Columnar honeycomb structure and method of producing the same

By integrating sintering aids into both partition walls and plugged portions of honeycomb filters, the mechanical strength and porosity gradient are stabilized, enhancing durability and filtration efficiency while reducing pressure loss.

JP2024143861AActive Publication Date: 2024-10-11NGK CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023056776
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Honeycomb filters with cordierite as the main component and ceria as a sintering aid face issues with mechanical strength due to the movement of sintering aids from the partition walls to the plugged parts, leading to increased porosity and potential damage during use.

Method used

Incorporating sintering aids like ceria, zirconia, and titania into both the partition walls and plugged portions of the honeycomb structure, while maintaining a specific porosity gradient and pore size distribution, to stabilize the structure and enhance mechanical strength.

Benefits of technology

The approach stabilizes the mechanical strength of the honeycomb structure, allowing for higher porosity without compromising durability, and achieves a sharper pore size distribution for improved filtration efficiency and reduced pressure loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143861000001_ABST
    Figure 2024143861000001_ABST
Patent Text Reader

Abstract

To suppress deterioration of mechanical strength of a columnar honeycomb structure containing a sintering aid and cordierite as a main component.SOLUTION: Provided is a columnar honeycomb structure that has a first cell and a second cell alternately arranged adjacent to each other with a partition wall therebetween, and sealing portions. The structure contains cordierite as a main component and one or more of sintering aids selected from ceria, zirconia, and titania, wherein when an average porosity of a portion in a range B from the deepest portion of the sealing portion of the first bottom face in the extending direction of the second cells to the first bottom face in a region of the partition wall in a range A from the deepest portion of the sealing portion of a second bottom face in an extending direction of the first cell to the second bottom face is defined as P1 (%), and when an average porosity of a portion of the partition wall in a range C from the deepest portion of the sealing portion of the second bottom face in the extending direction of the first cell to the deepest portion of the sealing portion of the first bottom face in the extending direction of the second cell is P2 (%), the relationship -4≤P1-P2≤7 is satisfied.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pillar-shaped honeycomb structure and a manufacturing method thereof. [Background technology]

[0002] Exhaust gas emitted from internal combustion engines such as diesel engines contains a large amount of particulate matter (particulate matter) whose main component is carbon, which causes environmental pollution. For this reason, the exhaust systems of diesel engines and other engines are generally equipped with a filter (Diesel Particulate Filter: DPF) to capture particulate matter. In recent years, particulate matter emitted from gasoline engines has also become a problem, and gasoline engines are now also being equipped with a filter (Gasoline Particulate Filter: GPF).

[0003] As a filter, a wall-flow type columnar honeycomb structure is known which has an outer peripheral sidewall, a plurality of first cells arranged on the inner peripheral sidewall, extending from a first bottom surface to a second bottom surface, having an open first bottom surface and a plugged portion on the second bottom surface, and a plurality of second cells arranged on the inner peripheral sidewall, extending from the first bottom surface to the second bottom surface, having a plugged portion on the first bottom surface and having an open second bottom surface, and which are alternately arranged adjacent to each other with partition walls between them.

[0004] Patent Document 1 describes an invention that aims to provide a honeycomb filter that can suppress an increase in pressure loss, has a large maximum soot deposition amount, and achieves high durability. The honeycomb filter comprises a cylindrical honeycomb structure having porous partition walls that partition and form a plurality of cells extending from one end face to the other end face, which serve as fluid flow paths, and plugging portions disposed at one open end of a given one of the cells and at the other open end of the remaining one of the cells, the porosity of the partition walls being 46% or less, and the permeability of the honeycomb structure being 0.8 μm 2or more, the pore volume ratio of pores having a pore diameter of 40 μm or more is 7.5% or less, and the pore volume ratio of pores having a pore diameter of 10 μm or less is 25% or less, and the thermal expansion coefficient of the honeycomb structure at 40° C. to 800° C. is 1.0×10 -6 / ℃ or less.

[0005] In addition, Patent Document 1 describes a method in which the partition walls are made of a porous body containing cordierite as a main component, It is described that the partition walls contain at least one selected from the group consisting of cerium oxide, zirconium oxide, and yttrium oxide, the cerium oxide content being 3.0 mass% or less, the zirconium oxide content being 2.5 mass% or less, and the yttrium oxide content being 2.0 mass% or less. Patent Document 1 describes that by configuring in this way, it is possible to suppress the formation of pores that are not related to gas permeability, and to manufacture a honeycomb structure with low porosity while maintaining permeability. It is also described that when the porosity of the honeycomb structure is reduced, the heat capacity of the honeycomb filter increases, and therefore the durability of the honeycomb filter is increased, and the maximum soot deposition amount can be improved. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2013 / 047908 Summary of the Invention [Problem to be solved by the invention]

[0007] As described in Patent Document 1, in a honeycomb filter mainly composed of cordierite, adding a small amount of ceria (cerium oxide) or the like is advantageous in suppressing the formation of pores that are not related to gas permeability and in producing a honeycomb structure with low porosity while maintaining permeability. However, since the plugging portions of the honeycomb filter described in Patent Document 1 are not fired, the strength is not sufficient and the plugging portions are easily damaged by ash or the like during use. Furthermore, there is a risk that the plugging portions will fall off if strong pressure is applied.

[0008] On the other hand, it was found that a honeycomb filter containing cordierite as a main component and containing sintering aids such as cerium oxide, even if the plugged portions are fired, has a problem in that sufficient mechanical strength cannot be obtained. For this reason, it has been difficult to adopt a high porosity in a honeycomb filter containing sintering aids such as cerium oxide.

[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to suppress a decrease in the mechanical strength of a columnar honeycomb structure containing a sintering aid and having cordierite as a main component, in one embodiment. Also, an object of the present invention is to provide a method for manufacturing a columnar honeycomb structure having improved mechanical strength, in another embodiment. [Means for solving the problem]

[0010] The inventors of the present invention conducted intensive research to solve the above problems and found that the porosity of the partition walls near the plugging parts increases locally due to the migration of sintering aid from the partition walls to the plugging parts during firing, resulting in a decrease in strength. The sintering aid gathers on the small pore side by capillary action and plugs the small pores, but at the same time, it also migrates to the plugging material. In addition, since the sintering aid has the effect of plugging the pores, a larger amount of pore-forming material is used than usual to maintain the porosity, and it was also found that the partition walls in the parts where the sintering aid was removed have a higher porosity.

[0011] As a result of discovering such a phenomenon, the present inventor came to believe that suppressing the migration of the sintering aid from the partition walls to the plugging portions and suppressing an increase in the porosity of the partition walls near the plugging portions would lead to suppressing a decrease in mechanical strength, and discovered that adding a sintering aid to the plugging portions as well is effective. The present invention was completed based on this finding, and is exemplified below.

