Polarizing film
By aligning the slow axis of the base material and absorption axis of the polarizing film at 45°±5° and controlling refractive index differences, the polarizing film effectively reduces interference unevenness from interfacial reflections, enhancing display device performance.
Patent Information
- Application Number
- JP2023214229
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2023-12-19
- Publication Date
- 2024-10-11
AI Technical Summary
Polarizing films used in flat panel display devices experience interference unevenness due to increased interface reflection of incident light between the polarizing film and the alignment film, as well as between the alignment film and the base material.
A polarizing film design where the slow axis direction of the base material and the absorption axis direction of the polarizing film are aligned at 45°±5°, with refractive index differences between the polarizing film and alignment film, and between the alignment film and the base material, controlled within specific ranges to minimize interfacial reflection.
Suppresses interference unevenness caused by interfacial reflection, ensuring a smoother and more efficient application of the polarizing film in display devices.
Smart Images

Figure 2024144086000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to polarizing films. [Background technology]
[0002] A polarizing film for the purpose of optical compensation is used in flat panel displays such as liquid crystal displays and organic electroluminescence displays. A polarizing film is generally composed of a substrate, an alignment film, and a polarizing film laminated in this order.
[0003] In recent years, there has been an increasing demand for thinner flat panel displays, and accordingly, thinner polarizing films are also required. An example of a thin polarizing film is the polarizing film described in Patent Document 1. This conventional polarizing film is made of a composition containing a polymerizable liquid crystal compound and a dichroic dye. As a thin polarizing film, a film having an absorption axis in an oblique direction to the longitudinal direction of the polarizing film is also known. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2007-510946 Summary of the Invention [Problem to be solved by the invention]
[0005] In the polarizing film as described above, there was a problem that interference unevenness becomes noticeable when the interfacial reflection of incident light between the polarizing film and the alignment film and between the alignment film and the substrate becomes strong.
[0006] The present disclosure has been made to solve the above-mentioned problems, and has an object to provide a polarizing film that can suppress interference unevenness caused by interfacial reflection of incident light. [Means for solving the problem]
[0007] A polarizing film according to one aspect of the present disclosure is a polarizing film comprising a substrate, an alignment film, and a polarizing film laminated in this order, wherein the angle between the slow axis direction of the substrate and the absorption axis direction of the polarizing film is 45°±5°, the refractive index difference between the polarizing film and the alignment film for visible light satisfies the following formula (1), and the refractive index difference between the alignment film and the substrate for visible light satisfies the following formula (2). |n(polarizing film)-n(alignment film)|≦0.06 … (1) |n(alignment film)-n(substrate)|≦0.06 … (2) (In formula (1), n (polarizing film) represents the refractive index in the transmission axis direction of the polarizing film.)
[0008] In this polarizing film, by controlling the refractive index difference between the alignment film and the substrate and between the alignment film and the substrate within the above range, it is possible to suppress the interfacial reflection of incident light between the alignment film and the substrate and between the alignment film and the substrate, and therefore, in this polarizing film, it is possible to suppress interference unevenness caused by interfacial reflection of incident light.
[0009] The thickness of the alignment film is preferably 10 nm to 400 nm, in which case, in a polarizing film having an alignment film thickness in this range, interference unevenness caused by interfacial reflection of incident light can be suitably suppressed.
[0010] A hard coat layer may be adjacent to the surface of the substrate opposite to the alignment film. In producing a polarizing film, it is considered that the substrate may warp due to shrinkage when the polarizing film is cured, and wrinkles may occur in the obtained polarizing film. By having a hard coat layer adjacent to the surface of the substrate opposite to the alignment film, warping of the substrate due to shrinkage when the polarizing film is cured can be suppressed, and wrinkles can be suppressed from occurring in the obtained polarizing film.
[0011] The substrate, the alignment film, and the polarizing film may be long. In this case, a long polarizing film capable of suppressing interference unevenness caused by interfacial reflection of incident light can be obtained. By continuously bonding the polarizing film cut out from the long polarizing film to various display devices, it is possible to efficiently manufacture display devices using a polarizing film in which interference unevenness caused by interfacial reflection of incident light is suppressed.
[0012] The angle between the longitudinal direction and the slow axis direction of the substrate is preferably 0°±5° or 90°±5°, which allows a polarizing film with high ellipticity to be obtained. Effect of the Invention
[0013] According to the present disclosure, it is possible to suppress interference unevenness caused by interfacial reflection of incident light. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic diagram showing a layer structure of a polarizing film according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a diagram showing layer structures of polarizing films according to examples and comparative examples. [Diagram 3] FIG. 1 is a diagram showing evaluation results of polarizing films according to Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, preferred embodiments of a polarizing film according to one aspect of the present disclosure will be described in detail with reference to the drawings.
[0016] Fig. 1 is a schematic diagram showing the layer structure of a polarizing film according to an embodiment of the present disclosure. As shown in Fig. 1, the polarizing film 1 is formed by laminating a substrate 2, an alignment film 3, and a polarizing film 4 in this order. In this embodiment, the substrate 2, the alignment film 3, and the polarizing film 4 are all long, and a long polarizing film 1 is formed.
