Decomposition method of polyhydroxyalkanoate, and production method of polyhydroxyalkanoate

The method efficiently decomposes PHA to low molecular weight using alcohol and a basic catalyst at controlled temperatures, addressing inefficiencies and costs of existing methods, particularly for P3HB3HH, with high throughput and low energy consumption.

JP2024144085APending Publication Date: 2024-10-11KANEKA CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023213981
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-12-19
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing PHA decomposition methods are inefficient, costly, and unable to handle polymers like P3HB3HH due to low solubility in organic solvents, requiring high energy and expensive solvents or catalysts, and face challenges with pH neutralization during decomposition.

Method used

A method involving mixing PHA particles with a specific particle size distribution in alcohol and a basic catalyst, then heating under controlled temperatures to achieve efficient decomposition without solvent dissolution, using inexpensive alcohol and catalysts.

Benefits of technology

PHA is decomposed to low molecular weight efficiently, reducing energy consumption and costs, enabling high throughput and suitable decomposition of low-solubility polymers like P3HB3HH.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a new decomposition technique of PHA, with which the polyhydroxyalkanoate can be decomposed to a low molecular weight at a low cost, low energy and high throughput.SOLUTION: A decomposition method of polyhydroxyalkanoate includes: a step to obtain a mixed liquid containing particulate polyhydroxyalkanoate by mixing polyhydroxyalkanoate particles which contains polyhydroxyalkanoate and in which a ratio of particles having a particle size of 0.5 μm or more and 1,000 μm or less is 90% or more in a volume-based particle size distribution measured by using a particle size distribution measuring device by a laser diffraction / scattering method with alcohol; and a step to heat the mixed liquid containing the particulate polyhydroxyalkanoate at 85°C or higher and 220°C or lower in the presence of a basic catalyst.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for decomposing polyhydroxyalkanoates (hereinafter also referred to as "PHA") for reuse as raw materials for chemical products. [Background technology]

[0002] It is known that various types of PHA, such as poly(3-hydroxybutyrate) (P3HB), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH), and polylactic acid (PLA), can be produced using biomass resources as raw materials. Biomass-derived PHA can also reduce greenhouse gas emissions because the raw materials, plants, absorb CO2, which is believed to be the cause of global warming, through photosynthesis during their growth. Even if biomass-derived PHA is incinerated, the amount of CO2 emitted is the same as the amount absorbed by the raw materials, plants, so it is thought that it will not affect the increase or decrease of CO2 in the atmosphere, and it is also a carbon-neutral material that is expected to help us break away from dependence on fossil fuels.

[0003] However, PHA derived from biomass resources is generally made from biomass resources that compete with food use, such as starch and vegetable oil, and some consider this to be undesirable. In addition, the ongoing development of natural forests to expand the production of biomass resources, for which demand is growing, is problematic, and it is preferable to establish technology to manufacture PHA using raw materials that have a low environmental impact and are in sufficient supply. Against this background, a method for manufacturing PHA using waste cooking oil has also been developed, but the supply of waste cooking oil is limited, and if the demand for PHA increases in the future, it will be difficult to cover all the raw materials with waste cooking oil.

[0004] Therefore, there is a demand for the development of a technology to reuse used PHA. Possible methods of reuse include reusing the PHA in the shape of the product as it is, or melting the PHA at high temperature and remolding it into a product of a different shape. However, these methods have the problem that the molecular weight of the PHA gradually decreases, resulting in a decrease in strength and inability to obtain the desired physical properties. Therefore, as a PHA recycling technology, it is preferable to establish a chemical recycling technology in which PHA is decomposed to a low molecular weight and then used as a raw material for chemical products.

[0005] As methods for decomposing PHA, techniques described in Patent Documents 1, 2 and 3 are disclosed. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2010 / 118955 [Patent Document 2] JP 2004-250414 A [Patent Document 3] Special table number 2004-513200 Summary of the Invention [Problem to be solved by the invention]

