of LiA oxide is Li2SO4, where the A element is Nb. x NbO y In the formula, x and y can take any value within the range according to the valence of the Nb element. Specifically, Li3NbO4, LiNbO3, LiNb3O8, and Li8Nb6O 19 etc. The above-mentioned various LiA oxides can be used alone or in combination of two or more.
[0021] When the coating portion contains other compounds in addition to the phosphorus-containing compound, regardless of the state of the phosphorus-containing compound and the other compounds in the coating portion, the abundance ratio of the phosphorus-containing compound to the other compounds, expressed as the mass ratio of the other compounds to the phosphorus-containing compound, may be, for example, 0.01 or more, 0.10 or more, or 0.30 or more. Furthermore, the abundance ratio of the phosphorus-containing compound to the other compounds, expressed as the mass ratio of the other compounds to the phosphorus-containing compound, may be 1.00 or less, 0.80 or less, or 0.60 or less. When the ratio of the phosphorus-containing compound to the other compounds is within the above range, the storage characteristics of the solid-state battery, which is a battery whose storage characteristics are easily affected by the storage environment, can be effectively improved, and an increase in the resistance of the solid-state battery, which becomes noticeable particularly when the storage environment is high temperature, can be effectively suppressed. The amount of phosphorus-containing compounds and other compounds contained in the coating can be measured by ICP atomic emission spectrometry.
[0022] The thickness of the coating portion is preferably, for example, 1 nm or more, more preferably 10 nm or more, and even more preferably 25 nm or more. When the thickness of the coating portion is within this lower limit, a reaction between the solid electrolyte and the active material, for example, an increase in resistance between the solid electrolyte and the active material, can be effectively suppressed. The thickness of the coating portion is preferably, for example, 100 nm or less, more preferably 50 nm or less, and even more preferably 35 nm or less. When the thickness of the coating portion has this upper limit, the movement of ions from the solid electrolyte to the active material can be effectively prevented from being hindered, and thus the charge transfer resistance can be effectively prevented from increasing. Considering the above, by setting the thickness of the covering portion within the above range, it is possible to effectively improve the storage characteristics of the solid-state battery, which is a battery whose storage characteristics are easily affected by the storage environment, and to effectively suppress an increase in the resistance of the solid-state battery, which becomes particularly noticeable when the storage environment is high temperature. The thickness of the coating layer can be measured, for example, by X-ray photoelectron spectroscopy (XPS). If necessary, it can also be observed and measured in combination with a scanning transmission electron microscope (STEM) or Auger electron spectroscopy (AES).
[0023] The core particle may have a portion on its surface where the coating portion is not present. In this case, it is preferable that the coating portion covers, for example, 10% or more of the total surface area of the core particle, more preferably 30% or more, and even more preferably 45% or more (this value is also called the "coverage ratio"). The fact that the coating portion covers the surface of the core particle can be confirmed, for example, by observing the surface of the core particle using X-ray photoelectron spectroscopy (XPS) in combination with a scanning transmission electron microscope (STEM) or energy dispersive X-ray analysis (EDS) as necessary, as well as Auger electron spectroscopy (AES), as described above. Furthermore, the thickness of the coating portion that coats the surface of the core particle does not need to be uniform.
[0024] [Core particles] The core particles are not particularly limited as long as they function as an active material. The core particles may contain, for example, a lithium metal composite oxide. As the lithium metal composite oxide, a known lithium metal composite oxide can be used. For example, it is preferable to include at least one selected from a lithium-containing composite oxide having a layered rock salt structure represented by the general formula LiMO2 (M represents a metal element), a lithium-excess layered rock salt type lithium-containing composite oxide, a lithium-containing composite oxide having a spinel structure represented by the general formula LiM2O4 (M represents a metal element), and a phosphate compound having an olivine structure represented by the general formula LiMPO4 (M represents a metal element). Alternatively, it may be a combination of two or more of these. However, it is not limited to these.
[0025] [Core particle A] The core particles are preferably particles made of a lithium transition metal composite oxide having a spinel structure containing Li, Mn, and O and one or more other elements (hereinafter, the core particles are also referred to as "core particles A"). When the active material of the present invention containing the core particles A is used as a positive electrode active material, it has an operating potential of 4.5 V or more based on a metal Li reference potential. "Having an operating potential of 4.5 V or more based on a metal Li reference potential" does not necessarily have to have only an operating potential of 4.5 V or more as a plateau region, but also includes a case where the operating potential is partially 4.5 V or more. Therefore, the present invention is not limited to a positive electrode active material consisting only of a 5 V class positive electrode active material having an operating potential of 4.5 V or more as a plateau region. For example, the active material of the present invention may contain a positive electrode active material having an operating potential of less than 4.5 V as a plateau region. Specifically, it is preferable that the 5V class positive electrode active material occupies, for example, 30% by mass or more, preferably 50% by mass or more, and particularly preferably 80% by mass or more (including 100% by mass) of the positive electrode active material.
[0026] As described above, the core particle A is preferably a particle made of a spinel-type composite oxide containing Li, Mn, and O and two or more other elements. At least one of the "two or more other elements" is preferably a metal element M1 selected from the group consisting of Ni, Co, and Fe, and the other element is preferably a metal element M2 consisting of one or a combination of two or more selected from the group consisting of Na, Mg, Al, K, Ca, Ti, V, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, In, Ta, W, Re, and Ce.
[0027] A preferred composition example of the core particle A is LiMnO 4-δ The lithium-manganese-containing spinel-type composite oxide may have a crystal structure in which a part of the Mn sites in the above formula (I) is replaced with Li, a metal element M1, and another metal element M2.
[0028] The metal element M1 is a substitution element that mainly contributes to realizing an operating potential of 4.5 V or more based on the metallic Li reference potential, and examples of such elements include Ni, Co, and Fe. The active material A may contain at least one of these elements, and it is particularly preferable that the active material A contains at least one of Ni and Co.
