Ferrite powder

A ferrite powder with controlled composition and shape is developed to address the issue of decreasing magnetic permeability over time, ensuring high stability and low loss, suitable for inductor applications.

JP2024143932AActive Publication Date: 2024-10-11POWDERTECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023056889
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-11
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

Conventional ferrite powders used in composite materials experience a decrease in magnetic permeability over time, known as disaccommodation, which affects their stability and performance in applications like inductors.

Method used

A ferrite powder composition with specific ranges of iron, manganese, and zinc content, along with controlled vacancy rates and particle shapes, including a spinel phase and a step structure, is developed to maintain high magnetic permeability and low loss.

Benefits of technology

The ferrite powder exhibits excellent stability of magnetic permeability over time, high magnetic permeability at high frequencies, and low loss, making it suitable for applications such as inductors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143932000001_ABST
    Figure 2024143932000001_ABST
Patent Text Reader

Abstract

To provide a ferrite powder excellent in stability of magnetic permeability with time while maintaining high fillability and high magnetic permeability and low loss at high frequencies.SOLUTION: A ferrite powder contains 56.0 mass% or more and 63.0 mass% or less iron (Fe), 7.0 mass% or more and 13.0 mass% or less manganese (Mn), and 1.0 mass% or more and 3.0 mass% or less zinc (Zn).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ferrite powder. [Background technology]

[0002] Composite materials made of ferrite powder and resin are widely used in a variety of applications, including inductors. Such composite materials are produced by kneading ferrite powder with resin. The composite material is molded into a sheet or other shape to form a composite (molded body). In this case, if the shape of the particles that make up the ferrite powder is close to spherical, the fluidity during molding is high and the filling rate of the ferrite powder in the composite is high. This results in good moldability and good magnetic properties. From this perspective, ferrite powder (particles) made up of spherical or polyhedral particles have been proposed.

[0003] For example, Patent Document 1 describes a Mn-Zn ferrite powder containing at least spherical or polyhedral ferrite particles having a spinel phase as a main phase, the ferrite particles having a step structure with a convex polygonal outline on the surface, and the ferrite powder has a BET specific surface area of ​​0.35 m 2 / g or more 10.00m 2 / g or less and a zinc oxide (ZnO) phase content of 0 mass% or more and 0.8 mass% or less is disclosed (claim 1 of Patent Document 1). Patent Document 1 also describes that the ferrite powder can suppress magnetic loss at high frequencies and can suppress particle shedding without impairing moldability and packing property when applied to composite materials or composites (

[0024] of Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2022 / 209640 Summary of the Invention [Problem to be solved by the invention]

[0005] Thus, it has been proposed to improve the moldability and filling property of composite materials and composite bodies by using spherical or polyhedral ferrite powder. However, the inventors have found that when the conventional ferrite powder is combined with a resin and then heated and molded to produce a resin molded body (composite body), there occurs a problem that the magnetic permeability of the resin molded body gradually decreases over time (disaccommodation).

[0006] As a result of further investigation, the inventors found that the change in magnetic permeability over time is significantly affected by γ-Fe2O3, which has vacancies, among the ferromagnetic iron (Fe) oxides contained in ferrite. They then discovered that by suppressing the formation of γ-Fe2O3 and controlling the vacancy rate, it is possible to obtain ferrite powder that has excellent stability of magnetic permeability over time while maintaining high filling properties, high magnetic permeability at high frequencies, and low loss.

[0007] Therefore, an object of the present invention is to provide a ferrite powder that has excellent stability of magnetic permeability over time while maintaining high filling properties, high magnetic permeability at high frequencies, and low loss. [Means for solving the problem]

[0008] The present invention encompasses the following aspects (1) to (4). In this specification, the expression "to" includes both ends of the expression. In other words, "X to Y" is synonymous with "X or more and Y or less."

[0009] (1) Ferrite powder containing iron (Fe) in an amount of 56.0 mass% or more and 63.0 mass% or less, manganese (Mn) in an amount of 7.0 mass% or more and 13.0 mass% or less, and zinc (Zn) in an amount of 1.0 mass% or more and 3.0 mass% or less.

[0010] (2) the ferrite powder contains spherical ferrite particles mainly composed of a spinel phase; The spinel phase has an iron (Fe) amount in excess of the stoichiometric ratio and a vacancy rate of 0 mol% or more and 90 mol% or less, The ferrite powder has a shape factor SF-1 of 100 or more and 110 or less, and a volume average particle size (D50) of 2.0 μm or more and 20 μm or less. The ferrite powder of (1) above.

[0011] (3) The ferrite powder of (1) or (2) above, having an α-iron oxide (α-Fe2O3) content of 0.0% by mass or more and 3.0% by mass or less.

[0012] (4) The ferrite powder according to any one of (1) to (3) above, having a copper (Cu) content of 0.0% by mass or more and 0.5% by mass or less. Effect of the Invention

[0013] According to the present invention, there is provided a ferrite powder that has excellent stability of magnetic permeability over time while maintaining high filling properties, high magnetic permeability at high frequencies, and low loss. [Brief description of the drawings]

[0014] [Figure 1] The change in the real part of magnetic permeability (μ') of ferrite powder over time is shown (Example 1). [Diagram 2] The change in the real part of magnetic permeability (μ') of ferrite powder over time is shown (Example 5). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the scope of the present invention.

[0016] <<1. Ferrite powder>> The ferrite powder of this embodiment contains iron (Fe) in an amount of 56.0 mass% or more and 63.0 mass% or less, manganese (Mn) in an amount of 7.0 mass% or more and 13.0 mass% or less, and zinc (Zn) in an amount of 1.0 mass% or more and 3.0 mass% or less.

[0017] Ferrite powder (hereinafter sometimes simply referred to as "powder") is composed of multiple ferrite particles (hereinafter sometimes simply referred to as "particles"). That is, ferrite powder is an aggregate of multiple ferrite particles. Furthermore, the ferrite particles that make up ferrite powder are basically independent. Therefore, ferrite powder by itself exhibits fluidity as a whole. However, as long as it exhibits fluidity as a whole, this does not exclude ferrite powder in which some particles are combined to form agglomerated particles (secondary particles).

[0018] The ferrite powder (particles) of this embodiment has a spinel phase as the main phase. That is, the content of the spinel phase is 50.0 mass% or more. The spinel phase is an iron oxide-based compound having a basic composition represented by MFe2O4 (where M is a metal element such as a transition metal element or a vacancy), and many of them are ferromagnetic. Therefore, the ferrite powder having a spinel phase as the main phase exhibits excellent magnetic properties.

[0019] The ferrite powder of the present embodiment has a composition of Mn-Zn ferrite containing iron (Fe), manganese (Mn) and zinc (Zn). Mn-Zn ferrite is generally characterized by high magnetic permeability. Therefore, when the ferrite powder is applied to an element such as an inductor, it is possible to obtain excellent magnetic properties.