[0007] In Patent Document 1, polylactic acid is decomposed by using a lactate ester as a solvent capable of dissolving polylactic acid and heating in the presence of a basic catalyst. However, this method has problems in that there is an upper limit to the amount of processing per batch due to the solubility of polylactic acid, the decomposition reaction takes a long time, and it is necessary to use a relatively expensive solvent, lactate ester. In addition, there is a problem that it cannot be applied to the decomposition of polymers such as P3HB3HH, which are not known to have a solvent that can dissolve them at a sufficient concentration. In Patent Document 2, supercritical carbon dioxide is used as a solvent for dissolving polylactic acid, and although this method can be applied to PHA, which has low solubility in organic solvents, it requires expensive equipment to handle supercritical carbon dioxide and a large amount of energy is required to maintain high temperature and high pressure conditions, so there is room for improvement. In Patent Document 3, PHA is decomposed by mixing a basic aqueous solution with PHA and heating it. To treat PHA at a sufficient decomposition rate using this method, a sufficiently high pH must be maintained during the decomposition reaction, but a large amount of basic compounds is required because the basic compounds are neutralized by the hydroxyalkanoic acids produced by the decomposition of PHA, causing the pH to decrease as the decomposition progresses. Since it is difficult to recover the neutralized basic compounds as useful compounds that can be reused at low cost, poor economics have been an issue.

[0008] Therefore, the object of the present invention is to provide a new PHA decomposition technology capable of decomposing PHA to a low molecular weight at low cost, with low energy and with a large throughput. Another object of the present invention is to decompose PHA such as P3HB3HH, which has extremely low solubility in organic solvents, in an appropriate manner. [Means for solving the problem]

[0009] The present inventors conducted extensive research to solve the above problems and have now completed the present invention.

[0010] That is, one aspect of the present invention is a method for decomposing a polyhydroxyalkanoate, comprising the steps of: (a) mixing polyhydroxyalkanoate particles, which contain polyhydroxyalkanoate and have a ratio of particles of 0.5 μm or more and 1000 μm or less of 90% or more in a volume-based particle size distribution measured using a particle size distribution measurement device using a laser diffraction / scattering method, with an alcohol to obtain a mixed liquid containing particulate polyhydroxyalkanoate; and (b) heating the mixed liquid containing the particulate polyhydroxyalkanoate at a temperature of 85° C. or more and 220° C. or less in the presence of a basic catalyst.

[0011] Moreover, one aspect of the present invention is a method for producing a polyhydroxyalkanoate with a number average molecular weight of 5,000 or less, comprising the steps of: (a) mixing polyhydroxyalkanoate particles containing polyhydroxyalkanoate and having a number average molecular weight of 10,000 or more and 1,500,000 or less, in which the proportion of particles of 0.5 μm or more and 1,000 μm or less as determined from a volume-based particle size distribution by a laser diffraction / scattering method is 90% or more, with an alcohol to obtain a mixed liquid containing particulate polyhydroxyalkanoate; and (b) heating the mixed liquid containing the particulate polyhydroxyalkanoate at a temperature of 85° C. or more and 220° C. or less in the presence of a basic catalyst. Effect of the Invention

[0012] According to one aspect of the present invention, PHA can be decomposed to a low molecular weight using inexpensive alcohol and a basic catalyst, enabling more efficient resource utilization. In addition, the present invention allows PHA to be decomposed under relatively mild conditions of 85°C to 220°C, i.e., with low energy, and is a decomposition process with low environmental impact. In addition, in the present invention, the amount of PHA treated per cycle does not depend on the solubility of PHA, so that decomposition at a high rate is possible. Furthermore, the present invention is capable of decomposing even PHA with extremely low solubility in organic solvents. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] One embodiment of the present invention will be described in detail below. Unless otherwise specified in this specification, "A~B" representing a numerical range means "A or more and B or less". Also, all the documents described in this specification are incorporated herein by reference as references.

[0014] 〔Method for decomposing PHA〕 A method for decomposing polyhydroxyalkanoate according to an embodiment of the present invention (hereinafter, also referred to as "this decomposition method") includes: (a) mixing polyhydroxyalkanoate particles containing polyhydroxyalkanoate and having a proportion of particles with a particle size of 0.5 μm or more and 1000 μm or less of 90% or more in the particle size distribution measured using a particle size distribution measuring device by laser diffraction / scattering method with alcohol to obtain a mixed solution containing particulate polyhydroxyalkanoate; (b) heating the mixed solution containing the particulate polyhydroxyalkanoate at 85°C or more and 220°C or less in the presence of a basic catalyst.

[0015] Hereinafter, this decomposition method will be described in more detail.

[0016] <Step (a)> Step (a) is a step of mixing polyhydroxyalkanoate particles (hereinafter, also referred to as "PHA particles") containing PHA and having a proportion of particles with a particle size of 0.5 μm or more and 1000 μm or less of 90% or more in the volume-based particle size distribution measured using a particle size distribution measuring device by laser diffraction / scattering method with alcohol to obtain a mixed solution containing particulate polyhydroxyalkanoate (hereinafter, also referred to as "PHA mixed solution").

