Prepreg, method for manufacturing prepreg and molding

By using a polyetherimide resin with tailored molecular weight distribution and high-temperature impregnation, the bending strength of prepregs is improved, resulting in stronger molded articles.

JP2024144073APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023209103
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-12-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing prepregs containing polyetherimide resin lack sufficient bending strength, limiting their application in demanding structural components.

Method used

Incorporating a polyetherimide resin with specific molecular weight distribution and peak structures in the prepreg, including a peak top (P2) with higher molecular weight than peak top (P1) in the GPC chromatogram, and manufacturing methods involving heating the resin film to 380°C or higher for impregnation.

Benefits of technology

The method enhances the bending strength of molded articles made from these prepregs, improving mechanical properties and moldability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144073000001
    Figure 2024144073000001
  • Figure 2024144073000002
    Figure 2024144073000002
  • Figure 2024144073000003
    Figure 2024144073000003
Patent Text Reader

Abstract

To improve flexural strength of a molding obtained by molding a prepreg containing a polyetherimide resin.SOLUTION: A prepreg contains a reinforcement fiber and a polyetherimide resin, wherein the polyetherimide resin has a peak top (P1) of a peak having a maximum area and a peak top (P2) having a molecular weight higher than that of the peak top (P1) in a GPC chromatogram.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a prepreg, a method for producing a prepreg, and a molded article. [Background technology]

[0002] Polyetherimide (hereinafter referred to as polyetherimide) resins have flame retardancy, heat resistance, and mechanical properties that exceed those of engineering plastics such as polyamide resins and polycarbonate resins, and therefore are being increasingly used as metal replacements. Therefore, in order to further expand the range of applications, fiber-reinforced composite materials in which matrix resins containing these resins are reinforced with reinforcing fibers have been proposed. For example, Patent Documents 1 and 2 disclose fiber-reinforced composite materials such as intermediate materials and prepregs that use polyetherimide resin as a matrix resin. In addition, when producing a prepreg containing polyetherimide by heating and melting, the melt viscosity of the resin is high, so there is a method of producing a prepreg by lowering the viscosity using a solvent that dissolves the polyetherimide resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-119506 A [Patent Document 2] JP 2012-246442 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to improve the bending strength of a molded article obtained by molding a prepreg containing a polyetherimide resin. The problems to be solved by each aspect of the present invention may be explicitly or implicitly disclosed in the present specification. [Means for solving the problem]

[0005] The prepreg of the present invention includes the following aspect [1], and the manufacturing method of the prepreg of the present invention includes the following aspect [2]. [1] A prepreg comprising reinforcing fibers and a polyetherimide resin, the polyetherimide resin having a peak top (P1) of a peak with a maximum area in a GPC chromatogram and a peak top (P2) having a higher molecular weight than the peak top (P1). [2] A method for producing a prepreg, comprising laminating a polyetherimide resin film on a fiber substrate and heating the laminate to impregnate the fiber substrate with a resin contained in the polyetherimide resin film, wherein the polyetherimide resin film has a thickness of 10 to 100 μm and is heated to 380° C. or higher. Effect of the Invention

[0006] According to the present invention, a molded article having improved bending strength can be obtained by molding a prepreg containing a polyetherimide resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] <Prepreg> The prepreg of the present invention contains reinforcing fibers and a polyetherimide resin, and the polyetherimide resin has at least one peak top (P2) having a higher molecular weight than the peak top (P1) of the peak with the largest area in a GPC chromatogram.

[0008] The prepreg of the present invention may further contain components (optional components) other than the polyetherimide resin and the reinforcing fibers. Examples of the form of the prepreg include a unidirectional prepreg (UD prepreg) in which a sheet-like reinforcing fiber bundle in which reinforcing fibers are aligned in one direction is impregnated with a matrix resin containing a polyetherimide resin, a cross prepreg in which a woven fabric of reinforcing fibers is impregnated with a matrix resin, and a tow prepreg in which a tow (reinforcing fiber bundle) is impregnated with a matrix resin in advance.

[0009] [Polyetherimide resin] The polyetherimide resin used in the prepreg of the present invention is a resin having a repeating unit containing an ether bond and an imide bond, and serves as a matrix resin in the prepreg of the present invention. The polyetherimide resin is a thermoplastic resin containing an aliphatic chain or an aromatic ring, as well as an ether bond and an imide bond. This polyetherimide may have a substituent within a range that does not impair the effects of the present invention. Of these, the polyetherimide resin used in the present invention preferably has a repeating unit represented by the following formula (3) (sometimes referred to as "repeating unit (3)").

[0010] [ka] ...Equation (3)

[0011] In formula (3), Y represents a divalent group having -O- or an ether bond, and Z represents an arylene group which may have a substituent. Examples of the arylene group include a phenylene group, a naphthylene group, a biphenylene group, etc. Examples of the divalent group having an ether bond include the groups shown below.

[0012] [ka]

[0013] Among the above, the polyetherimide resin of the present invention preferably contains a polyetherimide resin having a repeating unit represented by the following formula (1) (hereinafter, sometimes referred to as "repeating unit (1)").

[0014] [ka] ...Equation (1)

[0015] In the above formula (1), n ​​(the number of repetitions) is usually an integer in the range of 10 to 1000, and is preferably 20 or more, and more preferably 50 or more, in order to achieve an excellent balance between heat resistance and moldability. Also, n is preferably 1000 or less, and more preferably 500 or less. When it is contained as a high molecular weight substance, n (the repeat number) is usually an integer in the range of 1,000 to 100,000, preferably at least 1,000, and more preferably at least 2,000. By making it at least the lower limit, the mechanical properties of the molded article are improved.