[0029] The metal element M2 is a substitution element that mainly contributes to stabilizing the crystal structure and improving the characteristics. For example, examples of substitution elements that contribute to improving the capacity retention rate include Na, Mg, Al, K, Ca, Ti, V, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, In, Ta, W, Re, and Ce, and among them, Na, Mg, Al, K, Ca, Ti, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, Ta, and W are preferably used. The metal element M2 may be one or a combination of two or more of the above-mentioned elements. The metal element M2 preferably contains at least one of the above-mentioned elements, and may contain a metal element other than the above-mentioned elements. The metal element M2 contained in the structure is an element type different from the metal element M1.
[0030] An example of the composition of the core particle A is represented by the formula (1): Li x (M1 y M2 z Mn 2-x-y-z )O 4-δ Examples include a spinel-type lithium manganese-containing composite oxide represented by the following formula (1): The metal element M1 and the metal element M2 in the formula (1) are as described above.
[0031] In the formula (1), "x" is preferably 1.00 or more, more preferably 1.01 or more, and even more preferably 1.02 or more. In the formula (1), "x" is preferably 1.20 or less, more preferably 1.10 or less, and even more preferably 1.08 or less. "y" indicating the content of the metal element M1 is preferably 0.20 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. In addition, "y" indicating the content of the metal element M1 is preferably 1.20 or less, more preferably 1.10 or less, and even more preferably 1.05 or less. "z" indicating the content of the metal element M2 is preferably 0.001 or more, more preferably 0.002 or more, more preferably 0.005 or more, and even more preferably 0.100 or more. In particular, by making it 0.100 or more, the cycle characteristics can be improved more effectively. Moreover, "z" indicating the content of the metal element M2 is, for example, preferably 0.400 or less, and more preferably 0.300 or less.
[0032] Another example of the composition of the core particle A is a compound represented by the formula (2): Li x (Ni y M3 z Mn 3-x-y-z )O 4-δExamples of the spinel-type lithium manganese-containing composite oxide include those represented by the formula (2). In formula (2), "x" is preferably 1.00 or more, more preferably 1.01 or more, and even more preferably 1.02 or more. In formula (2), "x" is preferably 1.20 or less, more preferably 1.10 or less, and even more preferably 1.08 or less. In formula (2), "y" is preferably 0.20 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. In formula (2), "y" is preferably 0.70 or less, more preferably 0.60 or less, and even more preferably 0.55 or less.
[0033] In the formula (2), examples of the metal element M3 include Na, Mg, Al, K, Ca, Ti, V, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, In, Ta, W, Re, and Ce, among which Na, Mg, Al, K, Ca, Ti, Cr, Fe, Co, Cu, Ga, Y, Zr, Nb, Mo, Ta, and W are preferred. The metal element M3 may be one or a combination of two or more of the above-mentioned elements. "z" indicating the molar ratio of the metal element M3 is preferably, for example, greater than 0, and more preferably greater than 0.01, and even more preferably 0.05 or more, and even more preferably 0.10 or more. By setting "z" to this lower limit or more, the cycle characteristics can be improved more effectively. In addition, "z" indicating the molar ratio of the metal element M3 is preferably, for example, 0.50 or less, and even more preferably 0.45 or less, and even more preferably 0.40 or less, and even more preferably 0.35 or less.
[0034] In addition, "4-δ" in the above formulas (1) and (2) indicates that oxygen vacancies may be included. In addition, a part of oxygen may be substituted with fluorine or other elements. In this case, δ is preferably 0 or more. In addition, δ is preferably, for example, 0.20 or less, more preferably 0.10 or less, and even more preferably 0.05 or less.
[0035] The core particle A may contain B (boron). The state of existence of B may include a composite oxide phase containing Ni, Mn, and B in addition to a spinel crystal phase. An example of the composite oxide phase containing Ni, Mn, and B is a Ni5MnO4(BO3)2 crystal phase. The presence of the Ni5MnO4(BO3)2 crystal phase can be confirmed by comparing a diffraction pattern obtained by X-ray diffraction (XRD) with PDF (Powder Diffraction File) number "01-079-1029".
[0036] Regarding the content of the complex oxide phase containing Ni, Mn and B, it is preferable to contain the complex oxide phase so that the content of the B element in the core particle A is 0.02 mass% or more, and more preferably, the complex oxide phase is contained so that the content is 0.05 mass% or more. If the content of the B element is 0.02 mass% or more, it is preferable because the discharge capacity at high temperatures can be maintained. In addition, it is preferable to contain the complex oxide phase so that the content of the B element in the core particle A is 0.80 mass% or less, and more preferably, the complex oxide phase is contained so that the content is 0.60 mass% or less, more preferably, 0.30 mass% or less, and particularly preferably, 0.25 mass% or less. If the content of the B element is 0.80 mass% or less, it is preferable because the rate characteristic can be maintained.
[0037] The core particle A may contain components other than the above-mentioned Li, Mn, metal element M1, metal element M2, metal element M3, O, and B. In particular, the other elements may each be contained in an amount of 0.5 mass% or less, because such amounts are considered to have little effect on the performance of the core particle.
[0038] In addition, when the core particle A is fitted to a cubic crystal structure model of the space group Fd-3m (Origin Choice 2), for example, the range of Rwp and S, which indicate the degree of agreement between the observed intensity and the calculated intensity, is Rwp<10 or S<2.5, and thus it can be confirmed that the core particle A has a spinel structure.
[0039] The primary particles of the core particles A are preferably polycrystalline rather than monocrystalline. A monocrystalline refers to a particle in which the primary particle is composed of one crystallite, and a polycrystalline refers to a particle in which multiple crystallites exist within the primary particle. Whether the core particles are polycrystalline or not can be confirmed by observing the cross section of the primary particle using electron backscatter diffraction (EBSD). In the case of a polycrystalline, it can be confirmed that crystals with multiple orientations exist within the primary particle.