[0017] <PHA particles> In this specification, "PHA" is a general term for polymers having hydroxyalkanoates (hydroxyalkanoic acids) as monomer units. Hydroxyalkanoic acids constituting PHA are not particularly limited, but examples thereof include 2-hydroxypropanoic acid, 3-hydroxybutanoic acid, 4-hydroxybutanoic acid, 3-hydroxypropionic acid, 3-hydroxypentanoic acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, and 3-hydroxyoctanoic acid. These polymers may be homopolymers or copolymers containing two or more types of monomer units.

[0018] More specifically, examples of PHA include polylactic acid (PLA), poly-L-lactic acid (PLLA), poly(3-hydroxybutyrate) (P3HB), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (P3HB3HV), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (P3HB4HB), poly(3 -hydroxybutyrate-co-3-hydroxyoctanoate) (P3HB3HO), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate) (P3HB3HOD), poly(3-hydroxybutyrate-co-3-hydroxydecanoate) (P3HB3HD), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) (P3HB3HV3HH), etc. are included. Among them, P3HB, P3HB3HH, P3HB3HV, and P3HB4HB are preferred because they have a high amorphous content and therefore decomposition proceeds rapidly. Furthermore, P3HB3HH is particularly preferred because it is possible to easily control the mechanical strength suitable for use as a product and the amorphous content for rapid decomposition by adjusting the copolymerization ratio. In conventional decomposition methods, it was necessary to dissolve PHA in a solvent, making it difficult to decompose P3HB3HH at high throughputs, as there are no known solvents that can suitably dissolve PHA at high concentrations.However, according to the present invention, there is no need to dissolve PHA in a solvent, making it possible to decompose P3HB3HH at high concentrations and in high throughputs.

[0019] When the PHA contained in the PHA particles is P3HB3HH, the composition ratio of the repeating units of P3HB3HH is not particularly limited, but in order to obtain a sufficient amorphous proportion for rapid decomposition, it is preferable that the 3-hydroxybutyrate unit / 3-hydroxyhexanoate unit ratio is 80 / 20 to 99.9 / 0.1 (mol / mol), and more preferably 85 / 15 to 97 / 3 (mol / mol).

[0020] The number average molecular weight of the PHA contained in the PHA particles is not particularly limited, and the number average molecular weight, as determined by gel chromatography (hereinafter also referred to as "GPC") using polystyrene as the molecular weight standard, may be 10,000 or more, 20,000 or more, 50,000 or more, 80,000 or more, 10,000 to 1.5 million, 80,000 to 1.5 million, or 80,000 to 500,000.

[0021] In the volumetric particle size distribution of the PHA particles of the present invention, measured using a particle size distribution measuring device by the laser diffraction / scattering method, the ratio of particles of 0.5 μm to 1000 μm is 90% or more, more preferably the ratio of particles of 3 μm to 500 μm is 90% or more, and even more preferably the ratio of particles of 10 μm to 250 μm is 90% or more. If the particle size of the PHA particles is 0.5 μm or more, the particles can be suitably prepared by crushing / pulverization, and if it is 1000 μm or less, decomposition proceeds in a sufficiently short time. The particle size of the present invention is measured by the method described in the Examples using a HORIBA laser diffraction / scattering type particle size distribution measuring device LA-950.

[0022] The PHA particles may contain additives. Examples of additives include inorganic fillers such as talc, calcium carbonate, mica, and silica, colorants such as pigments and dyes, odor absorbers such as activated carbon and zeolite, fragrances such as vanillin and dextrin, plasticizers, antioxidants, weather resistance improvers, UV absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, and sliding property improvers. Among these additives, those that are not soluble in alcohol and cannot be decomposed by the present invention can be removed by a separation process such as a strainer after decomposition. In addition, water-soluble ones can be removed by extracting them into the aqueous phase by mixing the decomposition product with water and stirring it, and then separating it.

[0023] PHA particles are obtained by crushing and / or pulverizing used PHA products. The crushing and / or pulverizing method is not particularly limited, and can be carried out by applying a conventionally known method, for example, crushing and / or pulverizing using a single-shaft crusher, a double-shaft crusher, a pusher crusher, a screw crusher, a high-speed single-shaft crusher, a pusher crusher, a high-pressure homogenizer, an ultrasonic crusher, an emulsifying disperser, a bead mill, etc.

