Carbon dioxide recovery method
By employing a porous solid material with supported cyclic diamines for carbon dioxide absorption and desorption using sunlight, the method addresses high energy consumption in existing recovery methods, achieving efficient and cost-effective carbon dioxide capture.
Patent Information
- Application Number
- JP2023180872
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2023-10-20
- Publication Date
- 2024-10-11
AI Technical Summary
Existing carbon dioxide recovery methods require significant energy input for desorption, leading to high operational costs and hindering the widespread adoption of carbon dioxide capture systems, which are crucial for reducing global warming.
A method involving a porous solid material with supported carbon dioxide absorption liquid, utilizing cyclic diamines, which allows for efficient carbon dioxide absorption and desorption with reduced energy consumption by harnessing thermal energy from sunlight or other low-cost heating sources.
The method enables low-energy desorption of carbon dioxide, reducing operational costs and enhancing the feasibility of carbon dioxide capture systems for environmental sustainability.
Smart Images

Figure 2024144031000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for recovering carbon dioxide via an absorbent exhibiting carbon dioxide absorption properties. [Background technology]
[0002] 2. Description of the Related Art In recent years, in order to reduce the concentration of carbon dioxide in the atmosphere, technologies have been considered for directly absorbing carbon dioxide in the atmosphere and for separating and capturing carbon dioxide contained in the combustion exhaust gas of fossil fuels and the like.
[0003] In the case of recovering carbon dioxide, a method has been proposed in which carbon dioxide is absorbed into an absorbent and the absorbed carbon dioxide is desorbed from the absorbent. For example, the following Patent Document 1 describes a method in which carbon dioxide is separated from combustion exhaust gas using a solution containing an amine as an absorbent, and then the solution is heated to desorb and recover the carbon dioxide. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-245339 Summary of the Invention [Problem to be solved by the invention]
[0005] In this way, in order to desorb and recover the absorbed carbon dioxide from the carbon dioxide absorber, it is necessary to input energy such as heating. If the energy required for this desorption is large, the cost of carbon dioxide recovery will be high. If it is not possible to desorb and recover the carbon dioxide absorbed by the absorber with low energy after the carbon dioxide is absorbed by the absorber, it will be difficult to comprehensively reduce carbon dioxide emissions. For example, if a large amount of electricity is consumed to desorb carbon dioxide, carbon dioxide will be released to generate this electricity. In addition, problems may arise regarding the handling of the absorber after carbon dioxide has been absorbed.
[0006] On the other hand, as mentioned above, if a high amount of energy is required to desorb and capture carbon dioxide from an absorbent that has already absorbed it, the running costs associated with operating the system become a concern. This is an obstacle to the introduction and widespread use of carbon dioxide capture systems. At present, the problem of global warming is considered to be one of the problems that must be solved worldwide. It can be said that reducing the amount of carbon dioxide emissions, which are considered to be one of the main causes of global warming, and thus reducing the carbon dioxide concentration in the atmosphere, is an urgent task.
[0007] In light of the above, it is believed that realizing a system that can absorb carbon dioxide into an absorbent and then desorb and capture it from the absorbent at low cost and with low energy consumption is important in promoting efforts to reduce the concentration of carbon dioxide in the atmosphere.
[0008] In view of the above circumstances, an object of the present invention is to provide a method and system for recovering carbon dioxide, which can desorb and recover absorbed carbon dioxide from an absorbent with less energy. [Means for solving the problem]
[0009] The method for recovering carbon dioxide according to the present invention comprises: A step (a) of preparing a first absorbent body which is an absorbent body before absorbing carbon dioxide by supporting a carbon dioxide absorbing liquid containing a cyclic diamine exhibiting basicity in a solid material made of a porous substance having pores on the surface of the solid material; A step (b) of absorbing carbon dioxide into the first absorbent to prepare a second absorbent which is an absorbent having absorbed carbon dioxide; (c) providing heat to the second absorbent; and a step (d) of recovering the carbon dioxide desorbed from the second absorbent body via the step (c).
[0010] In this specification, "recovery" means transferring the carbon dioxide desorbed from the absorbent from the area where the absorbent is placed to another area. For example, the carbon dioxide may be stored in a storage tank such as a cylinder, or may be sent to a carbon dioxide utilization facility via a pipe. Examples of the utilization facility include a plant factory.
[0011] In addition, in this specification, the term "first absorbent" refers to the state of an absorbent exhibiting carbon dioxide absorbency before absorbing carbon dioxide. Furthermore, the term "second absorbent" refers to the state of an absorbent exhibiting carbon dioxide absorbency after absorbing carbon dioxide. Note that the first absorbent also includes a state in which the absorbent absorbs carbon dioxide to become a second absorbent and then receives a supply of thermal energy to desorb the carbon dioxide.
[0012] In this specification, the term "pore" refers to a minute hole having a diameter of about several nm to several tens of μm, and the term "porous material" refers to a material having numerous pores on its surface.
[0013] As described above, in order to desorb carbon dioxide from the second absorbent that has already absorbed carbon dioxide, it is necessary to supply thermal energy to the second absorbent. In other words, in order to reduce the energy required for capturing carbon dioxide, it is essential to reduce the energy consumed in supplying this thermal energy.
[0014] By supporting a carbon dioxide absorbing liquid in the pores of a porous material, it can be used as a carbon dioxide absorber. In addition, by supporting the carbon dioxide absorbing liquid in the pores, the contact area between the carbon dioxide contained in the gas to be treated and the carbon dioxide absorbing liquid can be increased, and carbon dioxide absorption can be performed efficiently. The specific surface area of the porous material is 10 m 2 / g or more, and 2 / g or more is more preferable. The specific surface area of the porous substance can be measured, for example, by a method conforming to JIS Z 8830 (method for measuring the specific surface area of powder (solid) by gas adsorption).
[0015] Materials that can be used as the porous material include ceramic materials such as silica, alumina, and zirconia, engineering plastic materials such as polypropylene, polyacetal, polyamide, and polycarbonate, carbon materials such as activated carbon and carbon fiber, and resins containing cellulose. The shape of the porous material is not particularly limited. Examples of the shape of the porous material include granular, plate-like, tubular, honeycomb, and pellet-like shapes.
[0016] In the present invention, the carbon dioxide absorbing liquid is prepared by dispersing a cyclic diamine as a carbon dioxide absorbent in a solvent such as water, polyethylene glycol (PEG), or dimethyl sulfoxide (DMSO). A plurality of types of these solvents may be combined. In addition, in order to reduce the viscosity of the carbon dioxide absorbing liquid and make it easier for the carbon dioxide absorbing liquid to enter the pores, an alcohol such as methanol may be added to the carbon dioxide absorbing liquid, and the alcohol may be evaporated after the carbon dioxide absorbing liquid is impregnated into the porous material.
[0017] In terms of reducing the energy consumed for increasing the temperature of the solvent in the thermal energy supplied during desorption of carbon dioxide, and increasing the utilization efficiency of the thermal energy, it is preferable that the concentration of the carbon dioxide absorbing liquid is high. On the other hand, for example, when the carbon dioxide absorbing liquid is used as it is as an absorbent, there is a situation that the viscosity increases and handling becomes difficult when the concentration of the carbon dioxide absorbing liquid is increased, and there is a certain restriction on increasing the concentration. In particular, in a material with high viscosity, the concentration of the carbon dioxide absorbing liquid is about 1% to 10%. In contrast, by supporting the carbon dioxide absorbing liquid on a solid material, even if the concentration of the carbon dioxide absorbing liquid is high (for example, several tens of%), it is possible to easily handle it. In other words, by using a solid absorbent, the concentration of the carbon dioxide absorbing liquid can be increased, and as a result, the utilization efficiency of the thermal energy can be increased. The preparation of the absorbent will be described in detail in the section "Mode for carrying out the invention".
[0018] Cyclic diamine refers to a cyclic compound having two primary or secondary amino groups in the molecule. Examples of cyclic diamine include isophorone diamine, cyclohexane-1,2-diamine, cyclohexane-1,3-diamine, 4,4-methylene bis(2-methylcyclohexylamine), 4,4-methylene bis(cyclohexylamine), etc. Cyclic diamines can be used alone or as a mixture.
[0019] Hereinafter, the absorption and desorption of carbon dioxide will be described using isophoronediamine as an example. The main reaction in which isophoronediamine absorbs carbon dioxide is represented by the following formula (1). [ka]
[0020] In this way, the isophoronediamine that has absorbed carbon dioxide can be given energy by supplying heat, and the reverse reaction of the reaction represented by formula (1) can be caused, thereby desorbing the absorbed carbon dioxide. Although isophoronediamine has been used as an example, the cyclic diamine may be 4,4-methylenebis(2-methylcyclohexylamine) or 4,4-methylenebis(cyclohexylamine).
[0021] The effect of recovering carbon dioxide by using an absorbent in which a carbon dioxide absorbing solution containing a cyclic diamine is supported on a solid material will be described in detail in the section "Mode for Carrying Out the Invention."
[0022] The step (a) may include a step of blowing a plasma gas or irradiating ultraviolet rays onto the pores of the solid material before the carbon dioxide absorbing liquid is supported in the pores.
[0023] According to the above method, the wettability of the pore surface with respect to the carbon dioxide absorbing liquid is improved, and the carbon dioxide absorbing liquid can be more suitably supported in the pore. More specifically, when the plasma gas is sprayed onto the pore, the nitrogen molecules or oxygen molecules in the atmosphere are plasmatized, and the plasmatized active species form hydrophilic functional groups (hydroxyl groups, carbonyl groups, carboxy groups, etc.) on the pore surface. When ultraviolet light is irradiated, radicals are generated in the atmosphere by the ultraviolet light (mainly oxygen radicals in the case of air). At the same time, the ultraviolet light irradiates the bonds between the molecules that constitute the pore surface, and the radicals react with the severing sites, resulting in the formation of hydrophilic functional groups on the pore surface.
[0024] The porous material may be a carbon material. Although details will be described later, by using a carbon material as the porous material constituting the solid material, the carbon dioxide absorbing liquid can be more suitably supported in the pores of the solid material. The above method has the effect of suppressing deterioration of the absorbent caused by the heat supply for desorption of absorbed carbon dioxide.