[0020] The amount of iron (Fe) in the ferrite powder is 56.0% by mass or more and 63.0% by mass or less. When the amount of Fe is less than 56.0% by mass, the amount of Mn and / or Zn becomes relatively large. In this case, depending on the composition ratio, the loss factor (tan δ) tends to increase from a relatively low frequency of about 50 MHz. Since the loss is large, it is not suitable for use in high-frequency applications such as inductors. The amount of Fe is preferably 57% by mass or more, and more preferably 58% by mass or more. On the other hand, when the amount of Fe exceeds 63.0% by mass, the amount of Mn and / or Zn becomes relatively small. The real part of the complex permeability (real part of permeability; μ') is low, and a high saturation magnetic flux density cannot be obtained. Therefore, it is still not suitable for use in applications such as inductors. The amount of Fe is preferably 62.5% by mass or less, and more preferably 62% by mass or less.

[0021] The manganese (Mn) content of the ferrite powder is 7.0% by mass or more and 13.0% by mass or less. If the Mn content is less than 7.0% by mass, the Fe content and / or Zn content will be relatively high. In this case, the real part of the magnetic permeability (μ') will be low, making it unsuitable for use in applications such as inductors. The Mn content is preferably 7.3% by mass or more, more preferably 7.5% by mass or more. On the other hand, if the Mn content exceeds 13.0% by mass, the Fe content and / or Zn content will be relatively low. Although it depends on the composition ratio, the loss factor (tan δ) tends to increase from a relatively low frequency of around 50 MHz. Therefore, it is still unsuitable for use in high-frequency applications such as inductors. The Mn content is preferably 12% by mass or less, more preferably 11% or less.

[0022] The amount of zinc (Zn) in the ferrite powder is 1.0% by mass or more and 3.0% by mass or less. If the amount of Zn is less than 1.0% by mass, the effect of adding Zn is less likely to be obtained, and the real part of magnetic permeability (μ') becomes low. On the other hand, if the amount of Zn is more than 3.0% by mass, the loss factor (tan δ) at 50 MHz becomes large. In addition, if the amount of Zn is excessively large, fine zinc oxide (ZnO) may adhere to the surface of the ferrite particles constituting the ferrite powder. This is because a part of the excess Zn volatilizes during the high-temperature heat treatment process (such as the thermal spraying process) during the production of the ferrite powder, and reprecipitates as fine ZnO on the surface of the ferrite particles. If ZnO adheres to the surface of the ferrite particles, when the ferrite powder and the resin are mixed and kneaded to produce a composite material, the viscosity of the composition may increase rapidly, making the production difficult.

[0023] Preferably, the ferrite powder contains spherical ferrite particles mainly composed of a spinel phase. Here, the spherical ferrite particles include not only spherical particles but also polyhedral particles. By controlling the shape of the particles contained in the ferrite powder to be spherical (spherical, polyhedral), the moldability and packing properties of the ferrite powder can be improved. This is because the spherical particles can smoothly avoid contact with other particles during molding. Therefore, the flowability during molding is improved and dense packing is possible. In contrast, particles having an anisotropic or irregular shape such as a plate or needle shape are inferior in moldability and packing properties.

[0024] The ferrite particles constituting the ferrite powder may be partly spherical ferrite particles, or may be entirely spherical ferrite particles. However, from the viewpoint of improving moldability and packing property, it is preferable that the proportion of spherical ferrite particles is high. Specifically, the proportion of spherical ferrite particles is preferably 50% by number or more.

[0025] Polyhedral particles basically have a shape in which a plurality of polygons are three-dimensionally combined. The polygons constituting the polyhedron are typically triangles, squares, hexagons, octagons, decagons, or combinations thereof, reflecting the crystal structure of the ferrite particles. Examples of such polyhedrons include rhombic truncated cuboctahedrons consisting of a square, a hexagon, and an octagon. The more faces a polyhedron has, the closer it is to a sphere. Therefore, the polyhedral particles preferably have a shape of 10 or more, more preferably 12 or more, and even more preferably 14 or more. The polyhedral particles typically have a shape of 100 or less, more typically 72 or less, and even more typically 24 or less.

[0026] In addition, particles in which one or more straight lines constituting a polygon are broken, or particles in which some straight lines are curved, are also included in the polyhedral particles, so long as they can be recognized as polyhedral when viewed as a whole particle. In addition, particles in which the straight lines constituting a polygon are finely jagged are also included in the polyhedral particles. Furthermore, spherical-like step particles may have a step structure on their surface. In this case, strictly speaking, they may not be completely spherical or polyhedral. However, this step structure is much smaller than the size of the particle. Therefore, even if they have such a microscopic step structure, particles that have a spherical or polyhedral shape when viewed macroscopically are considered to be spherical or polyhedral particles.

[0027] Preferably, the ferrite powder contains ferrite particles (spherical step particles) that have a step structure on their surface. By including particles with such a step structure, when the ferrite powder is applied to a composite material or composite, the adhesion to the resin is improved and particle dropout is suppressed. Although the detailed mechanism is unclear, it is speculated that the presence of the step structure increases the surface area of ​​the particles, i.e., the contact area with the resin, and as a result, the chemical bonding strength between the particles and the resin is increased. It is also speculated that the step structure allows the particles and the resin to fit together, which causes the anchor effect of the resin to work and increases the physical bonding strength between the particles and the resin.

[0028] The step structure has a convex polygonal outline on the ferrite particle surface. That is, when the particle is viewed from the surface, the step structure has a convex polygonal outline. In other words, the step structure is provided so as to surround a region of the particle surface with a combination of straight lines. By providing such a step structure, it is possible to more effectively prevent the particles from falling off. Here, the convex polygon is a polygon in which any interior angle is 180° or less. It can also be said to be a polygon in which a line segment connecting any two points inside or on the boundary does not go outside. In other words, it is not a concave polygon (non-convex polygon) such as a star. The outline of the step structure is not limited as long as it is a convex polygon. However, reflecting the crystal structure of ferrite, the outline is typically a triangle, a square, a hexagon, an octagon, or a decagon. The ferrite particle may also have a plurality of step structures on its surface. This makes it possible to more effectively prevent the particles from falling off.

[0029] Preferably, the spinel phase contained in the ferrite powder has an iron (Fe) amount in excess of the stoichiometric composition. That is, the spinel phase has a composition in which the iron (Fe) amount is in excess of the stoichiometric composition. As described above, the spinel phase has a basic composition represented by MFe2O4 (where M is a metal element such as a transition metal element or a vacancy). Therefore, in a stoichiometric composition in which M is an element other than Fe, the molar ratio of the Fe amount to the total amount of M and Fe contained in the spinel phase is 2 / 3. When the ratio of the Fe amount is more than 2 / 3, Fe is incorporated in the M site, and the composition of the spinel phase becomes (M,Fe)Fe2O4. By increasing the amount of Fe contained in the spinel phase to that of the stoichiometric composition, the loss factor (tan δ) at high frequencies can be lowered, and as a result, low loss of the ferrite powder is realized.