[0040] [Core particle B] The core particles are also preferably particles made of a lithium transition metal composite oxide having a layered rock-salt structure containing Li, M element (M includes at least one or a combination of two or more elements selected from the group consisting of Ni, Co, Mn, and Al), and O (hereinafter, the core particles are also referred to as "core particles B"). The active material of the present invention may contain other components in addition to core particles B. However, from the viewpoint of effectively obtaining the characteristics of core particles B, it is preferable that core particles B account for, for example, 80% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more (including 100% by mass).
[0041] The core particle B is represented by the formula (3): Li 1+x M 1-x O2 (wherein M is a combination of one or more elements selected from the group consisting of Ni, Co, Mn, and Al, or includes a combination of one or more elements selected from the group consisting of Ni, Co, Mn, and Al and a combination of one or more elements selected from the group consisting of transition metal elements present between Groups 3 and 11 of the periodic table, and typical metal elements from Periods 1 to 3 of the periodic table).
[0042] Formula (3): Li 1+x M 1-x In O2, "1+x" is, for example, 0.95 or more, preferably 0.97 or more, and more preferably 0.98 or more.1+x M 1-x In O2, "1+x" is, for example, preferably 1.09 or less, more preferably 1.07 or less, and even more preferably 1.05 or less.
[0043] "M" in the formula (3) may contain the three elements Mn, Co, and Ni. For example, it may be composed of only the three elements Mn, Co, and Ni, or may contain one or more of the other elements in addition to the three elements, or may have another composition.
[0044] Examples of transition metal elements present among the elements of Groups 3 to 11 of the periodic table, and typical metal elements from Period 1 to Period 3 of the periodic table include Al, V, Fe, Ti, Mg, Cr, Ga, In, Cu, Zn, Nb, Zr, Mo, W, Ta, and Re, and among these, V, Fe, Ti, Mg, Cr, Ga, Cu, Zn, Nb, Zr, Mo, W, and Ta are preferred.
[0045] When "M" in the above formula (3) contains the three elements Mn, Co, and Ni, the molar ratios of Mn, Co, and Ni are preferably Mn:Co:Ni=more than 0.00 and not more than 0.45:more than 0.00 and not more than 0.40:0.30 to 1.00, and more preferably Mn:Co:Ni=0.01 to 0.45:0.01 to 0.40:0.30 to 0.95, and more preferably Mn:Co:Ni=0.05 to 0.40:0.03 to 0.40:0.30 to 0.85, and even more preferably Mn:Co:Ni=0.05 to 0.40:0.03 to 0.40:0.30 to 0.75.
[0046] In the above formula (3), the atomic ratio of the oxygen amount is described as "2" for convenience, but may have some non-stoichiometry. That is, the atomic ratio of the oxygen amount may be "2-δ", where "-δ" indicates oxygen deficiency. In this case, δ is preferably 0 or more. In addition, δ is preferably, for example, 0.20 or less, more preferably 0.10 or less, and even more preferably 0.05 or less.
[0047] The core particles B may contain impurities. For example, the impurity elements may each be contained in an amount of 0.17 mass % or less. This is because it is believed that such amounts have almost no effect on the properties of the core particles B.
[0048] In addition, when the core particle B is fitted to a hexagonal crystal structure model of space group R-3m, for example, the ranges of Rwp and S, which indicate the degree of agreement between the observed intensity and the calculated intensity, are Rwp<10 or S<2.5, and thus it can be confirmed that the core particle B has a layered structure.
[0049] The primary particles of the core particles B are preferably polycrystalline rather than single crystal, like the core particles A. The definitions of single crystal and polycrystalline are the same as those for the core particles A.
[0050] [Core particle C] The core particles are preferably particles made of a lithium-rich layered rock-salt type lithium-containing composite oxide containing Li, Ma (Ma necessarily contains Mn and contains at least one selected from Ni and Co), Mb (Mb contains at least one selected from Al, Mg, Ti, Fe and Nb), and O (hereinafter, the core particles are also referred to as "core particles C"). The active material of the present invention may contain other components in addition to the core particles C. However, from the viewpoint of effectively obtaining the characteristics of the core particles C, it is preferable that the core particles C occupy, for example, 50% by mass or more, particularly 70% by mass or more, of which 90% by mass or more, and of which 95% by mass or more (including 100% by mass) is included.
[0051] The core particle C is represented by the formula (5): Li 1+x Ma 1-x-y Mb y O2 (wherein Ma necessarily contains Mn and contains at least one selected from Ni and Co. Mb contains at least one selected from Al, Mg, Ti, Fe and Nb).
[0052] In the above formula (5), "x" is, for example, preferably 0.10 or more, more preferably 0.11 or more, and even more preferably 0.12 or more. Also, in the above formula (5), "x" is, for example, preferably 0.33 or less, more preferably 0.32 or less, and even more preferably 0.31 or less. In the above formula (5), "y" is, for example, preferably 0.000 or more, more preferably 0.005 or more, and even more preferably 0.010 or more. Also, in the above formula (5), "y" is, for example, preferably 0.300 or less, more preferably 0.295 or less, and even more preferably 0.290 or less.
[0053] Regarding the content of Ma in the core particles, the content of Mn in Ma is, for example, preferably 30% by mass or more, more preferably 31% by mass or more, and even more preferably 32% by mass or more. Also, the content of Mn in Ma is, for example, preferably 80% by mass or less, more preferably 79% by mass or less, and even more preferably 78% by mass or less.
[0054] In the above formula (5), the atomic ratio of the oxygen amount is described as "2" for convenience, but may have some non-stoichiometry. That is, the atomic ratio of the oxygen amount may be "2-δ", where "-δ" indicates oxygen deficiency. In this case, δ is preferably 0 or more. In addition, δ is preferably, for example, 0.20 or less, more preferably 0.10 or less, and even more preferably 0.05 or less.
[0055] The core particles C may contain impurities. For example, when the impurity is SO4, the impurity may be 1.0 mass% or less. Alternatively, when the impurity is an element other than SO4, the impurity may be 0.5 mass% or less. This is because such an amount is considered to have almost no effect on the properties of the core particles C.
