Production method of division light fiber ribbon

By applying controlled resin coating and ultraviolet irradiation to form a tape and bind layer on bundled optical fibers, the method enhances the splittability of optical fiber ribbons, ensuring effective separation of optical fiber tapes without damage.

JP2024144007APending Publication Date: 2024-10-11FURUKAWA ELECTRIC CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023147016
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-09-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The divisibility between the tape layer and the bind layer in existing optical fiber ribbons is insufficient, affecting the splittability of optical fiber tapes.

Method used

A method involving the application of a first and second resin coating step followed by ultraviolet irradiation to form a tape layer and a bind layer on bundled optical fibers, with controlled temperature and irradiation conditions to enhance the splitting properties of the optical fiber ribbon.

Benefits of technology

The method results in a splittable optical fiber ribbon with improved splitting properties, allowing for effective separation of bundled optical fiber tapes without damage to the tape layer or the optical fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144007000001_ABST
    Figure 2024144007000001_ABST
Patent Text Reader

Abstract

To provide a production method of division light fiber ribbon having preferable splittable properties.SOLUTION: There is provided a production method of a division light fiber ribbon in one embodiment comprising: a first resin coating step for coating a first resin on surfaces of multiple light fiber colored cores which are arranged almost in parallel; a first ultraviolet radiating step for radiating light having a prescribed wavelength to the first resin, by a first UV light source, then forming a tape layer on the surface for forming a batch type light fiber tape core; a second resin coating step for coating a second resin on the surfaces of the multiple batch type light fiber tape cores arranged almost parallel; and a second ultraviolet radiating step for radiating the light of the prescribed wavelength to the second resin by a second UV light source, for forming a bind layer on the multiple batch type light fiber tape cores. A surface temperature immediately after the first ultraviolet radiating step is 88°C or greater.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a splittable optical fiber ribbon. [Background technology]

[0002] Patent Document 1 proposes an optical fiber ribbon in which the ribbon layer and the bind layer each use an ultraviolet-curable resin having different properties. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 2820693 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the optical fiber ribbon according to Patent Document 1 may have insufficient divisibility between the ribbon layer and the bind layer. The divisibility of the optical fiber ribbon means the ease of dividing the bundled optical fiber ribbons from the bind layer that covers the outer periphery of the bundled optical fiber ribbons with an ultraviolet curable resin into the individual bundled optical fiber ribbons.

[0005] The present invention has been made in consideration of the above problems, and an object of the present invention is to improve the splitting properties of a splittable optical fiber ribbon. [Means for solving the problem]

[0006] According to one aspect of the present invention, there is provided a method for manufacturing a splittable optical fiber ribbon, comprising: a first resin application step of applying a first resin to the surfaces of a plurality of colored optical fiber cores arranged approximately parallel to each other; a first ultraviolet irradiation step of irradiating the first resin with light of a predetermined wavelength using a first UV light source to form a tape layer on the surface, thereby forming an integrated optical fiber ribbon core; a second resin application step of applying a second resin to the surfaces of a plurality of the integrated optical fiber ribbon cores arranged approximately parallel to each other; and a second ultraviolet irradiation step of irradiating the second resin with light of the predetermined wavelength using a second UV light source to form a binding layer on the plurality of integrated optical fiber ribbon cores, wherein the surface temperature of the tape layer immediately after the first ultraviolet irradiation step is 88°C or higher. Effect of the Invention

[0007] According to the present invention, a method for producing a splittable optical fiber ribbon having excellent splittability can be provided. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a cross-sectional view of a colored optical fiber according to the present embodiment. [Figure 2A] FIG. 2A is a cross-sectional view of an integrated optical fiber ribbon according to the present embodiment. [Figure 2B] FIG. 2B is a cross-sectional view of an integrated optical fiber ribbon in this embodiment. [Figure 3A] FIG. 3A is a cross-sectional view of a splittable optical fiber ribbon in this embodiment. [Figure 3B] FIG. 3B is a cross-sectional view of a splittable optical fiber ribbon in this embodiment. [Figure 4] FIG. 4 is a schematic diagram of a manufacturing apparatus for a splittable optical fiber ribbon according to this embodiment. [Diagram 5] FIG. 5 is a block diagram of the control device in this embodiment. [Figure 6]FIG. 6 is a flowchart of a method for producing a splittable optical fiber ribbon in this embodiment. [Figure 7] FIG. 7 is a flowchart of a method for manufacturing a tape layer in this embodiment. [Figure 8] FIG. 8 is a flowchart of a method for manufacturing a bind layer in this embodiment. [Figure 9A] FIG. 9A shows an example of a division pattern of a split-type optical fiber ribbon in this embodiment. [Figure 9B] FIG. 9B shows an example of a division pattern of the split type optical fiber ribbon in this embodiment. [Figure 9C] FIG. 9C shows an example of a division pattern of a split-type optical fiber ribbon in this embodiment. [Figure 9D] FIG. 9D shows an example of a division pattern of a split-type optical fiber ribbon in this embodiment. [Figure 9E] FIG. 9E shows an example of a division pattern of a split-type optical fiber ribbon in this embodiment. [Figure 9F] FIG. 9F shows an example of a division pattern of a split-type optical fiber ribbon in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the specification, the same reference numerals refer to substantially the same components.

[0010] FIG. 1 is a cross-sectional view of a colored optical fiber 1 in this embodiment. The colored optical fiber 1 includes a bare optical fiber 11, a primary layer 12, a secondary layer 13, and a colored layer 14. The bare optical fiber 11 is made of, for example, quartz glass. The primary layer 12 is made of an ultraviolet-curable resin and is coated on the outer periphery of the bare optical fiber 11. The secondary layer 13 is made of an ultraviolet-curable resin and is coated on the outer periphery of the primary layer 12. The primary layer 12 and the secondary layer 13 are each formed by curing the ultraviolet-curable resin by irradiation with ultraviolet light. The bare optical fiber 11, the primary layer 12, and the secondary layer 13 are collectively referred to as an optical fiber strand.

[0011] The colored layer 14 is formed of an ultraviolet-curable resin and is coated on the outer periphery of the secondary layer 13. Like the primary layer 12 and the secondary layer 13, the colored layer 14 is formed by curing the ultraviolet-curable resin by irradiation with ultraviolet rays. The ultraviolet-curable resin forming the colored layer 14 is an oligomer, a monomer, or the like, and may contain additives such as a photoinitiator, a photosensitizer, an ultraviolet absorber, an antioxidant, a chain transfer agent, a lubricant such as silicone, and titanium oxide.

[0012] The colored layer 14 is the outermost layer of the colored optical fiber core 1, and has the function of protecting the bare optical fiber 11, the primary layer 12, and the secondary layer 13 from external forces. The colored layer 14 is colored with a coloring agent mixed with a pigment or a lubricant so that the multiple colored optical fiber cores 1 can be distinguished from one another. The color types can be, for example, white, black, gray, purple, blue, light blue, green, brown, yellow, orange, pink, red, and the like. The colored layer 14 may be the secondary layer 13 colored with a coloring agent. When the colored secondary layer 13 also serves as the colored layer 14, the colored layer 14 protects the bare optical fiber 11 and the primary layer 12 from external forces.

[0013] In this embodiment, the case where the secondary layer 13 and the colored layer 14 are formed separately will be described, but it is also possible to color the secondary layer 13 without forming the colored layer 14, and have the secondary layer 13 function as the colored layer 14. In this case, the secondary layer 13 can be colored by adding a colorant similar to the colorant that is used to color the ultraviolet-curable resin used in the colored layer 14 to the ultraviolet-curable resin used in the secondary layer 13.

[0014] The ultraviolet curing resin is not particularly limited as long as it is polymerizable by irradiation with ultraviolet rays. The ultraviolet curing resin may be, for example, a resin that can be polymerized by photoradical polymerization. The ultraviolet curing resin may include, for example, an ultraviolet curing resin having a polymerizable unsaturated group such as an ethylenically unsaturated group that is polymerized and cured by ultraviolet rays, such as urethane (meth)acrylate such as polyether-based urethane (meth)acrylate and polyester-based urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, etc. It is preferable that the ultraviolet curing resin has at least two polymerizable unsaturated groups.

[0015] Examples of the polymerizable unsaturated group in the ultraviolet curable resin include groups having an unsaturated double bond such as vinyl group, allyl group, acryloyl group, methacryloyl group, etc., and groups having an unsaturated triple bond such as propargyl group, etc. Among the above, an acryloyl group or a methacryloyl group is preferable as the polymerizable unsaturated group in terms of polymerizability.

[0016] The ultraviolet curable resin may be a monomer, oligomer, or polymer that initiates polymerization and hardens upon irradiation with ultraviolet light, but the ultraviolet curable resin is preferably an oligomer. An oligomer is a polymer having a degree of polymerization of 2 to 100. In this specification, "(meth)acrylate" means one or both of acrylate and methacrylate. The ultraviolet curable resin contains any photopolymerization initiator (hereinafter referred to as "photoinitiator") that has sensitivity in the ultraviolet region.