[0030] Preferably, the spinel phase has a vacancy rate of 0 mol% or more and 90 mol% or less. The vacancy rate is the ratio of γ-Fe2O3 (magnetite) to the total number of moles of Fe3O4 (magnetite) and γ-Fe2O3 (maghematite) contained in the ferrite powder (spinel phase). 3のIt is defined as the ratio of moles (γ-Fe2O3 moles / (Fe3O4 moles + γ-Fe2O3 moles)). By suppressing the vacancy rate, it is possible to reduce the change in magnetic permeability of ferrite powder over time. In contrast, if the vacancy rate exceeds 90 mol%, the change in magnetic permeability over a long period of time becomes large. Therefore, when ferrite powder is used as a filler in an inductor magnetic core, the performance of the inductor changes over time. In this case, it becomes difficult to obtain the performance that was initially designed, which can lead to malfunctions of electronic devices.

[0031] To explain this point, as mentioned above, the iron (Fe)-excess spinel phase has a composition of (M,Fe)Fe2O4. In other words, the crystals of the spinel phase, which is an oxide, contain a large amount of Fe. Meanwhile, Fe oxides exist in various forms, such as α-Fe2O3 (hematite), γ-Fe2O3 (maghematite), and Fe3O4 (magnetite). Of these, α-Fe2O3 and FeO are antiferromagnetic and do not exhibit ferromagnetic properties. In addition, they do not have a spinel structure.

[0032] In contrast, Fe3O4 (magnetite) and γ-Fe2O3 (maghematite) are ferromagnetic. The composition formula of Fe3O4 is Fe 3+ (Fe 2+ ,Fe 3+ )2O4, and the formula of γ-Fe2O3 is Fe 3+ (Fe 3+ 5 / 6 V 1 / 6 )2O4 (where V is vacant). They therefore have a spinel structure. Iron (Fe)-rich spinel phases can therefore be said to contain either or both of Fe3O4 (magnetite) and γ-Fe2O3 (maghematite).

[0033] Fe3O4 (magnetite) with a spinel structure does not have vacancies in its crystal structure, whereas γ-Fe2O3 (maghematite) has vacancies (V). Therefore, ferrite powder containing γ-Fe2O3 has vacancies (V) in the spinel phase, and the more γ-Fe2O3 there is, the more vacancies there are. Also, the more vacancies there are, that is, the more γ-Fe2O3 there is, the greater the change in permeability over time. The reason for this is believed to be related to the interaction between the vacancies present in the ferrite crystal lattice moving within the crystal lattice over time and settling into an energetically stable state (position), and the presence of the vacancies preventing the movement of the domain walls.

[0034] Therefore, the amount of γ-Fe2O3 in the spinel phase, that is, the vacancy rate, can be reduced to reduce the change in magnetic permeability over time. From the viewpoint of suppressing the change in magnetic permeability over time, it is desirable for the vacancy rate to be small. A vacancy rate of 90 mol% or less is more preferable, and a vacancy rate of 85 mol% or less is even more preferable. On the other hand, by increasing the vacancy rate to a certain level, the loss factor (tan δ) can be kept low. A vacancy rate of 20 mol% or more is preferable, a vacancy rate of 30 mol% or more is more preferable, and a vacancy rate of 40 mol% or more is even more preferable.

[0035] As mentioned above, the vacancy rate is the ratio of the number of moles of γ-Fe2O3 to the total number of moles of Fe3O4 and γ-Fe2O3. There are two types of Fe oxides that exhibit ferromagnetism: Fe3O4 and γ-Fe2O3. It is believed that these two types of Fe oxides exist as non-stoichiometric compounds in spinel. Therefore, the spinel hollow lattice rate can be estimated by using the ratio (vacancy rate) of vacant Fe oxides (γ-Fe2O3) in ferromagnetic Fe oxides (Fe3O4, γ-Fe2O3) as an index.

[0036] The vacancy rate is determined as follows. First, the ferrite powder is subjected to chemical analysis to determine the amounts of Fe, Mn, Zn, and Cu in the powder as mass percentages (mass%). Separately, the amount of divalent iron (Fe 2+Furthermore, the ferrite powder is subjected to X-ray diffraction (XRD) analysis to determine the amount of α-Fe2O3 (hematite) in the powder.

[0037] Next, the atomic weight of Fe (55.85), the atomic weight of Mn (54.94), the atomic weight of Zn (65.39), the atomic weight of Cu (63.55), and the formula weight of α-Fe2O3 (159.70) were used to calculate the amount of Fe (A), the amount of Mn (B), the amount of Zn (C), and the amount of Fe (D), converted into moles according to the following formulas (1) to (6). 2+ The amount of excess Fe, D, the amount of α-Fe2O3, E, and the amount of Cu, F, are calculated. Then, the amount of excess Fe, G (moles), and the amount of Fe compounds (γ-Fe2O3) with vacancies, H (moles), are calculated according to the following formulas (7) and (8). Finally, the vacancy rate, I (mol%), is calculated according to the following formula (9).

[0038]

number

[0039]

number

[0040] In addition, the ferrite powder may contain α-Fe2O3 (hematite). In addition, when the ferrite powder contains copper (Cu), CuOFe5O8 (copper-iron composite oxide) may be formed. α-Fe2O3 and CuOFe5O8 are not ferromagnetic materials with a spinel structure. Therefore, when calculating the amount of excess Fe in the spinel phase using the above formula (7), the Fe content contained in α-Fe2O3 and CuOFe5O8 is excluded. In addition, Fe3O4 (magnetite) contains divalent iron ions (Fe 2+ ), whereas γ-Fe2O3 (maghematite) contains Fe 2+ Therefore, when calculating the amount of γ-Fe2O3 using the above formula (8), the Fe contained in Fe3O4 is not included. 2+ minutes are excluded.

[0041] The amount of excess Fe calculated according to the above formula (7) should be greater than zero (0). In this case, the amount of iron (Fe) in the spinel phase contained in the ferrite powder is in excess of the stoichiometric composition.

[0042] Preferably, the excess iron (Fe) ratio of the ferrite powder is 25 mol% or more and 70 mol% or less. If the excess Fe ratio is less than 25 mol%, the real part of magnetic permeability (μ') becomes high, but the loss factor (tan δ) becomes large. Therefore, the ferrite powder is not suitable for use as a filler for the magnetic core of an inductor. If the excess Fe ratio exceeds 70 mol%, the loss factor (tan δ) becomes small, but the real part of magnetic permeability (μ') also becomes low. Therefore, the ferrite powder is also not suitable for use as a filler for the magnetic core of an inductor. The excess Fe ratio is more preferably 35 mol% or more and 70 mol% or less, and even more preferably 40 mol% or more and 70 mol% or less. The excess Fe ratio is the ratio of the amount of excess Fe to the total amount of Fe, and is calculated according to the following formula (10).