[0016] In the repeating unit represented by the above formula (1), the imide bond position is at the meta position. On the other hand, there are also polyetherimide resins in which the imide bond position is at the para position, such as the repeating unit represented by the following formula (2). As the polyetherimide resin used in the present invention, those containing a polyetherimide resin having a repeating unit represented by the following formula (2) (hereinafter, sometimes referred to as "repeating unit (2)") are also preferred. Therefore, it is preferable that the polyetherimide resin used in the present invention contains at least one structural unit of formula (1) and formula (2).

[0017] [ka] ...Equation (2)

[0018] In the above formula (2), n (the number of repetitions) of the polyetherimide resin present in the peak with the largest area derived from the polyetherimide resin in the GPC chromatogram is an integer in the range of 10 to 1000, and is preferably 50 or more, more preferably 100 or more, in order to provide an excellent balance between heat resistance and moldability. Also, it is preferably 1000 or less, more preferably 500 or less. When it is contained as a high molecular weight substance, n (the repeat number) is an integer in the range of 1000 to 100000, preferably at least 2000, and more preferably at least 5000. By making it at least the lower limit, the mechanical properties of the molded article are improved. The inclusion of a high molecular weight component can suppress interfacial cracking between the reinforcing fiber and the polyetherimide resin, improving the mechanical properties of the molded article.

[0019] The polyetherimide resin contained in the prepreg of the present invention has at least one peak top (P2) having a higher molecular weight than the peak top (P1) of the maximum area peak derived from the polyetherimide resin in a GPC chromatogram. By having the peak top (P2), interfacial cracking between the reinforcing fiber and the polyetherimide resin is suppressed, and the mechanical properties of the molded article are improved. In this GPC chromatogram, the peak area including the peak top (P2) relative to the total peak area derived from the polyetherimide resin is preferably 0.10% or more, more preferably 0.25% or more, even more preferably 0.30% or more, particularly preferably 0.50% or more, and especially preferably 0.55% or more. On the other hand, it is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably 2.0% or less. When it is above the lower limit, a high strength of the molded product is obtained, and when it is below the upper limit, it is easily softened when heated and the moldability is improved. The content of the high molecular weight substance is calculated from the area ratio of the total peak area derived from the polyetherimide resin in the GPC (gel permeation chromatography) chromatogram to the sum of the peak areas having peak tops with a molecular weight higher than the peak top (P1) of the peak with the largest area in the chromatogram.

[0020] The molecular weight distribution of the polyetherimide resin present in the peak with the largest area derived from the polyetherimide resin in the GPC chromatogram is preferably 1.1 or more, more preferably 1.5 or more, and particularly preferably 2.0 or more. The molecular weight distribution is preferably 8.0 or less, more preferably 5.0 or less, and particularly preferably 4.0 or less. If the molecular weight distribution is within the above range, the high molecular weight component and the low molecular weight component are in appropriate amounts, and the balance between mechanical properties and chemical resistance tends to be excellent.

[0021] In the GPC chromatogram of the polyetherimide resin contained in the prepreg, the weight average molecular weight (Mp1) of the peak top (P1) with the largest area is 1.0×104 More preferably, it is 3.0×10 4 More preferably, it is 8.0×10 or more. 5 It is preferable that the value is less than 6.0×10 5 It is more preferable that the molecular weight is not more than the lower limit. When the molecular weight is not less than the upper limit, the mechanical properties of the molded product are excellent, and when the molecular weight is not more than the upper limit, the productivity of the prepreg can be increased. In addition, in a GPC chromatogram of the polyetherimide resin used in the prepreg of the present invention, there is at least one peak top (P2) having a higher molecular weight than the peak top (P1) of the peak with the largest area. The weight average molecular weight (Mp2) of the peak top (P2) is 1.0×10 6 More than 1.5×10 is preferable. 6 More preferably, 2.0×10 6 More preferably, it is 1.0×10 or more. 8 When the content is equal to or more than the lower limit, the strength of the molded article is improved.

[0022] The ratio of the weight average molecular weight of the peak top (P1) to the peak top (P2) is preferably 20 or more, more preferably 25 or more, and even more preferably 30 or more, while it is preferably 100 or less, more preferably 70 or less, and even more preferably 60 or less. When the ratio of the weight average molecular weight of P1 to P2 is within the above range, both strength and moldability of the molded body are achieved.

[0023] In the present invention, the mass average molecular weight and molecular weight distribution are values ​​measured by gel permeation chromatography (GPC) under the following conditions.

[0024] (GPC measurement conditions) Equipment used: Tosoh Corporation HLC-8320GPC system Column: TSKgel guard column SuperH-H (4.6 mm l.D. x 3.5 cm) + TSKgel SuperHM-H (6.0 mm l.D. x 15 cm) x 2 (Tosoh Corporation) Eluent: PFP (pentafluorophenol) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) / chloroform (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. HPLC grade) = 1 / 2 (weight ratio) Column temperature: 40℃ Detector: Differential refractometer (RI detector), polarity=(+) Calibration curve: A cubic approximation curve using standard polystyrene (manufactured by Tosoh) (the value obtained is the molecular weight converted into polystyrene)

[0025] As the polyetherimide resin, commercially available products can be used, and examples of the product names available from SABIC Innovative Plastics include "Ultem (registered trademark; the same applies below) CRS5001," "Ultem CRS5011," "Ultem 1000," "Ultem 1010," and "Ultem 1040A." The polyetherimide resin may be used alone or in combination of two or more kinds.