[0017] Polyether-based urethane (meth)acrylate is a compound having a polyether segment, (meth)acrylate, and urethane bond, such as a reaction product of a polyol having a polyether skeleton with an organic polyisocyanate compound and a hydroxyalkyl (meth)acrylate. Polyester-based urethane (meth)acrylate is a compound having a polyester segment, (meth)acrylate, and urethane bond, such as a reaction product of a polyol having a polyester skeleton with an organic polyisocyanate compound and a hydroxyalkyl (meth)acrylate.

[0018] The ultraviolet curable resin may contain, in addition to the oligomer and the photoinitiator, for example, a diluting monomer, a photosensitizer, an ultraviolet absorber, an antioxidant, a silane coupling agent, a chain transfer agent, and various additives. The diluting monomer is a monofunctional (meth)acrylate or a polyfunctional (meth)acrylate. Here, the diluting monomer means a monomer for diluting the ultraviolet curable resin. It is possible to UV cure the ultraviolet curable resin using a UV-LED light source by adding a photoinitiator and a photosensitizer that have absorption in UV-LED to the ultraviolet curable resin. The photoinitiator may be, for example, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, and the like. The photosensitizer can be, for example, 2,4-diethyl-9H-thioxanthen-9-one, 2-isopropylthioxanthone, and the like.

[0019] The ultraviolet curable resin may contain a mercapto group-containing compound. The mercapto group-containing compound is a compound having at least one mercapto group in one molecule. The mercapto group-containing compound has the effect of terminating the polymerization of the polymerizable compound by reacting the mercapto group with a polymerizable compound such as urethane (meth)acrylate contained in the ultraviolet curable resin. The mercapto group-containing compound is not particularly limited, and examples thereof include (3-mercaptopropyl)trimethoxysilane, 3-mercaptopropionate isooctyl, 1-pentanethiol, as well as ethyl mercaptan, 1-butanethiol, 1-heptanethiol, 1-undecanethiol, 4-hydroxybenzenethiol, (2-mercaptoethyl)pyrazine, 2,3-butanedithiol, 3-methyl-2-butanethiol, 3-mercaptopropyltrimethoxysilane ... The thiol group may be, for example, butyronitrile, butyronitrile, butyl-1,2,4-triazole, 1,3,4-thiadiazole-2-thiol, isobutyl mercaptan, 4-methoxy-α-toluene thiol, 4,4′-biphenyl dithiol, trimethylsilyl methane thiol, 1,4-butanedithiol, 1,8-octanedithiol, (3-mercaptopropyl) triethoxy silane, 3-ethoxybenzene thiol, pentaerythritol tetra(3-mercaptopropionate), and the like.

[0020] The ultraviolet light is irradiated at an appropriate illuminance and dose using, for example, a mercury lamp or a UV-LED light source, etc. The Young's moduli of the primary layer 12, the secondary layer 13, and the colored layer 14 vary depending on the optical fiber manufacturing conditions (for example, linear speed, UV irradiation intensity, UV light source type, resin application temperature, etc.) and cannot be determined uniquely by the ultraviolet-curable resin used.

[0021] The primary layer 12 is a soft layer having a Young's modulus preferably between 0.1 MPa and 2.0 MPa, and has a function of buffering external forces applied to the bare optical fiber 11. The secondary layer 13 is a hard layer having a Young's modulus preferably between 500 MPa and 2000 MPa, and has a function of protecting the bare optical fiber 11 and the primary layer 12 from external forces.

[0022] The diameter of the bare optical fiber 11 may be, for example, 80 μm or more and 150 μm or less, and preferably 124 μm or more and 126 μm or less. The thickness of the primary layer 12 may be preferably 5 μm or more and 60 μm or less. The thickness of the secondary layer 13 may be preferably 5 μm or more and 60 μm or less. The thickness of the colored layer 14 may preferably be about several μm. Here, the diameter of the optical fiber strand may be determined by the sum of the diameter of the bare optical fiber 11, the length twice the thickness of the primary layer 12, and the length twice the thickness of the secondary layer 13. Therefore, the diameter of the bare optical fiber 11, the thickness of the primary layer 12, and the thickness of the secondary layer 13 may be selected so that the diameter of the optical fiber strand is, for example, about 190 to 250 μm.

[0023] FIG. 2A is a cross-sectional view of an integrated optical fiber ribbon 2 in this embodiment. The integrated optical fiber ribbon 2 includes M colored optical fibers 1A to 1M. Here, the number M of the colored optical fibers 1 is a natural number equal to or greater than 2. FIG. 2A shows the integrated optical fiber ribbon 2 when M=2. The colored optical fibers 1A and 1B are bundled in a belt shape via a tape layer 21. The tape layer 21 is formed by curing an ultraviolet-curable resin by irradiating ultraviolet rays. In a cross-sectional view, the tape layer 21 is formed in a substantially elliptical shape on the outer periphery of the colored optical fibers 1A and 1B, and extends along the longitudinal direction of the colored optical fibers 1A and 1B. The ultraviolet-curable resin forming the tape layer 21 may be the same material as the ultraviolet-curable resin forming the primary layer 12 and the secondary layer 13.

[0024] In this embodiment, the colored optical fiber core wires 1A, 1B have colored layers 14 of different colors. In an integrated optical fiber ribbon core wire 2 where M=3 or more, multiple colored optical fiber core wires 1 may have colored layers 14 of the same color. It is desirable that the colored optical fiber core wires 1A-1M have colored layers 14 of colors that allow the colored optical fiber core wires 1A-1M to be distinguished from one another.

[0025] FIG. 2B is a cross-sectional view of another bundled optical fiber ribbon 2 in this embodiment. Like the bundled optical fiber ribbon 2 in FIG. 2A, the bundled optical fiber ribbon 2 includes M colored optical fibers 1A to 1M. The colored optical fibers 1A and 1B are bundled in a belt shape via a tape layer 21. The tape layer 21 is formed by curing an ultraviolet-curable resin by irradiating ultraviolet rays. In a cross-sectional view, the tape layer 21 is formed in a substantially elliptical shape on the outer periphery of the colored optical fibers 1A and 1B, and extends along the longitudinal direction of the colored optical fibers 1A and 1B. The tape layer 21 is formed very thinly on the outer periphery of the colored optical fibers 1A and 1B.

[0026] FIG. 3A is a cross-sectional view of a splittable optical fiber ribbon 3 in this embodiment. The splittable optical fiber ribbon 3 includes N bundled optical fiber ribbons 2A to 2N. Here, the number N of the bundled optical fiber ribbons is a natural number equal to or greater than 2. FIG. 3A shows the splittable optical fiber ribbon 3 when N=2. The splittable optical fiber ribbon 3 includes bundled optical fiber ribbons 2A and 2B. The bundled optical fiber ribbon 2A and the bundled optical fiber ribbon 2B include colored optical fiber cores 1A and 1B and colored optical fiber cores 1C and 1D, respectively, and are bundled in a band shape via a binding layer 31. The binding layer 31 is formed by curing an ultraviolet-curable resin by irradiation with ultraviolet light. In a cross-sectional view, the binding layer 31 is formed in a substantially elliptical shape on the outer periphery of the bundled optical fiber ribbon 2A and 2B, and extends along the longitudinal direction of the bundled optical fiber ribbon 2A and 2B.

[0027] FIG. 3B is a cross-sectional view of another splittable optical fiber ribbon 3 in this embodiment. As with the splittable optical fiber ribbon 3 in FIG. 3A, the splittable optical fiber ribbon 3 includes N bundled optical fiber ribbons 2A to 2N. The bundled optical fiber ribbon 2A and the bundled optical fiber ribbon 2B each include colored optical fiber 1A, 1B and colored optical fiber 1C, 1D, and are bundled in a band shape via a binding layer 31. The binding layer 31 is formed by curing an ultraviolet-curable resin by irradiating ultraviolet rays. In a cross-sectional view, the binding layer 31 is formed in a substantially elliptical shape on the outer periphery of the bundled optical fiber ribbon 2A, 2B, and extends along the longitudinal direction of the bundled optical fiber ribbon 2A, 2B. The binding layer 31 is formed very thin on the outer periphery of the bundled optical fiber ribbon 2A, 2B. The thickness of the splittable optical fiber ribbon 3 can be, for example, 0.28 to 0.40 mm. The ultraviolet-curable resin forming the bind layer 31 may be the same material as the ultraviolet-curable resin forming the tape layer 21, but may have a different blend of additives such as photoinitiators, photosensitizers, ultraviolet absorbers, antioxidants, chain transfer agents, lubricants such as silicone, etc., a different type of monomer or oligomer, a different blend of monomers or oligomers, or a different degree of polymerization of the oligomers.