[0056] [Active material] The active material of the present invention preferably has a peak in a specific range in the infrared absorption spectrum obtained by Fourier transform infrared spectroscopy (FT-IR). By measuring the active material of the present invention by FT-IR, the chemical state of the phosphorus-containing compound forming the coating portion arranged on the surface of the core particle can be observed. As a result of the inventor's investigation, it was found that by observing a specific peak in the phosphorus-containing compound by FT-IR, it is possible to improve the storage characteristics of a solid-state battery, whose storage characteristics are easily affected by the storage environment (especially high-temperature storage). From this viewpoint, the active material of the present invention preferably has an infrared absorption spectrum obtained by FT-IR at 1290±50 cm -1 It is preferable that the peak is in the range of 1290±30 cm -1 More preferably, the peak is in the range of 1290±15 cm -1 It is more preferable that the peak is in the range of 1290±50 cm. -1 "Having a peak in the range of 1290±50 cm" means that the peak top position is 1290±50 cm -1 The presence or absence of a peak can be judged, for example, by the following criteria. Specifically, the wave number on the spectrum is (1290-50) cm -1 , i.e., 1240 cm -1 The point and the wave number on the spectrum are (1290+50) cm -1 , i.e., 1340 cm -1 Draw a straight line through the points 1290±50cm and 290±50cm. Subtract the absorbance based on this straight line to obtain a spectrum. -1 If the maximum value obtained by subtracting the absorbance on the straight line from the absorbance of the peak in the range is 0.02 or more, preferably 0.05 or more, then 1290±50 cm -1 It can be determined that a peak exists in the range of 1290±50 cm. The above absorbance values are values measured using the apparatus and conditions used in the examples described below. -1 The present inventors believe that the peak observed in this range is a peak derived from the stretching vibration of the bond between phosphorus (P) and oxygen (O) elements contained in the phosphorus-containing compound.
[0057] It is required for the active material to improve the storage characteristics of a solid-state battery, whose storage characteristics are easily affected by the storage environment, but the active material described in the above-mentioned Patent Document 1 could not solve this problem. In detail, although the active material described in the same document is treated to coat its surface with lithium metaphosphate, it is considered that the lithium metaphosphate is heat-treated after the treatment, and therefore its chemical structure is changed, and it is considered that the surface of the active material is coated with a phosphorus-containing compound different from lithium metaphosphate. Due to this, unlike the active material of the present invention, the active material described in the same document does not observe a peak in a specific range in the infrared absorption spectrum obtained by FT-IR. This is clear from the result of Comparative Example 1 described later. As a result, the active material described in the same document does not sufficiently improve the storage characteristics of a solid-state battery. In contrast, the active material of the present invention, whose surface is coated with a specific phosphorus-containing compound, can further improve the above-mentioned storage characteristics compared to the active material described in Patent Document 1.
[0058] The active material has an infrared absorption spectrum of 1290±50 cm -1 In order to have a peak in this range, it is preferable to dry mix the core particles and the compound that forms the coating portion while cooling in the manufacturing method described below, to include a phosphorus-containing compound in the coating portion, or to control the moisture content as described below.
[0059] It is also preferable that the active material of the present invention has a peak in a specific range in the P2p spectrum measured by X-ray photoelectron spectroscopy (XPS). XPS is a measurement method that can analyze the constituent elements of the sample surface and their electronic state by measuring the photoelectron energy generated from the sample surface by irradiating the sample with X-rays. Therefore, by measuring the active material of the present invention by XPS, the chemical state of the phosphorus-containing compound forming the coating portion arranged on the surface of the core particle can be observed. As a result of the inventor's investigation, it was found that the generation of a high resistance layer that may occur between the core particle and the electrolyte due to contact between them when charging and discharging at high temperatures, for example, can be suppressed by observing a specific binding energy in the phosphorus-containing compound by XPS measurement. From this viewpoint, it is preferable that the active material of the present invention has a peak in the P2p spectrum measured by XPS in the range of 134±0.45 eV, more preferably in the range of 134±0.40 eV, and even more preferably in the range of 134±0.20 eV. In this specification, "having a peak in the range of 134±0.45 eV" means that the position of the peak top is in the range of 134±0.45 eV. The presence or absence of a peak can be determined, for example, using the following criteria. Specifically, in an XPS spectrum, the average value of the photoelectron intensity (counts / s) in the range of (134-5.0)±0.5 eV, i.e., the range of 129±0.5 eV, and the average value of the photoelectron intensity (counts / s) in the range of (134+5.0)±0.5 eV, i.e., the range of 139±0.5 eV, is taken as the background intensity A, and the photoelectron intensity (counts / s) of the peak top in the range of 134±0.45 eV is taken as the peak intensity B. If the ratio (B / A) is 1.15 or more, preferably 1.20 or more, and more preferably 1.25 or more, it can be determined that a peak exists in the range of 134±0.45 eV. The above photoelectron intensity values are values measured using the apparatus and conditions used in the examples described later.
[0060] In order to make the active material have a peak in the range of 134±0.45 eV in the P2p spectrum measured by XPS, it is preferable to dry mix the core particles and the compound that forms the coating portion while cooling in the manufacturing method described below, to include a phosphorus-containing compound in the coating portion, or to control the moisture content as described below.
[0061] The active material of the present invention is generally in the form of particles, 50 That is, the volume cumulative particle size at 50% by volume of cumulative volume measured by a volume particle size distribution measurement method obtained by a laser diffraction scattering type particle size distribution measurement method is, for example, preferably 0.5 μm or more, more preferably 1.0 μm or more, even more preferably 2.0 μm or more, and even more preferably 2.5 μm or more. 50 For example, it is preferable that the thickness is 15.0 μm or less, more preferably 10.0 μm or less, and particularly preferably 8.0 μm or less. 50 By setting the range above, it is possible to reduce the resistance when Li ions diffuse into the particles of the active material, and as a result, it is possible to improve the end-of-discharge characteristics.