[0025] The average pore size of the porous material may be in the range of 30 nm to 0.1 μm.
[0026] The average pore size of a porous material (also expressed as "4V / A") can be measured by a known gas adsorption method in accordance with JIS Z 8831-2 (Powder (solid) pore size distribution and pore characteristics), where V is the pore volume and A is the specific surface area.
[0027] Moreover, the step (a) may include a step of adding a carbon material to the carbon dioxide absorbing liquid.
[0028] The porous material may be a material that uses cellulose. When the porous material constituting the solid material contains cellulose, the carbon dioxide absorbing liquid can be more suitably supported in the pores of the solid material.
[0029] In addition, from the viewpoint of reducing the energy consumed in supplying thermal energy, a solar heat collecting member that converts received solar light into heat may be used to supply thermal energy derived from the heat to the second absorber. By using heat derived from solar light to supply thermal energy, it is possible to reduce the energy consumed in supplying the thermal energy. Specific embodiments will be described later in the "Mode for Carrying Out the Invention".
[0030] From the viewpoint of reducing the energy required for heating, a method of driving a heater for heating by a so-called solar power generation system is also envisaged. However, currently, in a solar power generation system, there is a problem with the wavelength range of light that can be used by a solar panel that absorbs sunlight. In particular, infrared rays account for more than half of sunlight, but a solar panel only uses visible light and some ultraviolet rays. In addition, there are influences from the conversion efficiency of the solar panel and the thermal efficiency of the heater and the like with respect to the input power, so that this method cannot be said to be able to effectively use sunlight. On the other hand, in the present invention, as described later, infrared rays in particular can be effectively used, so that the wavelength range of light that can be used is wide, and sunlight can be used more efficiently than, for example, a solar power generation system. Effect of the Invention
[0031] According to the present invention, there is provided a method for recovering carbon dioxide, which can desorb absorbed carbon dioxide from an absorbent with less energy. [Brief description of the drawings]
[0032] [Figure 1A] FIG. 1 is a cross-sectional view showing a schematic configuration of a first embodiment of a carbon dioxide recovery system. [Figure 1B] 1B is a diagram showing a different scene from that of FIG. 1A in the recovery system according to FIG. 1A; [Diagram 2] 1B is a view of the recovery system of FIG. 1A from a different angle. [Diagram 3] FIG. 1 is a flow diagram showing an example of a recovery method according to the present invention. [Figure 4A] FIG. 2 is a cross-sectional view that illustrates a structure of a substrate that supports a carbon dioxide absorbing liquid. [Figure 4B] FIG. 2 is a cross-sectional view showing a schematic structure of a first absorbent body. [Figure 4C] FIG. 4 is a cross-sectional view showing a schematic example of another structure of the first absorbent body. [Diagram 5] FIG. 1 is a conceptual diagram of the experimental system used in the verification. [Figure 6] This is the spectrum of the halogen lamp used in the verification. [Figure 7A] 1 is a graph showing the carbon dioxide desorption results of Verification 1. [Figure 7B] 13 is a graph showing the carbon dioxide desorption results of Verification 2. [Figure 8] 13 is a diagram illustrating a configuration of a second embodiment of the recovery system. [Figure 9] FIG. 4 is a cross-sectional view illustrating a structure of a reaction tank according to a second embodiment. [Figure 10] 10 is a view showing a different scene from that of FIG. 9 in the reaction vessel according to FIG. [Figure 11] FIG. 6 is a cross-sectional view illustrating a schematic structure of a heat source according to a second embodiment. [Figure 12] 12 is a view of the heat source according to FIG. 11 as seen from the Z direction. [Figure 13] 13 is a diagram illustrating a configuration of another embodiment of the recovery system. [Figure 14] 14 is a diagram showing a different scene from that of FIG. 13 in the recovery system according to FIG. 13. [Figure 15] 13 is a diagram illustrating a schematic configuration example of a recovery system. [Figure 16A] FIG. 16 is a perspective view showing a schematic configuration of a heat source in FIG. [Figure 16B] 16B is a ZY cross-sectional view of the heat source in FIG. 16A when viewed from the X direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] The carbon dioxide capture method according to the present invention (hereinafter simply referred to as the "capture method") will be described below with reference to the drawings. Note that the drawings are all schematic illustrations, and the dimensional ratios and numbers in the drawings do not necessarily match the actual dimensional ratios and numbers.
[0034] [First embodiment] 1A and 1B are cross-sectional views showing a schematic configuration of a first embodiment of a carbon dioxide capture system (hereinafter, simply referred to as a "capture system") capable of carrying out a capture method according to the present invention. Fig. 1A corresponds to a scene in which a step (step S2 described later) of absorbing carbon dioxide contained in a gas G1 to be treated such as the atmosphere is carried out, and Fig. 1B corresponds to a scene in which a step (step S4 described later) of desorbing the absorbed carbon dioxide is carried out.
[0035] Moreover, Fig. 2 is a drawing showing the capture system of Fig. 1A viewed from a different direction. The configuration of the capture system 1 will be described with reference to Figs. 1A, 1B and 2, and then a carbon dioxide capture method executed by the capture system 1 will be described.
[0036] In each of the following figures, an XYZ coordinate system consisting of mutually orthogonal X, Y, and Z directions is also shown as appropriate. Typically, the Z direction is the vertical direction. Based on this definition, FIG. 2 corresponds to a drawing of the recovery system according to FIG. 1A as viewed from the Z direction. Note that, as will be described later, FIG. 2 omits the illustration of a part of the configuration of the reaction tank 2.
[0037] As shown in FIG. 1A, the recovery system 1 includes a reaction vessel 2, an absorber 3 that is located inside the reaction vessel 2 and exhibits carbon dioxide absorption properties, and a heat source 4 that supplies thermal energy to the absorber 3.
[0038] As described above, the absorbent 3 is configured to include a carbon dioxide absorbent having a property of absorbing carbon dioxide and a property of desorbing the absorbed carbon dioxide by the supply of heat H1. The absorbent 3 is made of, for example, a granular porous material having pores on the surface, and the carbon dioxide absorbent is supported in the pores.
[0039] The reaction vessel 2 accommodates therein an absorber 3, a solar heat collecting member 15 (hereinafter simply referred to as "heat collecting member 15") as a heat source 4, and a heat transfer member 19 for efficiently transferring heat H1 of the heat collecting member 15 to the absorber 3. In addition, the reaction vessel 2 has a light transmitting part 20 made of a glass material such as quartz glass on the +Z side so that the heat collecting member 15 can receive solar light C2 (see also FIG. 1B).
[0040] In this embodiment, as shown in Fig. 2, a plurality of plate-shaped heat transfer members 19 are arranged in the X direction. Moreover, from the viewpoint of efficiently transferring heat from the heat collecting member 15 to the absorber 3, the heat transfer members 19 are connected on the +Z side and arranged directly with respect to the heat collecting member 15 (see Fig. 1B). Note that, for convenience of illustration, the connection portions between the light transmitting portion 20, the heat collecting member 15, and the heat transfer members 19 are omitted in Fig. 2.
[0041] In this embodiment, an example is shown in which the heat source 4 is disposed inside the reaction tank 2, but as will be described later in the section on the second embodiment, the arrangement of the heat source 4 is not limited to this example.
[0042] Next, an example of a collection method that can be performed by the collection system 1 will be described.
[0043] 3 is a flow diagram showing an example of a recovery method according to the present invention. This recovery method 1a includes a step S1 of preparing an absorber (hereinafter, for convenience, referred to as "first absorber 3a") in a state before absorbing carbon dioxide, a step S2 of making the first absorber 3a absorb carbon dioxide to prepare an absorber (hereinafter, for convenience, referred to as "second absorber 3b") in a state in which carbon dioxide has been absorbed, a step S3 of converting solar light C2 into heat H1, a step S4 of supplying the heat obtained in the step S3 to the second absorber 3b, and a step S5 of recovering a gas containing carbon dioxide desorbed from the second absorber 3b by carrying out S4 (hereinafter, for convenience, referred to as "recovered gas G2").
[0044] By performing steps S4 and S5, the second absorber 3b desorbs the absorbed carbon dioxide and then becomes the first absorber 3a. That is, in the recovery method 1a, the steps from step S2 onwards can be repeated after performing step S5.
[0045] (Step S1: Preparation of first absorbent body) First, an absorbent (first absorbent 3a) is prepared before absorbing carbon dioxide. The first absorbent 3a is prepared by supporting a carbon dioxide absorbing solution containing a cyclic diamine, which is an amine-based material, on a substrate made of a porous material having pores on the surface. An example of the cyclic diamine is isophorone diamine (IPDA).
[0046] The carbon dioxide absorbing liquid is prepared by dispersing an amine-based material in a solvent such as PEG. As an example, when the solvent is PEG, the ratio of the solvent to the amine-based material is 1:1. Depending on the viscosity of the amine-based material, an alcohol such as methanol may be added to the carbon dioxide absorbing liquid. For example, by mixing methanol, the viscosity of the carbon dioxide absorbing liquid in which PEG and the amine-based material are mixed can be reduced.
[0047] FIG. 4A is a cross-sectional view showing a structure of the substrate 10. As shown in FIG. 4A, the substrate 10 is a solid material having numerous pores 11 on the surface. Then, the carbon dioxide absorbing liquid having the amine-based material dispersed therein is contacted with the substrate 10, and the carbon dioxide absorbing liquid is supported in the pores 11. FIG. 4B is a cross-sectional view showing a structure of the first absorbent 3a prepared through the above-mentioned operation. For example, the diameter D2 of the pores 11 is set to 15 nm or less. In FIG. 4A and FIG. 4B, the diameter D2 is exaggerated with respect to the particle diameter D1 of the substrate 10 for convenience of illustration.
[0048] 4C is a cross-sectional view showing a structure of the first absorbent body 3a when the aperture D2 is relatively large (for example, about several μm) following FIG. 4B. The aperture D2 is appropriately designed according to, for example, the surface tension of the carbon dioxide absorbing liquid 12 supported in the pores 11 and the carbon dioxide absorption capacity. From the viewpoint of preventing the supported carbon dioxide absorbing liquid 12 from peeling off from the pores 11, the aperture D2 is preferably 0.1 μm or less.