[0024] <Alcohol> In the present invention, alcohol reduces the molecular weight of PHA by transesterification with PHA, and produces an ester of hydroxyalkanoic acid and alcohol. Since no acid is produced as a product, the basic catalyst is not neutralized, and PHA can be efficiently decomposed with a small amount of basic catalyst. In the present specification, the term "alcohol" is not particularly limited as long as it can transesterify with PHA and is liquid at the temperature and pressure during the decomposition treatment, and examples thereof include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, and ethylene glycol. These alcohols may be used alone or in the form of a mixture of two or more alcohols. Among these, it is preferable to use inexpensive methanol or ethanol. In particular, it is more preferable to use bioethanol produced with low environmental impact in order to promote a breakaway from fossil fuel dependency in the production and use process of plastics. The alcohol consumed in the decomposition of PHA by the present invention can be effectively used as a carbon source in the production of chemical products using the decomposition products as raw materials.

[0025] The content of PHA particles in the PHA mixed liquid is not particularly limited, but if it is too small, the amount of PHA particles processed per cycle will be small, resulting in high costs, and if it is too large, decomposition may not proceed sufficiently, so it is preferable that the PHA particles be 5 parts by weight or more and 70 parts by weight or less, more preferably 15 parts by weight or more and 60 parts by weight or less, and even more preferably 30 parts by weight or more and 50 parts by weight or less, per 100 parts by weight of alcohol.

[0026] The amount of water contained in the PHA mixed liquid is not particularly limited, but the less the better. If the PHA mixed liquid contains a large amount of water, hydroxyalkanoic acid is generated by decomposition, which may neutralize and inactivate the basic catalyst, slowing down the progress of the decomposition reaction. Therefore, specifically, the water content is preferably 1% or less, more preferably 0.5% or less, and even more preferably 0.2% or less, relative to the PHA mixed liquid. The lower limit of the water content is not particularly limited, but is preferably 0.0001% or more, and even more preferably 0.001% or more, relative to the PHA mixed liquid. The water content in the PHA mixed liquid can be measured by gas chromatography.

[0027] The PHA mixture of the present invention contains particulate PHA. In this specification, particulate refers to a state in which the PHA is not completely dissolved. Particulate PHA may be partially dissolved. Particulate PHA can be confirmed by the presence or absence of turbidity in the PHA mixture.

[0028] The temperature in step (a) is not particularly limited, but is preferably at room temperature (about 15°C) or higher since cooling consumes energy. Heating is not required in step (a), but heating is required in step (b), so heating may be performed in advance from step (a). If heating is performed, it is preferable to heat the mixture to a temperature below the boiling point of the alcohol used at atmospheric pressure. It is more preferable to mix the mixture by stirring so that the PHA particles are thoroughly dispersed.

[0029] <Process (b)> Step (b) is a step of heating the PHA mixed liquid obtained in step (a) at 85° C. or higher and 220° C. or lower in the presence of a basic catalyst.

[0030] <Basic catalyst> In the present specification, the "basic catalyst" is not particularly limited as long as it is a basic compound capable of promoting transesterification with PHA, and examples thereof include sodium hydroxide, potassium hydroxide, calcium hydroxide, calcium oxide, magnesium hydroxide, etc. These basic catalysts may be used alone or in combination of two or more basic catalysts. Among them, it is particularly preferable to use sodium hydroxide, which is inexpensive and strongly basic. The amount of the basic catalyst used in step (b) is not particularly limited, but if the amount is too small, the reaction rate will be slow, and if the amount is too large, the cost will be high. Therefore, the amount is preferably 0.01 to 15 parts by weight, more preferably 0.05 to 5 parts by weight, and even more preferably 0.1 to 2 parts by weight, per 100 parts by weight of PHA particles.

[0031] In step (b), heating can be performed in a sealed vessel under a pressure condition higher than atmospheric pressure, or under reflux conditions. From the viewpoint of facility simplicity and operational stability, heating in a sealed vessel is preferred. The heating method is not particularly limited, and can be performed by applying a conventionally known method, such as heating with steam, hot water, or heat transfer oil, low-frequency induction heating, or electromagnetic wave heating.