[0062] The active material of the present invention may have a moisture content (mass ppm) up to 250°C measured by the Karl Fischer method of, for example, 1200 ppm or less, 1000 ppm or less, or 900 ppm or less. The moisture content may be, for example, 1 ppm or more, 5 ppm or more, 10 ppm or more, 20 ppm or more, 100 ppm or more, 200 ppm or more, or 400 ppm or more. The amount of moisture contained in the active material is preferably as small as possible from the viewpoint of reducing structural deterioration of the active material due to reaction with lithium and reducing reaction with the electrolyte during battery operation. In order to reduce the amount of moisture contained in the active material as much as possible, for example, the active material may be dried at a temperature of 250°C or the like, under vacuum, or in an inert atmosphere. The procedure for measuring the moisture content by the Karl Fischer method is as follows: using a Karl Fischer moisture meter capable of coulometric titration, the measurement sample is heated to 110°C, the released moisture content (ppm by mass) is measured, and then the measurement sample is heated to 250°C, the released moisture content (ppm by mass) is measured, and the sum of these values is taken as the moisture content. The measurement is performed in an argon atmosphere, and for example, an 860 KF Thermoprep (manufactured by Metrohm) and an 899 Coulometer (manufactured by Metrohm) are used as the measurement device.
[0063] The active material of the present invention can be used in a battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer. Specifically, the active material of the present invention can be used in the positive electrode layer or the negative electrode layer, and it is particularly preferable that the positive electrode layer contains the active material of the present invention. The active material of the present invention is preferably used in a solid battery containing a solid electrolyte. In a solid battery, the effect of the present invention can be enjoyed by the presence of a contact portion between the active material of the present invention and the solid electrolyte. The term "solid-state battery" refers not only to solid-state batteries that do not contain any liquid or gel-like substance as an electrolyte, but also to batteries that contain, for example, 50% by mass or less, 30% by mass or less, or 10% by mass or less of a liquid or gel-like substance as an electrolyte.
[0064] The active material of the present invention can be mixed with a solid electrolyte and a conductive material to obtain an electrode mixture. The solid electrolyte may be the same as the solid electrolyte used in a general solid-state battery. For example, a sulfide solid electrolyte, an oxide solid electrolyte, a nitride solid electrolyte, a halide solid electrolyte, etc. are listed. Among them, it is preferable to use a sulfide solid electrolyte containing elemental sulfur (S). The sulfide solid electrolyte may contain, for example, Li element and S element and have lithium ion conductivity, or may contain Li element, P element and S element and have lithium ion conductivity. The sulfide solid electrolyte may be any of a crystalline material, glass ceramics, and glass. The sulfide solid electrolyte may have a crystalline phase of an argyrodite-type structure. Examples of such sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiX (where "X" represents one or more halogen elements), Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 、Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 、Li 3.25 P 0.95 S4, Li 7-x PS 6-x X x (a solid electrolyte having a crystalline phase of an argyrodite-type structure, "X" represents one or more halogen elements, and 0.2 < x < 2.0 or 0.2 < x < 1.8). etc. can be mentioned. As the conductive material, for example, electronically conductive carbonaceous materials such as carbon black and acetylene black can be used.
[0065] The electrode binder can be used to prepare a paste by mixing it with a solvent and a binder, and applying the paste onto a current collector such as an aluminum foil and drying it to prepare an electrode (a positive electrode layer and / or a negative electrode layer). The electrode thus prepared contains the electrode binder and the binder.
[0066] [Manufacturing method of the active material] The manufacturing method of the active material is roughly classified into a manufacturing method of the core material particles and a forming method of the coating portion on the surface of the core material particles. An example of the method for producing the core particles includes a manufacturing method including a raw material mixing step, a wet grinding step, a granulation step, a firing step, a heat treatment step, a washing / drying step and a grinding step, although this manufacturing method is merely a preferred example and is not limited to this manufacturing method.
[0067] The method for forming the coating portion is appropriately selected depending on the type of phosphorus-containing compound that constitutes the coating portion. For example, when the coating portion contains lithium metaphosphate as the phosphorus-containing compound, it is preferable to dry-mix a mixture containing the core particles and a phosphorus-containing compound containing lithium (Li), phosphorus (P) and oxygen (O) elements, and to arrange the coating portion containing the phosphorus-containing compound on the surface of the core particles. In particular, when the dry mixing is performed while cooling, the phosphorus-containing compound is less likely to be altered. As a result, the obtained active material is preferable because it can improve the storage characteristics of a solid-state battery, which is a battery whose storage characteristics are easily affected by the storage environment. When dry mixing is performed with cooling, for example, a dry mixer equipped with a water-cooling jacket can be used. The temperature of the mixture during dry mixing is preferably maintained at 10°C or higher and 50°C or lower.
[0068] For example, when the coating portion includes other compounds in addition to the phosphorus-containing compound, a mixture containing the core particles, the above-mentioned phosphorus-containing compound, and other compounds may be dry-mixed to arrange the coating portion containing these compounds on the surface of the core particles. Alternatively, a mixture containing the core particles and the above-mentioned phosphorus-containing compound may be dry-mixed, and other compounds may be dry-mixed to arrange the coating portion containing these compounds on the surface of the core particles. Alternatively, one compound may be arranged on the surface of the core particles by a wet method, and then the core particles on which the compound is arranged and the other compound may be dry-mixed to arrange the coating portion containing these compounds on the surface of the core particles.
[0069] In the past, when a coating portion containing a compound is arranged on the surface of a core particle, it was common to contact the core particle with a solution containing the compound. This method aims to uniformly coat the surface of the core particle with a compound. However, the conventional method had the problem that a drying process and a heat treatment process may be required after the coating portion is arranged. In addition, there was a problem that the chemical structure of the compound changes, especially due to the heat treatment process. As a result of intensive research by the present inventors into these problems, it was found that when a coating portion containing a compound is arranged on a core particle, these problems can be solved by performing dry mixing while cooling as described above.