[0049] Here, the diameter D2 may correspond to the average pore size of the substrate 10.
[0050] Furthermore, by adding an alcohol such as methanol to the carbon dioxide absorbing liquid 12, the viscosity of the carbon dioxide absorbing liquid 12 is reduced, and as a result, the carbon dioxide absorbing liquid 12 can be suitably introduced into the pores 11. In this case, it is preferable to heat the substrate 10 after the carbon dioxide absorbing liquid 12 is supported on the substrate 10 to evaporate the alcohol. For example, the heating condition when methanol is used is about 60° C. When evaporating the alcohol, it is preferable that the substrate 10 is placed in a reduced pressure atmosphere of, for example, about 60 kPa.
[0051] Furthermore, before the substrate 10 is made to support the carbon dioxide absorbing liquid 12, the substrate 10 may be sprayed with plasma gas or irradiated with ultraviolet light. This can improve the hydrophilicity of the surfaces of the pores 11 contained in the substrate 10, and the carbon dioxide absorbing liquid 12 can be favorably supported. The hydrophilization treatment of these pore surfaces will be described in detail in the section [Verification] below.
[0052] The first absorbent 3a obtained through the above-mentioned operations is placed inside the reaction vessel 2 (see FIG. 1A).
[0053] Thus, the step S1 of preparing the first absorbent body 3a corresponds to the step (a).
[0054] (Step S2: Carbon dioxide absorption step) As shown in FIG. 1A, a gas to be treated G1 containing carbon dioxide is introduced from an inlet 5 into a reaction vessel 2 in which a first absorber 3a is located, and is brought into contact with the first absorber 3a. FIG. 2 shows a schematic view of a state in which the gas to be treated G1 flows through the reaction vessel 2. As a result, the first absorber 3a absorbs carbon dioxide in the gas to be treated G1, and a second absorber 3b in which carbon dioxide has been absorbed is obtained. Note that, from the viewpoint of facilitating understanding, the second absorber 3b in which carbon dioxide has been absorbed is hatched in each drawing (see FIG. 1B, etc.). The gas to be treated G1 in which the carbon dioxide concentration has been reduced by the absorption of carbon dioxide is discharged, for example, to an outside space through an outlet 6.
[0055] As described later, it is assumed that the reaction vessel 2 is irradiated with sunlight C2 (step S3). On the other hand, from the viewpoint of efficiently absorbing carbon dioxide by the first absorber 3a, it is preferable to set the atmosphere in the reaction vessel 2 to a low temperature. For this reason, in step S2, the sunlight C2 irradiated to the reaction vessel 2 may be shielded by an arbitrary shielding member (not shown). In addition, step S2 may be performed during a time period when there is no or little irradiation of sunlight C2, such as at night.
[0056] Examples of the gas G1 to be treated include the atmosphere, exhaust gas from a factory, etc. In particular, when the gas G1 to be treated is an exhaust gas, the gas G1 to be treated may be pretreated before being introduced into the reaction tank 2, for example by cooling the gas G1 to be treated or screening for substances contained in the gas G1 to be treated that inhibit the absorption of carbon dioxide.
[0057] Thus, step S2 of preparing the second absorbent body 3b by causing the first absorbent body 3a to absorb carbon dioxide corresponds to step (b).
[0058] (Step S3: Converting sunlight into heat) As described above, energy is required to desorb the absorbed carbon dioxide from the second absorber 3b. For this reason, heat H1 is supplied to the second absorber 3b. In this embodiment, the heat H1 is obtained by converting the sunlight C2.
[0059] 1B, the heat source 4 is composed of a heat collecting member 15 disposed vertically above (on the +Z side of) the reaction vessel 2. The heat collecting member 15 is heated by absorbing the sunlight C2 taken in through the light transmitting portion 20. For example, the heat collecting member 15 is typically composed of a metal such as aluminum or copper that is coated with a black color in order to efficiently absorb the sunlight C2. The heat collecting member 15 may also be coated with a black body material such as graphite that exhibits a high absorptivity for light.
[0060] 1B, the light-transmitting portion 20 is composed of a plurality of transparent members 21 made of a glass material such as quartz glass. Furthermore, a reduced-pressure space 22 is formed between these transparent members 21. The pressure of the low-pressure space 22 is, for example, 10 kPa or less, and typically approximately 0 atmospheres. The low-pressure space 22 is provided from the viewpoint of making it difficult for the heat H1 converted by the heat collecting member 15 to be transmitted to the +Z side, but the present invention is not limited to whether or not the low-pressure space 22 is formed.
[0061] (Step S4: Supplying heat to the second absorbent) The heat H1 obtained in the above step S3 is supplied to the second absorber 3b. As shown in FIG. 1B, the reaction vessel 2 has a heat transfer member 19 for efficiently supplying the heat H1 of the heat collecting member 15 to the second absorber 3b. Typically, the heat transfer member 19 is disposed directly on the heat collecting member 15 and is heated by the heat of the heat collecting member 15. For example, a material having a high thermal conductivity, such as aluminum, copper, or ceramics, can be used as the heat transfer member 19. Note that the heat transfer member 19 may be integrally formed with the heat collecting member 15 using the same material.
[0062] 1B, heat H1 radiated from the heat transfer member 19 at a high temperature is supplied to the second absorber 3b, and the second absorber 3b is heated. That is, in this embodiment, the step S3 of converting the solar light C2 into heat H1 and the step S4 of supplying the heat H1 to the second absorber 3b are automatically executed.
[0063] In addition, the carbon dioxide concentration is locally high in the vicinity of the second absorber where the carbon dioxide desorption reaction proceeds. In order to efficiently proceed with the carbon dioxide desorption reaction, it is preferable to lower the carbon dioxide concentration in the vicinity of the second absorber. This is because, in the carbon dioxide desorption reaction, by lowering the carbon dioxide concentration in the system on the carbon dioxide production (desorption) side, the reaction system is more likely to proceed to the carbon dioxide production side. For this reason, as shown in FIG. 1B, a desorption-promoting gas B1 such as air or nitrogen gas may be introduced into the reaction tank 2 from an inlet 5 at the same time as the supply of heat H1.
[0064] In step S4, a heat transfer medium made of a fluid may be used to supply the heat H1 to the second absorbent 3b, and this configuration will be described in detail in the second embodiment described later.
[0065] Thus, the step S4 of supplying the heat H1 to the second absorbent body 3b corresponds to the step (c).
[0066] (Step S5: Recovering desorbed carbon dioxide) The recovered gas G2 containing the carbon dioxide desorbed in step S4 is sent to a carbon dioxide utilization facility such as a plant factory through a pipe (not shown) via the exhaust port 6. However, in the present invention, the destination of the recovered gas G2 is not limited.
[0067] Thus, the step S5 of recovering carbon dioxide corresponds to the step (d).
[0068] [Verification 1] The fact that carbon dioxide can be efficiently recovered through the above-mentioned steps S1 to S5 will be described with reference to examples. Specifically, verification was carried out on the recovery of carbon dioxide from the atmosphere as the gas to be treated G1 using the configuration described with reference to Figs. 1A, 1B, and 2.
[0069] Fig. 5 is a cross-sectional view showing a schematic diagram of the experimental system used in this verification, following Fig. 1B. Fig. 5 shows the execution scene of steps S3 to S5. The reaction vessel 2 in this experimental system has the same configuration as that described with reference to Fig. 1A etc., and therefore the above description will be omitted as appropriate. The internal dimensions of the reaction vessel 2 used in this verification are length (X direction) 5 cm, width (Y direction) 2 cm, and height (Z direction) 0.7 cm.
[0070] As the heat collecting member 15, an aluminum plate-shaped member coated with a black body material, measuring 5 cm in length, 2 cm in width, and 0.2 cm in height, was placed at a height of 0.5 cm.
[0071] In this verification, isophoronediamine was used as the carbon dioxide absorbent, and PEG was used as its solvent. That is, the carbon dioxide absorbing liquid 12 was an isophoronediamine solution adjusted to have a volume ratio of 1:1 with respect to the PEG solvent.
[0072] Granular silica manufactured by Fuji Silysia was used as the solid material for supporting the isophoronediamine solution. This silica has an average particle size of 1 to 5 mm and a specific surface area of 100 to 200 m 2 / g.
[0073] First, the weight of the isophorone diamine solution was weighed out so that it was several tens of wt% per 1 g of the solid material, and methanol was added to the isophorone diamine solution at a certain ratio to prepare a mixed solution. Then, 1 g of the solid material was put into this mixed solution and stirred. The stirring was performed in a reduced pressure atmosphere of 50 kPa while heating at about 50°C. In this way, the isophorone diamine solution was impregnated into the solid material, and then the solution was heated in a reduced pressure atmosphere to evaporate the methanol, thereby obtaining a first absorbent 3a.
[0074] In this verification, from the viewpoint of desorbing carbon dioxide absorbed during the preparation of the first absorbent 3a, a process of evaporating methanol was performed, and then the first absorbent 3a was heated at 70°C for several hours while flowing nitrogen gas (purity 99.9%) at 0.5 L / min. After that, the weight of the first absorbent 3a was weighed to estimate the amount of isophoronediamine supported on the solid material, which was 18 wt%.
[0075] Several grams of the first absorbent 3a obtained through the above-mentioned operations were placed inside the reaction tank 2. Then, air (having a carbon dioxide concentration of about 400 pm) was introduced into the reaction tank 2 as the gas to be treated G1 at a flow rate of 7.5 mL / min for several tens of hours to obtain a second absorbent 3b that had absorbed carbon dioxide (step S2).
[0076] Since carbon dioxide is absorbed by the first absorbent 3a, the carbon dioxide concentration of the gas to be treated G1 after contact with the first absorbent 3a decreases. Thereafter, when the absorption of carbon dioxide by the first absorbent 3a is completed (second absorbent 3b), the carbon dioxide concentration of the gas to be treated G1 that has passed through the reaction tank 2 becomes approximately the same as the state before being introduced into the reaction tank 2. Therefore, in this verification, it was determined that the first absorbent 3a had sufficiently absorbed carbon dioxide when the carbon dioxide concentration of the gas to be treated G1 measured downstream of the exhaust port 6 reached 400 ppm.