[0028] [Young's modulus measurement] The Young's modulus of the primary layer 12 corresponds to the ISM (In Situ Modulus). The Young's modulus of the primary layer 12 is measured by the following method. A commercially available stripper is used to strip off the primary layer 12 and the secondary layer 13 from the middle of the optical fiber by a length of several mm. One end of the optical fiber on which the coating layer is formed is fixed on a slide glass with an adhesive, and a load F is applied to the other end of the optical fiber on which the coating layer is formed. In this state, the displacement δ of the primary layer 12 at the boundary between the part where the coating layer is stripped off and the part where the coating layer is formed is read with a microscope. The load F applied to the other end of the optical fiber is set to 10, 20, 30, 50, and 70 gF (i.e., 98, 196, 294, 490, and 686 mN), and the rate (slope) of change in the load F with respect to the displacement δ is calculated. The calculated slope and the following formula (1) are used to calculate the primary elastic modulus. Since the primary elastic modulus corresponds to the ISM, the primary elastic modulus will be appropriately referred to as P-ISM below. P-ISM=(3F / δ)*(1 / 2πl)*ln(DP / DG)···(1)

[0029] The unit of P-ISM is [MPa]. In the right side of formula (1), F / δ is the rate (slope) of change of load (F) [gF] with respect to displacement δ [μm], l is the sample length (e.g., 10 mm), and DP / DG is the ratio of the outer diameter (DP) [μm] of the primary layer 12 to the outer diameter (DG) [μm] of the cladding of the optical fiber. Therefore, when calculating P-ISM using F, δ, l, and formula (1), a predetermined unit conversion is required. The outer diameter of the primary layer 12 and the outer diameter of the cladding can be measured by observing the cross section of the optical fiber cut by a fiber cutter with a microscope.

[0030] The Young's modulus (S-ISM) of the secondary layer 13 is measured by the following method. The optical fiber is immersed in liquid nitrogen, and the coating layer of the optical fiber is stripped off using a commercially available stripper. A hollow cylindrical sample consisting of only the coating layer is prepared, and the end of the sample is fixed to an aluminum plate. The aluminum plate portion is chucked using a Tensilon universal tensile tester in an atmosphere with a temperature of 23°C and a relative humidity of 50%. The sample is pulled with a width of 6 mm, a gauge interval of 25 mm, and a pulling speed of 1 mm / min, and the force at 2.5% elongation is measured to calculate the elastic modulus of the secondary layer 13. Note that the hollow cylindrical sample also includes the primary layer 12, but since the value of S-ISM is sufficiently large compared to P-ISM, the effect of the elastic modulus of the primary layer 12 on the S-ISM can be ignored.

[0031] The Young's modulus of the tape layer 21 is measured by the following method. The tape layer 21 is peeled off from the integrated optical fiber ribbon 2 with a single-edged blade or the like, and the peeled off tape layer 21 is adjusted under constant temperature and humidity conditions (for example, a temperature of 23°C and a humidity of 50%). The tape layer 21 is cut into a sample piece having a length of 25 mm, and pulled at a pulling speed of 1 mm / min to calculate the Young's modulus at 2.5% strain. The cross-sectional area of ​​the sample piece is then measured under a microscope. The Young's modulus of the bind layer 31 is measured by the same method as that of the tape layer 21. The bind layer 31 is peeled off from the split optical fiber ribbon 3, and the Young's modulus is measured by the same procedure as that of the tape layer 21. In this embodiment, the Young's modulus of the primary layer 12 can be in the range of 0.1 to 2.0 MPa, the Young's modulus of the secondary layer 13 can be in the range of 500 to 2000 MPa, and the Young's modulus of the tape layer 21 and the bind layer 31 can be in the range of 1.0 to 2000 MPa.

[0032] [Effective core area and microbend loss] The effective core area (Aeff) is an index that indicates the susceptibility of an optical fiber to microbend loss. The effective core area (Aeff) is expressed by the formula (2). The effective core area (Aeff) is described in, for example, C-3-76 and C-3-77 of the 1999 Electronics Society Conference Proceedings of the Institute of Electronics, Information and Communication Engineers. Aeff = (πk / 4) * (MFD)2 (2)

[0033] Here, the effective core area Aeff is a value at a wavelength of 1550 nm, the MFD (Mode-field diameter) is the mode field diameter (μm), and k is a constant. The effective core area Aeff represents the area of ​​a portion of a cross section perpendicular to the axis of the bare optical fiber 11 through which light passes and has a predetermined intensity. In general, the larger the effective core area Aeff of the bare optical fiber 11, the weaker the optical confinement in the cross section of the bare optical fiber 11. That is, when the effective core area Aeff of the bare optical fiber 11 is large, the light in the bare optical fiber 11 is more likely to leak out due to an external force applied to the bare optical fiber 11. Therefore, when the effective core area Aeff of the bare optical fiber 11 is large, the microbend loss of the colored optical fiber 1 is more likely to occur.

[0034] In this embodiment, a bare optical fiber 11 having an effective core area Aeff of 80 μm2 or more is used. In an optical fiber, Aeff is an index of microbending sensitivity, and the larger Aeff, the higher the microbending sensitivity. In general, if Aeff>100 μm2, it is said that the microbending sensitivity is high. In particular, if Aeff is 130 μm2 or more and 150 μm2 or less, the optical fiber has a high microbending sensitivity without any problems.

[0035] There are various methods for measuring microbend loss. For example, an optical fiber of 400 m or more in length is wound in a single layer with no overlapping at a tension of 100 gF around a large bobbin wrapped with #1000 grit sandpaper (state A). Meanwhile, an optical fiber of the same length as in state A is wound in a single layer with no overlapping at the same tension around a bobbin not wrapped with sandpaper (state B). The difference between the transmission loss of the optical fiber in state A and the transmission loss of the optical fiber in state B can be defined as the value of microbend loss. Here, the transmission loss of the optical fiber in state B does not include microbend loss and is considered to be a transmission loss specific to the optical fiber being measured.

[0036] The above measurement method is similar to the fixed diameter drum method defined in JIS C6823: 2010, and is called the sandpaper method. Since this measurement method measures the transmission loss at a wavelength of 1550 nm, in this embodiment, the microbend loss at a wavelength of 1550 nm is measured.

[0037] In this embodiment, the microbend loss of the bare optical fiber and the colored optical fiber 1 is preferably 0.15 dB / km or less, and more preferably 0.1 dB / km or less.

[0038] [Measurement of absorbance] In this embodiment, the absorbance of the ultraviolet curable resin is measured by the following method. Two spacers are placed at a predetermined interval between two quartz glass pieces forming a rectangular parallelepiped. The ultraviolet curable resin used in the tape layer 21 is placed between the two spacers, and the two spacers and the ultraviolet curable resin are sandwiched between the two quartz glass pieces to form a sample. Here, the thickness of the spacer can be, for example, 50 μm. A spectrophotometer (PerkinElmer Lambda900 (registered trademark)) is used to irradiate the ultraviolet curable resin with a beam from a light source and measure the absorbance of the sample. The absorbance of the quartz glass measured in advance is subtracted from the measured absorbance to obtain the absorbance of the ultraviolet curable resin used in the tape layer 21 at a thickness of 50 μm. The absorbance A can be obtained by the following formula. A=-log(I / I0)=-log(T / 100)=εcl···(3)

[0039] where T is the transmittance, I is the transmitted light intensity, I0 is the light intensity incident on the sample, ε is the molar extinction coefficient, c is the concentration of the absorbing substance, and l is the distance through the medium that the light passes.

[0040] 4 is a schematic diagram of a manufacturing apparatus 5 used in the manufacturing method of the splittable optical fiber ribbon 3 in this embodiment. The manufacturing apparatus 5 includes a core wire holding device 51, a guide roller 52, a tape layer coating device 53, a binding layer coating device 54, a guide roller 55, a winding device 56, and a control device 7.

[0041] The core wire holding device 51 winds and holds the manufactured colored optical fiber core wire 1. The colored optical fiber core wire 1 is pulled out from the core wire holding device 51, guided by the guide roller 52, and transported to the tape layer covering device 53. The number of core wire holding devices 51 and guide rollers 52 can be changed according to the number of colored optical fiber core wires 1 that the segmented optical fiber ribbon core wire 3 has. In this embodiment, the bundled optical fiber ribbon core wire 2 is manufactured using two colored optical fiber core wires 1, and the segmented optical fiber ribbon core wire 3 is manufactured using two bundled optical fiber ribbon core wires 2. Therefore, the number of core wire holding devices 51 and the number of guide rollers 52 are four. The core wire holding devices 51A, 51B, 51C, and 51D hold the colored optical fiber core wires 1A to 1D, respectively, and the guide rollers 52A, 52B, 52C, and 52D transport the colored optical fiber core wires 1A, 1B, 1C, and 1D to the tape layer covering device 53, respectively.

[0042] The tape layer coating device 53 includes a resin coating device 531 and an ultraviolet ray irradiation device 532. The resin coating device 531 holds an ultraviolet ray curing resin and coats the ultraviolet ray curing resin on the outer circumference of the colored optical fiber core wires 1A, 1B, 1C, and 1D. The resin coating device 531 is called a coating die or a die. The ultraviolet ray irradiation device 532 includes an arbitrary UV light source 533 such as a metal halide lamp, a mercury lamp, a UV-LED light source, and is provided downstream of the resin coating device 531 (corresponding to the lower part in FIG. 4). The ultraviolet ray irradiation device 532 is called a curing furnace, and irradiates ultraviolet rays onto the colored optical fiber core wires 1A, 1B, 1C, and 1D coated with the ultraviolet ray curing resin, thereby forming the tape layer 21. The UV light source 533 is provided so as to surround the outer circumference of the colored optical fiber core wires 1A, 1B, 1C, and 1D. A plurality of ultraviolet ray irradiation devices 532 may be provided in the tape layer coating device 53. When multiple ultraviolet irradiators 532 are provided, the multiple ultraviolet irradiators 532 are provided in series in the transport direction of the optical fiber colored core 1. By providing multiple ultraviolet irradiators 532, the time for irradiating the ultraviolet curable resin with ultraviolet rays can be made longer. Note that by measuring the surface temperature of the tape layer 21 (described later) immediately after ultraviolet irradiation by the UV light source 533 (at the outlet 534 of the ultraviolet irradiator 532 in FIG. 4), the temperature of the tape layer 21 immediately after the ultraviolet curable resin is cured can be measured.