[0070] Although the present invention has been described based on the preferred embodiment, the present invention is not limited to the above embodiment.
[0071] In relation to the above-described embodiment, the following active material and its manufacturing method, as well as an electrode mixture, an electrode, and a battery each containing the same are further disclosed. [1] An active material having a core particle and a coating portion disposed on the surface of the core particle, The coating portion includes a compound containing lithium (Li), phosphorus (P), and oxygen (O), The compound has a molar ratio of lithium (Li) element to phosphorus (P) element of 0.5 or more and 2.5 or less, and a molar ratio of oxygen (O) element to phosphorus (P) element of 2.5 or more and 3.5 or less, In the infrared absorption spectrum obtained by Fourier transform infrared spectroscopy (FT-IR), -1 The active material has a peak in the range of
[0072] [2] The active material according to [1], which has a peak in the range of 134±0.45 eV in a P2p spectrum measured by X-ray photoelectron spectroscopy. [3] The active material according to [1] or [2], wherein the proportion of the compound contained in the coating portion is 50 mass % or more. [4] The active material according to any one of [1] to [3], wherein the core particles contain at least one selected from the group consisting of a lithium transition metal composite oxide having a spinel structure, a lithium transition metal composite oxide having a layered rock-salt structure, and a phosphate compound having an olivine structure. [5] The active material according to any one of [1] to [4], wherein the coating portion has a thickness of 1 nm or more and 100 nm or less. [6] The active material according to any one of [1] to [5], which has a moisture content of 1,200 ppm or less at up to 250° C. as measured by the Karl Fischer method.
[0073] [7] The active material according to any one of [1] to [6], wherein the coating portion contains lithium metaphosphate. [8] An electrode mixture comprising the active material according to any one of [1] to [7], a solid electrolyte, and a conductive material. [9] An electrode comprising the electrode mixture according to [8] and a binder.
[10] A battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, A battery, wherein the positive electrode layer contains the active material according to any one of [1] to [7].
[11] A method for producing an active material, comprising dry-mixing a mixture containing core particles and a compound containing lithium (Li), phosphorus (P), and oxygen (O) while cooling, to dispose a coating portion containing the compound on the surface of the core particles. EXAMPLES
[0074] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".
[0075] Example 1 (1) Preparation of core particles As the core particles, a spinel-type lithium transition metal composite oxide (hereinafter also referred to as "LNMO") having a composition of Li: 4.1%, Mn: 41.3%, Ni: 13.3%, and Ti: 5.4% was prepared.
[0076] (2) Formation of the coating The core particles and lithium metaphosphate were mixed using a dry particle composite device NOB-MINI manufactured by Hosokawa Micron Corporation, and the lithium metaphosphate was attached to the surface of the core particles to form a coating portion containing lithium metaphosphate. The amount of the core particles and lithium metaphosphate was adjusted so that the ratio of lithium metaphosphate to the active material was 5.0%. During mixing, the device was cooled and maintained at 30°C. In this manner, active material particles were obtained.
[0077] Example 2 In step (1) of Example 1, a lithium transition metal composite oxide (hereinafter also referred to as "NCM") having a composition of Ni: 60%, Co: 20%, Mn: 20% was prepared as the core material particles. Except for this, the active material particles were obtained in the same manner as in Example 1.
[0078] Comparative Example 1 This comparative example corresponds to an example of Patent Document 1. Instead of the step (2) in Example 1, the following step was added. First, an aqueous solution of lithium metaphosphate was prepared. The concentration of lithium metaphosphate in the aqueous solution was 0.1 mol / L. The concentration was set so that the ratio of lithium metaphosphate to the active material was 5.0%. The core particles were added to the obtained aqueous solution, and the two were mixed at 10,000 rpm for 30 minutes using a homogenizer (IKA T-25). After that, the solvent was removed using an evaporator while irradiating ultrasonic waves in a thermostatic chamber at 55°C. The core particles were then dried at 120°C for 1 hour, and dried at normal pressure under an air flow at 400°C for 1 hour to obtain active material particles.
[0079] Comparative Example 2 Instead of step (2) of Example 1, the following step was added. First, 29.5 g of LiOH·H2O was dissolved in 214 g of water to obtain a lithium hydroxide aqueous solution. After this aqueous solution was heated to 100°C, 2 mL of 30% hydrogen peroxide and 0.862 g of niobium hydroxide were dissolved in the aqueous solution. The concentration of the aqueous solution was adjusted so that the ratio of lithium niobate to the active material was 1.3%. After stirring the aqueous solution for 30 minutes while keeping it at 100°C, 50 g of core particles were added to the aqueous solution and stirred for another 20 minutes. Next, the heating and stirring were stopped and the solution was left to stand, and the active material was allowed to settle in the aqueous solution. The aqueous solution was decanted, and the active material was washed twice with 200 mL of 0.14 mol / L lithium sulfate solution. Then, the active material was dried at 80°C to obtain active material particles with lithium niobate present on the surface. As a result of XPS measurement, no P2p peak was observed. Since the active material of this comparative example does not contain phosphorus (P), the molar ratio of lithium (Li) to phosphorus (P) and the molar ratio of oxygen (O) to phosphorus (P) could not be calculated.