[0026] The glass transition temperature (Tg) of the polyetherimide resin is preferably 160°C or higher, more preferably 170°C or higher, and particularly preferably 180°C or higher. When the glass transition temperature is equal to or higher than the lower limit, the heat resistance of the prepreg is sufficient. In addition, the glass transition temperature is preferably 300°C or lower, more preferably 290°C or lower, and particularly preferably 280°C or lower. When the glass transition temperature is equal to or lower than the upper limit, the prepreg can be molded at a relatively low temperature. The glass transition temperature (Tg) of the prepreg indicates the inflection point (E'-Tg: Tg at E'-Onset) of the storage modulus measured by dynamic viscoelasticity measurement (DMA: Dynamic Mechanical Analysis), and can be measured by a method conforming to ASTM D7028.

[0027] The prepreg may further contain additives other than the reinforcing fibers. Examples of the additives include flame retardants, weather resistance improvers, antioxidants, heat stabilizers, UV absorbers, plasticizers, lubricants, colorants, compatibilizers, conductive fillers, etc. The additives may be used alone or in combination of two or more.

[0028] When the prepreg contains an additive, the polyetherimide resin and the additive are mixed to prepare a polyetherimide resin composition, and the carbon fiber is impregnated with the polyetherimide resin composition. When the prepreg contains a plurality of reinforcing fibers, a reinforcing fiber layer containing a plurality of reinforcing fibers may be impregnated with a polyetherimide resin or a polyetherimide resin composition.

[0029] From the viewpoint of maintaining mechanical strength, the volume content of the additive in the prepreg is preferably 5 vol % or less, more preferably 1 vol % or less, and even more preferably 0.5 vol % or less. The total volume content of the matrix resin, carbon fibers, other fibers and additives in the prepreg is 100% by volume. The thickness of one prepreg sheet is preferably 0.04 mm or more, and more preferably 0.07 mm or more, while it is preferably 0.7 mm or less, and more preferably 0.4 mm or less.

[0030] [Thermoplastic resins other than polyetherimide resin] The prepreg of the present invention may further contain a thermoplastic resin other than the polyetherimide resin (hereinafter also referred to as "other resin") within a range that does not impair the effects of the present invention. Examples of the other resins include polyamide (nylon 6, nylon 66, etc.) resins, polyolefin (polyethylene, polypropylene, etc.) resins, modified polyolefin resins, polyester (polyethylene terephthalate, polybutylene terephthalate, etc.) resins, polycarbonate resins, polyamideimide resins, polyphenylene oxide resins, polysulfone resins, polyethersulfone resins, polyetheretherketone resins, polyetherketoneketone resins, polyaryletherketone resins, polystyrene resins, ABS resins, polyphenylene sulfide resins, liquid crystal polyester resins, and copolymers of acrylonitrile and styrene, etc. The other resins may be used alone or in combination of two or more.

[0031] The content of the polyetherimide resin used in the prepreg of the present invention is preferably 85% by mass or more, more preferably 90% by mass or more, based on the total amount of the polyetherimide resin and other resins (total mass of the matrix resin). The upper limit of the content of the polyetherimide resin is usually 100% by mass based on the total mass of the matrix resin. If the content of the polyetherimide resin is equal to or more than the lower limit, the chemical resistance of the molded product is further improved. If the content of the polyetherimide resin is equal to or less than the upper limit, the impregnation of the matrix resin into the carbon fiber can be well maintained.

[0032] [Reinforced fiber] The reinforcing fibers used in the prepreg may be inorganic, organic or metal fibers. Examples of inorganic fibers include carbon fibers, graphite fibers, silicon carbide fibers, glass fibers, alumina fibers, tungsten carbide fibers, boron fibers, and metal fibers such as stainless steel and iron. Examples of organic fibers include aramid fibers, high density polyethylene fibers, and other general nylon fibers and polyester fibers. In addition, a hybrid reinforcing fiber that combines the above fibers can be used. An example of a hybrid reinforcing fiber is a metal-coated carbon fiber. These can be used alone or in combination of two or more. As for the form of the reinforcing fiber, continuous fiber is preferred from the viewpoint of strength and rigidity. Among the above, the prepreg of the present invention preferably contains carbon fibers as reinforcing fibers.

[0033] (Carbon Fiber) The carbon fiber is not particularly limited, but examples thereof include polyacrylonitrile (PAN)-based carbon fiber, petroleum / coal pitch-based carbon fiber, rayon-based carbon fiber, lignin-based carbon fiber, etc. Among these, PAN-based carbon fiber is preferred. The carbon fiber is preferably a continuous fiber. Carbon fibers are typically used in the form of a carbon fiber bundle in which a plurality of single fibers (filaments) are bundled. The number of filaments in the carbon fiber bundle is preferably 1000 to 60000, more preferably 1000 to 50000, and further preferably 12000 to 48000. If it is within the above range, it is preferable because it has excellent productivity and mechanical properties on an industrial scale. The obtained carbon fiber bundle can be used to make a fiber substrate such as a fiber form in which the carbon fiber bundles are aligned in one direction or a woven form (for example, plain weave, twill weave, satin weave, etc.). From the viewpoint of the rigidity and strength of the molded product, the strand elastic modulus of the carbon fiber is preferably 200 to 400 GPa, more preferably 250 to 380 GPa, and more preferably 280 to 350 GPa. The strand elastic modulus of the carbon fiber bundle is measured by a method conforming to ASTM D4018.