[0043]

number

[0044] Preferably, the mass ratio of iron (Fe) to manganese (Mn) contained in the ferrite powder (Fe / Mn mass ratio) is 5.5 to 8.0. If the amount of Zn is in the range of 1 mass% to 3 mass% and the Fe / Mn mass ratio is 5.5 to 8.0, the ferrite powder can achieve a good balance between high magnetic permeability and low loss. Therefore, it becomes possible to increase the μ'Q product.

[0045] Preferably, the copper (Cu) content of the ferrite powder is 0% by mass or more and 1.0% by mass or less. Cu is easily segregated in ferrite particles. If segregation occurs, the magnetic properties of the ferrite powder may deteriorate. By suppressing the Cu amount to 1.0% by mass or less, it is possible to suppress the generation of segregation that causes the deterioration of magnetic properties. On the other hand, Cu has the effect of stabilizing the valence of Fe. Although it depends on the manufacturing method of the ferrite powder, by adding an appropriate amount of Cu, it is possible to suppress the generation of vacancies and to suppress the change in magnetic permeability over time over a long period of time. The Cu content is more preferably 0% by mass or more and 0.50% by mass or less, and even more preferably 0% by mass or more and 0.35% by mass or less.

[0046] The ferrite powder may have a composition containing iron (Fe), manganese (Mn), zinc (Zn), copper (Cu) and oxygen (O), with the remainder being inevitable impurities. Alternatively, it may contain other component elements other than Fe, Mn, Zn, Cu and O. Examples of such component elements include lithium (Li), magnesium (Mg), aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co) and nickel (Ni). However, from the viewpoint of utilizing the excellent magnetic properties of Mn-Zn ferrite, it is preferable that the ferrite powder does not contain a large amount of other component elements other than Fe, Mn, Zn, Cu and O. The content of other component elements is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less.

[0047] Preferably, the spinel phase content in the ferrite powder (ferrite particles) is 80.0% by mass or more. The spinel phase, which is a ferromagnetic material, is the crystal phase that is the main component of the magnetic properties of the ferrite powder. By increasing the spinel phase ratio, it is possible to increase the saturation magnetization (σs) and magnetic permeability (μ) of the ferrite powder. The spinel phase ratio is more preferably 85.0% by mass or more, even more preferably 90.0% by mass or more, particularly preferably 95.0% by mass or more, and most preferably 99.0% by mass or more.

[0048] Preferably, the zinc oxide (ZnO) content in the ferrite powder is 0.0% by mass or more and 1.0% by mass or less. Zinc oxide (ZnO) is a heterophase derived from zinc (Zn) that has not been ferritized. Ferrite powder containing a large amount of ZnO has poor magnetic properties. In addition, when this ferrite powder is applied to a resin composition, it may cause a problem of increasing the viscosity of the composition. Therefore, the less ZnO as a heterophase, the better. The ZnO content is more preferably 0.0% by mass or more and 0.8% by mass or less, and even more preferably 0.0% by mass or more and 0.5% by mass or less.

[0049] Preferably, the α-iron oxide (α-Fe2O3) content in the ferrite powder is 0.0% by mass or more and 3.0% by mass or less. α-Fe2O3 is a heterophase that is an antiferromagnetic material. If there is an excessive amount of α-Fe2O3, the magnetic properties of the ferrite powder are degraded. If the amount of α-Fe2O3 is within the above-mentioned range, the effect on the magnetic properties is small. Therefore, by keeping the amount of α-Fe2O3 within this range, it is possible to prevent a decrease in the magnetic properties, particularly the saturation magnetization (σs), and a decrease in the saturation magnetic flux density when used in an inductor.

[0050] The particles constituting the ferrite powder may be either single crystal or polycrystalline. However, polycrystalline is preferable. The average crystallite size of the particles constituting the ferrite powder is preferably 150 nm or more and 220 nm or less.

[0051] Preferably, the volume average particle size (D50) of the ferrite powder is 2.0 μm or more and 20 μm or less. Here, the volume average particle size refers to the cumulative 50% diameter (D50) in the volume particle size distribution. By increasing D50 to 2.0 μm or more, it is possible to suppress the aggregation of the ferrite powder, and it is possible to further improve the moldability and packing properties. In addition, although it depends on the manufacturing conditions, by increasing the particle size to a certain extent, it is possible to control the vacancy rate of the ferrite powder. That is, ferrite particles with a small particle size have a large specific surface area. Therefore, oxidation is likely to progress in the high-temperature heat treatment process such as thermal spraying during the production of the ferrite powder, and γ-Fe2O3 having vacancies tends to be easily generated. From the viewpoint of improving the moldability and packing properties and controlling the vacancy rate, D50 is more preferably 2.3 μm or more, more preferably 2.5 μm or more, particularly preferably 2.8 μm or more, and most preferably 3.0 μm or more. On the other hand, by keeping D50 at 20 μm or less, the generation of interparticle voids can be suppressed, resulting in better packing properties. From the viewpoint of improving packing properties, D50 is more preferably 12 μm or less, even more preferably 10 μm or less, particularly preferably 8.0 μm or less, and most preferably 7.0 μm or less.

[0052] Preferably, the shape factor SF-1 of the ferrite powder is 100 or more and 110 or less. SF-1 is an index of the sphericity of the particles constituting the powder. For a perfect sphere, SF-1 is 100, and the more it deviates from a sphere, the higher it becomes. By suppressing SF-1 to 110 or less, the fluidity of the powder is increased and the moldability and packability are improved, regardless of whether the particles are spherical or polyhedral. SF-1 is more preferably 105 or less, and even more preferably 103 or less.

[0053] Preferably, the shape factor SF-2 of the ferrite powder is 100 or more and 110 or less. SF-2 is an index showing the degree of unevenness of the particle surface constituting the powder. If there is no surface unevenness, SF-2 is 100, and the deeper the unevenness, the higher it becomes. If the ferrite powder has a microscopic step structure on the particle surface, when it is made into a composite material or composite, the adhesion with the resin is improved and the falling off of the particles is suppressed. Therefore, SF-2 is moderately high, specifically, 101 or more is more preferable. On the other hand, if SF-2 is excessively high, the flowability of the powder decreases, which may lead to a decrease in moldability and filling ability. SF-2 is more preferably 105 or less, and even more preferably 103 or less.

[0054] Preferably, the ferrite powder has a BET specific surface area of ​​0.2 m 2 / g or more 2.0m 2 / g or less. BET specific surface area is 0.2 m 2 By increasing the BET specific surface area to 0.3 m / g or more, the generation of voids between particles is suppressed, and the packing property can be further improved. In addition, by keeping the BET specific surface area within the above range, the adhesion to resins is improved when the ferrite powder is applied to composite materials or composites. From the viewpoint of packing property and improved adhesion, the BET specific surface area is set to 0.3 m 2 On the other hand, the BET specific surface area is preferably 2.0 m 2 By keeping the BET specific surface area at 1.5 m or less, aggregation of the ferrite powder is suppressed, which leads to improved moldability and packing properties. In addition, although it depends on the manufacturing conditions, by reducing the BET specific surface area to a certain extent, it becomes possible to control the vacancy rate of the ferrite powder within an appropriate range. From the viewpoint of improving moldability and packing properties and controlling the vacancy rate, the BET specific surface area is set to 1.5 m 2 / g or less is more preferable, and 1.0m 2 / g or less is more preferable.