[0080] Comparative Example 3 In the step (1) of Example 1, NCM was prepared as the core material particles. In addition, the following step was provided instead of the step (2). First, 0.027 g of ethoxylithium was dissolved in 10 g of anhydrous ethanol to obtain an ethoxylithium solution. 0.167 g of pentaethoxyniobium was dissolved in 10 g of anhydrous ethanol to obtain a pentaethoxyniobium solution. The concentration of the solution was adjusted so that the ratio of lithium niobate to the active material was 0.8%. 10 g of NCM was added to 140 g of anhydrous ethanol, and dispersed using a homogenizer at 10,000 rpm for 30 minutes to obtain an ethanol solution in which NCM was dispersed. Next, the ethoxylithium solution was added to the ethanol solution in which NCM was dispersed, and the mixture was stirred at 10,000 rpm for 2 minutes. The pentaethoxyniobium solution was further added to this solution, and the mixture was stirred at 10,000 rpm for 8 minutes. The solution was ultrasonically treated at 55°C to evaporate the ethanol, and active material particles with lithium niobate present on the surface were obtained. No P2p peak was observed in the XPS measurement. Since the active material of this comparative example does not contain phosphorus (P), the molar ratio of lithium (Li) to phosphorus (P) and the molar ratio of oxygen (O) to phosphorus (P) could not be calculated.
[0081] [Rating 1] For the active materials obtained in the examples, FT-IR was performed by the following method to determine the peak position of the infrared absorption spectrum. For Examples 1 and 2, and Comparative Example 2, graphs of the obtained infrared absorption spectra are shown in FIG. 1. In addition, XPS measurement was performed by the following method to determine the P2p peak position. For Examples 1 and 2, and Comparative Example 2, graphs of the obtained P2p spectra are shown in FIG. 2. In addition, the coverage and thickness of the coating portion were measured by the following method. Furthermore, the moisture content was measured by the above-mentioned method. The results are shown in Table 1 below.
[0082] [Infrared absorption spectrum peak position] The active materials obtained in the examples and comparative examples were measured using a NICOLET iZ10 Fourier transform infrared spectrophotometer manufactured by Thermo Fisher Scientific Co., Ltd. The conditions used for the measurement are as follows. Measurement method: Diffuse reflection method (background: Au mirror) Number of times accumulated: 256 Resolution: 4cm -1
[0083] [P2p peak position] The particle surfaces of the active materials obtained in the examples and comparative examples were analyzed using a PHI Quantes XPS device manufactured by ULVAC-PHI, Inc. The conditions used for the measurements are as follows. Excitation X-ray: Monochromatic Al line (1486.7 eV) Output: 50W Acceleration voltage: 15 kV X-ray irradiation diameter: 200μmφ Measurement area: 1000μm x 300μm Take Angle: 45° Pass energy: 26.0 eV Energy step: 0.1 eV
[0084] The XPS data was analyzed using data analysis software (ULVAC-PHI "MultiPakVer9.9"). The background mode used was Iterated Shirley. P2p was selected as the orbital used for calculation. Energy correction was performed using the C1s hydrocarbon peak (correction position: 284.8 eV).
[0085] [Covering rate of the coated part] The coverage of the coating portion was measured using PHI Quantes, an XPS device used to measure the P2p peak position. Specifically, the ratio of the quantitative value of the element present only in the coating portion to the sum of the quantitative value of the element present only in the coating portion and the quantitative value of the element present only in the core material particle was calculated. For example, when LNMO was used as the core material particle and lithium metaphosphate was used as the coating portion, the coverage was calculated by P / (Ni+Mn+Ti+P)×100. Similarly, for example, when NCM was used as the core material particle and lithium metaphosphate was used as the coating portion, the coverage was calculated by P / (Co+Ni+Mn+P)×100. The conditions used for the measurement were the same as those used for measuring the P2p peak position.
[0086] [Thickness of Covering Part] The thickness of the coating was measured using PHI Quantes, the XPS device used to measure the P2p peak position. Specifically, Ar ion sputtering was performed and XPS measurement was performed to obtain a depth profile. The SiO2-equivalent sputtering depth at which the area of the peak derived from the elements specific to the coating, not the main elements constituting the core particles, was halved compared to before sputtering, was defined as the thickness of the coating. The conditions used for the measurement were the same as those used for measuring the P2p peak position.
[0087] [Evaluation 2] Using the active materials obtained in the Examples and Comparative Examples, solid-state batteries were manufactured by the following method, and the resistance increase rate after storage at 60°C, which is an evaluation of storage characteristics, was measured. The results are shown in Table 1 below. In Table 1, "-" indicates that the value could not be calculated or that there was no infrared absorption spectrum peak or P2p peak in a specific range.
[0088] [Fabrication of solid-state batteries] The active materials obtained in the examples and comparative examples were used as the positive electrode active material, and graphite (Gr) powder was used as the negative electrode active material. A sulfide solid electrolyte having an argyrodite structure was used as the solid electrolyte powder. The positive electrode composite powder was prepared by mixing the positive electrode active material, the solid electrolyte powder, and a carbon-based material serving as a conductive assistant in a mass ratio of 70:27:3 in a mortar. The negative electrode composite powder was prepared by mixing the negative electrode active material and the solid electrolyte powder in a mass ratio of 1:1 in a mortar. The lower opening of a polypropylene cylinder (opening diameter 10.5 mm, height 18 mm) with openings at the top and bottom was blocked with a positive electrode (made of SUS), solid electrolyte powder was placed on top of it, and it was blocked with a negative electrode (made of SUS), and then uniaxially pressed at 10 MPa to form a solid electrolyte layer. Next, the negative electrode was temporarily removed, and a negative electrode composite powder was placed on the solid electrolyte layer and blocked again with the negative electrode. Then, the cylinder was turned upside down, the positive electrode was temporarily removed, and a positive electrode composite powder was placed on the solid electrolyte layer and blocked again with the positive electrode, and then uniaxially pressed at 60 MPa to produce a solid battery consisting of a three-layer structure of a positive electrode composite, a solid electrolyte layer, and a negative electrode composite.