[0034] The volume content (Vf) of the reinforcing fibers in the prepreg is preferably 20 to 75 volume%, more preferably 40 to 70 volume%, and more preferably 50 to 65 volume%. When the volume content (Vf) of the reinforcing fibers is equal to or greater than the lower limit, the reinforcing effect of the reinforcing fibers is sufficiently exhibited, and the rigidity and strength of the molded article are further increased. When the volume content (Vf) of the reinforcing fibers is equal to or less than the upper limit, the adhesion between the reinforcing fibers and the matrix resin can be sufficiently ensured. The fatigue properties of the molded article are more excellent. In this specification, the volume content (Vf) of the reinforcing fibers is a value obtained by a measurement method in accordance with JIS K 7075.

[0035] (Prepreg manufacturing method) The prepreg of the present invention can be produced, for example, by processing a polyetherimide resin into a film having a thickness of about 10 to 100 μm, a fiber having a fiber diameter of about 5 to 50 μm, or a powder having an average particle diameter of about 10 to 100 μm, attaching it to carbon fibers, and heating it to impregnate them. Alternatively, a prepreg can be produced by dissolving a polyetherimide resin in an appropriate solvent and impregnating the reinforcing fibers with the resin. Among these, the method of processing the polyetherimide resin into a film having a thickness of about 10 to 100 μm and impregnating the reinforcing fibers by heating and melting is preferred because it stabilizes the resin content in the prepreg. The thickness of the film is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more, while it is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 40 μm or less. By having the film thickness within the above range, a film with a stable thickness can be efficiently produced.

[0036] Since polyetherimide resin has a high melt viscosity when heated, in order to efficiently impregnate the reinforcing fibers, it is necessary to include a step of heating to 380°C or higher, preferably 400°C or higher, and more preferably 420°C or higher. In order to sufficiently form a polymer, the heating step is preferably for 1 minute or more, more preferably for 2 minutes or more, further preferably for 4 minutes or more, and particularly preferably for 5 minutes or more. The heating step is usually for 10 minutes or less.

[0037] Therefore, a preferred method for producing the prepreg of the present invention is a method for producing a prepreg in which a polyetherimide resin film is laminated on a fiber substrate and heated to impregnate the fiber substrate with a resin contained in the polyetherimide resin film, the polyetherimide resin film having a thickness of 10 to 100 μm, and heated to 380° C. or higher during the heating. The types of resin constituting the polyetherimide resin film and the types of fiber substrates preferably used in this production method are as described above.

[0038] The polyetherimide film has a peak (F2) having a higher molecular weight than the peak (F1) having the maximum area in a GPC chromatogram, and the ratio of F2 to the area of ​​the polyetherimide is preferably 0.1% or less, more preferably 0.09% or less, and more preferably 0.08% or less. When the ratio of F2 is within the above range, impregnation into the reinforcing fibers becomes easy.

[0039] The weight-average molecular weight (Mf1) of the maximum peak (F1) derived from the matrix resin in the GPC chromatogram of the polyetherimide film is 1.0×10 4 ~8.0×10 4 is preferred, and 3.0×10 4 ~6.0×10 4 is more preferable. When the value is equal to or higher than the lower limit, the mechanical properties of the molded product are excellent, and when the value is equal to or lower than the upper limit, the productivity of the prepreg can be increased. In addition, the weight average molecular weight (Mf2) of one or more peaks (f2) present at a higher molecular weight than the maximum peak (f1) in the GPC chromatogram of the polyetherimide film is 1.0×10 6 More than 2.0×10 is preferable. 6 is more preferable. The strength of the molded article is improved when the content is equal to or higher than the lower limit. In the GPC analysis of polyetherimide resin, a PFP (pentafluorophenol) / chloroform = 1 / 2 (weight ratio) is used as the eluent, and the weight average molecular weight and the like can be obtained as polystyrene equivalent values.

[0040] Hereinafter, one embodiment of the method for producing a prepreg will be described. In the method for producing a prepreg of this embodiment, a resin film made of the above-mentioned matrix resin is laminated on a carbon fiber substrate and heated and pressurized to impregnate the carbon fiber substrate with the resin contained in the resin film, thereby producing a prepreg. Specifically, a carbon fiber substrate and a resin film are overlapped, and the matrix resin is impregnated into the carbon fiber substrate by one or more heating rolls heated to the melting point (or flow start temperature) or higher of the matrix resin, and the matrix resin is brought into contact with a cooling roll, thereby producing a prepreg in which the matrix resin is solidified. It is preferable to select a release film or release paper that is heat resistant to the heating roll temperature during production. In addition, for matrix resins that are difficult to impregnate with the heating roll, a double belt press combining a metal belt and a heating roll, or a heating press can be used to produce a prepreg. The heating roll and the heating press, or the cooling roll and the cooling press may be combined to produce the prepreg. Specifically, the roll and the press may be included in the same production device, and after forming a partially impregnated prepreg precursor in a production device including a heating roll, the prepreg may be produced in another production device including a heating press.

[0041] When producing a prepreg, the resin film to be laminated on the carbon fiber substrate may be laminated on one side or on both sides, and the resin films may be the same type or different types.

[0042] [Molded body] The molded article of the present invention is obtained by molding the above-mentioned prepreg of the present invention. The molded article of the present invention is preferably a molded article obtained by molding a laminate in which two or more sheets of the prepreg of the present invention are laminated together. Note that the molded article of the present invention may also be a molded article obtained by molding a laminate in which the prepreg of the present invention and a prepreg other than the prepreg of the present invention are combined and laminated together.

[0043] The lamination configuration of the prepregs in the laminate is not particularly limited. The number of prepregs in the laminate can be appropriately set depending on the thickness of the prepregs and the thickness required for the molded article. In the case of UD prepregs in which the reinforcing fibers in the prepregs are aligned in one direction, the fiber direction of the carbon fibers in each UD prepreg to be laminated can be appropriately set depending on the physical properties required for the molded article.