[0043] While the colored optical fiber core wires 1A, 1B, 1C, and 1D pass through the inside of the ultraviolet irradiation device 532, the UV light source 533 irradiates ultraviolet light onto the ultraviolet curing resin applied to the outer periphery of the colored optical fiber core wires 1A, 1B, 1C, and 1D. The ultraviolet curing resin applied to the outer periphery of the colored optical fiber core wires 1A and 1B and the outer periphery of the colored optical fiber core wires 1C and 1D is cured to form the tape layer 21. In this way, the integrated optical fiber ribbon core wires 2A and 2B are formed. The integrated optical fiber ribbon core wires 2A and 2B are transported from the tape layer coating device 53 to the bind layer coating device 54.

[0044] The binding layer coating device 54 has the same configuration as the tape layer coating device 53, and includes a resin coating device 541 and an ultraviolet ray irradiation device 542. The resin coating device 541 holds an ultraviolet ray curing resin and applies the ultraviolet ray curing resin to the outer circumference of the bundled optical fiber ribbon core wires 2A and 2B. The resin coating device 541 is called a coating die or a die. The ultraviolet ray irradiation device 542 includes an arbitrary UV light source 543 such as a metal halide lamp, a mercury lamp, a UV-LED light source, or the like, and is provided downstream of the resin coating device 541 (corresponding to the lower part in FIG. 4). The ultraviolet ray irradiation device 542 is called a curing furnace, and irradiates ultraviolet rays to the bundled optical fiber ribbon core wires 2A and 2B to which the ultraviolet ray curing resin has been applied, to form the binding layer 31. The UV light source 543 is provided so as to surround the outer circumference of the bundled optical fiber ribbon core wires 2A and 2B. As with the tape layer coating device 53, the binding layer coating device 54 may also include a plurality of ultraviolet ray irradiation devices 542. When a plurality of ultraviolet irradiation devices 542 are provided, the plurality of ultraviolet irradiation devices 542 are provided in series in the transport direction of the integrated optical fiber ribbon 2. By providing a plurality of ultraviolet irradiation devices 542, the time for irradiating the ultraviolet curing resin with ultraviolet rays can be extended. As with the tape layer coating device 53, the surface temperature of the binding layer 31 can be measured immediately after the ultraviolet light is irradiated by the UV light source 543 (at the outlet 544 of the ultraviolet irradiation device 542 in FIG. 4), thereby measuring the temperature of the binding layer 31 immediately after the ultraviolet curing resin is cured.

[0045] While the integrated optical fiber ribbons 2A, 2B pass through the inside of the ultraviolet irradiation device 542, the UV light source 543 irradiates the ultraviolet curing resin applied to the outer periphery of the integrated optical fiber ribbons 2A, 2B with ultraviolet light. The ultraviolet curing resin applied to the outer periphery of the integrated optical fiber ribbons 2A, 2B is cured to form a binding layer 31. Through the above steps, the split type optical fiber ribbon 3 is manufactured. The split type optical fiber ribbon 3 is transported from the binding layer coating device 54, transported via a guide roller 55 to a winding device 56, and wound up.

[0046] The control device 7 controls, for example, the conveying speed of the guide rollers 52A, 52B, 52C, 52D and the guide roller 55, the pressure when the ultraviolet curing resin is pressurized and supplied to the tape layer coating device 53 and the bind layer coating device 54, the temperature of the ultraviolet curing resin supplied to the resin applicator 531 and the resin applicator 541, the outlet diameter of the tape layer coating device 53 and the bind layer coating device 54, the intensity of the UV light source of the ultraviolet irradiator 532 and the ultraviolet irradiator 542, the internal temperature of the tape layer coating device 53 and the bind layer coating device 54, the take-up torque of the take-up device 56, and the like. Control of luk etc.

[0047] 5 is a block diagram of the control device 7 in this embodiment. The control device 7 has a CPU (Central Processing Unit) 701, a ROM (Read Only Memory) 702, a RAM (Random Access Memory) 703, a storage device 704, a display 705, a touch sensor 706, an input device 707, a communication I / F 708, and a sensor I / F 709. Each part is connected to each other via a bus 710.

[0048] The CPU 701 controls each part of the manufacturing apparatus 5 by an application program. The ROM 702 is composed of a non-volatile memory, and stores an application program for controlling each part of the manufacturing apparatus 5. The RAM 703 provides a memory area necessary for the operation of the CPU 701. The storage device 704 is composed of a hard disk, a semiconductor memory, etc.

[0049] The display 705 is composed of, for example, a liquid crystal display, an OLED (Organic Light Emitting Diode) display, an LED (Light Emitting Diode) display, or the like. A touch sensor 706 is disposed on the surface of the display 705. The touch sensor 706 includes a capacitive or resistive detection circuit. The input device 707 is a user I / F, and may be, for example, a keyboard, a mouse, or the like.

[0050] The communication I / F 708 is a communication unit that transmits and receives data, and communicatively connects the control device 7 to the tape layer coating device 53 and the bind layer coating device 54. The communication between the control device 7 and the manufacturing device 5 via the communication I / F 708 may be either wired communication or wireless communication. The wireless communication method may be, for example, third generation mobile communication, LTE (Long Term Evolution), fourth generation mobile communication, fifth generation mobile communication, short-range wireless communication such as Bluetooth (registered trademark), wireless communication via a wireless LAN connection such as Wi-Fi, etc.

[0051] The sensor I / F 709 acquires various data from sensors included in the manufacturing apparatus 5 and stores the data in the storage device 704 or the like. The various data may be, for example, the temperature of the ultraviolet curing resin supplied to the resin coating apparatus 531 and the resin coating apparatus 541, the pressure when the ultraviolet curing resin is pressurized and supplied, the temperature of a tank storing the ultraviolet curing resin, the intensity of the UV light sources 533 and 543, the internal temperatures of the tape layer coating apparatus 53 and the bind layer coating apparatus 54, the surface temperature of the optical fiber colored core wire 1, the surface temperature of the bundled optical fiber ribbon core wire 2, the surface temperature of the division type optical fiber ribbon core wire 3, and the like.

[0052] The control device 7 receives control parameters of the manufacturing device 5 through the operation of the operator, and controls the manufacturing device 5. The control device 7 also receives information from a sensor (not shown) provided in the manufacturing device 5 via a sensor I / F 709, and can calculate the conveying speed of the guide rollers 52A, 52B, 52C, 52D and the guide roller 55, the temperature of a tank storing the ultraviolet-curable resin supplied to the resin applicator 531 and the resin applicator 541, the surface temperature of the optical fiber colored core wire 1, the surface temperature of the bundled optical fiber ribbon core wire 2, the surface temperature of the divisional optical fiber ribbon core wire 3, the internal temperature of the tape layer coating device 53, the internal temperature of the bind layer coating device 54, and the like, and can reflect these in the control of the manufacturing device 5.

[0053] FIG. 6 is a flow chart of a method for manufacturing the split type optical fiber ribbon 3 in this embodiment. First, an optical fiber preform is placed in a drawing device (not shown) (step S101). The optical fiber preform is heated by a heater to draw the bare optical fiber 11 (step S102). An ultraviolet curing resin is applied to the outer periphery of the drawn bare optical fiber 11, and ultraviolet rays are irradiated to form the primary layer 12 (step S103). An ultraviolet curing resin is applied to the outer periphery of the primary layer 12, and ultraviolet rays are irradiated to form the secondary layer 13 (step S104). An optical fiber is obtained by the steps S101 to S104. A colored ultraviolet curing resin is applied to the outer periphery of the optical fiber, and ultraviolet rays are irradiated to form the colored layer 14 (step S105). A colored optical fiber 1 is obtained by the steps S101 to S105. The manufactured colored optical fiber 1 is wound up on a core wire holding device 51. It should be noted that steps S101 to S105 are performed for each of the colored optical fibers 1A, 1B, 1C, and 1D.

[0054] The manufacturing apparatus 5 transfers the colored optical fiber core wires 1A, 1B, 1C, 1D from the core wire holding devices 51A, 51B, 51C, 51D to the tape layer coating device 53, which then forms the tape layer 21 on the colored optical fiber core wires 1A, 1B and the tape layer 21 on the colored optical fiber core wires 1C, 1D (step S106). By forming the tape layer 21 on the outer circumference of the colored optical fiber core wires 1A, 1B and the outer circumference of the colored optical fiber core wires 1C, 1D, the integrated optical fiber ribbon core wires 2A, 2B are obtained. The specific process of forming the tape layer 21 in step S106 will be described in detail with reference to FIG. 7.