[0012] [Aspect 1] A columnar honeycomb structure comprising an outer peripheral side wall, a plurality of first cells arranged on the inner peripheral side of the outer peripheral side wall, extending from a first bottom surface to a second bottom surface, having openings on the first bottom surface and having plugging portions on the second bottom surface, and a plurality of second cells arranged on the inner peripheral side of the outer peripheral side wall, extending from the first bottom surface to the second bottom surface, having plugging portions on the first bottom surface and having openings on the second bottom surface, wherein the plurality of first cells and the plurality of second cells are alternately arranged adjacent to each other with partition walls interposed therebetween, the outer peripheral side wall, the partition walls, and the plugging portions are fired and contain cordierite as a main component and one or more sintering aids selected from ceria, zirconia, and titania; In the partition wall, an average porosity of a portion in a range A from the deepest portion of the plugging portion of the second bottom surface in the extension direction of the first cells to the second bottom surface and an average porosity of a portion in a range B from the deepest portion of the plugging portion of the first bottom surface in the extension direction of the second cells to the first bottom surface are defined as P1 (%), When the average porosity of a portion of the partition wall in a range C from the deepest portion of the plugging portion of the second bottom surface in the extension direction of the first cells to the deepest portion of the plugging portion of the first bottom surface in the extension direction of the second cells is P2 (%), -4≦P1-P2≦7 is satisfied; Columnar honeycomb structure. [Aspect 2] 2. The pillar-shaped honeycomb structure according to embodiment 1, wherein P1-P2 satisfies −2≦P1−P2≦5. [Aspect 3] 3. The pillar-shaped honeycomb structure according to embodiment 1 or 2, wherein 55≦P2≦70 is satisfied. [Aspect 4] A columnar honeycomb structure according to any one of aspects 1 to 3, wherein the average total content of one or more sintering aids selected from ceria, zirconia, and titania in the portions of the partition walls in the range A and the portions of the partition walls in the range B is S1 (%), the average total content of one or more sintering aids selected from ceria, zirconia, and titania in the portions of the partition walls in the range C is S2 (%), and the cumulative 50% pore size of the partition walls in the volume-based cumulative pore size distribution measured by mercury intrusion porosimetry is D50 (μm), satisfying (S2-S1) / D50×100≦6. [Aspect 5] A columnar honeycomb structure according to any one of aspects 1 to 4, wherein the partition walls in the region C have a cumulative pore size distribution on a volume basis measured by mercury intrusion porosimetry, in which the cumulative 10% pore size (D10), cumulative 50% pore size (D50) and cumulative 90% pore size (D90) from the small pore side satisfy the relationship (D90-D10) / D50≦1.2. [Aspect 6] A method for manufacturing a columnar honeycomb structure comprising: an outer peripheral side wall; a plurality of first cells arranged on an inner peripheral side of the outer peripheral side wall, extending from a first bottom surface to a second bottom surface, having openings on the first bottom surface and having plugging portions on the second bottom surface; and a plurality of second cells arranged on the inner peripheral side of the outer peripheral side wall, extending from the first bottom surface to the second bottom surface, having plugging portions on the first bottom surface and having openings on the second bottom surface, wherein the plurality of first cells and the plurality of second cells are arranged adjacent to each other alternately with partition walls interposed therebetween, a step of kneading a raw material composition containing a cordierite raw material, a dispersion medium, a pore-forming material, a binder, and one or more sintering aids selected from ceria, zirconia, and titania to form a puddle, and then extruding the puddle to obtain a columnar honeycomb formed body having an outer peripheral side wall and a first bottom surface and a second bottom surface, the first bottom surface and the second bottom surface both having openings; a step of filling a plugging portion forming slurry containing a cordierite raw material, a dispersion medium, a pore former, a binder, and one or more sintering aids selected from ceria, zirconia, and titania into openings of the first bottom surface and the second bottom surface where the plugging portions are to be formed after drying the columnar honeycomb formed body; A step of firing the columnar honeycomb formed body filled with the plugging portion forming slurry; Including, Regarding the sintering aid in the raw material composition, the total amount added with respect to 100 parts by mass of the cordierite-forming raw material is C1 parts by mass, and regarding the sintering aid in the slurry for forming plugging portions, the total amount added with respect to 100 parts by mass of the cordierite-forming raw material is C2 parts by mass, and thus -8≦C1−C2≦1 is satisfied. Manufacturing method. [Aspect 7] The method according to embodiment 6, wherein −6≦C1−C2≦0 is satisfied. [Aspect 8] The method according to aspect 6 or 7, wherein 1≦C2≦10 is satisfied. [Aspect 9] The manufacturing method according to any one of aspects 6 to 8, wherein the sintering aid in the raw material composition and the sintering aid in the slurry for forming plugging portions have a median diameter (D50) of 0.1 to 10 μm in a volume-based cumulative particle size distribution determined by a laser diffraction / scattering method. Effect of the Invention

[0013] According to one embodiment of the present invention, it is possible to suppress the decrease in mechanical strength of a columnar honeycomb structure mainly composed of cordierite by containing a sintering aid such as ceria. As a result, even if the porosity of the partition walls is increased to achieve even lower pressure loss, it is possible to ensure the mechanical strength required for the product. In addition, the addition of a sintering aid such as ceria sharpens the pore size distribution, in other words, it is possible to obtain pores with a highly uniform pore size. A sharp pore size distribution is considered to be advantageous in improving the balance between low pressure loss and collection performance. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a perspective view showing a typical wall-flow type columnar honeycomb structure. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a wall-flow type columnar honeycomb structure observed from a cross section parallel to the cell extension direction. [Diagram 3] 1 is an example of a profile of porosity when the porosity (%) is measured along the thickness direction D of the partition walls from one surface to the other surface. [Figure 4] 11 is a conceptual diagram illustrating a method for identifying the position of one surface of a partition on a cross-sectional image. FIG. [Diagram 5] FIG. 4 is a schematic partial enlarged view of the vicinity of plugging portions when a partition wall of a pillar-shaped honeycomb structure is observed in a cross section parallel to the cell extension direction. [Figure 6] FIG. 3 is a schematic partial enlarged view of a partition wall of a pillar-shaped honeycomb structure observed in a cross section perpendicular to the cell extension direction. [Figure 7] FIG. 1 is an explanatory diagram illustrating an example of a method for forming plugging portions by a squeegee method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Next, an embodiment of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiment, and that appropriate changes and improvements in the design may be made based on the ordinary knowledge of a person skilled in the art without departing from the spirit of the present invention.

[0016] (1. Pillar-shaped honeycomb structure) 1 and 2 are schematic perspective and cross-sectional views of a columnar honeycomb structure 100 applicable as a wall-flow type exhaust gas filter and / or catalyst carrier for automobiles. The columnar honeycomb structure 100 includes an outer peripheral side wall 102, a plurality of first cells 108 arranged on the inner peripheral side of the outer peripheral side wall 102, extending in parallel from a first bottom surface 104 to a second bottom surface 106, the first bottom surface 104 being open and having plugging portions 109 on the second bottom surface 106, and a plurality of second cells 110 arranged on the inner peripheral side of the outer peripheral side wall 102, extending in parallel from the first bottom surface 104 to the second bottom surface 106, having plugging portions 109 on the first bottom surface 104, and having an open second bottom surface 106. In the columnar honeycomb structure 100, the first cells 108 and the second cells 110 are arranged alternately adjacent to each other with partition walls 112 interposed therebetween.

[0017] For example, when exhaust gas containing particulate matter such as soot is supplied to the first bottom surface 104 on the upstream side of the columnar honeycomb structure 100, the exhaust gas is introduced into the first cells 108 and proceeds downstream within the first cells 108. Since the second bottom surface 106 on the downstream side of the first cells 108 is plugged, the exhaust gas passes through the porous partition walls 112 that separate the first cells 108 and the second cells 110 and flows into the second cells 110. Since the particulate matter cannot pass through the partition walls 112, it is collected and deposited within the first cells 108. After the particulate matter is removed, the clean exhaust gas that has flowed into the second cells 110 proceeds downstream within the second cells 110 and flows out from the second bottom surface 106 on the downstream side.

[0018] The bottom shape of the columnar honeycomb structure 100 is not limited, and may be, for example, a circular shape, an elliptical shape, a racetrack shape, an oval shape, or other round shape, a triangular shape, a rectangular shape, or other polygonal shape, or other irregular shape. The illustrated columnar honeycomb structure 100 has a circular bottom shape and is cylindrical as a whole.

[0019] The height of the columnar honeycomb structure (the length from the first bottom surface to the second bottom surface) is not particularly limited, and may be appropriately set depending on the application and required performance. The height of the columnar honeycomb structure may be, for example, 40 mm to 450 mm. There is also no particular limit to the relationship between the height of the columnar honeycomb structure and the maximum diameter of each bottom surface (referring to the maximum length of the diameters passing through the center of gravity of each bottom surface of the columnar honeycomb structure). Therefore, the height of the columnar honeycomb structure may be longer than the maximum diameter of each bottom surface, or the height of the columnar honeycomb structure may be shorter than the maximum diameter of each bottom surface.

[0020] The outer peripheral side wall, partition walls and plugging portions of the columnar honeycomb structure are fired and each contains cordierite as a main component. This means that the total mass ratio of cordierite (2MgO·2Al2O3·5SiO2) in 100% by mass of the material constituting each of the outer peripheral side wall, partition walls and plugging portions is 50% by mass or more. The mass ratio of cordierite in 100% by mass of the material constituting each of the outer peripheral side wall, partition walls and plugging portions is preferably 70% by mass or more, more preferably 80% by mass or more. The mass ratio of cordierite is measured by X-ray diffraction (XRD).