[0089] [Resistance increase rate after storage at 60℃] <When the core particles are LNMO> The solid-state batteries prepared in Example 1 and Comparative Examples 1 and 2 were used to carry out charge / discharge tests as follows. In detail, the batteries were placed in an environmental tester set so that the environmental temperature for charging / discharging the batteries was 25° C., and the batteries were prepared for charging / discharging, and were left to stand until the battery temperature reached the environmental temperature. The conditions for charging / discharging the solid-state batteries were as follows. Next, the battery was charged at a constant current and constant potential to 5.0 V at 0.1 C, and then discharged at a constant current to 3.0 V at 0.1 C, and this cycle was repeated for three cycles. After that, the battery was charged until the state of charge (SOC) reached 50%, and the resistance value before the storage test was measured by impedance measurement. After that, the battery was charged at a constant current and constant potential to 4.9 V at 0.1 C, discharged at a constant current to 3.0 V at 0.1 C, and then charged at a constant current and constant potential to 4.9 V at 0.1 C again. The battery was charged at a constant current and constant potential to 4.9 V at 0.1 C, and placed in a thermostatic chamber set at 60 ° C. and stored for 168 hours. After 168 hours, the battery was removed and returned to room temperature, then placed in an environmental tester set to 25 ° C., and discharged at a constant current to 3.0 V at 0.1 C. Thereafter, the battery was charged at a constant current and constant potential to 4.9 V at 0.1 C, and discharged at a constant current to 3.0 V at 0.1 C. After charging until the SOC was 50%, the resistance value after the storage test was measured by impedance measurement. The resistance value after the storage test was calculated relative to the resistance value before the storage test, and this value was taken as the resistance increase rate after storage at 60°C.
[0090] <When the core particles are NCM> A charge / discharge test was carried out as follows using the solid-state batteries produced in Example 2 and Comparative Example 3. In detail, the batteries were placed in an environmental tester in which the environmental temperature for charging and discharging the batteries was set to 25° C., and prepared for charging and discharging, and were left to stand until the battery temperature reached the environmental temperature. Next, the battery was charged at a constant current and constant potential to 4.5 V at 0.1 C, and then discharged at a constant current to 2.5 V at 0.1 C, and this cycle was repeated for three cycles. After that, the battery was charged until the state of charge (SOC) reached 50%, and the resistance value before the storage test was measured by impedance measurement. After that, the battery was charged at a constant current and constant potential to 4.5 V at 0.1 C, discharged at a constant current to 2.5 V at 0.1 C, and then charged at a constant current and constant potential to 4.5 V at 0.1 C again. The battery was charged at a constant current and constant potential to 4.5 V at 0.1 C, and placed in a thermostatic chamber set at 60 ° C. and stored for 168 hours. After 168 hours, the battery was removed and returned to room temperature, then placed in an environmental tester set to 25 ° C. and discharged at a constant current of 0.1 C to 2.5 V. Thereafter, the battery was charged at a constant current and constant potential to 4.5 V at 0.1 C, and discharged at a constant current of 0.1 C to 2.5 V. After charging until the SOC was 50%, the resistance value after the storage test was measured by impedance measurement. The resistance value after the storage test was calculated relative to the resistance value before the storage test, and this value was taken as the resistance increase rate after storage at 60°C.
[0091] [Table 1]
[0092] As is clear from the results shown in FIG. 1, the active material obtained in Comparative Example 1 had a capacitance of 1290±50 cm -1 In contrast, no peak was observed in the range of 1290±50 cm for the active materials obtained in Examples 1 and 2. -1 A peak was observed in the range of 2, no peak was observed in the range of 134±0.45 eV in the active material obtained in Comparative Example 1. In contrast, peaks were observed in the range of 134±0.45 eV in the active materials obtained in Examples 1 and 2. Furthermore, as is clear from the results shown in Table 1, the solid-state batteries obtained using the active materials obtained in each Example showed a low resistance increase rate after storage at 60° C. This shows that the active materials obtained in each Example improve the storage characteristics of solid-state batteries.
Claims
1. An active material having a core particle and a coating portion disposed on a surface of the core particle, The coating portion includes a compound containing lithium (Li), phosphorus (P), and oxygen (O), The compound has a molar ratio of lithium (Li) element to phosphorus (P) element of 0.5 or more and 2.5 or less, and a molar ratio of oxygen (O) element to phosphorus (P) element of 2.5 or more and 3.5 or less, In the infrared absorption spectrum obtained by Fourier transform infrared spectroscopy (FT-IR), -1 The active material has a peak in the range of
2. 2. The active material of claim 1, having a peak in the range of 134±0.45 eV in a P2p spectrum measured by X-ray photoelectron spectroscopy.
3. The active material according to claim 1 , wherein the compound is contained in the coating portion at a ratio of 50 mass % or more.
4. 2. The active material according to claim 1, wherein the core particles contain at least one selected from the group consisting of a lithium transition metal composite oxide having a spinel structure, a lithium transition metal composite oxide having a layered rock salt structure, and a phosphate compound having an olivine structure.
5. The active material according to claim 1 , wherein the coating portion has a thickness of 1 nm or more and 100 nm or less.
6. 2. The active material according to claim 1, which has a moisture content of 1200 ppm or less at up to 250° C. as measured by the Karl Fischer method.
7. The active material according to claim 1 , wherein the coating portion contains lithium metaphosphate.
8. An electrode mixture comprising the active material according to claim 1 , a solid electrolyte, and a conductive material.
9. An electrode comprising the electrode mixture according to claim 8 and a binder.
10. A battery having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, A battery, wherein the positive electrode layer comprises the active material according to claim 1 .
11. A method for producing an active material, comprising dry-mixing a mixture containing core particles and a compound containing lithium (Li), phosphorus (P) and oxygen (O) while cooling, and disposing a coating portion containing the compound on the surface of the core particles.
Citation Information
Patent Citations
Method for producing composite active material
JP2021099918A
Positive electrode active material for lithium secondary batteries, positive electrode for lithium secondary batteries, lithium secondary battery, method for producing positive electrode active material for lithium secondary batteries, and method for manufacturing lithium secondary battery
WO2017094416A1
Active material, positive electrode mixture using same, and solid-state battery
WO2020175506A1
Cited By
Active material, method for producing same, electrode mixture, electrode, and battery
WO2025205689A1