[0032] The heating temperature in step (b) is 85°C or higher and 220°C or lower, preferably 90°C or higher and 200°C or lower, more preferably 100°C or higher and 180°C or lower, and even more preferably 110°C or higher and 150°C or lower. If the temperature is lower than 85°C, the decomposition reaction does not proceed at a sufficient rate, and if the temperature is higher than 220°C, the saturated vapor pressure of the alcohol becomes very high, so that the manufacturing cost of a sealed container having high pressure resistance becomes very high and there is a safety risk. If the temperature is set to 110°C or higher and 150°C or lower, the decomposition can be performed in a short time using a relatively inexpensive sealed container.

[0033] From the viewpoint of energy utilization efficiency, the heating time in step (b) is preferably as short as possible under conditions in which the PHA is sufficiently decomposed, for example, from 10 minutes to 15 hours, more preferably from 30 minutes to 5 hours, and even more preferably from 1 hour to 3 hours. By setting the heating time to 3 hours or less, a significant effect can be obtained in terms of the amount of PHA decomposed per unit time and unit weight of the PHA mixed solution, as compared with existing technologies.

[0034] Regarding the pressure in step (b), in the case of heating in a sealed container, the pressure in the sealed container is equal to or higher than the saturated vapor pressure of the alcohol at the heating temperature. The pressure in the sealed container may be the saturated vapor pressure of the alcohol, or may be pressurized to be equal to or higher than the saturated vapor pressure by air, nitrogen, carbon dioxide, or the like. When heating in a sealed container in step (b), it is desirable from the viewpoint of safety that the saturated vapor pressure of the alcohol to be heated is lower than the withstand pressure of the sealed container used. In the case of heating under reflux conditions, the pressure in step (b) is atmospheric pressure.

[0035] In order to promote rapid decomposition, it is preferable that the PHA particles are sufficiently dispersed in the alcohol during heating in step (b). Although the PHA particles are dispersed in the alcohol by convection caused by heating, it is preferable to stir the PHA mixture during heating in order to promote more uniform and rapid decomposition.

[0036] From the viewpoints of economy and environmental load reduction, it is preferable to recover and reuse the alcohol not consumed in the decomposition reaction. The alcohol can be easily recovered by heating the solution obtained in step (b) to volatilize the alcohol, and then cooling and condensing the resulting alcohol vapor.

[0037] The process may further include a separation step subsequent to the step (b) for removing undecomposed PHA particles, additives, etc., by a separation process using a strainer, etc. In particular, when the PHA particles used in the step (a) contain 0.1% or more particles larger than 1000 μm in the volume-based particle size distribution measured using a particle size distribution measuring device by a laser diffraction / scattering method, it is preferable to include a separation step subsequent to the step (b).

[0038] The number average molecular weight of the polyhydroxyalkanoate obtained by step (b) is preferably 5000 or less, as determined by GPC using polystyrene as the molecular weight standard, more preferably 3000 or less, and even more preferably 1500 or less. If the molecular weight is 5000 or less, the low molecular weight compound produced by decomposition can be suitably used as a carbon source for chemical production by microbial culture or chemical synthesis. The lower limit of the number average molecular weight may be the molecular weight of the monomer.

[0039] By incorporating the above-mentioned steps, this decomposition method can produce low molecular weight compounds that can be used as raw materials for chemical products from used or unnecessary PHA, thereby reducing the amount of waste and the amount of fossil fuel used.

[0040] In one embodiment of the present invention, in addition to the above steps, the decomposition method can further utilize various devices, tanks, etc. used in the art. The present invention is not limited to the above-described embodiment, and various modifications are possible within the scope of the claims.

[0041] [Method for producing polyhydroxyalkanoate] A method for producing a polyhydroxyalkanoate having a number average molecular weight of 5,000 or less according to one embodiment of the present invention (hereinafter referred to as "this production method") comprises the steps of: (a) mixing PHA particles having a number average molecular weight of 10,000 or more and 1,500,000 or less, in which the proportion of particles having a size of 0.5 μm or more and 1,000 μm or less as determined from a volume-based particle size distribution by a laser diffraction / scattering method is 90% or more, with alcohol to obtain a mixed liquid containing particulate polyhydroxyalkanoate; and (b) heating the mixed liquid containing the particulate polyhydroxyalkanoate at a temperature of 85° C. or more and 220° C. or less in the presence of a basic catalyst.

[0042] In one embodiment of the present invention, the production method may include steps (a) and (b) described in the above section "Method for decomposing PHA."