[0077] In this verification, light L1 was irradiated onto the heat collecting member 15 using a halogen lamp 30 to simulate sunlight C2 (see FIG. 5). FIG. 6 shows the spectrum of the halogen lamp 30 used in this verification. As shown in FIG. 6, the halogen lamp 30 used in this verification has a peak intensity at which the emission intensity is maximum near 1000 nm, and shows a light intensity of 40% or more of the peak intensity in the range of 500 nm to 2000 nm. In this verification, the power input to the halogen lamp 30 was 50 W.
[0078] When the halogen lamp 30 was turned on to desorb the absorbed carbon dioxide, air was passed through the reaction vessel 2 as the desorption-promoting gas B1 at a flow rate of 7.5 mL / min.
[0079] 7A is a graph showing the results of carbon dioxide desorption in this experiment. In Fig. 7A, the horizontal axis shows the time elapsed since the halogen lamp 30 was turned on, and the vertical axis shows the carbon dioxide concentration measured at the position of the exhaust port 6.
[0080] As shown in FIG. 7A, the carbon dioxide concentration of the recovered gas G2 exceeded 400 ppm (0.04%), which is a typical carbon dioxide concentration in the atmosphere. This is because the second absorber 3b desorbed carbon dioxide by receiving heat H1 from the heat collecting member 15 heated by irradiation with light L1. The carbon dioxide concentration of the recovered gas G2 reached a maximum of approximately 9600 ppm (0.96%). This is 24 times the carbon dioxide concentration of the atmosphere. From this point of view, it can be said that carbon dioxide was desorbed suitably from the second absorber 3b in this verification.
[0081] In this way, it is clear from this verification that at least light L1 in the wavelength range of 500 nm to 2000 nm was converted into heat H1 and used for desorption of carbon dioxide. On the other hand, it is known that sunlight C2 has a high intensity especially in the wavelength range of 500 nm to 2500 nm. In other words, although light L1 from the halogen lamp 30 was used in this verification, it can be understood that carbon dioxide desorption can be performed similarly suitably even if light L1 is replaced with sunlight C2.
[0082] [Verification 2] Next, the use of isophoronediamine as a carbon dioxide absorbent to efficiently recover carbon dioxide will be described with reference to an example. In this verification, similar to the above verification 1, verification was performed using different carbon dioxide absorbents when recovering carbon dioxide from the atmosphere as the gas G1 to be treated. Specifically, verification was performed in a case where isophoronediamine was used as the carbon dioxide absorbent (Example 1) and, as a comparative example, a case where polyethyleneimine was used as the carbon dioxide absorbent (Comparative Example 1).
[0083] Example 1 During carbon dioxide desorption, the same operations as those described in Verification 1 above were performed, except that heat was supplied so that the temperature inside reaction tank 2 became approximately 60°C.
[0084] Comparative Example 1 The experiment was carried out under the same conditions as in Example 1, except that polyethyleneimine was used as the carbon dioxide absorbent instead of isophoronediamine.
[0085] FIG. 7B is a graph showing the carbon dioxide desorption results of this verification, following FIG. 7A. In FIG. 7B, the results of Example 1 are shown by a solid line, and the results of Comparative Example 1 are shown by a dashed line. As shown in FIG. 7B, in Example 1 and Comparative Example 1, the carbon dioxide concentration of the recovered gas G2 exceeded the carbon dioxide concentration of the atmosphere (0.04%). From this point, it can be seen that in both cases, the second absorbent 3b desorbed carbon dioxide due to the supply of heat. Furthermore, in both Example 1 and Comparative Example 1, the carbon dioxide concentration of the recovered gas G2 reached a maximum value at about 4 hours.
[0086] However, in Comparative Example 1, after the carbon dioxide concentration of the recovered gas G2 reached its maximum value, it took more than about 25 hours for it to approach the carbon dioxide concentration of the atmosphere (0.04%). In contrast, in Example 1, the carbon dioxide concentration approached that of the atmosphere after about 10 hours had elapsed. The fact that the carbon dioxide concentration of the recovered gas G2 approached that of the atmosphere indicates that the carbon dioxide absorbent had completed the reaction of desorbing the absorbed carbon dioxide. In other words, it can be seen that isophoronediamine can desorb absorbed carbon dioxide in a shorter time than polyethyleneimine.
[0087] As described above, in the recovery of carbon dioxide, the carbon dioxide absorption process and desorption process are repeated (see FIG. 3). At this time, from the viewpoint of efficiently absorbing carbon dioxide in the absorption process, it is preferable to desorb as much of the absorbed carbon dioxide as possible from the absorber in the desorption process that precedes the absorption process.
[0088] In view of this, isophoronediamine is suitable as a carbon dioxide absorbent because it can desorb absorbed carbon dioxide in a few hours, or at most about 10 hours, even in a relatively low temperature environment of 60°C. On the other hand, polyethyleneimine takes a long time to desorb carbon dioxide in a temperature environment of 60°C (Figure 7B), so it is presumed that a temperature of 80°C to 100°C or higher is required to desorb absorbed carbon dioxide in about a few hours. In this way, by using isophoronediamine as a carbon dioxide absorbent, a large amount of carbon dioxide can be desorbed with less thermal energy.
[0089] It was also found that isophorone diamine absorbs a large amount of carbon dioxide per mole. Specifically, the amount of carbon dioxide absorbed per mole of isophorone diamine was 0.7 mol in Example 1. Since polyethyleneimine is a polymer, it is not easy to calculate the amount of carbon dioxide absorbed per mole, but even if this is taken into consideration, the amount of carbon dioxide absorbed per mole of isophorone diamine is small. As described above, in Example 1 and Comparative Example 1, the volumes of isophorone diamine and polyethyleneimine are set to be equal. For ease of understanding, if 1 L of each is used and the weights are calculated from the respective densities, the isophorone diamine is 920 g and the polyethyleneimine is 1080 g. Since the molecular weight of isophorone diamine is 170.3 g / mol, 920 g of isophorone diamine is 5.4 mol. On the other hand, polyethyleneimine is a polymer of ethyleneimine with a molecular weight of 43.1 g / mol. On this basis, 1080 g of polyethyleneimine can be considered as 25.1 mol of ethyleneimine.
[0090] In view of the above, although isophorone diamine has a molar amount of about 1 / 5 of polyethyleneimine, the amount of absorbed carbon dioxide desorbed is about the same as that of polyethyleneimine (see FIG. 7B). The fact that the amount of absorbed carbon dioxide desorbed is about the same indicates the absorption of carbon dioxide at the same level. In other words, based on the above molar amount, the amount of carbon dioxide absorbed by isophorone diamine is considered to be about 5 times that of polyethyleneimine. This also shows that isophorone diamine has a high carbon dioxide absorption capacity and is suitable as a carbon dioxide absorbent. Incidentally, the amount of carbon dioxide absorbed per mole of monoethanolamine, which is conventionally known as a carbon dioxide absorbent, is about 0.5 mol. From this comparison, it can be understood that isophorone diamine has a high carbon dioxide absorption capacity.
[0091] The present inventors speculate as follows regarding the fact that isophoronediamine absorbs a large amount of carbon dioxide and that isophoronediamine can desorb the absorbed carbon dioxide with a small amount of thermal energy. Isophoronediamine reacts with carbon dioxide to form carbamic acid, as shown in the above formula (1). Here, the carbamic acid obtained by reacting isophoronediamine with carbon dioxide has the characteristic of precipitating as a solid phase from the isophoronediamine solution and separating from the liquid phase. In other words, in the reaction of absorbing carbon dioxide, the generated carbamic acid is sequentially removed from the reaction system (liquid phase), so that the concentration of the product carbamic acid in the reaction system is unlikely to increase, and it is considered that the carbon dioxide absorption reaction in formula (1) is likely to proceed. It is speculated that this is the reason why isophoronediamine exhibits excellent carbon dioxide absorption properties.
[0092] In addition, in the desorption reaction of absorbed carbon dioxide, the temperature of the liquid phase of the isophoronediamine solution increases due to the supply of heat. This increases the solubility of carbamic acid, which was in the solid phase, and the carbamic acid dissolves in the liquid phase. Since the carbamic acid separates as a solid phase when produced, the solid phase is considered to be more stable than the liquid phase. In light of this, it is expected that carbamic acid, which is stable in the solid phase, becomes unstable in the liquid phase, and the energy required for the reaction is reduced. It is presumed that this is the reason why isophoronediamine exhibits a carbon dioxide desorption reaction even in a relatively low temperature environment of 60°C.
[0093] In this verification, isophorone diamine was used as the carbon dioxide absorbent. However, in view of the structure of isophorone diamine, it is presumed that a cyclic diamine, which is a cyclic compound and has two primary or secondary amino groups in the molecule, will generate solid-phase carbamic acid when reacted with carbon dioxide. Therefore, based on this verification, it can be understood that the energy required for carbon dioxide capture can be reduced by adopting a cyclic diamine as a carbon dioxide absorbent.
[0094] Furthermore, as shown in the first embodiment described above and the second embodiment described below, the energy required for carbon dioxide capture can be further reduced by obtaining the thermal energy for carbon dioxide desorption from sunlight. Although the amount of sunlight irradiation is dependent on the weather, as described above, by employing a cyclic diamine as a carbon dioxide absorbent, absorbed carbon dioxide can be desorbed with less energy than before, so that absorbed carbon dioxide can be desorbed suitably even when heat derived from sunlight is supplied.
[0095] [Verification 3] As described above, by supporting the carbon dioxide absorbing solution on a solid material, the concentration of the cyclic diamine in the carbon dioxide absorbing solution can be increased, and carbon dioxide can be desorbed with less energy. This point will be described with reference to the following examples.