[0055] Preferably, the tap density of the ferrite powder is 0.50 g / cm 3 More than 3.50g / cm 3The tap density can be increased by mixing small and large particles, resulting in better overall packing of the ferrite powder. The tap density is 1.00 g / cm 3 More than 3.00g / cm 3 The following is more preferred:

[0056] Preferably, the true specific gravity of the ferrite powder is 5.00 g / cm 3 That's all. By increasing the true specific gravity, it is possible to improve the magnetic properties of the ferrite powder, particularly the saturation magnetization (σs) and magnetic permeability (μ). The true specific gravity is 5.05 g / cm 3 The above is more preferable.

[0057] Preferably, the real part of magnetic permeability (μ') of the ferrite powder at 50 MHz is 7.0 or more. By increasing μ', the magnetic properties of elements such as inductors containing the ferrite powder can be improved. μ' is more preferably 7.5 or more, and even more preferably 8.0 or more.

[0058] Preferably, the μ'Q product of the ferrite powder at 50 MHz is 400 or more. By increasing the μ'Q product, it is possible to achieve a good balance between high magnetic permeability and low loss of the ferrite powder. The μ'Q product is more preferably 450 or more, and even more preferably 500 or more. The μ'Q product is calculated according to the following formula (11) using the real part (μ') of the complex permeability and the loss factor (tan δ) of the ferrite powder. The loss factor (tan δ) is calculated according to the following formula (12) using the real part (μ') and imaginary part (μ'') of the complex permeability.

[0059]

number

[0060] Preferably, the permeability change rate of the ferrite powder at 50 MHz is 0.040 or less. The permeability change rate is an index of the degree of change in permeability over time, and the smaller the permeability change rate, the smaller the change in permeability over time, that is, the better the stability over time. The change in permeability over a long period of time is considered to be a relaxation phenomenon and is approximated by a power law. Therefore, the permeability μ'(t) after an elapsed time t (unit: hr) is in an approximate linear relationship with the natural logarithm ln(t) of time t, as shown in the following formula (13). In the following formula (13), A represents the slope of the line, and B represents the intercept. Then, as shown in the following formula (14), the absolute value of the slope A of the line is defined as the permeability change rate.

[0061]

number

[0062] If the rate of change in magnetic permeability is 0.040 or less, it can be determined that the change in magnetic permeability over a long period of time is small. On the other hand, if the rate of change in magnetic permeability exceeds 0.040, the performance of the inductor changes over time when ferrite powder is used as the magnetic core filler of the inductor. This makes it difficult to obtain the performance (output) that was initially designed, and may lead to malfunction of the electronic device.

[0063] <<2. Ferrite powder manufacturing method>> The ferrite powder of the present embodiment is not limited in its manufacturing method as long as it satisfies the above-mentioned requirements, but is preferably manufactured by spraying a mixture of ferrite raw materials under predetermined conditions and then quenching, as shown below.

[0064] <Raw material mixture> First, the ferrite raw materials are mixed to prepare a raw material mixture. As the ferrite raw materials, known ferrite raw materials such as oxides, carbonates, hydroxides and / or chlorides can be used. The raw materials can be mixed using a known mixer such as a Henschel mixer in either a dry or wet manner, or both.

[0065] <Pre-calcination and grinding> Next, the obtained raw material mixture is pre-calcined to obtain a pre-calcined product. The pre-calcination may be performed by a known method. For example, it may be performed under known conditions using a furnace such as a rotary kiln, a continuous furnace, or a batch furnace. For example, the pre-calcination may be performed under an atmosphere such as air at a temperature of 700°C to 1300°C for a period of 2 hours to 12 hours.

[0066] <Granulation> The resulting calcined product is then pulverized and granulated to obtain a granulated product. The pulverization method is not particularly limited. For example, a known pulverizer such as a vibration mill, a ball mill, or a bead mill may be used, and either or both of a dry method and a wet method may be used. The granulation method may also be a known method. For example, water and, if necessary, additives such as a binder such as polyvinyl alcohol (PVA), a dispersant, and / or an antifoaming agent may be added to the calcined product after pulverization to adjust the viscosity, and then the product is granulated using a granulator such as a spray dryer.

[0067] In the production of normal ferrite powder (particles), the binder component is generally removed before the main sintering. In contrast, in the production method of the present embodiment, it is preferable not to perform the binder removal process. By performing thermal spraying in a state in which the binder component is contained and controlling the amount of carbon contained in the granulated material, the vacancy rate of the finally obtained ferrite powder can be adjusted to be within an appropriate range.

[0068] Preferably, the carbon content of the granulated material is 0.08% by mass or more and 0.20% by mass or less. Although it depends on the thermal spraying conditions, the vacancy rate of the ferrite powder can be controlled to a desired value by limiting the carbon content of the granulated material within the above-mentioned range. On the other hand, if the carbon content is too low, the oxygen concentration in the surrounding environment of the particles passing through the flame in the subsequent thermal spraying process increases. As a result, the oxidation of the ferrite powder advances, promoting the generation of γ-Fe2O3, which may lead to an increase in the vacancy rate. On the other hand, if the carbon content is too high, the decomposition of the binder component of the granulated material does not proceed sufficiently. As a result, there is a risk of particles having an excessively large particle size and an uneven shape being generated.

[0069] <Thermal spraying> Next, the obtained granules are sprayed to produce a sprayed material. In the spraying process, the granules transported by gas pass through a spray flame and melt to form ferrite. The ferrite particles are then quenched and solidified with a cooling gas, and collected by a cyclone or filter. The cooling gas may be air at room temperature, or air or an inert gas (nitrogen gas, helium gas, argon gas, etc.) at a temperature lower than room temperature may be used to prevent quenching and oxidation. If necessary, the collected ferrite particles may be classified. In the classification process, the particle size is adjusted to the desired particle size using existing methods such as air classification (air flow classification), mesh filtration, sieve classification, and sedimentation. It is also possible to separate and collect large particle size particles in one process using air flow classification such as a cyclone.

[0070] In order to obtain ferrite particles with a step structure (spherical-like step particles), it is important to spray the granulated material under specified conditions. During spraying, the entire granulated material is melted and then rapidly cooled. Although the detailed mechanism is unknown, it is speculated that a polygonal step structure reflecting the crystal structure of ferrite is formed on the particle surface when melted at high temperatures, and that this structure is maintained by rapid cooling. In contrast, if the granulated material is sintered at a temperature below the melting temperature to produce ferrite particles, it is believed that the polygonal step structure is difficult to form, and even if it is formed, the step structure will disappear when cooled slowly.