[0021] From the viewpoint of making the pore size distribution sharp, the outer peripheral side wall and the partition wall of the columnar honeycomb structure each preferably contain one or more sintering aids selected from ceria, zirconia, and titania, and more preferably contain at least ceria. Also, from the viewpoint of suppressing a decrease in mechanical strength, the plugged portion of the columnar honeycomb structure preferably contains one or more sintering aids selected from ceria, zirconia, and titania, and more preferably contains at least ceria.

[0022] When the partition walls contain one or more sintering aids selected from ceria, zirconia, and titania, it is desirable to have a small difference between the porosity (%) in the vicinity of the plugged portions of the partition walls and the porosity (%) at the locations away from the plugged portions of the partition walls in order to suppress the decrease in mechanical strength of the columnar honeycomb structure. Specifically, it is preferable to satisfy P1-P2≦7, more preferably to satisfy P1-P2≦5, and even more preferably to satisfy P1-P2≦4. By setting the upper limit of P1-P2 to 7 or less, the advantage of suppressing the decrease in mechanical strength of the columnar honeycomb structure is obtained. However, even if P1-P2 is made too small, the adverse effect of a decrease in mechanical strength of the honeycomb structure due to the difference in rigidity may occur, so it is preferable to satisfy -4≦P1-P2, more preferably to satisfy -2≦P1-P2, and even more preferably to satisfy 0≦P1-P2. Therefore, for example, it is preferable that −4≦P1−P2≦7 is satisfied, it is more preferable that −2≦P1−P2≦5 is satisfied, and it is even more preferable that 0≦P1−P2≦3 is satisfied.

[0023] P1 indicates the average porosity (%) of a portion of the partition 112 in a range A from the deepest portion of the plugging portion 109 of the second bottom surface 106 in the extension direction of the first cell 108 to the second bottom surface 106, and a portion of a range B from the deepest portion of the plugging portion 109 of the first bottom surface 104 in the extension direction of the second cell 110 to the first bottom surface 104. P2 indicates the average porosity (%) of a portion of the partition wall 112 in a range C from the deepest portion of the plugging portion 109 of the second bottom surface 106 in the extension direction of the first cell 108 to the deepest portion of the plugging portion 109 of the first bottom surface 104 in the extension direction of the second cell 110.

[0024] From the viewpoint of realizing low pressure loss, P2 preferably satisfies 55≦P2, more preferably satisfies 57≦P2, and even more preferably satisfies 59≦P2. From the viewpoint of ensuring mechanical strength, P2 preferably satisfies P2≦70, more preferably satisfies P2≦68, and even more preferably satisfies P2≦66. Thus, for example, it is preferable to satisfy 55≦P2≦70, more preferably satisfies 57≦P2≦68, and even more preferably satisfies 59≦P2≦66.

[0025] P1 and P2 are measured in the following procedure. First, the measurement procedure for P2 will be described. Three partition wall samples (cross-sectional size (length 20 mm × width 2 mm) × depth 0.3 mm) with a cross section parallel to the cell extension direction exposed are taken without bias from the partition wall part in the above-mentioned range C. Next, the cross section of each sample is observed by an X-ray microscope and CT scanned, and then the obtained three-dimensional cross-sectional image is binarized based on the brightness and divided into a number of voxels (size of one voxel = length in the wall surface direction of the partition wall (Y direction): 0.8 μm, length in the thickness direction of the partition wall (X direction): 0.8 μm, length in the depth direction of the partition wall (Z direction): 0.8 μm cube) of the space part and the solid part. The measurement conditions for the X-ray microscope were a magnification of 4x. The binarization process is carried out using Otsu's binarization method.

[0026] Next, for a given region of any one of the partitions on the three-dimensional cross-sectional image (length in the wall direction (Y direction) of the partition: 340 μm, length in the thickness direction (X direction) of the partition: length including the entire thickness and having space portions of 50 μm or more on both sides of the partition, length in the depth direction (Z direction) of the partition: 300 μm), a profile of porosity (%) is obtained at 0.8 μm intervals along the thickness direction (X direction) of the partition from one surface to the other surface based on the binarized voxel data (see FIG. 3). The porosity of a thickness of 0.8 μm is calculated according to the formula of porosity=(number of voxels in the space portion) / (total number of voxels in the region)×100(%) for a thickness region of 0.8 μm (length in the wall direction (Y direction) of the partition: 340 μm, length in the thickness direction (X direction) of the partition: 0.8 μm, length in the depth direction (Z direction) of the partition: 300 μm). By performing this calculation for the entire predetermined region at 0.8 μm intervals from the left end of the screen, a profile of the porosity (%) at 0.8 μm intervals along the thickness direction (X direction) of the partition wall from one surface to the other surface can be obtained.

[0027] In this case, the position of one surface of the partition wall is determined as the most frequent position when measuring the distance M in the thickness direction D (X direction) from a line segment parallel to the wall surface direction of the partition wall to one surface of the partition wall to be measured, as shown in Fig. 4. The distance M is measured at 0.8 µm intervals over a length of 340 µm in the wall surface direction of the partition wall (Y direction perpendicular to the thickness direction (X direction)) on the binarized image. The position of the other surface of the partition wall is identified in the same manner.

[0028] In this manner, a profile of the porosity of any one partition wall is obtained from each sample, and the average porosity of the partition wall is calculated from the profile. Then, the average value of the total of three partition wall samples in the above range C is defined as the average porosity P2 (%).

[0029] Next, the measurement procedure for P1 will be described. Three partition samples (cross-sectional size (length 20 mm × width 2 mm) × depth 0.3 mm) with cross sections parallel to the cell extension direction are taken from the partition parts in the above-mentioned ranges A and B without bias, for a total of six samples. Next, in the same manner as in the measurement of P2, the cross sections of each sample are observed with an X-ray microscope and CT scanned, and the obtained three-dimensional cross-sectional images are then binarized based on brightness to separate them into a large number of voxels for spatial and solid parts.

[0030] Next, for a predetermined region of any one of the partition walls on the three-dimensional cross-sectional image (length in the wall surface direction (Y direction) of the partition wall: 340 μm, length in the thickness direction (X direction) of the partition wall: length including the entire thickness and having space portions of 50 μm or more on both sides of the partition wall, length in the depth direction (Z direction) of the partition wall: 300 μm), a profile of porosity (%) at 0.8 μm intervals along the thickness direction (X direction) of the partition wall from one surface to the other surface is obtained based on the binarized voxel data in the same manner as in the measurement of P2. However, in the partition walls in the above ranges A and B, one surface 112a is adjacent to the cell space, while the other surface 112b is adjacent to the plugged portion 109. It is difficult to identify the boundary between the plugged portion 109 and the partition wall 112. Therefore, the position of the partition wall surface 112c in the range C where the plugging portions 109 on the other surface 112b of the partition wall 112 are not adjacent is identified by the above-mentioned method, and a straight line L is drawn along the surface 112c to define the boundary with the plugging portions. Fig. 5 shows a schematic partial enlarged view of the vicinity of the plugging portions when the partition walls of the columnar honeycomb structure are observed at a cross section parallel to the cell extension direction.

[0031] In this manner, a profile of the porosity of any one partition wall is obtained from each sample, and the average porosity of the partition wall is calculated from the profile. Then, the average value of a total of six partition wall samples in the above ranges A and B is defined as the average porosity P1 (%).

[0032] In a columnar honeycomb structure containing cordierite as a main component and the above-mentioned sintering aid, in order to suppress a decrease in mechanical strength, it is advantageous to suppress the migration of the sintering aid from the partition walls to the plugging portions and suppress a local decrease in porosity in the vicinity of the plugging portions of the partition walls. The migration of the sintering aid is considered to be caused by the concentration difference of the sintering aid between the plugging portions and the partition walls, and can be suppressed by adding the same amount of sintering aid to the plugging portions as the partition walls, preferably more than the partition walls. This concentration difference is preferably set appropriately according to the cumulative 50% pore size (D50) of the partition walls described later.