[0096] Example 2 After desorption of the absorbed carbon dioxide was performed in the same manner as in Example 1, the amount of carbon dioxide recovered was obtained from the flow rate of the recovery gas G2 and the carbon dioxide concentration. Based on the amount of carbon dioxide, the amounts of isophoronediamine, PEG, and silica required to recover 100 kg of carbon dioxide per day were estimated. Based on the specific heat of each, the temperature of the second absorbent 3b made of these materials was heated from room temperature to 60°C, and the energy required to desorb carbon dioxide (hereinafter, for convenience, referred to as "desorption energy") was theoretically calculated. The specific heat of isophoronediamine and PEG was 2.5 kJ / kg K, and the specific heat of silica was 0.92 kJ / kg K.
[0097] Comparative Example 2 An approximately 15 wt% aqueous solution of isophoronediamine was prepared using water as a solvent, and carbon dioxide gas for experiments was bubbled into the solution to absorb carbon dioxide. More specifically, carbon dioxide was absorbed until no additional carbon dioxide absorption was observed, and then the solution was left to stand in an air atmosphere for about 1 hour to reach an equilibrium state. The aqueous solution was then heated from room temperature to 60°C to desorb carbon dioxide.
[0098] The amount of carbon dioxide desorbed was obtained from the flow rate of the gas containing carbon dioxide desorbed from the isophoronediamine aqueous solution and the carbon dioxide concentration. Then, the amount of isophoronediamine aqueous solution required to recover 100 kg of carbon dioxide per day was estimated in accordance with Example 2. In addition, based on the specific heat of the isophoronediamine aqueous solution, the desorption energy required to heat the aqueous solution from room temperature to 60°C was theoretically calculated.
[0099] Comparative Example 3 The experiment was carried out under the same conditions as Comparative Example 2, except that an approximately 1 wt% azobenzene solution in ethanol was used as the carbon dioxide absorption liquid instead of the isophoronediamine aqueous solution, and the temperature during carbon dioxide desorption was 40°C.
[0100] (Results of verification 3) Table 1 below shows the conditions for Example 2 and Comparative Examples 2 and 3, and the calculation results obtained in this verification. [Table 1]
[0101] According to Table 1, the desorption energy of Example 2 is less than half that of Comparative Example 2. This is believed to be because in Example 2, the carbon dioxide absorbing liquid containing isophorone diamine is supported on a solid material, thereby increasing the concentration of isophorone diamine in the carbon dioxide absorbing liquid, and as a result, the energy consumed to increase the temperature of the solvent is reduced. More specifically, in Comparative Example 2, the concentration of the isophorone diamine aqueous solution is about 15 wt%. In contrast, in Example 2, the concentration of isophorone diamine relative to PEG and isophorone diamine is high at about 50 wt%. In addition, in Example 2, the proportion (supported amount) of isophorone diamine when silica is included is about 20 wt%.
[0102] As mentioned above, when the concentration of the carbon dioxide absorbing liquid is increased, the viscosity increases, making it difficult to handle. However, by supporting the carbon dioxide absorbing liquid on a solid material, it is possible to easily handle the carbon dioxide absorbing liquid even when the concentration is high. In other words, by making it a solid absorbent (Example 2), the concentration of the carbon dioxide absorbing liquid can be increased, which increases the efficiency of thermal energy utilization and reduces the carbon dioxide desorption energy.
[0103] In addition, Example 2 differs from Comparative Example 2 in that the solvent is PEG. As described above, PEG has a smaller specific heat than water. In other words, the fact that the solvent of Example 2 is PEG is also a factor in the reduction in the desorption energy of Example 2 compared to Specific Heat Example 2. However, as described above, Example 2 and Comparative Example 2 have a large difference in the concentration of isophoronediamine in the carbon dioxide absorbing solution. In view of this, it can be understood that the reason why the desorption energy of Example 2 is reduced compared to Comparative Example 2 is that the effect of increasing the concentration of isophoronediamine, which increases the utilization efficiency of thermal energy, is greater than the effect of the specific heat of the solvent being reduced. In other words, the above discussion does not depend on whether the solvent is PEG or water.
[0104] In Comparative Example 3, when the temperature during carbon dioxide desorption was set to about 40°C, a certain amount of carbon dioxide desorption was confirmed. Therefore, in Comparative Example 3, the desorption energy was calculated with ΔT set to 20K. In addition, Comparative Example 3 uses ethanol, which has a smaller specific heat than water, as the solvent. In view of these circumstances, it is expected that the desorption energy of Comparative Example 3 will be a relatively small value. However, the desorption energy of Comparative Example 3 was 23.2 GJ, which was a larger value than that of Comparative Example 2.
[0105] That is, according to Table 1, it can be seen that by using isophoronediamine as the carbon dioxide absorbent (Comparative Example 2), the desorption energy can be reduced to about 1 / 5, even compared to Comparative Example 3, which has a low ΔT and a small specific heat of the solvent. Thus, the reason that the desorption energy of Comparative Example 2 is smaller than that of Comparative Example 3 is considered to be because the concentration of the isophoronediamine aqueous solution of Comparative Example 2 is higher than that of Comparative Example 3. That is, even by comparing Comparative Example 2 and Comparative Example 3, it can be seen that the desorption energy is reduced by increasing the concentration of the carbon dioxide absorbent.
[0106] In addition, the azobenzene used in Comparative Example 3 is a material that has low solubility in solvents such as water and ethanol and has high viscosity. For this reason, it was difficult to use the azobenzene solution for absorbing carbon dioxide even at a concentration of, for example, about 5 wt %.
[0107] From the viewpoint of providing the carbon dioxide absorbent with an increased concentration for carbon dioxide absorption, it is also assumed that the azobenzene solution is supported on a solid material. However, in order to easily prepare a solid absorbent, it is desirable that the concentration of the carbon dioxide absorbing solution before impregnating the solid material is high. In this regard, as shown in Comparative Example 2, an aqueous solution of isophorone diamine can be easily prepared at a concentration of, for example, about 15 wt%. In addition, by supporting an isophorone diamine solution on a solid material, it is also possible to increase the concentration of isophorone diamine in the solvent to several tens of wt% (Example 2). In other words, the fact that it has an amino group and has high solubility in the solvent is also an advantage of using a cyclic diamine such as isophorone diamine as a carbon dioxide absorbent.
[0108] [Verification 4] As described above, in the step S1 of preparing the first absorbent body 3a, before the carbon dioxide absorbing liquid 12 is supported on the substrate 10, the substrate 10 may be sprayed with a plasma gas or irradiated with ultraviolet rays. The effect of irradiating the substrate 10 with ultraviolet rays was verified, and will be described below.
[0109] Specifically, when preparing the first absorber 3a in the same manner as described above in Verification 1, the solid material was irradiated with ultraviolet light having a peak wavelength of about 172 nm using a Xe excimer lamp before being put into the mixed liquid. The ultraviolet light irradiation was performed at a radiance of several tens of mW / cm. 2 This took place for a few seconds.
[0110] Thereafter, the first absorbent 3a was weighed after the treatments such as evaporation of methanol and heating, and the amount of isophoronediamine supported on the solid material was estimated, in the same manner as described above in Verification 1. The results are compared with the amount of support obtained in Verification 1 without UV irradiation, and are shown in Table 1 below.
[0111] [Table 2]
[0112] According to Table 2, by irradiating the solid material with ultraviolet light, the amount of isophoronediamine supported in the solid material became about 1.2 times that in the case of no ultraviolet light irradiation (Verification 1). This is considered to be because ultraviolet light irradiation formed hydrophilic functional groups on the pore surfaces of the solid material, improving the wettability of the pore surfaces to the carbon dioxide absorbing solution containing isophoronediamine.
[0113] By increasing the amount of carbon dioxide absorbent supported in the solid material, the carbon dioxide absorption capacity of the absorber can be improved. Also, as a result of improving the wettability of the pore surface to the carbon dioxide absorbing liquid, it is presumed that peeling off of the carbon dioxide absorbing liquid from the pore surface is suppressed when the operations related to the carbon dioxide absorption process and desorption process are repeated (see Figure 3). In other words, by supporting the carbon dioxide absorbing liquid after irradiating the solid material with ultraviolet rays, deterioration of the absorber due to peeling off of the carbon dioxide absorbing liquid is suppressed even when carbon dioxide capture is repeated. This is expected to maintain the carbon dioxide capture capacity when looking at the entire capture system.
[0114] Hydrophilic functional groups can also be formed on the pore surfaces of solid materials by spraying plasma gas onto the pores. In other words, based on the results of this verification, it is inferred that spraying plasma gas can also hydrophilize the pore surfaces and increase the amount of carbon dioxide absorbent supported in solid materials.
[0115] [Verification 5] A case was examined in which a cyclic diamine other than isophoronediamine was used as the carbon dioxide absorbent, and this will be described below as Example 3.
[0116] Example 3 In Example 3, 4,4-methylenebis(2-methylcyclohexylamine) was used as the carbon dioxide absorbent instead of isophoronediamine. Hereinafter, for convenience, this amine-based material is referred to as "MBMCA".
[0117] In Example 3, the operations of absorbing and desorbing carbon dioxide were carried out in accordance with Example 2 of Verification 3, and the desorption energy was calculated from the experimental values. In addition, in consideration of the characteristics of the amine-based material, the weight change of the first absorbent body 3a when the operations of absorbing and desorbing carbon dioxide were repeated was evaluated.
[0118] Specifically, as described in Verification 1, the weight of the MBMCA solution was weighed out so that it was several tens of wt% per 1 g of solid material, and then the methanol added for stirring was evaporated and the solution was heated, etc., to obtain a first absorbent 3a.
[0119] Next, the first absorbent 3a obtained through the above operation was placed in the reaction tank 2, and carbon dioxide was absorbed into the first absorbent 3a (step S2). Then, heat was supplied to desorb the absorbed carbon dioxide (step S4). The operations of the carbon dioxide absorption step S2 and the heat supply step S4 were the same as those in Example 1 of the above-mentioned verification 2.
[0120] Using the same method as described in Verification 3, we evaluated the carbon dioxide desorption energy of MBMCA, which was approximately 2 GJ, which was almost the same as the desorption energy of isophoronediamine. In addition, the amount of carbon dioxide absorbed per mole of MBMCA was also approximately the same as that of isophoronediamine.
[0121] That is, even when the cyclic diamine MBMCA is used as the carbon dioxide absorbent instead of isophoronediamine, it can be understood that the desorption energy of carbon dioxide is reduced, as described in Example 2 of Verification 3. As described above, the use of the cyclic diamine can reduce the desorption energy of carbon dioxide.