[0071] In thermal spraying, a mixture of combustion gas and oxygen can be used as a combustible gas combustion flame source. The volume ratio of the combustion gas to oxygen is preferably 1:3.5 to 1:6.0, more preferably 1:4.9 to 1:6.0, and even more preferably 1:4.9 to 1:5.3. This allows the volatilized raw material to condense, and the formation of small-diameter particles can be favorably promoted. For example, a combustion gas flow rate of 7 Nm 3 / hr total oxygen flow rate 35Nm 3 / hour (the volume ratio of combustion gas to oxygen is 1:5).

[0072] If there is an excessive amount of combustion gas or oxygen during combustion, the gas not used in the combustion may take away the heat during combustion, causing the flame temperature to drop. The amount of excess combustion gas not used in the combustion is preferably 20% or less of the amount of combustion gas supplied. Also, the amount of excess oxygen not used in the combustion is preferably 20% or less of the amount of oxygen supplied.

[0073] The amount of combustion gas relative to the amount of raw material supplied is also important. Specifically, the net fuel gas ratio is 1.05 Nm 3 / kg or more 2.00Nm 3 / kg or less is preferable. Here, the net gas amount ratio is the ratio of the net combustion gas amount to the raw material supply amount, and is calculated according to the following formula (15). Also, the net combustion gas amount is the amount of combustion gas used for net combustion, and is calculated according to the following formula (16) or (17).

[0074]

number

number

number

[0075] Examples of the combustion gas used in thermal spraying include flammable gases such as propane gas, propylene gas, and acetylene gas, and among these, propane gas is preferred. In order to transport the granulated material into the flammable gas, a carrier gas such as nitrogen, oxygen, or air can be used. The flow rate of the transported granulated material is preferably 20 m / sec or more and 60 m / sec or less. The thermal spraying temperature is preferably 1000°C or more and 3500°C or less, and more preferably 2000°C or more and 3500°C or less.

[0076] The amount of raw material supplied during thermal spraying is also important. That is, the mechanism of the appearance of the step structure changes depending on the time it takes for the raw material particles to cool down from the temperature when passing through the thermal spray flame (the amount of heat given to the raw material particles) to room temperature. In particular, the step structure appears when the primary raw material particles that have passed through the high-temperature flame are rapidly cooled. Even with the same temperature flame, the step structure becomes less likely to appear if the number of passes per unit time of the primary raw material particles (the amount of processing per hour) increases. From the viewpoint of appearing the step structure, it is preferable to supply a small amount of raw material for thermal spraying. For example, the supply amount is preferably 20 kg / hour or less, more preferably 10 kg / hour or less, and most preferably 7 kg / hour or less.

[0077] When ferrite powder contains elements with high vapor pressure such as zinc (Zn), the step structure is effectively generated. However, in addition to the contained elements, the conditions during thermal spraying are also important. In other words, the step structure is easily generated when the sprayed material that has passed through the thermal spray flame cools from a high temperature at an appropriate speed. The cooling rate in sintering, which is different from thermal spraying, is relatively slow. Therefore, as the grain boundaries of the particles grow, the periphery of the step structure becomes non-linear.

[0078] The cooling rate also has a large effect on magnetic properties, especially the frequency characteristics of magnetic permeability. That is, particles that are rapidly cooled during thermal spraying have a relatively small grain size. Therefore, the loss factor (tan δ) is small at frequencies higher than 10 MHz. On the other hand, particles that are slowly cooled during sintering have a large grain size, so the loss factor at high frequencies is large.

[0079] In this way, it is possible to adjust the properties of the ferrite powder by controlling the thermal spraying conditions. By performing thermal spraying under preferred conditions, it is possible to suitably adjust the shape of the obtained ferrite particles. In addition, it is possible to control the vacancy rate of the ferrite particles within a desired range.

[0080] <<3. Ferrite-resin composite material>> The ferrite resin composite material of the present embodiment contains the above-mentioned ferrite powder and resin. This composite material prevents the ferrite particles from falling off without impairing moldability and packing properties.

[0081] Examples of resins constituting the composite material include epoxy resins, urethane resins, acrylic resins, silicone resins, polyamide resins, polyimide resins, polyamideimide resins, fluororesins, and combinations thereof. The silicone resin may be a modified silicone resin modified with acrylic, urethane, epoxy, and / or fluorine.

[0082] The composite material may contain components other than the ferrite powder and the resin, such as, for example, a solvent, a filler (organic filler, inorganic filler), a plasticizer, an antioxidant, a dispersant, a colorant such as a pigment, and / or thermally conductive particles.

[0083] The ratio of the ferrite powder to the total solid content in the composite material is preferably 50% by mass to 95% by mass, more preferably 80% by mass to 95% by mass. The ratio of the resin to the total solid content in the composite material is preferably 5% by mass to 50% by mass, more preferably 5% by mass to 20% by mass. By setting the ratio of the ferrite powder and the resin within the above ranges, the dispersion stability of the ferrite powder in the composite material, as well as the storage stability and moldability of the composite material, become excellent, and the mechanical strength and magnetic properties of the composite (molded body) obtained by molding the composite material become excellent.

[0084] <<4. Ferrite-resin composite>> The ferrite resin composite of the present embodiment includes a molded body of the above-mentioned ferrite resin composition. That is, the composite is produced by molding the ferrite resin composition. The molding method is not particularly limited, and examples thereof include compression molding, extrusion molding, injection molding, blow molding, and calendar molding. Alternatively, a coating film of the composite material may be formed on a substrate.

[0085] <<5. Electronic Components>> The electronic component of the present embodiment includes the above-mentioned ferrite resin composite. The electronic component may be a known component that utilizes the magnetic properties of ferrite. Examples of such components include inductors such as transformers and communication coils. The electronic component of the present embodiment includes ferrite powder with small time change in magnetic permeability, and therefore has the advantage of excellent stability over time. EXAMPLES

[0086] The present embodiment will be described in more detail with reference to the following examples and comparative examples, however, the present invention is not limited to the following examples.

[0087] (1) Preparation of ferrite powder [Examples 1-10] <Raw material mixture> The raw materials α-iron oxide (α-Fe2O3), manganese tetroxide (Mn3O4), zinc oxide (ZnO) and copper oxide (CuO) were weighed and mixed using a Henschel mixer. The raw materials were weighed so that the raw material blend amounts calculated as Fe2O3, MnO, ZnO and CuO were the molar amounts shown in Table 1 below.

[0088] <Pre-calcination and grinding> The resulting mixture was pre-fired in a rotary kiln. The pre-fired mixture was held for 4 hours under the conditions (temperature and atmosphere) shown in Table 1 below. The pre-fired product was then coarsely pulverized using a dry bead mill (3 / 16 inch steel ball beads). Water was then added and the mixture was finely pulverized using a wet bead mill (0.65 mm zirconia beads) to obtain a slurry. The particle size of the pulverized powder in the slurry is shown in Table 1 below.