[0044] (Method of Manufacturing Molded Product) The molded article can be obtained by molding the prepreg of the present invention. The method for molding the prepreg is not particularly limited, but examples thereof include methods in which a single prepreg of the present invention or a laminate of multiple prepregs of the present invention is molded by a mold pressing method, an autoclave method, a hot / cold pressing method, etc. Examples of a method for laminating prepregs include an automatic lamination method using a robot. EXAMPLES

[0045] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. The values ​​of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​of the examples.

[0046] [Evaluation method for 90° bending strength] A test piece was obtained from the obtained molded plate, and a 90° bending test was performed in accordance with ASTM D790 using a universal testing machine (INSTRON 5565, manufactured by INSTRON) equipped with a three-point bending jig (indenter R = 5.0 mm, support R = 3.2 mm) under the conditions of L / d = 16, the ratio of the distance between supports (L) to the thickness (d) of the test piece, and crosshead speed = (L2 × 0.01) / (6 × d), to measure the 90° bending strength. The dimensions of the test piece used in the measurement were 12.7 mm wide and 50 mm long.

[0047] (material) The carbon fibers and polyetherimide resins used in this example are shown below. Carbon fiber 1: Mitsubishi Chemical Corporation, product name "MR50R", strand elastic modulus: 285GPa Carbon fiber 2: Mitsubishi Chemical Corporation, product name "TR50S", strand elastic modulus: 235GPa Polyetherimide resin 1: SABIC Innovative Plastics, product name "Ultem TM CRS5001" (a polyetherimide resin having the repeating unit (2) Polyetherimide resin 2: SABIC Innovative Plastics, product name "Ultem TM 1000", (a polyetherimide resin having the repeating unit (1))

[0048] Example 1 A unidirectional fiber substrate using the carbon fiber 1 and a 23 μm-thick PEI resin 1 film extruded from the polyetherimide resin 1 using a T-die are bonded by heat fusion, and the carbon fiber area weight (FAW) is 64 g / m 2 Thus, a precursor prepreg for a fiber reinforced composite material was obtained, with 100% unimpregnated fiber remaining.

[0049] The temperature of the mold in the hydraulic press was adjusted to 400 to 440°C, and two pressurized bodies (C / C composite plates with a thickness of about 3 mm) were placed in the mold. Next, three sheets of the fiber-reinforced composite material precursor prepreg were stacked, and a release film (Upilex 50S, manufactured by Ube Industries) was stacked on both sides of the stack. The stack was then passed between the pressurized bodies, and the hydraulic press was used to pressurize the stack at an average pressure of 4.1 MPa for 5.0 minutes. The stack was then cooled and solidified to obtain an impregnated unidirectional prepreg with a thickness of about 0.2 mm and a fiber content of about 60% by volume.

[0050] (GPC analysis) About 9 mg of each of the film and prepreg was weighed, and a chromatogram was obtained using a GPC device (HLC-8320GPC manufactured by Tosoh Corporation). From the film, a peak derived from the matrix resin was detected from the GPC chromatogram. The peak with the largest area was designated as F1, and the peak detected on the higher molecular weight side than F1 was designated as F2, and the weight average molecular weight (Mf1) of the maximum peak (F1) was obtained. In addition, the content of the high molecular weight substance contained in the film was calculated as (area of ​​F2) / (total area of ​​peaks derived from polyetherimide). Next, peaks derived from polyetherimide resin were detected from the prepreg in the GPC chromatogram. The peak with the largest area was designated P1, and the peak detected on the higher molecular weight side than P1 was designated P2. The weight average molecular weights of the maximum peak (P1) and the high molecular weight peak (P2) were obtained as Mp1 and Mp2, respectively. The content of the high molecular weight material contained in the prepreg was calculated as (area of ​​P2) / (total area of ​​peaks derived from polyetherimide). Comparing the film and prepreg, the weight average molecular weight (Mf1) of the film and the weight average molecular weight of the prepreg were both 4.8×10 4 No decrease in molecular weight was observed due to the heating process. On the other hand, the content of polymers was 0.07% in the film and 0.67% in the prepreg, indicating an increase in polymers due to the heating process.

[0051] (Production of Molded Body) The prepreg was cut into 11 pieces measuring 118 mm x 198 mm, and laminated so that all the fiber directions were oriented in the 0° direction to produce a laminate. The resulting laminate was sandwiched between steel dies and compression molded for 15 minutes under molding conditions of 5 MPa in the heating platen of a two-stage heating and cooling press (manufactured by Shinto Metal Industries, output: 50 tons) set at 320°C. The die was then transferred to the press platen surface set at 80°C, and the temperature was lowered to 150°C in about 2 minutes, yielding a molded body of 120 mm x 200 mm (thickness 2 mm). The 90° bending strength of the obtained molded article was measured by a method in accordance with ASTM D790, and the results are shown in Table 1. Furthermore, the polymer content of Mf1, Mp1, Mp2, the film, and the prepreg was measured, and the results are shown in Table 1.