[0055] The manufacturing apparatus 5 transfers the integrated optical fiber ribbons 2A, 2B from the tape layer coating device 53 to the binding layer coating device 54, which then forms a binding layer 31 on the integrated optical fiber ribbons 2A, 2B (step S107). By forming the binding layer 31 on the outer periphery of the integrated optical fiber ribbons 2A, 2B, a separable optical fiber ribbon 3 is obtained. The separable optical fiber ribbon 3 is taken up by a take-up device 56. The specific process of forming the binding layer 31 in step S107 will be described in detail with reference to FIG. 8.

[0056] FIG. 7 is a flow chart of the manufacturing method of the tape layer 21 in this embodiment. First, the manufacturing device 5 sets the light source output of the UV light source 533, the irradiation time of ultraviolet rays to the ultraviolet curing resin, the temperature of the ultraviolet curing resin, and the like (step S201). The output of the UV light source 533 is set in the range of 0 to 100%, with the maximum output of the UV light source 533 being 100%. The irradiation time of ultraviolet rays to the ultraviolet curing resin is set by controlling the linear speed of the optical fiber colored cores 1A, 1B, 1C, and 1D when passing through the ultraviolet irradiation device 532. Also, as described in FIG. 4, the irradiation time of ultraviolet rays to the ultraviolet curing resin can be controlled by providing a plurality of ultraviolet irradiation devices 532. The temperature of the ultraviolet curing resin is set by an operator or the like via the control device 7. The predetermined temperature can be, for example, in the range of room temperature to 50°C.

[0057] The manufacturing apparatus 5 heats the ultraviolet curable resin held in the tape layer coating apparatus 53 to a predetermined temperature based on the temperature of the ultraviolet curable resin set in step S201 (step S202). The ultraviolet curable resin may be heated inside the tape layer coating apparatus 53, or may be heated in a tank (not shown) that stores the ultraviolet curable resin and supplies the ultraviolet curable resin to the tape layer coating apparatus 53. When applying the ultraviolet curable resin to the optical fiber colored cores 1A, 1B, 1C, and 1D, it is preferable that the ultraviolet curable resin is heated so that the temperature of the ultraviolet curable resin is the temperature set in step S201. The temperature of the ultraviolet curable resin is measured using a thermocouple-type thermometer.

[0058] When the temperature of the ultraviolet curing resin reaches a predetermined temperature, the manufacturing device 5 conveys the colored optical fiber core wires 1A, 1B, 1C, and 1D wound around the core wire holding device 51 to the tape layer coating device 53. The tape layer coating device 53 applies ultraviolet curing resin to the outer circumference of the colored optical fiber core wires 1A and 1B and the outer circumference of the colored optical fiber core wires 1C and 1D in the resin coating device 531 (step S203). Furthermore, the ultraviolet irradiation device 532 irradiates the ultraviolet curing resin with ultraviolet light for a predetermined irradiation time to form the tape layer 21 on the outer circumference of the colored optical fiber core wires 1A and 1B and the outer circumference of the colored optical fiber core wires 1C and 1D (step S204). The UV light source provided in the ultraviolet irradiation device 532 may be, for example, a mercury lamp, a UV-LED light source, or the like.

[0059] Through the steps S201 to S204, the tape layer 21 is formed on the outer circumference of the colored optical fiber cores 1A and 1B and on the outer circumference of the colored optical fiber cores 1C and 1D, and the bundled optical fiber tape cores 2A and 2B are obtained. In step S201, the output of the UV light source 533 is adjusted, and the irradiation time of the ultraviolet curing resin with ultraviolet rays is adjusted. In step S202, the ultraviolet curing resin is heated, so that the temperature and the conversion rate of the tape layer 21 when the ultraviolet curing resin undergoes a curing reaction in step S204 can be controlled. For example, when the absorbance of the ultraviolet curing resin at a wavelength of 395 nm of ultraviolet rays is 0.22, the temperature of the ultraviolet curing resin is 50.0°C, the output of the UV light source is 75%, and the irradiation time of the ultraviolet curing resin with ultraviolet rays is 54 msec, the surface temperature of the tape layer 21 immediately after the ultraviolet irradiation can be about 93.6°C, and the conversion rate of the tape layer 21 can be 85.1%. When the absorbance of the ultraviolet curing resin at a wavelength of 395 nm of ultraviolet light is 0.07, the temperature of the ultraviolet curing resin is 50.0° C., the output of the UV light source is 100%, and the irradiation time of ultraviolet light to the ultraviolet curing resin is 108 msec, the surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light is approximately 122.0° C., and the conversion rate of the tape layer 21 can be 84.1%. The surface temperature of the tape layer 21 is measured by using a non-contact thermometer at the exit 534 of the UV light source 533 shown in FIG. 4 when the integrated optical fiber ribbons 2A and 2B are carried out from the ultraviolet irradiation device 532.

[0060] As described above, by appropriately setting the absorbance of the UV-curable resin when forming the ribbon layer around the outer periphery of the colored optical fiber, the supply temperature of the colored optical fiber, the temperature of the UV-curable resin, the output of the UV light source, and the irradiation time of UV rays to the UV-curable resin, it is possible to control the temperature during the curing reaction of the UV-curable resin and the conversion rate of the ribbon layer, thereby improving the splittability of the splittable optical fiber ribbon.

[0061] 8 is a flowchart of a method for manufacturing the bind layer 31 in this embodiment. First, the manufacturing apparatus 5 sets the light source output of the UV light source 543 and the irradiation time of the ultraviolet ray to the ultraviolet curing resin (step S301). The output of the UV light source 543 is set in the range of 0 to 100%, with the maximum output of the UV light source 543 being 100%. The output of the UV light source 543 when forming the bind layer 31 is preferably smaller than the output of the UV light source 533 when forming the tape layer 21.

[0062] The irradiation time of the ultraviolet curing resin with ultraviolet rays is set by controlling the linear speed when the bundled optical fiber ribbons 2A and 2B pass through the ultraviolet irradiation device 542. The irradiation time of the ultraviolet curing resin with ultraviolet rays when forming the binding layer 31 is preferably shorter than the irradiation time of the ultraviolet curing resin with ultraviolet rays when forming the tape layer 21. By providing a plurality of ultraviolet irradiation devices 532 in the tape layer coating device 53, the irradiation time of the ultraviolet rays when forming the binding layer 31 may be shorter than the irradiation time of the ultraviolet rays when forming the tape layer 21. For example, when two ultraviolet irradiation devices 532 are provided in the tape layer coating device 53 and one ultraviolet irradiation device 542 is provided in the binding layer coating device 54, the irradiation time of the ultraviolet rays when forming the binding layer 31 is approximately half of the irradiation time of the ultraviolet rays when forming the tape layer 21. Furthermore, the temperature of the ultraviolet curing resin may be set, and for example, the temperature of the ultraviolet curing resin may be room temperature or the like.

[0063] The manufacturing device 5 transports the bundled optical fiber ribbons 2A and 2B from the tape layer coating device 53 to the binding layer coating device 54. The binding layer coating device 54 coats the outer periphery of the bundled optical fiber ribbons 2A and 2B with an ultraviolet curing resin in a resin coating device 541 (step S302). When coating the ultraviolet curing resin, the ultraviolet curing resin may be heated to a predetermined temperature. The ultraviolet curing resin may be heated inside the binding layer coating device 54, or in a tank (not shown) that stores the ultraviolet curing resin and supplies the ultraviolet curing resin to the binding layer coating device 54. Furthermore, the ultraviolet irradiation device 542 irradiates the ultraviolet curing resin with ultraviolet light for a predetermined irradiation time to form a binding layer 31 on the outer periphery of the bundled optical fiber ribbons 2A and 2B (step S303). The UV light source provided in the ultraviolet irradiation device 542 may be, for example, a mercury lamp, a UV-LED light source, or the like.

[0064] Through the steps S301 to S303, the binding layer 31 is formed on the outer circumference of the bundled optical fiber ribbon 2A, 2B, and the split optical fiber ribbon 3 is obtained. In step S301, the output of the UV light source 543 is adjusted, and the irradiation time of the ultraviolet ray to the ultraviolet curable resin is adjusted, so that the conversion rate of the binding layer 31 when the ultraviolet curable resin undergoes a curing reaction in step S303 can be controlled. For example, when the output of the UV light source is 40% and the irradiation time of the ultraviolet ray to the ultraviolet curable resin is 27 msec, the conversion rate of the binding layer 31 can be 80.6%. When the output of the UV light source is 20% and the irradiation time of the ultraviolet ray to the ultraviolet curable resin is 54 msec, the conversion rate of the binding layer 31 can be 83.0%.

[0065] If the adhesion between the colored layer 14 and the tape layer 21 is strong (many chemical bonds) and the adhesion between the tape layer 21 and the bind layer 31 is weak (few chemical bonds), the tape layer 21 will not easily peel off from the colored optical fiber 1, and the bind layer 31 will easily peel off from the integrated optical fiber ribbon 2. Therefore, by increasing the conversion rate of the tape layer 21 and decreasing the conversion rate of the bind layer 31, the splittability of the splittable optical fiber ribbon 3 can be improved.