[0033] Specifically, the average value S1 (%) of the total content of one or more sintering aids selected from ceria, zirconia, and titania in the vicinity of the plugged portions of the partition walls, the average value S2 (%) of the total content of the sintering aids in the locations away from the plugged portions of the partition walls, and the cumulative 50% pore size (D50) (μm) of the partition walls preferably satisfy the following relationship. Specifically, it is preferable to satisfy (S2-S1) / D50×100≦6, more preferably to satisfy (S2-S1) / D50×100≦4, and even more preferably to satisfy (S2-S1) / D50×100≦2. By setting the upper limit of (S2-S1) / D50×100 to 6 or less, an advantage is obtained in that the decrease in mechanical strength of the columnar honeycomb structure is suppressed. Although the lower limit of (S2-S1) / D50×100 is not particularly set, if it is made too small, the effect of suppressing the decrease in mechanical strength is saturated, while considering the range of S2 shown below, it is common to satisfy -6≦(S2-S1) / D50×100, typically to satisfy -4≦(S2-S1) / D50×100, and more typically to satisfy -2≦(S2-S1) / D50×100. Therefore, for example, it is preferable to satisfy -6≦(S2-S1) / D50×100≦6, more preferably to satisfy -4≦(S2-S1) / D50×100≦4, and even more preferably to satisfy -2≦(S2-S1) / D50×100≦2.

[0034] S1 refers to the average value (%) of the total content of one or more sintering aids selected from ceria, zirconia, and titania in a portion of the partition 112 in a range A from the deepest portion of the plugging portion 109 of the second bottom surface 106 in the extension direction of the first cell 108 to the second bottom surface 106, and in a portion of the partition 112 in a range B from the deepest portion of the plugging portion 109 of the first bottom surface 104 in the extension direction of the second cell 110 to the first bottom surface 104. S2 indicates the average value (%) of the total content of one or more sintering aids selected from ceria, zirconia, and titania in a region C of the partition wall 112 from the deepest part of the plugging portion 109 of the second bottom surface 106 in the extension direction of the first cell 108 to the deepest part of the plugging portion 109 of the first bottom surface 104 in the extension direction of the second cell 110.

[0035] From the viewpoint of making the pore size distribution sharp, it is preferable that S2 be 1≦S2, it is more preferable that S2 be 2≦S2, and it is even more preferable that S2 be 3≦S2. Moreover, from the viewpoint of suppressing a decrease in the melting point of the partition walls, it is preferable that S2 be 10, it is more preferable that S2 be 8, and it is even more preferable that S2 be 6. Therefore, for example, it is preferable that S2 be 1≦S2≦10, it is more preferable that S2 be 8≦2, and it is even more preferable that S2 be 6≦S2.

[0036] In addition, from the viewpoint of suppressing the movement of the sintering aid from the partition walls to the plugged portions, the plugged portions of the columnar honeycomb structure preferably contain one or more sintering aids selected from ceria, zirconia, and titania, and more preferably contain at least ceria. If the average value of the total content of one or more sintering aids selected from ceria, zirconia, and titania in the plugged portions is S3 (%), from the viewpoint of suppressing the movement of the sintering aid from the partition walls to the plugged portions, it is preferable that S3 is 1≦S3, more preferably that S3 is 2≦S3, and even more preferably that S3 is 3≦S3. In addition, from the viewpoint of suppressing the melting point of the plugged portions from decreasing, it is preferable that S3 is 10, more preferably that S3 is 8, and even more preferably that S3 is 6. Therefore, for example, it is preferable that S3 is 1≦S3≦10, more preferably that S3 is 8, and even more preferably that S3 is 6.

[0037] The total content of sintering aids is measured by an energy dispersive X-ray analyzer (EDS) attached to a scanning electron microscope (SEM). Specifically, a sample (size: 15mm x 15mm x 15mm) in which a cross section parallel to the cell extension direction is exposed is taken from the measurement points of the outer peripheral side wall, partition wall, and plugging part, and the cross section is mirror-polished using diamond slurry to obtain an observation sample. This polished surface is observed (size of one field of view: 700μm x 700μm) and elementally mapped by SEM-EDS analysis at 200x magnification. The area of ​​the solid part excluding the space part on the SEM image is taken as 100%, and the area occupied by Ce is obtained by image analysis, which is regarded as the ceria content. Similarly, the area of ​​the solid part excluding the space part on the SEM image is taken as 100%, and the area occupied by Zr is obtained by image analysis, which is regarded as the zirconia content. The area of ​​the solid part on the screen excluding voids is taken as 100%, and the area occupied by Ti is determined by image analysis, which is regarded as the titania content.

[0038] The measurement method of S1 will be described. Using the method described above, two samples of the partition walls in which cross sections parallel to the cell extension direction are exposed are taken from each of the partition wall portions in the above-mentioned range A and range B without bias, for a total of four samples, and observation samples are prepared for each. Each observation sample is subjected to element mapping by the above-mentioned SEM-EDS analysis to determine the total content of one or more sintering aids selected from ceria, zirconia, and titania. The average value of the total content in all observation samples is taken as S1 (%).

[0039] The measurement method of S2 will be described. Using the method described above, two samples of the partition walls in which a cross section parallel to the cell extension direction is exposed are taken without bias from the partition wall portion in the above-mentioned range C, and observation specimens are prepared for each. Each observation specimen is subjected to element mapping by the above-mentioned SEM-EDS analysis to determine the total content of one or more sintering aids selected from ceria, zirconia, and titania. The average value of the total content in all the observation specimens is taken as S2 (%).

[0040] The measurement method of S3 will be explained. Using the method described above, two samples of the plugging portion where the cross section parallel to the cell extension direction is exposed are taken from the vicinity of the first bottom surface and the second bottom surface without bias, for a total of four samples, and observation samples are prepared for each. Each observation sample is subjected to element mapping by the SEM-EDS analysis described above, and the total content of one or more sintering aids selected from ceria, zirconia, and titania is obtained. The average value of the total content in all the observation samples is taken as S3 (%).

[0041] The average thickness of the partition walls in the columnar honeycomb structure is preferably 152 μm or more from the viewpoint of ensuring strength, more preferably 178 μm or more, and even more preferably 203 μm or more. In addition, the average thickness of the partition walls is preferably 305 μm or less, more preferably 279 μm or less, and even more preferably 254 μm or less from the viewpoint of suppressing pressure loss. FIG. 6 shows a schematic partial enlarged view of the partition walls 112 of the columnar honeycomb structure 100 observed in a cross section perpendicular to the cell extension direction. The thickness of the partition walls refers to the length of the line segment N that crosses the partition walls when the line segment N connects the centers of gravity O of adjacent cells in a cross section perpendicular to the cell extension direction (height direction of the columnar honeycomb structure). The thickness direction D of the partition walls refers to the direction parallel to the line segment N. The average thickness of the partition walls refers to the average value of the thicknesses of all the partition walls.

[0042] In one embodiment, the plugging portions of both the first bottom face and the second bottom face have an average depth of 2 to 8 mm. When the average depth of the plugging portions is 2 mm or more, the strength of the plugging portions can be ensured. The average depth of the plugging portions is preferably 3 mm or more. Furthermore, when the average depth of the plugging portions is 8 mm or less, the area of ​​the partition walls that capture particulate matter in the cells can be prevented from becoming small. The average depth of the plugging portions is preferably 7 mm or less. The depth of the plugging portions in the cell extension direction is measured at any 20 points on each bottom face, and the average value is taken as the average depth of the plugging portions on each bottom face.

[0043] There is no particular restriction on the cell density (the number of cells per unit cross-sectional area) of the columnar honeycomb structure, and it is, for example, 6 to 2000 cells / square inch (0.9 to 311 cells / cm 2 ), more preferably 50 to 1000 cells / in2 (7.8 to 155 cells / cm2). 2 ), and particularly preferably 100 to 600 cells / square inch (15.5 to 92.0 cells / cm 2 Here, the cell density is calculated by dividing the total number of cells (including plugged cells) by one of the bottom areas excluding the outer peripheral side wall of the pillar-shaped honeycomb structure.

[0044] It is desirable for the partition walls to have a sharp pore size distribution in order to balance low pressure loss and collection performance. Specifically, in the partition walls, particularly in the portion of the partition walls in range C, in the cumulative pore size distribution on a volume basis measured by mercury intrusion porosimetry, the cumulative 10% pore size (D10), cumulative 50% pore size (D50), and cumulative 90% pore size (D90) from the small pore side preferably satisfy the relationship (D90-D10) / D50≦1.2, more preferably satisfy the relationship (D90-D10) / D50≦1.1, and even more preferably satisfy the relationship (D90-D10) / D50≦1.0. Although the lower limit of (D90-D10) / D50 is 0, it is normal to satisfy 0.5≦(D90-D10) / D50 from the viewpoint of ease of production.