[0043] In this production method, the "PHA particles," "alcohol," "PHA mixed liquid," "basic catalyst," and the like are the same as those described in the above "PHA decomposition method."

[0044] The low molecular weight PHA obtained by the present production method may contain a monomeric hydroxyalkanoic acid and / or an ester formed by dehydration condensation of a hydroxyalkanoic acid and an alcohol.

[0045] According to this production method, low molecular weight PHA can be produced from waste PHA, and the amount of resources competing with edible resources such as starch and vegetable oil used in chemical production can be reduced, resulting in a process with low environmental impact. The obtained low molecular weight PHA can be suitably used as a raw material for chemical production by chemical synthesis or culture process.

[0046] In one embodiment of the present invention, in addition to the above steps, the present manufacturing method can further utilize various devices, tanks, etc. used in the art. The present invention is not limited to the above-mentioned embodiment, and various modifications are possible within the scope of the claims.

[0047] That is, one embodiment of the present invention is as follows. <1> (a) mixing polyhydroxyalkanoate particles, which contain polyhydroxyalkanoate and have a ratio of particles having a particle diameter of 0.5 μm or more and 1000 μm or less of 90% or more in a volume-based particle size distribution measured using a particle size distribution measuring device by a laser diffraction / scattering method, with alcohol to obtain a mixed solution containing particulate polyhydroxyalkanoate; (b) heating the mixture containing the particulate polyhydroxyalkanoate at 85° C. or more and 220° C. or less in the presence of a basic catalyst; A method for decomposing polyhydroxyalkanoates. <2> The polyhydroxyalkanoate particles contained in the mixed liquid containing the polyhydroxyalkanoate are 5 parts by weight or more and 70 parts by weight or less per 100 parts by weight of alcohol. <1> The method for decomposing polyhydroxyalkanoate according to claim 1. <3> The step (b) is carried out in a sealed vessel under a pressure higher than atmospheric pressure or under reflux conditions. <1> ~ <2> The method for decomposing polyhydroxyalkanoate according to claim 1. <4> The alcohol is at least one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, and ethylene glycol. <1> ~ <3> The method for decomposing polyhydroxyalkanoate according to claim 1. <5> The basic catalyst is at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, calcium hydroxide, calcium oxide, and magnesium hydroxide. <1> ~ <4> The method for decomposing polyhydroxyalkanoate according to claim 1. <6> The amount of the basic catalyst added is 0.01 parts by weight or more and 15 parts by weight or less based on 100 parts by weight of the polyhydroxyalkanoate particles. <1> ~ <5> The method for decomposing polyhydroxyalkanoate according to claim 1. <7> The polyhydroxyalkanoate particles comprise poly(3-hydroxyalkanoate); <1> ~ <6> The method for decomposing polyhydroxyalkanoate according to claim 1. <8>The method for decomposing polyhydroxyalkanoate according to <7>, wherein the polyhydroxyalkanoate particles contain poly-3-hydroxybutyrate-3-hydroxyhexanoate. <9>(a) A step of mixing polyhydroxyalkanoate particles having a number average molecular weight of 10,000 or more and 1,500,000 or less, wherein the proportion of particles having a particle size of 0.5 μm or more and 1000 μm or less obtained from the volume-based particle size distribution by the laser diffraction / scattering method is 90% or more, in alcohol to obtain a mixed solution containing particulate polyhydroxyalkanoate. (b) A step of heating the mixed solution containing the particulate polyhydroxyalkanoate in the presence of a basic catalyst at 85°C or higher and 220°C or lower. A method for producing polyhydroxyalkanoate having a number average molecular weight of 5000 or less.

Examples

[0048] Hereinafter, the present invention will be described more specifically with reference to examples, but the present invention is not limited to these examples.

[0049] <Number average molecular weight of PHA particles> 10 mg of P3HB3HH powder, which is PHA particles, was dissolved in 10 mL of chloroform, and then insoluble matters were removed by filtration. The number average molecular weight of this solution (filtrate) was measured using a GPC system manufactured by Shimadzu Corporation equipped with "Shodex K805L (300x8 mm, 2 connected)" (manufactured by Showa Denko KK), with chloroform as the mobile phase. As the molecular weight standard sample, Shodex K-804 (polystyrene gel) manufactured by Showa Denko K.K. was used.

[0050] <Number average molecular weight of decomposed PHA> After the PHA mixed solution after step (b) was heated at 60°C for 3 hours, a dry powder was obtained. The number average molecular weight of this dry powder was measured by the same method as described in

[0049] .