[0052] Example 2 A prepreg and a molded body were produced in the same manner as in Example 1, except that the pressing time was changed to 6.7 minutes. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and the high molecular weight peak (P2) of the maximum area peak in the GPC chromatogram of the polyetherimide resin contained in the film used and the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0053] Example 3 A prepreg and a molded body were produced in the same manner as in Example 1, except that the pressing time was changed to 8.3 minutes. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and the high molecular weight peak (P2) of the maximum area peak in the GPC chromatogram of the polyetherimide resin contained in the film used and the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0054] Example 4 A prepreg and a molded body were produced in the same manner as in Example 1, except that the pressing time was changed to 3.0 minutes. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and the high molecular weight peak (P2) of the maximum area peak in the GPC chromatogram of the polyetherimide resin contained in the film used and the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0055] Example 5 A prepreg and a molded body were produced in the same manner as in Example 1, except that the pressing time was changed to 3.5 minutes. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and the high molecular weight peak (P2) of the maximum area peak in the GPC chromatogram of the polyetherimide resin contained in the film used and the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0056] Example 6 A prepreg and a molded body were produced in the same manner as in Example 1, except that the mold in the hydraulic press was changed to 380 to 420°C and the pressurization time was changed to 3.9 minutes. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and the high molecular weight peak (P2) of the maximum area peak in the GPC chromatogram of the polyetherimide resin contained in the film used and the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0057] Example 7 A prepreg and a molded body were produced in the same manner as in Example 6, except that the pressing time was changed to 4.6 minutes. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and the high molecular weight peak (P2) of the maximum area peak in the GPC chromatogram of the polyetherimide resin contained in the film used and the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0058] Example 8 A prepreg and a molded body were produced in the same manner as in Example 6, except that the average pressure was changed to 5.8 MPa and the pressurization time was changed to 2.8 minutes. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and the high molecular weight peak (P2) of the maximum area peak in the GPC chromatogram of the polyetherimide resin contained in the film used and the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0059] Example 9 A unidirectional fiber substrate using the carbon fiber 2 and a 23 μm thick PEI resin 2 film extruded from the matrix resin 2 using a T-die are bonded by heat fusion, and the carbon fiber area weight (FAW) is 64 g / m 2 Thus, a precursor prepreg for a fiber reinforced composite material was obtained, with 100% unimpregnated fiber remaining.

[0060] The temperature of the mold in the hydraulic press was adjusted to 390 to 410°C, and in the same manner as in Example 1, the hydraulic press was used to apply an average pressure of 4.1 MPa for 2.3 minutes, after which the mixture was cooled and solidified to obtain an impregnated unidirectional prepreg having a thickness of approximately 0.2 mm and a fiber content of approximately 60% by volume.

[0061] (GPC analysis) In the GPC chromatograms of the film using matrix resin 2 and the prepreg, two peaks derived from the matrix resin were detected, as in Example 1. As a result of the GPC measurement, when the film and the prepreg were compared, the weight average molecular weight (Mf1) of the film was 5.8×10 4 The weight average molecular weight of the prepreg is 5.5 × 10 4 Thus, no significant decrease in molecular weight was observed due to the heating process. On the other hand, the content of polymers was 0.08% in the film and 1.67% in the prepreg, indicating an increase in polymers due to the heating process.

[0062] The 90° bending strength of the molded article obtained in the same manner as in Example 1 was measured by a method in accordance with ASTM D790, and the results are shown in Table 1. Furthermore, the polymer content of Mf1, Mp1, Mp2, the film, and the prepreg was measured, and the results are shown in Table 1.

[0063] Example 10 A prepreg and a molded body were produced in the same manner as in Example 9, except that the mold in the hydraulic press was changed to 400 to 440°C and the pressurization time was changed to 1.0 minute. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and the high molecular weight peak (P2) of the maximum area peak in the GPC chromatogram of the polyetherimide resin contained in the film used and the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0064] Example 11 A unidirectional fiber substrate using the carbon fiber 1 and a 15 μm thick film obtained by extruding the polyetherimide resin 1 using a T-die under the same conditions as in Example 1 were bonded together by heat fusion, and the carbon fiber area weight (FAW) was 40 g / m 2 Thus, a precursor prepreg for a fiber reinforced composite material was obtained, with 100% unimpregnated fiber remaining.

[0065] As in Example 1, the temperature of the mold in the hydraulic press was adjusted to 400 to 440°C, and two pressurized bodies (C / C composite plates with a thickness of about 3 mm) were placed therein. Next, four sheets of the fiber-reinforced composite material precursor prepreg were stacked, and a release film (Upilex 50S, manufactured by Ube Industries) was further stacked on both sides of the stack, which was then passed between the pressurized bodies, and the hydraulic press was used to pressurize the stack at an average pressure of 4.1 MPa for 1.0 minute, after which the stack was cooled and solidified to obtain an impregnated unidirectional prepreg with a thickness of about 0.15 mm and a fiber content of about 60% by volume.

[0066] (Production of Molded Body) The prepreg was cut into 14 pieces, and molded bodies (thickness 2 mm) were obtained in the same manner as in Example 1. The film used in Example 11 was different in thickness from the film used in Example 1, but was produced under the same conditions, and the GPC chromatograms were considered to be almost the same. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and high molecular weight peak (P2) of the peak with the largest area in the GPC chromatogram of the polyetherimide resin contained in the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0067] Example 12 A prepreg and a molded body were produced in the same manner as in Example 11, except that the mold in the hydraulic press was changed to 380 to 420°C and the pressurization time was changed to 1.3 minutes. The weight average molecular weights (Mp1, Mp2) of the peak top (P1) and the high molecular weight peak (P2) of the peak with the largest area in the GPC chromatogram of the polyetherimide resin contained in the obtained prepreg, the high molecular weight content of the prepreg, and the 90° bending strength of the molded plate were measured. The results are shown in Table 1.

[0068] From Examples 1 to 12, a molded article having good bending strength can be obtained by using a prepreg containing P1 and P2. Furthermore, when the polymer content of the prepreg is 0.25% by area or more, a molded article having higher bending strength can be obtained.

[0069] [Table 1] [Industrial Applicability]

[0070] The prepreg of the present invention can give a molded article having excellent chemical resistance and mechanical properties. Therefore, the prepreg and molded article of the present invention are useful as members for sporting goods, automobiles, aircraft, industrial equipment, etc.