[0089] <Granulation> To the obtained slurry, polyvinyl alcohol (PVA, 10% aqueous solution) was added as a binder. At this time, the amount of PVA added was adjusted. The amount of PVA added in terms of solid content relative to the pulverized powder is shown in Table 1 below. The slurry to which the binder was added was then granulated using a spray dryer.

[0090] <Thermal spraying> The obtained granules were sprayed and quenched in a combustible gas combustion flame. The spraying was performed under the conditions shown in Table 1 below (propane gas flow rate, total oxygen flow rate, raw material supply oxygen flow rate, combustion oxygen flow rate, raw material supply amount, air volume, and spraying temperature). In addition, air for cooling was introduced into the combustion gas immediately after spraying to quench the product. Furthermore, the product was collected using a cyclone installed downstream to obtain a sprayed material. Coarse powder was removed from the obtained sprayed material using a sieve, and fine powder was further removed using a classification device to obtain a ferrite powder consisting of Mn-Zn ferrite particles.

[0091] The manufacturing conditions of the ferrite powders of Examples 1 to 10 are summarized in the following Table 1. Examples 1 and Examples 7 to 10 are embodiment samples, and Examples 2 to 6 are comparative examples.

[0092] [Table 1]

[0093] (2) Evaluation The ferrite powders produced in Examples 1 to 10 were evaluated for various properties as follows.

[0094] <Chemical analysis> The ferrite powder was subjected to chemical analysis to determine the metal content. First, 0.2 g of ferrite powder was weighed, and 60 ml of pure water, 20 ml of 1N hydrochloric acid, and 20 ml of 1N nitric acid were added to it, and then heated to prepare an aqueous solution in which the sample was completely dissolved. The obtained aqueous solution was set in an ICP analyzer (Shimadzu Corporation, ICPS-10001V) to measure the metal content.

[0095] <Oxidation-reduction titration> The divalent iron (Fe) contained in the ferrite powder was determined by redox titration. 2+ The amount of 1,2-dichloromethane (1,2,3,4-trifluoroethylene) was determined. The redox titration was performed according to JIS M 8213, using potassium permanganate instead of potassium dichromate.

[0096] <xrd> The ferrite powder was analyzed by X-ray diffraction (XRD) under the following conditions.

[0097] - X-ray diffraction equipment: PANalytical X'pert MPD (including high-speed detector) - Source: Co-Kα - Tube voltage: 45kV -Tube current: 40mA - Scan speed: 0.002° / sec (continuous scan) - Scan range (2θ): 15~90°

[0098] Based on the obtained X-ray diffraction profile, the content ratio of each of the spinel phase, ZnO phase, and α-Fe2O3 phase in the ferrite powder was determined. In addition, the X-ray diffraction profile was subjected to Rietveld analysis to estimate the lattice constant of the spinel phase, and the crystallite size of the spinel phase was calculated according to Scherrer's formula.

[0099] In addition, the amounts of Fe, Mn, Zn, and Cu (unit: mass%) determined by chemical analysis, and the amount of divalent iron (Fe 2+ The vacancy rate and Fe excess ratio of the spinel phase were calculated using the amount of α-Fe2O3 (unit: mass%) obtained by XRD analysis and the amount of α-Fe2O3 (unit: mass%) obtained by XRD analysis. Specifically, the calculations were performed according to the above formulas (1) to (10).

[0100] <Particle shape and surface structure> The shape and surface structure of particles in the ferrite powder were evaluated as follows. First, the ferrite powder was observed using a scanning electron microscope (SEM; Hitachi High-Technologies Corporation, SU-8020). During observation, the magnification was set to 50,000 times. Then, an image was taken with 1 to 30 particles, preferably 1 to 10 particles, in the field of view. The images were taken randomly from 10 fields of view to confirm the presence or absence of a polygonal step structure.

[0101] <shape factor> The shape factors (SF-1 and SF-2) of the ferrite powder were determined using a particle image analyzer (Malvern Panalytical, Morphologi G3). First, the ferrite powder was analyzed using the particle image analyzer. During the analysis, image analysis was performed for each of 30,000 particles in the powder, and the circularity, perimeter, and equivalent circle diameter (CE Diameter) were automatically measured. At this time, an objective lens with a magnification of 10 times was used, and the sample amount was 3 mm 3 、 and the particles were dispersed on a slide glass using the dispersion jig attached to this apparatus under the condition that the dispersion pressure was 5 bar.

[0102] Among the obtained data, the average of the data of the particles within ±5% of the volume average particle diameter was determined as the average circularity, average perimeter, and average equivalent circle diameter (CE Diameter), and using these, SF-1 and SF-2 were calculated according to the following equations (18) and (19).

[0103]

Equation

Equation

[0104] <Tap density> The tap density of the ferrite powder was measured in accordance with JIS Z 2512-2012 using a USP tap density measuring device (Hosokawa Micron Corporation, Powder Tester PT-X).

[0105] <True specific gravity> The true specific gravity of the ferrite powder was measured in accordance with JIS Z8807:2012 using the gas displacement method. Specifically, the measurement was performed using a fully automatic true density measuring device (Mounttech Co., Ltd., Macpycno).

[0106] <BET specific surface area> The BET specific surface area of ​​the ferrite powder was measured using a specific surface area measuring device (Mountec Co., Ltd., Macsorb HM model-1208). First, about 10 g of the ferrite powder was placed on a medicine packing paper and degassed in a vacuum dryer. After confirming that the degree of vacuum was 0.1 MPa or less, the powder was heated at 200°C for 2 hours to remove moisture adhering to the particle surface. Then, the ferrite powder from which moisture had been removed (about 0.5 to 4 g) was placed in a standard sample cell dedicated to the measuring device and accurately weighed with a precision balance. The weighed ferrite powder was then set in the measuring port of the measuring device and measured by the one-point method. The measuring atmosphere was set at a temperature of 10 to 30°C and a relative humidity of 20 to 80% (no condensation).

[0107] <Particle size distribution> The particle size distribution of the ferrite powder was measured as follows. First, 10 g of ferrite powder and 80 ml of water were placed in a 100 ml beaker, and two drops of sodium hexametaphosphate were added as a dispersant. Then, the mixture was dispersed using an ultrasonic homogenizer (SMT Corporation, UH-150 type). The output level of the ultrasonic homogenizer was set to 4 and dispersion was performed for 20 seconds. After that, bubbles formed on the surface of the homogenizer were removed, and the resulting dispersion was introduced into a laser diffraction particle size distribution measuring device (Shimadzu Corporation, SALD-7500nano) and measured. The measurement conditions were pump speed 7, built-in ultrasonic irradiation time 30, and refractive index 1.70-050i. From this measurement, the 10% diameter (D10), 50% diameter (volume average particle size, D50), and 90% diameter (D90) in the volume particle size distribution were obtained.