[0051] <Particle size> The particle size was measured under the following conditions using a HORIBA laser diffraction / scattering type particle size distribution analyzer LA-950.

[0052] 5 g of a dispersion liquid in which 10 parts by weight of PHA particles were dispersed in water was prepared and injected into the LA-950 at a temperature of 25°C to obtain the particle size distribution. From the obtained particle size distribution, the particle size detected with a frequency of 0.05% or more was designated as the particle size of the particles present in the measured PHA particles.

[0053] Example 1 P3HB3HH particles, in which the ratio of 3-hydroxybutyrate units to 3-hydroxyhexanoate units is 99 / 11 and all particles detected have a particle size in the range of 30 μm to 200 μm when measured using a particle size distribution measuring device by the laser diffraction / scattering method, were mixed with 30 parts by weight of ethanol. Sodium hydroxide was further added to the obtained PHA mixture in an amount of 0.5 parts by weight based on the weight of the P3HB3HH particles, and the mixture was heated at 120°C for 2 hours while stirring in a closed container. When the treated liquid was hot-filtered at 50°C, almost no P3HB3HH particles remained. When the molecular weight was evaluated by GPC, the number average molecular weight of the original P3HB3HH was 173,000, whereas that of the treated P3HB3HH was 1,305.

[0054] Example 2 P3HB3HH particles, in which the ratio of 3-hydroxybutyrate units to 3-hydroxyhexanoate units is 99 / 11 and all particles detected have a particle size in the range of 30 μm to 200 μm when measured using a particle size distribution measuring device using a laser diffraction / scattering method, were mixed with 30 parts by weight of ethanol. Sodium hydroxide was further added to the obtained PHA mixture in an amount of 3 parts by weight based on the weight of the P3HB3HH particles, and the mixture was heated at 90°C for 10 hours while stirring in a closed container. When the treated liquid was hot-filtered at 50°C, almost no P3HB3HH particles remained. When the molecular weight was evaluated by GPC, the number average molecular weight of the original P3HB3HH was 173,000, whereas that of the treated P3HB3HH was 1,930.

[0055] Example 3 P3HB3HH particles, in which the ratio of 3-hydroxybutyrate units to 3-hydroxyhexanoate units is 99 / 11 and all particles detected have a particle size in the range of 30 μm to 200 μm when measured using a particle size distribution measuring device by laser diffraction and scattering method, were mixed with 30 parts by weight of ethanol. Calcium oxide was further added to the obtained PHA mixture in an amount of 0.5 parts by weight based on the weight of the P3HB3HH particles, and the mixture was heated at 120°C for 2 hours while stirring in a closed container. When the treated liquid was hot-filtered at 50°C, almost no P3HB3HH particles remained. When the molecular weight was evaluated by GPC, the number average molecular weight of the original P3HB3HH was 173,000, whereas that of the treated P3HB3HH was 1689.

[0056] Example 4 P3HB3HH particles, in which the ratio of 3-hydroxybutyrate units to 3-hydroxyhexanoate units is 99 / 11 and all particles detected have a particle size in the range of 30 μm to 200 μm when measured using a particle size distribution measuring device by the laser diffraction / scattering method, were mixed with 30 parts by weight of ethanol. Sodium hydroxide was further added to the obtained PHA mixture at 2 parts by weight based on the weight of the P3HB3HH particles, and the mixture was heated at 100°C for 10 hours while stirring under reflux conditions. When the treated liquid was hot-filtered at 50°C, almost no P3HB3HH particles remained. When the molecular weight was evaluated by GPC, the number average molecular weight of the original P3HB3HH was 173,000, whereas that of the treated P3HB3HH was 1520.

[0057] Comparative Example 1 P3HB3HH particles with a 3-hydroxybutyrate unit / 3-hydroxyhexanoate unit ratio of 99 / 11 and a particle size ranging from 5 mm to 1 cm were mixed with 30 parts by weight of ethanol. Sodium hydroxide was further added to the resulting PHA mixture in an amount of 0.5 parts by weight based on the weight of the P3HB3HH particles, and the mixture was heated at 120°C for 2 hours while stirring in a sealed container. A large amount of undecomposed P3HB3HH particles were visually confirmed in the liquid after the treatment, confirming that decomposition had not progressed sufficiently.