[0071] [summary] In summary, the present invention may have the following embodiments. [Embodiment 1] Embodiment 1 is a prepreg including reinforcing fibers and a polyetherimide resin, the polyetherimide resin having a peak top (P1) of the peak with the largest area in a GPC chromatogram and a peak top (P2) having a higher molecular weight than the peak top (P1). [Embodiment 2] A second embodiment is the prepreg according to the first embodiment, wherein the polyetherimide resin contains at least one structural unit of the following formulas (1) and (2):

[0072] [ka] (1)

[0073] [ka] (2) [Embodiment 3] Embodiment 3 is the prepreg according to embodiment 1 or 2, in which a peak area including the peak top (P2) is 0.10% or more, 0.25% or more, 0.30% or more, 0.50% or more, or 0.55% or more of the total peak area derived from the polyetherimide resin in the GPC chromatogram. [Embodiment 4] A fourth embodiment is a prepreg comprising reinforcing fibers and a polyetherimide resin, the polyetherimide resin having a peak top (P1) of the maximum area peak in a GPC chromatogram and a peak top (P2) having a higher molecular weight than the peak top (P1), and the peak area including the peak top (P2) is 0.10% or more, 0.25% or more, 0.30% or more, 0.50% or more, or 0.55% or more of the total peak area derived from the polyetherimide resin in the GPC chromatogram. [Embodiment 5] A fifth embodiment is the prepreg according to the fourth embodiment, wherein the polyetherimide resin contains at least one structural unit of the following formulas (1) and (2):

[0074] [ka] (1)

[0075] [ka] (2) [Embodiment 6] In embodiment 6, the weight average molecular weight (Mp2) of the peak top (P2) is 1.0 × 10 6 or more than 1.5×106 The prepreg according to any one of embodiments 1 to 5 is as described above. [Embodiment 7] Embodiment 7 is the prepreg according to any one of embodiments 1 to 6, in which the peak area including the peak top (P2) of the peak area derived from the polyetherimide resin in the GPC chromatogram is 5.0% or less, 3.0% or less, or 2.0% or less. [Embodiment 8] In embodiment 8, the weight average molecular weight (Mp1) of the peak top (P1) is 1.0 to 8.0 × 10 4 or more than 3.0×10 4 The prepreg according to any one of embodiments 1 to 7 is as described above. [Embodiment 9] In embodiment 9, the weight average molecular weight (Mp1) of the peak top (P1) is 8.0 × 10 5 or less than 6.0×10 5 9. A prepreg according to any one of embodiments 1 to 8, wherein [Embodiment 10] A tenth embodiment is a prepreg according to any one of the first to ninth embodiments, comprising carbon fibers as the reinforcing fibers. [Embodiment 11] An eleventh embodiment is a prepreg according to any one of the first to tenth embodiments, in which the ratio (Mp2 / Mp1) of the weight average molecular weights calculated from the peak top (P1) and the peak top (P2) is 20 or more, 25 or more, or 30 or more. [Embodiment 12] Embodiment 12 is a prepreg according to any one of embodiments 1 to 12, in which the ratio (Mp2 / Mp1) of the weight average molecular weight calculated from the peak top (P1) and the peak top (P2) is 100 or less, 70 or less, or 60 or less. [Embodiment 13] A thirteenth embodiment is a molded article using the prepreg according to any one of the first to twelfth embodiments. [Embodiment 14] Embodiment 14 is a method for producing a prepreg in which a polyetherimide resin film is laminated on a fiber base material and heated to impregnate the fiber base material with a resin contained in the polyetherimide resin film, wherein the polyetherimide resin film has a thickness of 10 to 100 μm and is heated to 380° C. or higher. [Embodiment 15] A fifteenth embodiment is the prepreg according to the fourth embodiment, wherein the polyetherimide resin contains at least one structural unit of the following formulas (1) and (2):

[0076] [ka] (1)

[0077] [ka] (2) [Embodiment 16] A sixteenth embodiment is the method for producing a prepreg according to the fourteenth or fifteenth embodiment, wherein the heating is performed for one minute or longer. [Embodiment 17] A seventeenth embodiment is a method for producing the prepreg according to any one of the fourteenth to sixteenth embodiments, in which a polyetherimide film having a thickness of 10 to 100 μm is used and impregnated by heating to 380° C. or higher. [Embodiment 18] Embodiment 18 is a method for producing a prepreg according to any one of embodiments 14 to 17, wherein the polyetherimide film has at least one peak top (F2) having a higher molecular weight than the peak top (F1) having the maximum area in a GPC chromatogram, and the peak area including F2 is 0.1% or less. [Embodiment 19] A nineteenth embodiment is a method for producing a prepreg according to any one of the fourteenth to eighteenth embodiments, in which pressure is applied simultaneously with the heating. [Embodiment 20] Embodiment 20 is a prepreg including reinforcing fibers and a polyetherimide resin, the polyetherimide resin having a peak top (P1) of the peak with the largest area in a GPC chromatogram and a peak top (P2) having a higher molecular weight than the peak top (P1). [Embodiment 21] Embodiment 21 is the prepreg according to embodiment 20, wherein the peak area including the peak top (P2) in the peak area derived from the polyetherimide resin in the GPC chromatogram is 0.1% or more, 0.25% or more, 0.3% or more, or 0.6% or more. [Embodiment 22] A twenty-second embodiment is the prepreg according to the twenty-first embodiment, wherein the polyetherimide resin contains at least one structural unit of the following formulas (1) and (2):

[0078] [ka] (1)