[0066] By appropriately setting not only the absorbance of the UV-curable resin when forming the tape layer, the supply temperature of the colored optical fiber, the temperature of the UV-curable resin, the output of the UV light source, and the irradiation time of UV rays on the UV-curable resin when forming the bind layer on the outer periphery of the bundled optical fiber ribbon, but also the output of the UV light source and the irradiation time of UV rays on the UV-curable resin when forming the bind layer on the outer periphery of the bundled optical fiber ribbon, it is possible to control the conversion rate of the bind layer when the UV-curable resin undergoes a curing reaction, thereby further improving the splittability of the splittable optical fiber ribbon.

[0067] In addition, compared to the UV light of a mercury lamp, the UV light of a UV-LED light source does not include IR light, so the curing temperature of the tape layer is lower when curing the ultraviolet-curable resin, and the curing reactivity may decrease. Therefore, when the tape layer is formed using a UV-LED light source, it is difficult to properly cure the tape layer, and the splitting property of the splittable optical fiber ribbon may deteriorate. In this embodiment, by controlling the curing temperature of the tape layer to an appropriate temperature range, the splitting property of the splittable optical fiber ribbon can be improved even when the tape layer is cured using a UV-LED light source.

[0068] [First embodiment] Table 1 shows, in the first embodiment, the absorbance of the ultraviolet-curable resin forming the tape layer 21 at a thickness of 50 μm for an ultraviolet wavelength of 395 nm, the temperature when the optical fiber colored core wire 1 is supplied during the manufacture of the split type optical fiber ribbon 3, the temperature of the ultraviolet-curable resin forming the tape layer 21, the light source output of the UV light source 533 in the tape layer coating device 53 and the irradiation time of ultraviolet rays to the ultraviolet-curable resin, the surface temperature of the tape layer 21 immediately after the tape layer 21 is formed (measured at the exit 534 of the ultraviolet irradiation device 532 in Figure 4), and an evaluation of the splittability of the split type optical fiber ribbon 3.

[0069] [Table 1]

[0070] Based on the manufacturing method of the splittable optical fiber ribbon 3 shown in Figs. 6 to 8, the splittable optical fiber ribbon 3 shown in Figs. 3A and 3B was manufactured. Furthermore, the splittability of the manufactured splittable optical fiber ribbon 3 was evaluated. In this embodiment, a splittable optical fiber ribbon 3 including two (N=2) bundled optical fiber ribbons 2A and 2B was used. The room temperature was in the range of 24.0 to 28.0°C.

[0071] In this embodiment, an ultraviolet curing resin having a Young's modulus in the range of 500 to 1400 MPa is used for the tape layer 21, and an ultraviolet curing resin having a Young's modulus in the range of 30 to 110 MPa is used for the bind layer 31. The ultraviolet curing resin used for the bind layer 31 has absorption for the wavelength of the UV light source 533.

[0072] The UV light source 533 used for ultraviolet irradiation was a UV-LED light source, and the wavelength of the UV light source 533 was 395±10 nm. A thermocouple-type thermometer was used to measure the temperature of the ultraviolet-curable resin, and a non-contact thermometer was used to measure the surface temperatures of the optical fiber colored core 1 and the tape layer 21. The non-contact thermometer was a thermograph with an emissivity set to 0.96.

[0073] The conversion rate of the tape layer 21 was measured by a microscopic ATR (Attenuated Total Reflection) method of Fourier Transform Infrared Spectroscopy (FT-IR). The conversion rate was measured by measuring the extent to which the peak area near 810 cm-1 decreased after UV curing from the state of the ultraviolet curable resin before UV curing, based on the peak area near 1500 cm-1.

[0074] Regarding the splittability of the splittable optical fiber ribbon 3, the binding layer 31 in a predetermined range other than the end of the splittable optical fiber ribbon 3 was rubbed with a mesh part of a dedicated jig (for example, QS ribbon single-core separation tool QS101), and it was evaluated whether the splittable optical fiber ribbon 3 could be split into the bundled optical fiber ribbons 2A and 2B within 5 rubs (evaluation method of splittability). When the splittable optical fiber ribbon 3 was split into the bundled optical fiber ribbons 2A and 2B, if the bundled optical fiber ribbons 2A and 2B could be split without peeling of the tape layer 21 or without the tape layer 21 being damaged to separate the colored optical fiber 1 into individual fibers, the splittability was evaluated as passing (evaluation of OK). If the damage to the tape layer 21 was so great that the damage to the tape layer 21 was visible, the splittability was evaluated as failing (evaluation of NG).

[0075] 9A to 9F show an example of a splittable optical fiber ribbon 3 split into bundled optical fiber ribbons 2A and 2B. Fig. 9A to 9E show an example of a result that passed (evaluated as OK) in the evaluation of splittability, and Fig. 9F shows an example of a result that failed (evaluated as NG) in the evaluation of splittability.

[0076] In the example of Fig. 9A, although pieces of the binding layer 31 remain in each of the integrated optical fiber ribbons 2A and 2B at the cross section of the binding layer 31, there is no damage to the tape layers 21 of the integrated optical fiber ribbons 2A and 2B. Similarly, in the example of Fig. 9B, although pieces of the binding layer 31 remain in each of the integrated optical fiber ribbons 2A and 2B at the cross section of the binding layer 31, there is no damage to the tape layers 21. Therefore, the examples of Fig. 9A and Fig. 9B are evaluated as OK in the evaluation of splittability.

[0077] In the example of Fig. 9C, a piece of the binding layer 31 remains in the integrated optical fiber ribbon 2A at the cross section of the binding layer 31, but there is no damage to the tape layers 21 of the integrated optical fiber ribbon 2A, 2B. Similarly, in the example of Fig. 9D, a piece of the binding layer 31 remains in the integrated optical fiber ribbon 2B, but there is no damage to the tape layers 21 of the integrated optical fiber ribbon 2A, 2B. Therefore, the examples of Fig. 9C and Fig. 9D are evaluated as OK in the evaluation of splittability.

[0078] In the example of Fig. 9E, although the pieces of the binding layer 31 are separated from the integrated optical fiber ribbons 2A and 2B, there is no damage to the tape layers 21 of the integrated optical fiber ribbons 2A and 2B. Therefore, the example of Fig. 9E is evaluated as OK in the evaluation of divisibility.

[0079] In the example of Fig. 9F, the tape layers 21 of the integrated optical fiber ribbons 2A and 2B are damaged, and the colored optical fiber 1A is separated from the integrated optical fiber ribbon 2A. Therefore, the example of Fig. 9F is rated as NG in the evaluation of divisibility. In addition to the example of Fig. 9F, the evaluation of divisibility is NG in cases where the integrated optical fiber ribbon 2A and the integrated optical fiber ribbon 2B cannot be separated, the tape layers 21 are damaged to a degree that can be seen with the naked eye, the tape layers 21 are damaged and the colored optical fiber 1 is separated from the integrated optical fiber ribbons 2A and 2B, the colored optical fiber 1A, 1B, 1C, and 1D are damaged, and so on.

[0080] In this embodiment, the optical fiber colored core wires 1A, 1B, 1C, and 1D are continuously connected by the tape layer 21 in the length direction of the optical fiber. When the optical fiber colored core wires 1A, 1B, 1C, and 1D are continuously connected by the tape layer 21 in the length direction of the optical fiber, an ultraviolet curable resin having a high Young's modulus is selected for the ultraviolet curable resin used in the tape layer 21, and the amount of ultraviolet curable resin used in the tape layer 21 is large, compared with the case where the optical fiber colored core wires 1A, 1B, 1C, and 1D are intermittently connected by the tape layer 21 in the length direction of the optical fiber. Therefore, it is more difficult to harden the ultraviolet curable resin. Furthermore, a plurality of bundled optical fiber ribbon core wires 2A and 2B are connected by the bind layer 31. When removing the bind layer 31, it is desirable that the tape layer 21 and the bind layer 31 are appropriately hardened so that only the bind layer 31 is removed and the tape layer 21 is not damaged.