[0122] In addition, MBMCA is characterized by having a large molecular weight of about 288 g / mol and a relatively high boiling point of about 340° C. In view of this, the weight change of the first absorbent body 3a when the operation of absorbing and desorbing carbon dioxide was repeated was evaluated.
[0123] Here, the supply of heat for desorbing the absorbed carbon dioxide may cause some of the amine-based material supported on the solid material to evaporate. More specifically, in the carbon dioxide absorption process, it is assumed that moisture in the gas G1 to be treated, such as the atmosphere, is adsorbed by the first absorber 3a together with carbon dioxide, and the amine-based material is locally converted into an aqueous solution state. In this state, it is believed that the supply of heat for desorbing carbon dioxide makes it easier for some of the amine-based material to evaporate together with the moisture.
[0124] When the evaporation of the amine-based material from the first absorbent body 3a becomes significant, it becomes necessary to replace the first absorbent body 3a earlier. Therefore, in consideration of maintaining the carbon dioxide recovery capacity of the first absorbent body 3a, it is preferable to suppress the weight change of the first absorbent body 3a caused by the evaporation of the amine-based material.
[0125] In contrast, when the operation of absorbing and desorbing carbon dioxide was repeated a predetermined number of times for the first absorbent body 3a carrying MBMCA, the weight change of the first absorbent body 3a was small, being less than 1%.
[0126] The reason why the weight change of the first absorbent 3a was suppressed to a small value of 1% or less is believed to be due to the high boiling point of MBMCA. In view of the large molecular weight and high boiling point, a cyclic diamine such as MBMCA may be used as the carbon dioxide absorbent. In other words, by using MBMCA as the amine-based material, it is believed that the amount of carbon dioxide absorbed can be increased while suppressing the evaporation of the amine-based material due to heat supply or the like.
[0127] In addition, in view of this verification, it is also suitable to adopt 4,4-methylenebis(cyclohexylamine) as the carbon dioxide absorbent. For the sake of convenience, this amine-based material will be referred to as "MBCA" below.
[0128] MBCA is a cyclic diamine with a similar structure to MBMCA, and is characterized by a large molecular weight of approximately 210 g / mol and a relatively high boiling point of approximately 330° C. In light of this, it is believed that even when MBCA is used as a carbon dioxide absorbent, it is possible to increase the amount of carbon dioxide absorbed while suppressing the evaporation of amine-based materials due to heat supply, etc., just like MBMCA.
[0129] In other words, MBMCA and MBCA are suitable materials in that the weight change of the first absorbent body 3a is suppressed when the operation of absorbing and desorbing carbon dioxide is repeated. In view of this, a cyclic diamine such as MBMCA or MBCA may be adopted as the amine-based material.
[0130] [Verification 6] Next, the effect of forming the solid material supporting the carbon dioxide absorbing liquid 12 from a carbon material was verified, and will be described below as Example 4. Specifically, when preparing the first absorbent 3a by the same method as described above in Verification 1, the solid material supporting the isophoronediamine solution was changed. In this verification, the weight change of the first absorbent 3a when the operation of absorbing and desorbing carbon dioxide was repeated was evaluated.
[0131] Example 4 The first absorbent 3a was prepared in the same manner as in the above-mentioned verification 1, except that pellet-shaped activated carbon was used as the solid material for supporting the isophoronediamine solution. The activated carbon had a cylindrical shape, an average particle size of 1.5 mm to 3.0 mm, and a height of about 5 mm. The specific surface area was about 3000 m 2 The pore size was 1.47 ml / g and the pore volume was 1.47 ml / g. Furthermore, the diameter D2 of the pores 11 of the activated carbon was 1.8 nm (see FIG. 4A).
[0132] As described in the Verification 1 section, the weight of the isophoronediamine solution was weighed out so that it was several tens of wt% per 1 g of solid material, and then the methanol added for stirring was evaporated and the solution was heated, etc., to obtain a first absorbent body 3a.
[0133] Next, the first absorbent 3a obtained through the above operation was placed in the reaction tank 2, and carbon dioxide was absorbed into the first absorbent 3a (step S2). Then, heat was supplied to desorb the absorbed carbon dioxide (step S4). The operations of the carbon dioxide absorption step S2 and the heat supply step S4 were the same as those in Example 1 of the above-mentioned verification 2.
[0134] When the operation of absorbing and desorbing carbon dioxide was repeated a predetermined number of times for the first absorbent 3a in which the solid material was activated carbon, the weight change of the first absorbent 3a was extremely small, being 0.1% or less.
[0135] The present inventors speculate as follows about the reason why the weight change of the first absorbent 3a in Example 4 was suppressed to an extremely small value of 0.1% or less. In a carbon material such as activated carbon, six-membered or five-membered ring structures formed by carbon atoms are stacked irregularly. On the other hand, a cyclic diamine such as isophoronediamine is also a cyclic compound and has a ring structure in its structure. Since both the carbon material and the cyclic diamine have a ring structure, it is speculated that a bonding force resulting from π-electron interaction is generated between the two ring structures.
[0136] In other words, in Example 4, the weight change of the first absorbent 3a was extremely small, and it is presumed that this is because the solid material was activated carbon, which generated a bonding force between isophoronediamine and the solid material due to π-electron interactions, resulting in isophoronediamine being more firmly supported on the solid material.
[0137] In addition, micropores smaller than the diameter D2 typically exist inside the pores 11 of a carbon material such as activated carbon. It is presumed that the anchor effect caused by the existence of the micropores also contributes to the support of isophoronediamine on the solid material.
[0138] As described in the above verification 5, when the evaporation of isophorone diamine from the first absorbent body 3a becomes significant, it becomes necessary to replace the first absorbent body 3a earlier. Therefore, from the viewpoint of maintaining the carbon dioxide recovery capacity of the first absorbent body 3a, it is preferable to suppress the weight change of the first absorbent body 3a caused by the evaporation of isophorone diamine.
[0139] In contrast, in Example 4, the weight change of the first absorbent 3a is small, and the evaporation of isophorone diamine is suppressed. In other words, in Example 4, it is presumed that the solid material is activated carbon, and as a result, isophorone diamine is more firmly supported on the solid material, and the evaporation of isophorone diamine is suppressed. From the viewpoint of suppressing the weight change of the first absorbent 3a, a carbon material such as activated carbon may be adopted as the solid material supporting the carbon dioxide absorbing liquid. In addition, although the above description is based on the assumption that the amine material is isophorone diamine, the same discussion is also possible in the case where the amine material is, for example, a cyclic diamine such as MBMCA.
[0140] Furthermore, if the diameter D2 of the pores 11 in the activated carbon is larger, the contact area between the carbon dioxide absorbing liquid 12 supported in the pores and the carbon dioxide contained in the gas to be treated G1 will be larger, and it is believed that carbon dioxide will be absorbed more efficiently.
[0141] Here, in Example 2, the diameter D2 of the pores 11 of the silica used as the solid material was 50 nm. As an example, the present inventors carried out the operation of absorbing and desorbing carbon dioxide by supporting the carbon dioxide absorbing liquid 12 in the same manner as in Example 2 on silica having pores 11 with diameters D2 of 10 nm and 30 nm, respectively, and confirmed that the amount of carbon dioxide absorbed increased as the diameter D2 of the pores 11 increased. It is considered that the same is true even when the solid material is activated carbon, in that the absorption of carbon dioxide is efficiently performed by increasing the diameter D2 of the pores 11 of the solid material.
[0142] On the other hand, the present inventors confirmed a phenomenon in which, in the case where the carbon dioxide absorbing liquid 12 is supported on silica, if the diameter D2 of the pores 11 of the silica exceeds 0.1 μm, a part of the supported carbon dioxide absorbing liquid 12 peels off from the pores 11. It is presumed that this phenomenon may also occur in the pores 11 of activated carbon.
[0143] In view of the above, it is preferable that the diameter D2 of the pores 11 in the carbon material such as activated carbon is in the range of 30 nm to 0.1 μm.
[0144] That is, an absorber that is a porous substance made of a carbon material and has a cyclic diamine supported in the pores can suitably absorb and desorb carbon dioxide using the cyclic diamine while suppressing evaporation of the cyclic diamine caused by heat supply, etc. As described above, the average pore size of the porous substance is preferably in the range of 30 nm to 0.1 μm.
[0145] Activated carbon can be produced by activating wood materials such as coconut shells and sawdust using a conventionally known method. As an example, activated carbon can be produced by activating wood materials using an activator such as potassium hydroxide (also called "alkali activation"). Another method for producing activated carbon is to activate wood materials using a gas such as water vapor (also called "gas activation"). The diameter D2 of the pores 11 in the activated carbon can be adjusted by appropriately changing the conditions of the activation treatment.
[0146] Furthermore, even when the solid material is made of a carbon material, in the step S1 of preparing the first absorbent 3a, the solid material may be sprayed with plasma gas or irradiated with ultraviolet rays before the carbon dioxide absorbing liquid 12 is supported thereon.
[0147] As described in the section on verification 4, hydrophilic functional groups are formed on the surfaces of the pores 11 in the solid material by irradiating them with ultraviolet light or spraying them with plasma gas. A specific example of such a functional group is a hydroxyl group (-OH), in which electrons are localized on the oxygen atom, and the oxygen atom is in a charged state.
[0148] For this reason, it is considered that a bonding force resulting from dipole interaction occurs between the hydroxyl groups formed in the pores and the carbon atoms and hydrogen atoms in the amine-based material such as isophoronediamine. It is considered that the bonding force causes the carbon dioxide absorbing liquid 12 to be more firmly supported in the pores 11 of the carbon material. This increases the support ratio when preparing the first absorbent 3a, and suppresses evaporation of the amine-based material when desorbing carbon dioxide.
[0149] In view of the above, it is preferable to blow plasma gas or irradiate ultraviolet rays onto the pores 11 of the carbon material such as activated carbon before supporting the carbon dioxide absorbing liquid 12.