[0079] [ka] (2) [Embodiment 23] In embodiment 23, the weight average molecular weight (Mp2) of the peak top (P2) is 1.0 × 10 6 or more than 1.5×10 6 The prepreg according to any one of embodiments 20 to 22 is as described above. [Embodiment 24] Embodiment 24 is the prepreg according to any one of embodiments 20 to 23, wherein the peak area including the peak top (P2) in the peak area derived from the polyetherimide resin in the GPC chromatogram is 5.0% or less, 3.0% or less, or 2.0% or less. [Embodiment 25] In the twenty-fifth embodiment, the weight average molecular weight (Mp1) of the peak top (P1) is 1.0 to 8.0 × 10 4 or more than 3.0×104 The prepreg according to any one of embodiments 20 to 24 is as described above. [Embodiment 26] In embodiment 26, the weight average molecular weight (Mp1) of the peak top (P1) is 8.0 × 10 5 or less than 6.0×10 5 26. A prepreg according to any one of embodiments 20 to 25, wherein [Embodiment 27] Example 27 is the prepreg of any one of examples 20 to 26, comprising carbon fibers as the reinforcing fibers. [Embodiment 28] Embodiment 28 is a prepreg according to any one of embodiments 20 to 27, in which the ratio (Mp2 / Mp1) of the weight average molecular weights calculated from the peak top (P1) and the peak top (P2) is 20 or more, 25 or more, or 30 or more. [Embodiment 29] Embodiment 29 is a prepreg according to any one of embodiments 20 to 28, in which the ratio (Mp2 / Mp1) of the weight average molecular weights calculated from the peak top (P1) and the peak top (P2) is 100 or less, 70 or less, or 60 or less. [Embodiment 30] Embodiment 30 is a molded article using the prepreg according to any one of embodiments 20 to 29. [Embodiment 31] Embodiment 31 is a method for producing a prepreg in which a polyetherimide resin film is laminated on a fiber base material and heated to impregnate the fiber base material with a resin contained in the polyetherimide resin film, wherein the polyetherimide resin film has a thickness of 10 to 100 μm and is heated to 380° C. or higher. [Embodiment 32] Embodiment 32 is a method for producing a prepreg according to embodiment 31, in which the heating is performed for one minute or more. [Embodiment 33] In a thirty-third embodiment, there is provided a method for producing the prepreg according to the thirty or twenty-second embodiment, in which a polyetherimide film having a thickness of 10 to 100 μm is used and impregnated by heating to 380° C. or higher. [Embodiment 34] Embodiment 34 is a method for producing a prepreg according to any one of embodiments 30 to 33, wherein the polyetherimide film has at least one peak top (F2) having a higher molecular weight than the peak top (F1) having the maximum area in a GPC chromatogram, and the peak area including F2 is 0.1% or less. [Embodiment 35] Embodiment 35 is a method for producing a prepreg according to any one of embodiments 30 to 34, in which pressure is applied simultaneously with the heating.

Claims

1. A prepreg comprising reinforcing fibers and a polyetherimide resin, the polyetherimide resin having a peak top (P1) of a peak with a maximum area in a GPC chromatogram and a peak top (P2) having a higher molecular weight than the peak top (P1).

2. 2. The prepreg according to claim 1, wherein the polyetherimide resin contains at least one structural unit represented by the following formulas (1) and (2): 【Chemistry 1】 ・・・(1) 【Chemistry 2】 ・・・(2)

3. The weight average molecular weight (Mp2) of the peak top (P2) is 1.0×10 6 ~1.0 x 10 8 The prepreg according to claim 1 or 2.

4. 3. The prepreg according to claim 1, wherein a peak area including the peak top (P2) is 0.10% or more relative to a total area of ​​peaks derived from a polyetherimide resin in the GPC chromatogram.

5. The weight average molecular weight (Mp1) of the peak top (P1) is 1.0×10 4 ~8.0 x 10 4 The prepreg according to claim 1 or 2.

6. The prepreg according to claim 1 or 2, comprising carbon fibers as the reinforcing fibers.

7. 3. The prepreg according to claim 1, wherein a ratio (Mp2 / Mp1) of the weight average molecular weights determined from the peak top (P1) and the peak top (P2) is 20 or more.

8. 3. The prepreg according to claim 1, wherein a ratio (Mp2 / Mp1) of the weight average molecular weights determined from the peak top (P1) and the peak top (P2) is 100 or less.

9. A molded article using the prepreg according to claim 1 or 2.

10. A method for producing a prepreg, comprising laminating a polyetherimide resin film on a fiber substrate and heating the laminate to impregnate the fiber substrate with a resin contained in the polyetherimide resin film, The polyetherimide resin film has a thickness of 10 to 100 μm, The method for producing a prepreg, wherein the heating is performed at 380° C. or higher.

11. The method for producing a prepreg according to claim 10, wherein the polyetherimide resin contains at least one structural unit of the following formulas (1) and (2): 【Chemistry 3】 ・・・(1) 【Chemistry 4】 ・・・(2)

12. The method for producing a prepreg according to claim 10 or 11, wherein the heating is performed for 1 minute or more.

13. The method for producing a prepreg according to claim 10 or 11, wherein the polyetherimide film has at least one peak top (F2) having a higher molecular weight than a peak top (F1) having a maximum area in a GPC chromatogram, and the peak area including F2 is 0.1% or less.

14. The method for producing a prepreg according to claim 10 or 11, wherein pressure is applied simultaneously with the heating.

Citation Information

Patent Citations

  • Prepreg sheet material and method for producing the same

    JP2012246442A

  • Structure for aircraft

    JP2017119506A