[0058] Comparative Example 2 P3HB3HH particles, in which the ratio of 3-hydroxybutyrate units to 3-hydroxyhexanoate units is 99 / 11 and all particles detected have a particle size in the range of 30 μm to 200 μm when measured using a particle size distribution measuring device by laser diffraction and scattering method, were mixed with water at 20 parts by weight. Sodium hydroxide was added to the resulting PHA mixture at 50 parts by weight based on the weight of the P3HB3HH particles, and the mixture was heated at 130°C for 3 hours while stirring in a closed container. A large amount of undecomposed P3HB3HH particles were visually confirmed in the liquid after the treatment, and it was confirmed that the decomposition had not progressed sufficiently. Since the pH of the mixture after the treatment had dropped to 8.0, it is considered that the sodium hydroxide was neutralized by the hydroxyalkanoic acid generated by the decomposition of P3HB3HH, and the mixture became close to neutral, so that the decomposition did not proceed sufficiently.

[0059] 〔result〕 Comparing Examples 1 to 4 with Comparative Example 1, it was found that by using particles with a particle size of 0.5 μm to 1000 μm, PHA can be decomposed under mild conditions, i.e., with low energy. Also, comparing Examples 1 to 4 with Comparative Example 2, it was found that by using alcohol, the amount of sodium hydroxide used as a basic catalyst could be reduced to less than 1 / 100 compared to the decomposition method using water, and costs could be significantly reduced. [Industrial Applicability]

[0060] The present invention can be suitably used in the fields of chemical production, plastic recycling, and other fields.

Claims

1. (a) mixing polyhydroxyalkanoate particles, which contain polyhydroxyalkanoate and have a ratio of particles having a particle diameter of 0.5 μm or more and 1000 μm or less of 90% or more in a volume-based particle diameter distribution measured using a particle diameter distribution measuring device by a laser diffraction / scattering method, with alcohol to obtain a mixed solution containing particulate polyhydroxyalkanoate; (b) heating the mixture containing the particulate polyhydroxyalkanoate at 85° C. or more and 220° C. or less in the presence of a basic catalyst; A method for decomposing polyhydroxyalkanoates.

2. 2. The method for decomposing a polyhydroxyalkanoate according to claim 1, wherein the polyhydroxyalkanoate particles contained in the mixed liquid containing the polyhydroxyalkanoate are 5 parts by weight or more and 70 parts by weight or less per 100 parts by weight of the alcohol.

3. 2. The method for decomposing a polyhydroxyalkanoate according to claim 1, wherein the step (b) is carried out in a sealed vessel under a pressure condition higher than atmospheric pressure or under a reflux condition.

4. The method for decomposing polyhydroxyalkanoate according to claim 1, wherein the alcohol is at least one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol and ethylene glycol.

5. 2. The method for decomposing polyhydroxyalkanoate according to claim 1, wherein the basic catalyst is at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, calcium hydroxide, calcium oxide, and magnesium hydroxide.

6. 2. The method for decomposing polyhydroxyalkanoate according to claim 1, wherein the amount of the basic catalyst added is 0.01 parts by weight or more and 15 parts by weight or less per 100 parts by weight of the polyhydroxyalkanoate particles.

7. 2. The method for decomposing a polyhydroxyalkanoate according to claim 1, wherein the polyhydroxyalkanoate particles comprise poly(3-hydroxyalkanoate).

8. 8. The method for decomposing a polyhydroxyalkanoate according to claim 7, wherein the polyhydroxyalkanoate particles comprise poly-3-hydroxybutyrate-3-hydroxyhexanoate.

9. (a) mixing polyhydroxyalkanoate particles having a number average molecular weight of 10,000 or more and 1,500,000 or less, which contain polyhydroxyalkanoate and have a particle diameter of 0.5 μm or more and 1,000 μm or less in a volume-based particle size distribution determined by a laser diffraction / scattering method of 90% or more, with an alcohol to obtain a mixed solution containing particulate polyhydroxyalkanoate; (b) heating the mixture containing the particulate polyhydroxyalkanoate at 85° C. or more and 220° C. or less in the presence of a basic catalyst; A method for producing polyhydroxyalkanoate having a number average molecular weight of 5,000 or less.

Citation Information

Patent Citations

  • Method for recovering monomer of polyester

    JP2004250414A

  • Method for treating plastic articles digestible by hot alkaline treatment

    JP2004513200A

  • Chemical recycling of PLA by alcoholysis

    WO2010118955A1