[0045] In this specification, D10, D50 and D90 of the partition walls are measured by the mercury intrusion method defined in JIS R1655:2003 using a mercury porosimeter. Mercury intrusion is a method in which a sample is immersed in mercury under vacuum and a uniform pressure is applied, mercury is forced into the sample while gradually increasing the pressure, and the pore size distribution is calculated from the pressure and the volume of mercury forced into the pores. When the pressure is gradually increased, mercury is forced into the pores starting from the larger diameter pores, and the cumulative volume of mercury increases, and when all the pores are finally filled with mercury, the cumulative volume reaches an equilibrium amount. The cumulative volume at this time is the total pore volume (cm 3 / g). The pore diameter at the time when 10% of the total pore volume of mercury is injected from the small pore side is the cumulative 10% pore diameter (D10), the pore diameter at the time when 50% of the total pore volume of mercury is injected from the small pore side is the cumulative 50% pore diameter (D50), and the pore diameter at the time when 90% of the total pore volume of mercury is injected from the small pore side is the cumulative 90% pore diameter (D90).

[0046] Six samples (0.3 g) were taken from the partition walls without bias from the above-mentioned area C of the columnar honeycomb structure, including the center and outer periphery in the radial direction, and the pore size distribution of each was measured to determine D10, D50 and D90, and the average value was taken as the measured value.

[0047] It is desirable to set the D50 of the partition walls to an appropriate range depending on the application. For example, when a columnar honeycomb structure is used for a filter, the D50 of the partition walls, particularly the portion of the partition walls in range C, is preferably 28 μm or less, more preferably 26 μm or less, and even more preferably 24 μm or less. When the D50 of the partition walls is in the above range, the particulate matter collection efficiency is significantly improved. In addition, the D50 of the partition walls is preferably 5 μm or more, more preferably 6 μm or more, and even more preferably 7 μm or more. When the D50 of the partition walls is in the above range, an increase in pressure loss can be suppressed.

[0048] One measure of the mechanical strength of a columnar honeycomb structure is the isostatic fracture strength. In measuring the isostatic fracture strength of a columnar honeycomb structure, a test is conducted in which the columnar honeycomb structure is submerged in water in a pressure vessel, and the water pressure is gradually increased to apply isotropic pressure to the columnar honeycomb structure. As the water pressure in the pressure vessel gradually increases, destruction eventually occurs in the partition walls and outer peripheral side walls of the columnar honeycomb structure. The value of the pressure (fracture strength) at which destruction occurs is the isostatic fracture strength. Isostatic fracture strength is measured based on the automobile standard (JASO M505-87) issued by the Automotive Engineering Society of Japan.

[0049] In applying the columnar honeycomb structure as an exhaust gas filter and / or a catalyst carrier for an automobile, the lower limit of the isostatic fracture strength is preferably 0.5 MPa or more, more preferably 1.0 MPa or more, and even more preferably 1.5 MPa or more. The upper limit of the isostatic fracture strength is not particularly set, but is usually 3.0 MPa or less, and typically 2.5 MPa or less.

[0050] When the columnar honeycomb structure is used as a catalyst carrier, the surface of the partition wall can be coated with a catalyst according to the purpose. Examples of the catalyst include, but are not limited to, an oxidation catalyst (DOC) for increasing the exhaust gas temperature by oxidizing and burning hydrocarbons (HC) and carbon monoxide (CO), a PM combustion catalyst for assisting the combustion of PM such as soot, an SCR catalyst and an NSR catalyst for removing nitrogen oxides (NOx), and a three-way catalyst capable of simultaneously removing hydrocarbons (HC), carbon monoxide (CO), and nitrogen oxides (NOx). The catalyst can appropriately contain, for example, precious metals (Pt, Pd, Rh, etc.), alkali metals (Li, Na, K, Cs, etc.), alkaline earth metals (Mg, Ca, Ba, Sr, etc.), rare earths (Ce, Sm, Gd, Nd, Y, La, Pr, etc.), transition metals (Mn, Fe, Co, Ni, Cu, Zn, Sc, Ti, Zr, V, Cr, etc.), etc.

[0051] (2. Manufacturing method) A method for manufacturing a columnar honeycomb structure according to an embodiment of the present invention will be described below by way of example. First, a raw material composition containing one or more sintering aids selected from ceria, zirconia, and titania in addition to a cordierite raw material, a dispersion medium, a pore former, and a binder is kneaded to form a clay, and then the clay is extruded to obtain a columnar honeycomb molded body having an outer peripheral side wall and an inner peripheral side of the outer peripheral side wall, extending from a first bottom surface to a second bottom surface, and both the first bottom surface and the second bottom surface having openings. Additives such as a dispersant and other ceramic raw materials may be mixed into the raw material composition as necessary. In the extrusion molding, a die having a desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used.

[0052] The cordierite-forming raw material is a raw material that becomes cordierite by firing, and can be provided, for example, in the form of a powder. The cordierite-forming raw material preferably has a chemical composition of 30 to 45 mass% alumina (Al2O3) (including aluminum hydroxide converted to alumina), 11 to 17 mass% magnesia (MgO), and 42 to 57 mass% silica (SiO2).

[0053] From the viewpoint of making the pore size distribution sharp, the total amount of one or more sintering aids selected from ceria, zirconia, and titania added is preferably 2 parts by mass or more, more preferably 3 parts by mass or more, and even more preferably 4 parts by mass or more, relative to 100 parts by mass of the cordierite raw material. From the viewpoint of suppressing a decrease in the melting points of the outer peripheral side wall and the partition walls, the total amount of one or more sintering aids selected from ceria, zirconia, and titania added is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less, relative to 100 parts by mass of the cordierite raw material.

[0054] From the viewpoint of increasing the compositional uniformity in the partition walls and the outer peripheral side walls of the columnar honeycomb structure, the sintering aid added to the raw material composition has an upper limit of the median diameter (D50) in the cumulative particle size distribution on a volume basis determined by a laser diffraction / scattering method of 10 μm or less, more preferably 8 μm or less, and even more preferably 6 μm or less. From the viewpoint of the occurrence of internal defects due to aggregation, the sintering aid in the raw material composition has a lower limit of the median diameter (D50) in the cumulative particle size distribution on a volume basis determined by a laser diffraction / scattering method of 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. Therefore, for example, the median diameter (D50) of the sintering aid in the raw material composition is preferably 0.1 to 10 μm, more preferably 0.3 to 8 μm, and even more preferably 0.5 to 6 μm.

[0055] The dispersion medium may be water or a mixed solvent of water and an organic solvent such as alcohol, with water being particularly preferred.

[0056] The content of the dispersion medium in the columnar honeycomb molded body before the drying step is preferably 20 to 110 parts by mass, more preferably 25 to 100 parts by mass, and even more preferably 30 to 90 parts by mass, relative to 100 parts by mass of the cordierite-forming raw material. When the content of the dispersion medium in the columnar honeycomb molded body is 20 parts by mass or more relative to 100 parts by mass of the cordierite-forming raw material, the advantage that the quality of the columnar honeycomb structure is easily stabilized is easily obtained. When the content of the dispersion medium in the columnar honeycomb molded body is 90 parts by mass or less relative to 100 parts by mass of the cordierite-forming raw material, the shrinkage amount during drying is small, and deformation can be suppressed. In this specification, the content of the dispersion medium in the columnar honeycomb molded body refers to a value measured by a drying loss method.

[0057] The pore-forming material is not particularly limited as long as it becomes pores after firing, and examples thereof include wheat flour, starch, foamed resin, water-absorbent resin, silica gel, carbon (e.g., graphite), ceramic balloons, polyethylene, polystyrene, polypropylene, nylon, polyester, acrylic resin, and phenol. The pore-forming material may be used alone or in combination of two or more. The content of the pore-forming material is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, and even more preferably 9 parts by mass or more, relative to 100 parts by mass of the cordierite raw material, from the viewpoint of increasing the porosity of the columnar honeycomb structure after firing. The content of the pore-forming material is preferably 30 parts by mass or less, more preferably 27 parts by mass or less, and even more preferably 24 parts by mass or less, relative to 100 parts by mass of the cordierite raw material, from the viewpoint of ensuring the strength of the columnar honeycomb structure after firing.