[0108] <Magnetic properties - saturation magnetization, residual magnetization and coercive force> The magnetic properties (saturation magnetization, residual magnetization, and coercivity) of the ferrite powder were measured as follows. First, the ferrite powder was packed into a cell with an inner diameter of 5 mm and a height of 2 mm, and set in a vibrating sample magnetic measurement device (Toei Industry Co., Ltd., VSM-C7-10A). A magnetic field was applied and swept up to 5 kOe, and then the applied magnetic field was reduced to draw a hysteresis curve. From the data of this curve, the saturation magnetization σs, residual magnetization σr, and coercivity Hc of the ferrite powder were obtained.

[0109] <Magnetic permeability> The magnetic permeability of the ferrite powder was measured using an RF impedance / material analyzer (Agilent Technologies, E4991B) and a magnetic material measurement electrode (16454A). First, 9 g of ferrite powder and 1 g of binder resin (Kynar301F: polyvinylidene fluoride) were placed in a polyethylene container (contents 100 ml), and the mixture was stirred and mixed using a ball mill at a rotation speed of 100 rpm. Next, the resulting mixture (about 0.6 g) was filled into a die (inner diameter 4.5 mm, outer diameter 13 mm) and pressed for 1 minute at a pressure of 40 MPa using a press machine to produce a molded body. The obtained molded body was heated and cured at 180 °C for 1 hour using a hot air dryer to prepare a measurement sample. The obtained measurement sample was set in the RF impedance / material analyzer, and the outer diameter, inner diameter, and height of the measurement sample that had been measured in advance were entered. During the measurement, the amplitude was set to 100 mV, and the measurement frequency range was swept from 1 MHz to 3 GHz on a logarithmic scale.Then, the real part (μ') and the imaginary part (μ'') of the complex permeability at a frequency of 50 MHz were obtained.

[0110] In addition, the loss factor (tan δ) and the μ′Q product were calculated according to the above formulas (11) and (12) using the real part (μ′) and imaginary part (μ″) of the complex permeability after 72 hours at 50 MHz.

[0111] Furthermore, the change over time of the real part of magnetic permeability (μ′) at 50 MHz was measured up to an elapsed time of 17,520 hours.Then, using the obtained data, the rate of change of magnetic permeability was calculated according to the above formulas (13) and (14).

[0112] (3) Evaluation results The evaluation results obtained for the ferrite powders of Examples 1 to 10 are shown in the following Tables 2 to 6. Moreover, the time changes in the real part of magnetic permeability (μ') of the ferrite powders of Examples 1 and 5 are shown in Figure 1 (Example 1) and Figure 2 (Example 5).

[0113] The ferrite powders of Comparative Examples 2 and 3 had a low Fe content of 54.53 mass% or less and a high Zn content of 3.64 mass% or more (Table 2). Therefore, the loss factor (tan δ) at 50 MHz was high, 0.028 or more, and the μ'Q product was low, 330 or less (Table 5). It was found that these ferrite powders had high loss and were unsuitable for use in high-frequency applications such as inductors.

[0114] The ferrite powder of Example 4, which is a comparative example, had a high Fe content of 63.11 mass % and a Zn content of zero (0) (Table 2). Therefore, the real part of magnetic permeability (μ') was low at 6.45 (Table 5). It was found that this ferrite powder had low magnetic permeability and was unsuitable for use in applications such as inductors.

[0115] The ferrite powder of Example 5, which is a comparative example, had a high Zn content of 3.30 mass% (Table 2). Therefore, the loss factor (tan δ) was high at 0.024 and the μ'Q product was low at 379 (Table 5). In addition, the vacancy rate was high at 100.0% and the rate of change in magnetic permeability was high at 0.061 (Tables 3 and 6). It was found that this ferrite powder had high loss and poor stability of magnetic permeability over time.

[0116] The ferrite powder of Example 6, which is a comparative example, contained aggregates (Table 4). Therefore, the shape factors SF-1 and SF-2 were large, 126 to 130, and the volume average particle size (D50) was large, 23.11 μm (Table 4). In addition, no step structure was confirmed on the particle surface (Table 4). This ferrite powder had a large loss factor (tan δ) of 0.084 and a small μ'Q product of 107 (Table 5). In addition, the rate of change in magnetic permeability was large, 0.081 (Table 6). It was found that this ferrite powder had a large loss and poor stability of magnetic permeability over time. In addition, this ferrite powder was considered to have poor filling properties when made into a composite material (composite material).

[0117] In contrast, the ferrite powders of Examples 1 and 7 to 10, which are working examples, had a true spherical shape (Table 4). Therefore, SF-1 and SF-2 were small at 101 to 102, had a polygonal step structure on the surface, and D50 was relatively small at 9.92 μm or less (Table 4). The vacancy rate was also 80.5 mol% or less (Table 3). These ferrite powders had a permeability real part (μ') of 8.23 ​​or more and a μ'Q product of 439 or more (Table 5). In addition, the permeability change rate was small at 0.038 or less, and in particular, the permeability change rate of the ferrite powder of Example 9 was very small at 0.005 (Table 6). Therefore, it was found that these ferrite powders had high permeability and low loss, as well as small permeability time change.

[0118] From the above results, it can be seen that according to this embodiment, a ferrite powder having excellent stability of magnetic permeability over time can be obtained while maintaining high filling properties, high magnetic permeability at high frequencies, and low loss.

[0119] [Table 2]

[0120] [Table 3]

[0121] [Table 4]

[0122] [Table 5]

[0123] [Table 6] < / xrd>

Claims

1. A ferrite powder containing iron (Fe) in an amount of 56.0 mass% or more and 63.0 mass% or less, manganese (Mn) in an amount of 7.0 mass% or more and 13.0 mass% or less, and zinc (Zn) in an amount of 1.0 mass% or more and 3.0 mass% or less.

2. The ferrite powder includes spherical ferrite particles mainly composed of a spinel phase, The spinel phase has an iron (Fe) amount in excess of the stoichiometric ratio and a vacancy rate of 0 mol% or more and 90 mol% or less, The ferrite powder has a shape factor SF-1 of 100 or more and 110 or less, and a volume average particle size (D50) of 2.0 μm or more and 20 μm or less. The ferrite powder according to claim 1.

3. α-iron oxide (α-Fe 2 O 3 The ferrite powder according to claim 1 or 2, wherein the content of said element (I) is 0.0 mass % or more and 3.0 mass % or less.

4. The ferrite powder according to claim 1 or 2, wherein the copper (Cu) content is 0.0 mass% or more and 0.5 mass% or less.

Citation Information

Patent Citations

  • Low-loss soft magnetic ferrite material for 5G and preparation method thereof

    CN113200741A

  • Mn-zn ferrite magnetic material

    JP1994290926A

  • Ferrite powder and method for producing the same

    JP2021066648A

  • Composite particle, powder, resin composition, and molded article

    WO2019159799A1

  • Ferrite powder, ferrite resin composite material, and electromagnetic shielding material, electronic material, or electronic component

    WO2022209640A1