[0081] [Example 1] An ultraviolet curing resin having an absorbance of 0.37 at a wavelength of 395 nm was heated to 35.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Then, the output of the UV light source 533 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 54 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 92.4°C. Furthermore, a binding layer 31 was formed in the process shown in Figure 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0082] [Example 2] An ultraviolet curing resin having an absorbance of 0.37 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Then, the output of the UV light source 533 was set to 100%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 162 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 140.0°C. Furthermore, a binding layer 31 was formed in the process shown in Figure 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0083] [Example 3] An ultraviolet curing resin having an absorbance of 0.37 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Then, the output of the UV light source 533 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 162 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 128.3°C. Furthermore, a binding layer 31 was formed in the process shown in Figure 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0084] [Example 4] An ultraviolet curing resin having an absorbance of 0.22 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Then, the output of the UV light source 533 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 54 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 93.6°C. Furthermore, a binding layer 31 was formed in the process shown in Figure 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0085] [Example 5] An ultraviolet curing resin having an absorbance of 0.15 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Then, the output of the UV light source 533 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 54 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 89.9°C. Furthermore, a binding layer 31 was formed in the process shown in Figure 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0086] [Example 6] An ultraviolet curing resin having an absorbance of 0.10 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Then, the output of the UV light source 533 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 54 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 89.5°C. Furthermore, a binding layer 31 was formed in the process shown in Figure 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0087] [Example 7] An ultraviolet curing resin having an absorbance of 0.10 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Then, the output of the UV light source 533 was set to 38%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 108 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 88.0°C. Furthermore, a binding layer 31 was formed in the process shown in Figure 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0088] [Example 8] An ultraviolet curing resin having an absorbance of 0.07 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Then, the output of the UV light source 533 was set to 100%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 108 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 122.0°C. Furthermore, a binding layer 31 was formed in the process shown in Figure 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0089] [Comparative Example 1] An ultraviolet curing resin having an absorbance of 0.10 at a wavelength of 395 nm was heated to room temperature and applied to the colored optical fiber 1 at the same temperature as the room temperature. Thereafter, the output of the UV light source 533 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 54 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 82.1°C. Furthermore, a binding layer 31 was formed in the process shown in Fig. 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as NG.

[0090] [Comparative Example 2] An ultraviolet curing resin having an absorbance of 0.07 at a wavelength of 395 nm was heated to 50°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 54 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 86.8°C. Furthermore, a binding layer 31 was formed in the process shown in Fig. 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as NG.

[0091] [Comparative Example 3] An ultraviolet curing resin having an absorbance of 0.15 at a wavelength of 395 nm was heated to 50°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 was set to 38%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 54 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 75.0°C. Furthermore, a binding layer 31 was formed in the process shown in Fig. 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as NG.

[0092] [Comparative Example 4] An ultraviolet curing resin having an absorbance of 0.37 at a wavelength of 395 nm was heated to 50°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 was set to 25%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 162 msec using the ultraviolet irradiation device 532 to form the tape layer 21. The surface temperature of the tape layer 21 immediately after irradiation with ultraviolet light was 87.5°C. Furthermore, a binding layer 31 was formed in the process shown in Fig. 8 to manufacture a splittable optical fiber ribbon 3, and the splittability was evaluated by the above-mentioned evaluation method. The splittability of the splittable optical fiber ribbon 3 was evaluated as NG.

[0093] As shown in Examples 1 to 8 in this embodiment, the absorbance of the ultraviolet curing resin at a wavelength of 395 nm was selected within a range of 0.07 to 0.37, the temperature of the ultraviolet curing resin was heated within a range of 35.0°C to 50°C, and the temperature of the colored optical fiber 1 was heated within a range of room temperature to 50°C. In the tape layer coating device 53, the output of the UV light source 533 was set within a range of 38 to 100%, and the irradiation time of the ultraviolet light was set within a range of 54 to 162 msec, to form the tape layer 21 on the colored optical fiber 1. The surface temperature of the tape layer 21 immediately after the tape layer 21 was formed was about 88°C to about 140°C. The evaluation of the splittability of the split type optical fiber ribbon 3 using the bundled optical fiber ribbon 2 manufactured under the conditions of Examples 1 to 8 was OK. In this way, when applying the ultraviolet curable resin to the colored optical fiber 1, the colored optical fiber 1 and the ultraviolet curable resin are heated to an appropriate temperature range, and the output of the UV light source and the irradiation time of the ultraviolet light are appropriately set, so that the temperature of the ribbon layer 21 when irradiating the ultraviolet curable resin with ultraviolet light can be controlled to an appropriate temperature range, and the ultraviolet curable resin can be appropriately cured. This makes it possible to provide a manufacturing method for a splittable optical fiber ribbon 3 with good splittability.

[0094] [Second embodiment] Next, the manufacturing conditions and the like of the split type optical fiber ribbon 3 in the second embodiment will be described. The following mainly describes the configuration different from the first embodiment.

[0095] Table 2 shows, in the second embodiment, the absorbance of the ultraviolet-curable resin forming the tape layer 21 at a thickness of 50 μm for an ultraviolet wavelength of 395 nm, the temperature when the optical fiber colored core wire 1 is supplied during the manufacture of the split type optical fiber ribbon core wire 3, the temperature of the ultraviolet-curable resin forming the tape layer 21, the light source output of the UV light source 533 in the tape layer coating device 53 and the irradiation time of ultraviolet rays to the ultraviolet-curable resin, the light source output of the UV light source 543 in the bind layer coating device 54 and the irradiation time of ultraviolet rays to the ultraviolet-curable resin, the surface temperature of the tape layer 21 immediately after the tape layer 21 is formed (measured at the exit 534 of the ultraviolet irradiation device 532 in Figure 4), the conversion rate of the tape layer 21 at the boundary between the tape layer 21 and the bind layer 31 and the conversion rate of the bind layer 31 at the outermost surface of the split type optical fiber ribbon core wire 3, and an evaluation of the splittability of the split type optical fiber ribbon core wire 3.

[0096] [Table 2]

[0097] In this embodiment, the UV light source 533 and the UV light source 543 used for ultraviolet irradiation are UV-LED light sources, and the wavelengths of the UV light source 533 and the UV light source 543 are 395±10 nm. The method for evaluating the splittability of the splittable optical fiber ribbon 3 is the same as that of the first embodiment.

[0098] [Example 1] The ultraviolet curing resin having an absorbance of 0.32 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 92.8°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 40%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 94.0%, and the conversion rate of the binding layer 31 was 79.3%. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0099] [Example 2] The ultraviolet curing resin having an absorbance of 0.30 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 100.0°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 40%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 94.3%, and the conversion rate of the binding layer 31 was 79.8%. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0100] [Example 3] The ultraviolet curing resin having an absorbance of 0.30 at a wavelength of 395 nm was heated to 35.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 90.0°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 40%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 91.1%, and the conversion rate of the binding layer 31 was 79.5%. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0101] [Example 4] The ultraviolet curing resin having an absorbance of 0.30 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 100.0°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 20%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 93.7%, and the conversion rate of the binding layer 31 was 75.2%. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0102] [Example 5] The ultraviolet curing resin having an absorbance of 0.22 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 93.6°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 40%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 85.1%, and the conversion rate of the binding layer 31 was 80.6%. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0103] [Example 6] The ultraviolet curing resin having an absorbance of 0.15 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 89.9°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 40%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 83.9%, and the conversion rate of the binding layer 31 was 80.3%. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0104] [Example 7] The ultraviolet curing resin having an absorbance of 0.10 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 89.5°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 40%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 82.6%, and the conversion rate of the binding layer 31 was 78.9%. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0105] [Example 8] The ultraviolet curing resin having an absorbance of 0.10 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 38%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 108 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet light irradiation was 88.0°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 20%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 54 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 81.9%, and the conversion rate of the binding layer 31 was 82.0%. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0106] [Example 9] The ultraviolet curing resin having an absorbance of 0.07 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 100%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 108 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 122.0°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 20%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 54 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 84.1%, and the conversion rate of the binding layer 31 was 83.0%. The splittability of the splittable optical fiber ribbon 3 was evaluated as OK.

[0107] [Comparative Example 1] The ultraviolet curing resin having an absorbance of 0.07 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet light irradiation was 86.8°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 40%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 81.7%, and the conversion rate of the binding layer 31 was 80.1%. The splittability of the splittable optical fiber ribbon 3 was evaluated as NG.

[0108] The ultraviolet curable resins of Comparative Example 1 and Example 9 have the same absorbance, but the output of the UV light source 533 in Comparative Example 1 is smaller than the output of the UV light source 533 in Example 9. As a result, the conversion rate of the tape layer 21 in Comparative Example 1 is smaller than the conversion rate of the tape layer 21 in Example 9, and the splittability of the splittable optical fiber ribbon 3 is deteriorated.

[0109] [Comparative Example 2] The ultraviolet curing resin having an absorbance of 0.15 at a wavelength of 395 nm was heated to room temperature and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 86.0°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 40%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 81.6%, and the conversion rate of the binding layer 31 was 79.6%. The splittability of the splittable optical fiber ribbon 3 was evaluated as NG.

[0110] The ultraviolet-curable resins of Comparative Example 2 and Example 6 have the same absorbance, but the temperature of the ultraviolet-curable resin of the tape layer 21 in Comparative Example 2 is lower than the temperature of the ultraviolet-curable resin of the tape layer 21 in Example 6. As a result, the curing temperature of the tape layer 21 is lowered, the conversion rate of the tape layer 21 is reduced, and the splittability of the splittable optical fiber ribbon 3 is deteriorated.

[0111] [Comparative Example 3] The ultraviolet curing resin having an absorbance of 0.22 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 50%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 54 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet irradiation was 88.0°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 27 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 83.5%, and the conversion rate of the binding layer 31 was 84.4%. The splittability of the splittable optical fiber ribbon 3 was evaluated as NG.

[0112] The conversion rates of the tape layer 21 in Comparative Example 3 and Example 6 are almost the same, 83.5% and 83.9%, respectively. The conversion rate of the binding layer 31 in Comparative Example 3 is larger than that of the binding layer 31 in Example 6, and the splittability of the splittable optical fiber ribbon 3 is deteriorated.