[0058] Examples of the binder include organic binders such as methyl cellulose, hydroxypropoxyl methyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, carboxymethyl cellulose, and polyvinyl alcohol. The content of the binder is preferably 4 parts by mass or more, more preferably 4.5 parts by mass or more, and even more preferably 5 parts by mass or more, relative to 100 parts by mass of the cordierite raw material, from the viewpoint of increasing the strength of the columnar honeycomb molded body before firing. The content of the binder is preferably 9 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 7 parts by mass or less, relative to 100 parts by mass of the cordierite raw material, from the viewpoint of suppressing the occurrence of breakage due to abnormal heat generation in the firing process. The binder may be used alone or in combination of two or more types.

[0059] The dispersant may be ethylene glycol, dextrin, fatty acid soap, polyether polyol, etc. The dispersant may be used alone or in combination of two or more. The content of the dispersant is preferably 0 to 2 parts by mass with respect to 100 parts by mass of the cordierite-forming raw material.

[0060] The columnar honeycomb formed body can be dried using a conventionally known drying method such as hot air drying, microwave drying, dielectric drying, reduced pressure drying, vacuum drying, freeze drying, etc. Among these, a drying method that combines hot air drying with microwave drying or dielectric drying is preferred because it can quickly and uniformly dry the entire columnar honeycomb formed body.

[0061] After drying the columnar honeycomb formed body, plugging portions are formed on both bottom surfaces of the columnar honeycomb formed body. Each plugging portion can be formed by filling the openings of the first cell and the second cell where the plugging portions are to be formed with a plugging portion forming slurry, and then drying and firing the filled slurry. The plugging portion forming slurry can contain one or more sintering aids selected from ceria, zirconia, and titania in addition to the cordierite-forming raw material, dispersion medium, pore-forming material, and binder.

[0062] For example, the plugging portion forming slurry contains 30 to 60 parts by mass of a dispersion medium, 5 to 20 parts by mass of a pore-forming material, and 0.2 to 2.0 parts by mass of a binder with respect to 100 parts by mass of a cordierite-forming raw material. In a preferred embodiment, the plugging portion forming slurry contains 35 to 50 parts by mass of a dispersion medium, 8 to 16 parts by mass of a pore-forming material, and 0.2 to 1.5 parts by mass of a binder with respect to 100 parts by mass of a cordierite-forming raw material.

[0063] The total amount of one or more sintering aids selected from ceria, zirconia, and titania in the plugging portion forming slurry is preferably adjusted according to the total amount of one or more sintering aids selected from ceria, zirconia, and titania in the raw material composition for obtaining the above-mentioned columnar honeycomb molded body. Specifically, when the total amount of the sintering aid in the raw material composition for obtaining the columnar honeycomb molded body is C1 parts by mass relative to 100 parts by mass of the cordierite raw material, and the total amount of the sintering aid in the plugging portion forming slurry is C2 parts by mass relative to 100 parts by mass of the cordierite raw material, from the viewpoint of suppressing the movement of the sintering aid from the partition wall to the plugging portion, it is preferable to satisfy C1-C2≦1, more preferably to satisfy C1-C2≦0, and even more preferably to satisfy C1-C2≦-1. However, even if C1-C2 is made too small, the effect of suppressing the migration of the sintering aid from the partition walls to the plugging portions becomes saturated, while the melting point of the partition walls is likely to decrease, so it is preferable to satisfy -8 ≦ C1-C2, more preferably to satisfy -6 ≦ C1-C2, and even more preferably to satisfy -4 ≦ C1-C2. Therefore, for example, it is preferable to satisfy -8 ≦ C1-C2 ≦ 1, more preferably to satisfy -6 ≦ C1-C2 ≦ 0, and even more preferably to satisfy -4 ≦ C1-C2 ≦ -1.

[0064] As long as C1 and C2 satisfy the above relationship, there are no particular restrictions on C2 itself, but it is normal for C2 to satisfy 1≦C2≦10, typically for C2 to satisfy 1.5≦C2≦8, and more typically for C2 to satisfy 2.0≦C2≦6.

[0065] From the viewpoint of uniformity of composition, the sintering aid in the plugging portion forming slurry has an upper limit of the median diameter (D50) in the volume-based cumulative particle size distribution obtained by the laser diffraction / scattering method of 10 μm or less, more preferably 8 μm or less, and even more preferably 6 μm or less. From the viewpoint of internal defects caused by aggregation, the sintering aid in the plugging portion forming slurry has a lower limit of the median diameter (D50) in the volume-based cumulative particle size distribution obtained by the laser diffraction / scattering method of 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. Therefore, for example, the median diameter (D50) of the sintering aid in the plugging portion forming slurry is preferably 0.1 to 10 μm, more preferably 0.3 to 8 μm, and even more preferably 0.5 to 6 μm.

[0066] The dispersion medium may be water or a mixed solvent of water and an organic solvent such as alcohol, with water being particularly preferred.

[0067] The pore-forming material is not particularly limited as long as it becomes pores after firing, and examples thereof include wheat flour, starch, foamed resin, water-absorbent resin, silica gel, carbon (e.g., graphite), ceramic balloons, polyethylene, polystyrene, polypropylene, nylon, polyester, acrylic resin, phenol, etc. The pore-forming material may be used alone or in combination of two or more kinds.

[0068] Examples of the binder include organic binders such as methyl cellulose, hydroxypropoxyl methyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, etc. The binder may be used alone or in combination of two or more kinds.

[0069] The plugging portion forming slurry may contain a dispersant as appropriate. The dispersant may be contained in an amount of, for example, 0.1 to 3 parts by mass, preferably 0.2 to 2 parts by mass, relative to 100 parts by mass of the cordierite forming raw material. Examples of the dispersant include ethylene glycol, dextrin, fatty acid soap, and polyalcohol. The dispersant may be used alone or in combination of two or more kinds.

[0070] The openings of the cells can be filled with the plugging portion forming slurry, for example, by the following "squeegee method." As shown in Fig. 7, a film 121 is attached to the upper bottom surface (here, the second bottom surface 106 in the figure) of the dried columnar honeycomb formed body 600 fixed using a chuck 120, and a laser is irradiated to the film 121 at positions corresponding to the arrangement conditions of the plugging portions (for example, "checkered pattern") to form a plurality of holes 126 in the film 121.

[0071] Thereafter, the plugging portion forming slurry 124 is placed on the film 121, and the squeegee 122 is moved along the film 121 in the direction of the arrow in Fig. 7. As a result, a certain amount of the plugging portion forming slurry 124 is filled into the cells 125 that are opened at positions corresponding to the holes 126 of the film 121.

[0072] The depth of the plugging portion can be changed by the number of times the squeegee 122 is moved, the contact angle between the squeegee 122 and the film 121, the pressing pressure of the squeegee 122 against the film 121, and the viscosity of the plugging portion forming slurry 124, etc.

[0073] After filling the plugging portion forming slurry 124, the film 121 is peeled off, and the entire columnar honeycomb formed body 600 is dried. As a result, the plugging portion forming slurry 124 filled in the cells 125 is dried, and the plugging portions before firing are formed. The drying can be performed, for example, under conditions of a drying temperature of 100 to 230°C for about 60 to 150 seconds. After drying, the plugging portions protrude from the bottom surface of the columnar honeycomb formed body by the thickness of the film, and can be scraped off as necessary.

[0074] The material of the film is not particularly limited, but is preferably polypropylene (PP), polyethylene terephthalate (PET), polyimide, or Teflon (registered trademark) because it is easy to heat process to form holes. The film also preferably has an adhesive layer, and the material of the adhesive layer is preferably an acrylic resin, a rubber-based material (e.g., a rubber whose main component is natural rubber or synthetic rubber), or a silicon-based resin. For example, an adhesive film having a thickness of 20 to 50 μm can be suitably used as the film.

[0075] In addition to the above-mentioned "squeegee method," another method for filling the openings of the cells with the plugging portion forming slurry is the "press-in method." The "press-in method" is a method in which the bottom surface of a columnar honeycomb formed body with a film attached and holes drilled therein is immersed in a liquid tank containing the plugging portion forming slurry, and the cells are filled with the plugging portion forming slurry. In this case, the depth of the plugging portions can be changed by the depth to which the columnar honeycomb formed body is immersed in the plugging portion forming slurry.