[0150] Furthermore, when adjusting the first absorbent 3a, the mode of utilizing the binding force derived from the π-electron interaction between the carbon material and the amine-based material, which is a cyclic diamine, is not limited to the example in which the solid material is a carbon material. For example, even when the solid material is composed of silica, a fibrous or powdery carbon material may be added to the mixed liquid into which the solid material is added when supporting the carbon dioxide absorbing liquid 12 in the pores 11. Examples of the carbon material include carbon fibers such as carbon nanotubes. As an example, the weight ratio of the amine-based material, the solvent such as PEG, and the carbon material is 75:25:100.
[0151] The carbon material added to the mixed liquid is supported in the pores 11 together with the carbon dioxide absorbing liquid 12. At this time, a bonding force resulting from the above-mentioned π electron interaction is generated between the carbon material and the amine material in the carbon dioxide absorbing liquid 12. It is considered that the bonding force suppresses the amine material from being desorbed from the carbon material, and as a result, even if heat is supplied for desorption of absorbed carbon dioxide, for example, the amine material is less likely to evaporate from the pores 11.
[0152] Additionally, in view of the above discussion, the solid material may be comprised of a porous material including cellulose.
[0153] An example of the molecular structure of cellulose is shown in the following formula (2). As shown in formula (2), cellulose has a six-membered ring structure containing carbon atoms, and is therefore considered to bind more strongly to cyclic diamines such as isophoronediamine through π-electron interaction. In addition, since cellulose has many hydroxyl groups, an increase in the binding force resulting from the above-mentioned dipole interaction between cellulose and amine-based materials can also be expected. In this way, by supporting the carbon dioxide absorbing liquid 12 on a porous substance containing cellulose, it is possible to efficiently support the carbon dioxide absorbing liquid 12 on a solid material, or to suppress deterioration of the carbon dioxide absorbing liquid 12 due to the carbon dioxide desorption operation. [ka]
[0154] The cellulose-containing porous material is produced by mixing cellulose fibers obtained by defibrating plant fibers (also called "pulp") obtained from wood and the like with a resin material, such as polypropylene or polyethylene.
[0155] More specifically, cellulose fiber is obtained by dispersing pulp in an aqueous solution and defibrating the pulp through chemical treatment such as TEMPO oxidation or mechanical treatment such as crushing. A granular or pellet-shaped solid material can be produced by mixing and molding the cellulose fiber and resin material. For example, the ratio of cellulose fiber to resin material is 7:3.
[0156] The solid material is a porous substance having pores formed by the gaps between fibrous cellulose fibers. The diameter of the pores is, for example, about 50 nm. The diameter of the pores can be appropriately adjusted by adjusting the defibration conditions of the cellulose fibers to change the thickness and length of the cellulose fibers. In the cellulose-containing porous substance, as in the carbon material, the diameter of the pores is preferably 50 nm to 1 μm.
[0157] Cellulose fiber is a carbon-neutral material that absorbs carbon dioxide emitted during exhaust incineration because it is made from wood and other raw materials. Cellulose fiber can also be produced from thinned wood and inedible parts of food ingredients such as corn. In other words, the use of cellulose fiber is advantageous because it can reduce carbon dioxide emissions resulting from the operation of a carbon dioxide capture system.
[0158] As described above, according to the present invention, it is possible to increase the efficiency of carbon dioxide capture while reducing the amount of energy input, as compared to conventional methods. This will also contribute greatly to Goal 13 of the Sustainable Development Goals (SDGs) led by the United Nations, which is to "take urgent action to combat climate change and its impacts."
[0159] [Second embodiment] Hereinafter, the second embodiment of the carbon dioxide recovery system will be described, focusing on the differences from the first embodiment.
[0160] In the above first embodiment, the heat source 4 is disposed inside the reaction tank 2, but the heat source 4 can also be disposed outside the reaction tank 2 at a position independent of the reaction tank 2. That is, in this embodiment, the heat transfer medium heated by the heat source 4 is introduced into the reaction tank 2 and supplies heat H1 to the second absorber 3b inside the reaction tank 2.
[0161] 8 is a diagram showing a schematic configuration of a second embodiment of the recovery system 1, and some components are shown in a block diagram. As shown in FIG. 8, the recovery system 1 according to this embodiment includes a reaction tank 2, a heat source 4, a first flow path 31 connecting the heat source 4 and the reaction tank 2, a second flow path 32 introducing the gas to be treated G1 into the reaction tank 2, and a third flow path 33 located downstream of the reaction tank 2 with respect to the flow direction of the gas to be treated G1, etc. In addition, FIG. 8 shows a scene of step S4 (see FIG. 3), in which the air as the heat transfer medium A1 is introduced into the reaction tank 2 from the first flow path 31.
[0162] In this embodiment, the air sent to the reaction tank 2 by a flow mechanism such as a blower fan (not shown) is used as the heat transfer medium A1. In this embodiment, the gas G1 to be treated is air. For this reason, the recovery system 1 includes a first valve V1 capable of controlling the flow rate of air flowing through the second flow path 32, a second valve V2 capable of controlling the flow rate of air flowing through the first flow path 31, and a control unit 8 that controls the open / closed states of each valve (V1, V2). In FIG. 8, the first valve V1 is in a closed state, and the second valve V2 is in an open state. In order to represent the open / closed states of the valves in a schematic manner, the positions of each valve relative to the piping are drawn to be different.
[0163] The reaction tank 2 also has a thermometer 9 that measures the temperature of the internal space of the reaction tank 2. The control unit 8 can transmit signals (d1, d2) to each valve (V1, V2) for adjusting the valve opening based on temperature information d0 in the reaction tank 2 from the thermometer 9, as described below.
[0164] The configuration of this embodiment will be described below with reference to Fig. 9 to Fig. 12. Fig. 9 and Fig. 10 are cross-sectional views that typically show the structure of the reaction tank 2, with Fig. 9 corresponding to the scene of step S2 and Fig. 10 corresponding to the scene of step S4 (see Fig. 3). Fig. 11 and Fig. 12 are cross-sectional views that typically show the structure of the heat source 4, with Fig. 12 being a drawing of the heat source 4 in Fig. 11 as viewed from the Z direction following Fig. 2.
[0165] 9, the first absorber 3a prepared through the above-mentioned step S1 is placed inside the reaction tank 2. Then, the second valve V2 is closed and the first valve V1 is open, and air as the gas to be treated G1 is introduced into the reaction tank 2 through the inlet 5b. The first absorber 3a absorbs carbon dioxide contained in the gas to be treated G1, thereby obtaining the second absorber 3b (step S2).
[0166] Next, step S3 is performed by the heat source 4. As shown in Fig. 11, the heat source 4 has a heating tank 4a, a heat collecting member 15 arranged vertically above (on the +Z side of) the heating tank 4a, a heat transfer member 19 arranged directly on the heat collecting member 15, and a light transmitting portion 20 for taking in solar light C2. Note that, for convenience of illustration, the light transmitting portion 20, the heat collecting member 15, and the heat transfer member 19 are partially omitted in Fig. 12. The heat source 4 has a structure common to the reaction tank 2 according to the first embodiment, and therefore the description of the common portions will be simplified.
[0167] As shown in Fig. 11, air as the heat transfer medium A1 is introduced into the heating tank 4a through the inlet 5. Then, the heat transfer medium A1 comes into contact with the heat transfer member 19, which has been heated by the heat H1 obtained by converting solar light C2 by the heat collecting member 15, and is heated. Thereafter, the heat transfer medium A1 is discharged from the outlet 6 and sent into the reaction tank 2 through the first flow path 31. Note that the same discussion as in the first embodiment can be applied to the light transmitting portion 20.
[0168] From the viewpoint of increasing the contact area between the heat transfer member 19 and the heat transfer medium A1, the heat transfer member 19 may be, for example, a plate-shaped member, and may be arranged so that its main surface is approximately perpendicular to the flow direction of the heat transfer medium A1, as shown in Fig. 12. From the same viewpoint, a flow passage section 25, which is located between the inner wall of the heating tank 4a and the heat transfer member 19 in the Y direction and through which the heat transfer medium A1 passes, may be configured to overlap with the main surface of the heat transfer member 19 located at the rear stage in the flow direction of the heat transfer medium A1 when viewed in the X direction (flow direction). Note that the "main surface" here refers to a surface of the plate-shaped heat transfer member 19 that has a much larger area than the other surfaces.
[0169] As shown in Fig. 10, air as the heat transfer medium A1 heated by the heat source 4 is introduced into the reaction tank 2 where the second absorbent 3b is located through the inlet 5a. At this time, typically, the second valve V2 is opened and the first valve V1 is closed. In this manner, the high-temperature heat transfer medium A1 is brought into contact with the second absorbent 3b, and heat H1 is supplied to the second absorbent 3b (step S4).
[0170] The recovered gas G2 containing the carbon dioxide desorbed from the second absorbent 3b by the supply of heat H1 is recovered via the outlet 6a (step S5).
[0171] In this embodiment, since the air is used as the heat transfer medium A1, the carbon dioxide concentration in the vicinity of the second absorber 3b can be reduced by introducing the heat transfer medium A1 into the reaction vessel 2. In other words, the air used as the heat transfer medium A1 also functions as a desorption-promoting gas B1 that promotes desorption of carbon dioxide.
[0172] By heating the second absorbent 3b with the air as the heat transfer medium A1, the absorbed carbon dioxide is desorbed. From the viewpoint of repeatedly using the absorbent 3 (see FIG. 3), it is preferable to reduce the thermal effect on the second absorbent 3b. For this reason, the control unit 8 receives temperature information d0 from the thermometer 9, and when the temperature in the reaction tank 2 is equal to or higher than a predetermined value, transmits a signal d1 to adjust the opening degree of the first valve V1. By adjusting the opening degree of the first valve V1, it is possible to introduce air at a lower temperature than the heat transfer medium A1, thereby lowering the temperature in the reaction tank 2 and reducing the thermal effect on the second absorbent 3b. That is, the air in this case corresponds to the "cooling gas". Also, from the viewpoint of promoting the cooling of the temperature in the reaction tank 2, the signal d2 may be transmitted to the second valve V2 to adjust the opening degree of the second valve V2. The predetermined value is, for example, a value determined in consideration of the heat resistance, such as the boiling point, of the carbon dioxide absorbent constituting the absorbent 3. The predetermined value may be, for example, 100°C or less, preferably 80°C or less, and more preferably 60°C or less.