[0113] [Comparative Example 4] The ultraviolet curing resin having an absorbance of 0.10 at a wavelength of 395 nm was heated to 50.0°C and applied to the colored optical fiber 1 at the same temperature as room temperature. Thereafter, the output of the UV light source 533 in the tape layer coating device 53 was set to 25%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 532 for an irradiation time of 162 msec to form the tape layer 21. The surface temperature of the tape layer 21 immediately after the ultraviolet light irradiation was 84.5°C. Furthermore, the output of the UV light source 543 in the binding layer coating device 54 was set to 20%, and the ultraviolet curing resin was irradiated with ultraviolet light using the ultraviolet irradiation device 542 for an irradiation time of 81 msec to form the binding layer 31. The conversion rate of the tape layer 21 of the manufactured splittable optical fiber ribbon 3 was 80.7%, and the conversion rate of the binding layer 31 was 88.9%. The splittability of the splittable optical fiber ribbon 3 was evaluated as NG.

[0114] Comparing Comparative Example 4 and Example 7, the conversion rate of the tape layer 21 in Comparative Example 4 is smaller than the conversion rate of the tape layer 21 in Example 7. Furthermore, the conversion rate of the bind layer 31 in Comparative Example 4 is larger than the conversion rate of the bind layer 31 in Example 7. The tape layer 21 and the bind layer 31 were cured at an inappropriate conversion rate, which resulted in poor splittability of the splittable optical fiber ribbon 3.

[0115] As shown in Examples 1 to 9 in this embodiment, the absorbance of the ultraviolet curing resin at a wavelength of 395 nm was selected within a range of 0.07 to 0.32, the temperature of the ultraviolet curing resin was heated within a range of 35.0°C to 50°C, and the temperature of the colored optical fiber 1 was room temperature. In the tape layer coating device 53, the output of the UV light source 533 was set within a range of 38 to 100%, and the irradiation time of the ultraviolet light was set within a range of 54 to 108 msec, to form the tape layer 21 on the colored optical fiber 1. The surface temperature of the tape layer 21 immediately after the tape layer 21 was formed was about 88°C to about 122°C. In the binding layer coating device 54, the output of the UV light source 543 was set within a range of 20 to 40%, and the irradiation time of the ultraviolet light was set within a range of 27 to 54 msec, to form the binding layer 31 on the bundled optical fiber ribbon 2. The evaluation of the splittability of the splittable optical fiber ribbon 3 manufactured under the conditions of Examples 1 to 9 was OK.

[0116] In this way, when applying the ultraviolet-curable resin to the colored optical fiber 1, the colored optical fiber 1 and the ultraviolet-curable resin are heated to an appropriate temperature range, and the output of the UV light source 533 and the irradiation time of ultraviolet light are appropriately set, so that the temperature of the tape layer 21 when irradiating the ultraviolet-curable resin with ultraviolet light can be controlled to an appropriate temperature range, and the ultraviolet-curable resin forming the tape layer 21 can be appropriately cured. Furthermore, when applying the ultraviolet-curable resin to the bundled optical fiber ribbon 2, the output of the UV light source 543 and the irradiation time of ultraviolet light can be appropriately set, so that the ultraviolet-curable resin forming the bind layer 31 can be appropriately cured. This makes it possible to provide a splittable optical fiber ribbon 3 with good splittability.

[0117] In the first and second embodiments, not only the optical fiber colored core 1 and the ultraviolet curing resin but also the resin applicator 531 and the resin applicator 541 may be heated to a predetermined temperature. For example, the resin applicator 531 and the resin applicator 541 may be heated to the same temperature as the ultraviolet curing resin. A portion through which the ultraviolet curing resin passes, such as a supply pipe (nozzle) of the ultraviolet curing resin, may be heated. In the first and second embodiments, a UV-LED light source having a wavelength of 395 nm is used as the UV light source 533 and the UV light source 543, but a UV-LED light source having a wavelength of, for example, 275 nm, 365 nm, 385 nm, etc. may be used.

[0118] In the second embodiment, the conversion rate of the bind layer 31 is controlled by setting the output of the UV light source 543 and the irradiation time of the ultraviolet light, but the conversion rate of the bind layer 31 may be controlled by other methods. For example, the conversion rate of the bind layer 31 can be controlled by setting the absorbance of the ultraviolet curing resin forming the bind layer 31, the curing temperature of the bind layer 31, the oxygen concentration during curing of the bind layer 31, and the like.

[0119] In the first and second embodiments, the UV light source 533 of the tape layer coating device 53 is a UV-LED light source, but the UV light source 533 may be a combination of a UV-LED and a mercury lamp. For example, an ultraviolet curing resin having an absorbance of 0.07 at a wavelength of 395 nm is heated to 50.0° C. and applied to the optical fiber colored core 1 at the same temperature as room temperature. After that, ultraviolet irradiation was performed using a UV-LED light source as the UV light source 533 in the tape layer coating device 53. The output of the UV-LED light source was set to 75%, and the ultraviolet curing resin was irradiated with ultraviolet light from the UV-LED light source for an irradiation time of 27 msec. Next, ultraviolet irradiation was performed using a mercury lamp as the UV light source 533 in the tape layer coating device 53. The output of the mercury lamp was set to 100%, and the ultraviolet curing resin was irradiated with ultraviolet light from the mercury lamp for an irradiation time of 27 msec. In this manner, the tape layer 21 was formed. Furthermore, the output of the UV light source 543 in the bind layer coating device 54 was set to 40%, and the ultraviolet curing resin was irradiated with ultraviolet light for an irradiation time of 27 msec using the ultraviolet irradiation device 542, thereby forming the bind layer 31. The splitting property of the manufactured splittable optical fiber ribbon 3 was evaluated as OK. The splitting property of the splittable optical fiber ribbon 3 was also evaluated as OK even if the irradiation order of the UV-LED light source and the mercury lamp of the UV light source 533 in the ribbon layer coating device 53 was reversed, but from the viewpoint of efficiently reacting the photoinitiator, it is preferable to irradiate in the order of the UV-LED light source and the mercury lamp. [Explanation of symbols]

[0120] 1: Colored optical fiber core 11: Optical fiber 12: Primary layer 13: Secondary layer 14: Colored layer 2: Integrated optical fiber ribbon 21: Tape layer 3: Split type optical fiber ribbon 31: Bind layer 5: Manufacturing equipment 53: Tape layer coating device 54: Binding layer coating device 7: Control device

Claims

1. a first resin application step of applying a first resin to surfaces of a plurality of colored optical fibers arranged substantially parallel to each other; a first ultraviolet irradiation step of irradiating the first resin with light of a predetermined wavelength by a first UV light source to form a tape layer on the surface to form an integrated optical fiber tape; a second resin application step of applying a second resin to the surfaces of the bundled optical fiber ribbons arranged substantially parallel to each other; a second ultraviolet ray irradiation step of irradiating the second resin with light of the predetermined wavelength by a second UV light source to form a binding layer on the surfaces of the plurality of bundled optical fiber ribbons; 2. The method for producing a splittable optical fiber ribbon, wherein the surface temperature of the ribbon layer immediately after the first ultraviolet ray irradiation step is 88° C. or higher.

2. 2. The method for manufacturing a split type optical fiber ribbon according to claim 1, wherein the first UV light source is a light emitting diode.

3. 2. The method for producing a split type optical fiber ribbon according to claim 1, wherein the second UV light source is a light emitting diode.

4. 2. The method for manufacturing a split type optical fiber ribbon according to claim 1, wherein the first UV light source is a combination of a light emitting diode and a mercury lamp.

5. the first UV light source is a light emitting diode and a mercury lamp; The first ultraviolet ray irradiation step includes: Irradiating with the light emitting diode; 2. The method for producing a splittable optical fiber ribbon according to claim 1, further comprising the step of irradiating with the mercury lamp after the step of irradiating with the light emitting diode.

6. 2. The method for producing a splittable optical fiber ribbon according to claim 1, wherein the first resin is heated to 35[deg.] C. or higher.

7. 2. The method for manufacturing a split optical fiber ribbon according to claim 1, wherein the first resin is heated to 70°C or less, and the temperature of the surface of the integrated optical fiber ribbon immediately after the first ultraviolet irradiation process is 140°C or less.

8. 2. The method for producing a split type optical fiber ribbon according to claim 1, wherein the plurality of colored optical fibers are once wound around a bobbin or the like.

9. 2. The method for manufacturing a split type optical fiber ribbon according to claim 1, wherein the time for irradiating the light of the predetermined wavelength in the first ultraviolet irradiation process is longer than the time for irradiating the light of the predetermined wavelength in the second ultraviolet irradiation process.

10. 2. The method for producing a split type optical fiber ribbon according to claim 1, wherein an output of the first UV light source is greater than an output of the second UV light source.

11. 2. The method for producing a splittable optical fiber ribbon according to claim 1, wherein the first resin has an absorption property with respect to the wavelength of the first UV light source.

12. 2. The method for producing a splittable optical fiber ribbon according to claim 1, wherein the second resin has an absorption property with respect to the wavelength of the second UV light source.

Citation Information

Patent Citations

  • split optical fiber tape

    JP2820693B2