[0076] The columnar honeycomb formed body filled with the plugging portion forming slurry is then subjected to a degreasing process and a firing process, thereby manufacturing a columnar honeycomb structure. The combustion temperature of the binder is about 200°C, and the combustion temperature of the pore-forming material is about 300 to 1000°C. Therefore, the degreasing process may be carried out by heating the honeycomb formed body to a temperature range of about 200 to 1000°C. The heating time is not particularly limited, but is usually about 10 to 100 hours. The honeycomb formed body after the degreasing process is called a calcined body. The firing process may be carried out by heating the calcined body to 1300 to 1450°C and holding it for 3 to 24 hours, for example, depending on the material composition of the columnar honeycomb structure. EXAMPLES

[0077] The following examples are provided to better understand the present invention and its advantages, but the present invention is not limited to these examples.

[0078] <Comparative Example 1-1> (1) Preparation of columnar honeycomb body A raw material composition was prepared by adding 80 parts by mass of a dispersion medium, 25 parts by mass of a pore former, 5 parts by mass of a binder, and 1 part by mass of a dispersant to 100 parts by mass of a cordierite raw material, and kneading the resulting composition to prepare a clay. Alumina, aluminum hydroxide, kaolin, talc, and silica were used as the cordierite raw materials. Water was used as the dispersion medium, water-absorbent resin and silica gel were used as the pore former, methylcellulose was used as the binder, and ethylene glycol was used as the dispersant.

[0079] The clay was put into an extrusion molding machine and extruded through a die of a predetermined shape to obtain a cylindrical honeycomb molded body. The obtained cylindrical honeycomb molded body was subjected to dielectric drying and hot air drying, and then both bottom surfaces were cut to the predetermined dimensions and further dried with hot air at 70°C for 2 hours.

[0080] (2) Formation of plugging parts 40 parts by mass of the dispersion medium, 10 parts by mass of the pore former, 2 parts by mass of the binder, and 1 part by mass of the dispersant were added to 100 parts by mass of the cordierite raw material, and the mixture was kneaded to prepare a slurry for forming plugged portions. Alumina, aluminum hydroxide, kaolin, talc, and silica were used as the cordierite raw material. Water was used as the dispersion medium, foamed resin was used as the pore former, methyl cellulose was used as the binder, and ethylene glycol was used as the dispersant. Using the "squeegee method" described above, the slurry for forming plugged portions was filled on both bottom surfaces so that the first cells and the second cells were alternately arranged adjacent to each other. After that, the mixture was dried under the conditions of 180°C x 200 seconds in an air atmosphere.

[0081] (3) Firing Next, the honeycomb structure was degreased by heating at about 200° C. in an air atmosphere, and then fired at 1400° C. for 10 hours in an air atmosphere to obtain a columnar honeycomb structure having plugged portions. The columnar honeycomb structures were manufactured in the number required for the following tests.

[0082] (4) Specifications of columnar honeycomb structure The specifications of the obtained pillar-shaped honeycomb structure are as follows. Overall shape: Cylinder with diameter 132mm x height 152mm Cell shape in cross section perpendicular to the flow direction: Square Cell density (number of cells per unit cross-sectional area): 300 cells / sq. in. (47 cells / cm 2 ) Average bulkhead thickness: 8.5 mil (216 μm) (nominal value based on cap specifications) Average plugging depth: 5mm The outer side walls, partition walls and plugging portions of the columnar honeycomb structure were subjected to X-ray analysis measurement in the range of 2θ=8 to 100° by X-ray diffraction using an X'pert PRO device manufactured by PANalytical Corporation using Cu Kα radiation, and the cordierite crystal phase ratio was determined by analysis using the Rietveld analysis program RIETAN, and was found to be 75 to 94 mass%.

[0083] <Comparative Examples 1-2 to 1-6, Examples 1-1 to 1-9> Three types of sintering aids were prepared: ceria, zirconia, and titania. These were in powder form, and the median diameter (D50) in the cumulative particle size distribution on a volume basis was determined by the laser diffraction / scattering method. The results are shown below. Ceria: 1μm Zirconia: 1μm Titania: 1μm

[0084] A columnar honeycomb structure was obtained under the same manufacturing conditions as those of Comparative Example 1-1, except that the amount C1 (parts by mass) of the sintering aid added to 100 parts by mass of the cordierite-forming raw material in the raw material composition for the honeycomb formed body and the amount C2 (parts by mass) of the sintering aid added to 100 parts by mass of the cordierite-forming raw material in the plugging portion forming slurry were set to the conditions shown in Table 1. The columnar honeycomb structure was manufactured in the number required for the following tests.

[0085] <Comparative Example 2-1> (1) Preparation of columnar honeycomb body A raw material composition was prepared by adding 80 parts by mass of a dispersion medium, 25 parts by mass of a pore former, 5 parts by mass of a binder, and 1 part by mass of a dispersant to 100 parts by mass of a cordierite raw material, and kneading the resulting composition to prepare a clay. Alumina, aluminum hydroxide, kaolin, talc, and silica were used as the cordierite raw materials. Water was used as the dispersion medium, water-absorbent resin and silica gel were used as the pore former, methylcellulose was used as the binder, and ethylene glycol was used as the dispersant.

[0086] The clay was put into an extrusion molding machine and extruded through a die of a predetermined shape to obtain a cylindrical honeycomb molded body. The obtained cylindrical honeycomb molded body was subjected to dielectric drying and hot air drying, and then both bottom surfaces were cut to the predetermined dimensions and further dried with hot air at 70°C for 2 hours.

[0087] (2) Formation of plugging parts 40 parts by mass of the dispersion medium, 10 parts by mass of the pore former, 2 parts by mass of the binder, and 1 part by mass of the dispersant were added to 100 parts by mass of the cordierite raw material, and the mixture was kneaded to prepare a slurry for forming plugged portions. Alumina, aluminum hydroxide, kaolin, talc, and silica were used as the cordierite raw material. Water was used as the dispersion medium, a foamed resin was used as the pore former, methylcellulose was used as the binder, and ethylene glycol was used as the dispersant. Using the "squeegee method" described above, the slurry for forming plugged portions was filled on both bottom surfaces so that the first cells and the second cells were alternately arranged adjacent to each other.

[0088] (3) Firing Then, the honeycomb structure was dried at 180°C for 200 seconds in an air atmosphere. The honeycomb structure was then degreased by heating at about 200°C in an air atmosphere, and then fired at 1400°C for 10 hours in an air atmosphere to obtain a honeycomb structure having plugged portions. The number of honeycomb structures required for the following tests was manufactured.

[0089] (4) Specifications of columnar honeycomb structure The specifications of the obtained pillar-shaped honeycomb structure are as follows. Overall shape: Cylinder with diameter 132mm x height 152mm Cell shape in cross section perpendicular to the flow direction: Square Cell density (number of cells per unit cross-sectional area): 340 cells / sq. in. (53 cells / cm 2 ) Average bulkhead thickness: 11mil (279μm) (nominal value based on base specifications) Average plugging depth: 5mm The outer side walls, partition walls and plugging portions of the columnar honeycomb structure were subjected to X-ray analysis measurement in the range of 2θ=8 to 100° by X-ray diffraction using an X'pert PRO device manufactured by PANalytical Corporation using Cu Kα radiation, and the cordierite crystal phase ratio was determined by analysis using the Rietveld analysis program RIETAN, and was found to be 75 to 94 mass%.

[0090] <Comparative Examples 2-2 to 2-6, Examples 2-1 to 2-9> Three types of sintering aids were prepared: ceria, zirconia, and titania. These were in powder form, and the median diameter (D50) in the cumulative particle size distribution on a volume basis was determined by the laser diffraction / scattering method. The results are shown below. Ceria: 1μm Zirconia: 1μm Titania: 1μm

[0091] A columnar honeycomb structure was obtained under the same manufacturing conditions as those of Comparative Example 2-1, except that the amount C1 (parts by mass) of the sintering aid added to 100 parts by mass of the cordierite-forming raw material in the raw material composition for the honeycomb molded body and the amount C2 (parts by mass) of the sintering aid added to 100 parts by mass of the cordierite-forming raw material in the plugging portion forming slurry were set to the conditions shown in Table 2. The columnar honeycomb structure was manufactured in the number required for the following tests.

[0092] <Characteristics evaluation> Various characteristics were evaluated for each of the pillar-shaped honeycomb structures obtained above.