[0173] In this embodiment, an example has been described in which the control unit 8 adjusts the opening of each valve (V1, V2) based on the temperature information d0 from the thermometer 9 to lower the temperature in the reaction tank 2 in step S4. However, the control unit 8 may also perform control to open the first valve V1 and close the second valve V2 for a predetermined time, for example, when the accumulated time during which V2 is in an open state reaches a preset time.
[0174] In this embodiment, a configuration for heating the heat transfer medium A1 introduced into the reaction tank 2 has been shown, but as described with reference to FIG. 1, a configuration of a heat source 4 disposed in the reaction tank 2 for heating the heat transfer medium A1 and the second absorber 3b may be used in combination.
[0175] [Another embodiment] 13 and 14 are diagrams showing a schematic configuration of another embodiment of the collection system 1, with a part of the configuration shown in a block diagram. Fig. 13 corresponds to a scene where step S2 is performed, and Fig. 14 corresponds to a scene where steps S4 and S5 are performed.
[0176] This embodiment includes a heat exchanger 36 that exchanges heat between the air as the heat transfer medium A1 and the recovered gas G2 containing carbon dioxide recovered from the reaction tank 2 (see FIG. 14). The recovery system 1 also includes a fourth flow path 34 (see FIG. 13) that branches off from the third flow path 33 and through which the gas to be treated G1 flows after passing through the reaction tank 2, and a fourth valve V4 arranged in the fourth flow path 34. Note that the configurations of the reaction tank 2 and the heat source 4 can be discussed in the same manner as described with reference to FIGS. 9 to 12.
[0177] 13, when step S2 is performed, the first valve V1 and the fourth valve V4 arranged in the second flow path 32 are opened, and a flow mechanism such as a fan (not shown) introduces the gas to be treated G1 into the reaction tank 2. In the reaction tank 2, the gas to be treated G1 from which carbon dioxide has been absorbed by the first absorber 3a is discharged via the fourth flow path 34, for example, to the outside space.
[0178] As shown in FIG. 14, when steps S4 and S5 are performed, the second valve V2 disposed in the first flow path 31 through which the air flows as the heat transfer medium A1 and the third valve V3 disposed in the third flow path 33 through which the recovered gas G2 flows are opened. In this embodiment, as shown in FIG. 14, the air in the space in which plants are grown in the plant factory 35 (hereinafter, for convenience, referred to as the "growth space 35a") is used as the heat transfer medium A1. Furthermore, the recovered gas G2 containing carbon dioxide desorbed from the second absorbent 3b in the reaction tank 2 can be used in the growth space 35a. The recovered gas G2 contains carbon dioxide desorbed by heating the second absorbent 3b, and therefore has a higher temperature than the air as the heat transfer medium A1. Therefore, it is preferable to perform heat exchange between the recovered gas G2 and the air as the heat transfer medium A1.
[0179] In addition, although the amount is small, the cyclic diamine contained in the second absorber 3b may evaporate due to the supply of heat H1. Therefore, it is assumed that the recovered gas G2 contains a small amount of cyclic diamine-derived components evaporated by the supply of heat H1. In view of this, it is preferable to cool the recovered gas G2 by performing heat exchange between the recovered gas G2 and wastewater for hydroponic cultivation (not shown) in the plant factory 35. By cooling the recovered gas G2, the cyclic diamine-derived components are cold-trapped, and the cyclic diamine-derived components can be prevented from flowing into the growth space 35a. In addition, in order to supply sufficient heat to the atmosphere as the heat transfer medium A1, it is preferable that the heat exchange as the cold trap is performed after the heat exchange between the atmosphere and the recovered gas G2.
[0180] In the plant factory 35, it is assumed that the growth lights are turned on or off in accordance with the circadian rhythm specific to the plants. That is, while the lights are turned on, the carbon dioxide concentration in the growth space 35a decreases due to photosynthesis by the plants. Therefore, from the viewpoint of enhancing the effect of the desorption promoting gas B1 described above, it is preferable to use the air in the growth space 35a as the heat transfer medium A1. When the carbon dioxide concentration in the growth space 35a is high due to respiration of the plants or the like (typically while the growth lights are turned off), the air in another space, such as an outside space, may be used as the heat transfer medium A1.
[0181] <2> In the second embodiment, in step S4, the air as the heat transfer medium A1 is introduced into the internal space of the reaction tank 2. However, as shown in FIG. 15, heat exchange may be performed between the heat transfer medium A1 flowing on the outside of the reaction tank 2 and the reaction tank 2 in which the second absorbent 3b is located. FIG. 15 is a diagram that shows a part of another configuration example of the recovery system 1. FIG. 16A is a perspective view that shows a configuration of the heat source 4 in FIG. 15, and FIG. 16B is a ZY cross-sectional view of the heat source 4 in FIG. 16A when viewed from the X direction. In FIG. 16A and FIG. 16B, the flow direction of the heat transfer medium A1 is the X direction.
[0182] The heat source 4 in FIG. 16A has an L-shaped cross section as shown in FIG. 16B, for example, and contains water as a heat transfer medium A1 inside. The heat source 4 has a flat heat collecting member 15 on a part of the outer wall surface, and the heat collecting member 15 is heated by absorbing solar light C2, and generates high-temperature water (hereinafter, referred to as "hot water"). Typically, the heat source 4 is placed on an inclined surface such as a stand 41 so that the heat collecting member 15 can efficiently receive the solar light C2. The hot water is configured to flow through a flow path 40, and heat H1 can be supplied to the second absorber 3b in the reaction tank 2 by performing heat exchange between the hot water as the heat transfer medium A1 and the reaction tank 2.
[0183] At this time, in order to reduce the carbon dioxide concentration in the reaction tank 2 and promote desorption of absorbed carbon dioxide from the second absorber 3b, air may be introduced into the reaction tank 2 as a desorption promotion gas B1, for example, from the second flow path 32 (see Figure 15).
[0184] 15 has described an example in which heat exchange is performed between hot water serving as heat transfer medium A1 flowing through flow path 40 and reaction tank 2. However, heat exchange may also be performed between the hot water and air serving as heat transfer medium A1 flowing through first flow path 31 described with reference to FIGS. 8 and 10. In other words, air that has been heated by the heat exchange is introduced into reaction tank 2, whereby heat H1 is supplied to second absorbent 3b (see FIG. 10), and absorbed carbon dioxide is desorbed.
[0185] <4> The above-mentioned embodiments can be realized by appropriately combining them. For example, a heat source 4 may be additionally disposed inside the reaction tank 2 according to Fig. 8 or Fig. 15. The reaction tank 2 may have the same configuration as that described with reference to Fig. 1.
[0186] <5> In the above description, the absorbent body 3 is described as being granular, but as mentioned above, the shape of the absorbent body 3 is not limited to this, and it may be, for example, in a plate shape.
[0187] <6> In the above, the heat H1 obtained by converting the solar light C2 is supplied to the second absorber 3b, but the present invention is not limited to a method for supplying heat to the second absorber 3b. For example, the second absorber 3b may be heated using a heater, a boiler, or the like. [Explanation of symbols]
[0188] 1: Collection system 1a: Collection method 2: Reactor 3: Absorber 3a: First absorbent 3b: Second absorbent 4: Heat source 4a: Heating tank 5,5a,5b: Inlet 6,6a: Outlet 8: Control section 9: Thermometer 10: Base material 11: Pore 12: Carbon dioxide absorbing liquid 15: Heat collecting member 19: Heat transfer materials 20 : Translucent part 21: Transparent material 22: Low pressure space 25: Flow section 30: Halogen lamp 31, 32, 33, 34, 40: Channel 35: Plant factory 35a: Growth space 36 : Heat exchanger 41: Mount A1: Heat transfer medium B1: Desorption promoting gas C1: Sun C2: Sunlight G1: Gas to be treated G2: Recovered gas
Claims
1. A step (a) of preparing a first absorbent body which is an absorbent body before absorbing carbon dioxide by supporting a carbon dioxide absorbing liquid containing a cyclic diamine exhibiting basicity in a solid material made of a porous substance having pores on the surface of the solid material; A step (b) of absorbing carbon dioxide into the first absorbent to prepare a second absorbent which is an absorbent having absorbed carbon dioxide; (c) providing heat to the second absorbent body; and a step (d) of recovering the carbon dioxide desorbed from the second absorbent via the step (c).
2. 2. The method for recovering carbon dioxide according to claim 1, wherein the step (a) includes a step of blowing a plasma gas or irradiating ultraviolet rays onto the pores of the solid material before the carbon dioxide absorbing liquid is supported in the pores.
3. 3. The method for recovering carbon dioxide according to claim 1, wherein the cyclic diamine is isophoronediamine.
4. 3. The method for recovering carbon dioxide according to claim 1, wherein the cyclic diamine is 4,4-methylenebis(2-methylcyclohexylamine) or 4,4-methylenebis(cyclohexylamine).
5. 3. The method for recovering carbon dioxide according to claim 1, wherein the porous substance is a carbon material.
6. The method for recovering carbon dioxide according to claim 5, wherein the average pore diameter of the porous material is in the range of 30 nm to 0.1 μm.
7. The method for recovering carbon dioxide according to claim 5, wherein the cyclic diamine is isophoronediamine, 4,4-methylenebis(2-methylcyclohexylamine), or 4,4-methylenebis(cyclohexylamine).
8. The method for recovering carbon dioxide according to claim 1 , wherein the step (a) includes a step of adding a carbon material to the carbon dioxide absorbing liquid.
9. 2. The method for recovering carbon dioxide according to claim 1, wherein the porous material comprises cellulose.
10. The method for recovering carbon dioxide according to claim 8 or 9, wherein the cyclic diamine is isophoronediamine, 4,4-methylenebis(2-methylcyclohexylamine), or 4,4-methylenebis(cyclohexylamine).
Citation Information
Patent Citations
Method for removing carbon dioxide and sulfur compounds in combustion exhaust gas
JP1993245339A
Cited By
CO2 Extraction and Storage System
JP7655605B1