[0093] (1. Porosity) The average porosity P1 (%) of the partition wall portion in the above-mentioned range A and range B (near the plugged portion) of the columnar honeycomb structure, and the average porosity P2 (%) of the partition wall portion in the above-mentioned range C (away from the plugged portion) were determined according to the method described above. Based on the measurement results, P1-P2 was calculated. The results are shown in Tables 1 and 2.

[0094] (2.SEM-EDS analysis) The average value S1 (%) of the total content of the sintering aid in the partition wall portion in the above-mentioned range A and range B (near the plugged portion) of the columnar honeycomb structure, the average value S2 (%) of the total content of the sintering aid in the partition wall portion in the above-mentioned range C (away from the plugged portion), and the average value S3 (%) of the total content of the sintering aid in the plugged portion were obtained according to the above-mentioned method. The device used for the SEM-EDS analysis was Hitachi High-Technologies Corporation Model S-3400N. The results are shown in Tables 1 and 2.

[0095] (3. Measurement of Pore Size Distribution) The pore size distribution (D10, D50 and D90) of the partition walls of the columnar honeycomb structure was measured by mercury intrusion porosimetry according to the method described above. Based on the measurement results, (D90-D10) / D50 was calculated. Based on the results of SEM-EDS analysis, (S2-S1) / D50×100 was calculated. The results are shown in Tables 1 and 2.

[0096] (4. Measurement of isostatic fracture strength) The isostatic fracture strength of the columnar honeycomb structure was measured based on the automobile standard (JASO M505-87) issued by the Automotive Engineers Association of Japan. The results are shown in Tables 1 and 2.

[0097] [Table 1]

[0098] [Table 2]

[0099] (5. Discussion) Comparative Examples 1-1 and 2-1, in which a specific sintering aid was not added, had excellent isostatic fracture strength, but the pore size distribution was broad. In contrast, Comparative Examples 1-2 to 1-7 and 2-2 to 2-7, in which a specific sintering aid was added, had sharp pore size distributions. However, in these examples, the manufacturing conditions C1-C2 were inappropriate, so that the average porosity P1 of the partition wall portion near the plugging portion increased, and the condition -4≦P1-P2≦7 was not satisfied. As a result, the isostatic fracture strength was significantly reduced.

[0100] On the other hand, in Examples 1-1 to 1-9 and Examples 2-1 to 2-9, the portions constituting the partition walls and the outer peripheral side walls of the columnar honeycomb structures contained a predetermined sintering aid, and satisfied -4≦P1-P2≦7. Therefore, it was possible to suppress the decrease in isostatic fracture strength while sharpening the pore size distribution. Furthermore, it can be seen that by optimizing P1-P2, it is possible to obtain isostatic fracture strength that is comparable to the examples (Comparative Examples 1-1 and 2-1) before the addition of the predetermined sintering aid. [Explanation of symbols]

[0101] 100: Pillar honeycomb structure 102: Outer wall 104: First bottom surface 106:Second bottom surface 108: First cell 109: Plugging part 110: Second cell 112: Bulkhead 112a: surface 112b: Surface 112c: surface 120: Zipper 121: Film 122: Squeegee 124: Plugging slurry 125: Cell 126: Hole 600: Columnar honeycomb formed body

Claims

1. A columnar honeycomb structure comprising an outer peripheral side wall, a plurality of first cells arranged on an inner peripheral side of the outer peripheral side wall, extending from a first bottom surface to a second bottom surface, having openings on the first bottom surface and plugging portions on the second bottom surface, and a plurality of second cells arranged on the inner peripheral side of the outer peripheral side wall, extending from the first bottom surface to the second bottom surface, having plugging portions on the first bottom surface and having openings on the second bottom surface, wherein the plurality of first cells and the plurality of second cells are alternately arranged adjacent to each other with partition walls interposed therebetween, the outer peripheral side wall, the partition walls, and the plugging portions are fired and contain cordierite as a main component and one or more sintering aids selected from ceria, zirconia, and titania; The average porosity of a portion of the partition wall in a range A from the deepest portion of the plugging portion of the second bottom surface in the extension direction of the first cells to the second bottom surface, and a portion of the partition wall in a range B from the deepest portion of the plugging portion of the first bottom surface in the extension direction of the second cells to the first bottom surface is P 1 (%)year, The average porosity of the portion of the partition wall in the range C from the deepest portion of the plugging portion of the second bottom surface in the extension direction of the first cell to the deepest portion of the plugging portion of the first bottom surface in the extension direction of the second cell is P 2 (%), -4≦P 1 -P 2 Satisfying ≦7, Columnar honeycomb structure.

2. -2≦P 1 -P 2 The pillar-shaped honeycomb structure according to claim 1 , which satisfies ≦5.

3. 55≦P 2 3. The pillar-shaped honeycomb structure according to claim 1 or 2, which satisfies ≦70.

4. The average value of the total content of one or more sintering aids selected from ceria, zirconia, and titania in the portion in the range A and the portion in the range B of the partition wall is S 1 (%), and the average of the total contents of one or more sintering aids selected from ceria, zirconia, and titania in the portions of the partition walls in the range C is S 2 (%), and the cumulative 50% pore diameter of the partition walls in the volume-based cumulative pore diameter distribution measured by mercury intrusion porosimetry is D50 (μm), (S 2 -S 1 3. The pillar-shaped honeycomb structure according to claim 1 or 2, which satisfies the relationship: D50×100≦6.

5. The partition wall in the region C has a cumulative pore size distribution on a volume basis measured by mercury intrusion porosimetry, in which the cumulative 10% pore size (D10), cumulative 50% pore size (D50) and cumulative 90% pore size (D90) from the small pore side satisfy the relationship of (D90-D10) / D50≦1.

2.

6. A method for manufacturing a columnar honeycomb structure comprising: an outer peripheral side wall; a plurality of first cells arranged on an inner peripheral side of the outer peripheral side wall, extending from a first bottom surface to a second bottom surface, having openings on the first bottom surface and plugging portions on the second bottom surface; and a plurality of second cells arranged on the inner peripheral side of the outer peripheral side wall, extending from the first bottom surface to the second bottom surface, having plugging portions on the first bottom surface and having openings on the second bottom surface, wherein the plurality of first cells and the plurality of second cells are arranged adjacent to each other alternately with partition walls interposed therebetween, a step of kneading a raw material composition containing a cordierite raw material, a dispersion medium, a pore-forming material, a binder, and one or more sintering aids selected from ceria, zirconia, and titania to form a puddle, and then extruding the puddle to obtain a columnar honeycomb formed body having an outer peripheral side wall and a first bottom surface and a second bottom surface, the first bottom surface and the second bottom surface both having openings; a step of filling a plugging portion forming slurry containing a cordierite raw material, a dispersion medium, a pore former, a binder, and one or more sintering aids selected from ceria, zirconia, and titania into openings of the first bottom surface and the second bottom surface where the plugging portions are to be formed after drying the columnar honeycomb formed body; A step of firing the columnar honeycomb formed body filled with the plugging portion forming slurry; Including, Regarding the sintering aid in the raw material composition, the total amount added to 100 parts by mass of the cordierite-forming raw material is C 1 parts by mass, and the total amount of the sintering aid in the slurry for forming the plugging portion is C 2 In parts by mass, -8≦C 1 -C 2 ≦1, Manufacturing method.

7. −6≦C 1 -C 2 The method according to claim 6, wherein the ratio of the two is ≦0.

8. 1≦C 2 The method according to claim 6 or 7, which satisfies ≦10.

9. The manufacturing method according to claim 6 or 7, wherein the sintering aid in the raw material composition and the sintering aid in the slurry for forming the plugging portion have a median diameter (D50) of 0.1 to 10 μm in a volume-based cumulative particle size distribution obtained by a laser diffraction / scattering method.

Citation Information

Patent Citations

  • Honeycomb structure and its production

    JP2000051710A

  • Sealed honeycomb structure and method for producing the same

    JP2005349269A

  • Method for producing plugged honeycomb structure and plugged honeycomb structure

    JP2016175810A

  • Encapsulated honeycomb structure and manufacturing method of encapsulated honeycomb structure

    JP2017145171A

  • High cordierite-to-mullite ratio cordierite-mullite-aluminum magnesium titanate compositions and ceramic articles comprising same

    US20160068441A1