[0017] The term "long" includes both a state in which the film is wound into a roll and a state in which the film is unwound from a roll. The length of the long polarizing film 1 in the longitudinal direction (the direction in which the polarizing film 1 extends) is, for example, 10 m to 3000 m, and preferably 100 m to 200 m. The length of the long polarizing film 1 in the transverse direction (the direction perpendicular to the direction in which the polarizing film 1 extends) is, for example, 0.1 m to 5 m, and preferably 0.2 m to 2 m.
[0018] The long polarizing film 1 is cut to a required size and used in various display devices. Examples of the display devices include liquid crystal display devices, organic EL display devices, inorganic EL display devices, electron emission displays, electronic paper, and piezoelectric ceramic displays. These display devices may display two-dimensional images or three-dimensional images.
[0019] The substrate 2 is made of, for example, resin. The substrate 2 is particularly transparent to visible light, and has a transmittance of 80% or more for light with a wavelength of 380 nm to 780 nm. In consideration of practical handling and processability, the thickness of the substrate 2 is, for example, 5 μm to 300 μm, and preferably 20 μm to 200 μm.
[0020] The substrate 2 is, for example, a retardation film having a function as a quarter-wave plate. The substrate 2 as a retardation film is obtained by stretching a long substrate having no retardation. The slow axis direction of the substrate 2 varies depending on the stretching method. Examples of the stretching method include uniaxial stretching, biaxial stretching, and oblique stretching. The angle between the longitudinal direction of the polarizing film 1 and the slow axis direction of the substrate 2 is preferably 0°±5° or 90°±5°.
[0021] The substrate 2 has optical properties represented by the following formulas (1) and (2). The substrate 2 may also have optical properties represented by the following formulas (3) and (4). In the following formulas (1) to (4), Re(λ) is a front retardation value for light with a wavelength of λ nm. 100nm <Re(550)<160nm …(1) 130nm <Re(550)<150nm …(2) Re(450) / Re(550)≦1.00 …(3) 1.00≦Re(650) / Re(550) …(4)
[0022] The front retardation value is determined by the following formula (5). In formula (5), d represents the thickness, and Δn(λ) represents the birefringence at a wavelength of λ nm. In order to obtain a desired front retardation value, d and Δn(λ) should be adjusted. By adjusting the front retardation value, the substrate 2 can be obtained as a ¼ wavelength plate. Re(λ)=d×Δn(λ) …(5)
[0023] Examples of the resin material constituting the substrate 2 include polyolefins such as polyethylene, polypropylene, and norbornene-based polymers; cyclic olefin-based resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide; and polyphenylene oxide. The substrate 2 is preferably a cyclic olefin-based resin, triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate, polyethylene naphthalate, polymethacrylic acid esters, polyacrylic acid esters, polyethylene, or polypropylene. The substrate 2 is more preferably a cyclic olefin-based resin, triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate, polymethacrylic acid esters, or polyacrylic acid esters.
[0024] The substrate 2 may be subjected to a surface treatment. Examples of the surface treatment include corona or plasma treatment under a vacuum atmosphere to an atmospheric pressure atmosphere, laser treatment, ozone treatment, saponification treatment, flame treatment, application of a coupling agent, primer treatment, and treatment by a graft polymerization method in which a reactive monomer or a reactive polymer is attached to the surface and then reacted by irradiating with radiation, plasma, or ultraviolet light.
[0025] A hard coat layer 5 may be adjacent to the surface of the substrate 2 opposite to the alignment film 3. The hard coat layer 5 is a cured resin layer that has a higher surface smoothness than the adjacent substrate 2 and is peelable from the substrate 2. The hard coat layer 5 can be formed from a material known in the art as long as the desired peel strength can be ensured in the substrate 2. Examples of the hard coat layer 5 include a layer formed from a resin composition containing a water-soluble polymer, and a cured resin layer formed from a resin composition containing an active energy ray-curable or thermosetting resin component.
[0026] The resin composition constituting the hard coat layer 5 usually contains a resin component (polymer). Examples of the resin component include (meth)acrylic polymers, urethane polymers, polyester polymers, silicone polymers, polyvinyl ether polymers, polyvinyl alcohol polymers, and the like. These resin components may be used alone or in combination of two or more.
[0027] The content of the resin component in the resin composition can be appropriately determined depending on the type of the resin component used. The content of the resin component is preferably 50 parts by mass or more, more preferably 60 parts by mass or more, and even more preferably 70 parts by mass or more, based on 100 parts by mass of the solid content of the resin composition. The content of the resin component is preferably 100 parts by mass or less, more preferably 95 parts by mass or less, and even more preferably 90 parts by mass or less.
[0028] The resin composition constituting the hard coat layer 5 may contain a crosslinking agent. As the crosslinking agent, a crosslinking agent usually used in the field can be used. The crosslinking agent can be appropriately selected depending on the resin components constituting the hard coat layer 5, the composition of the layer adjacent to the hard coat layer 5, etc. Examples of the crosslinking agent include methylol compounds, polyfunctional thiol compounds, polyfunctional (meth)acrylates, etc. These may be used alone or in combination of two or more. In addition, the hard coat layer 5 may contain an additive for improving the strength of the substrate 2. Examples of the additive include inorganic fine particles, organic fine particles, and mixtures thereof.
[0029] The alignment film 3 is a film having a regulating force for aligning the dichroic dye in a desired direction. The alignment film 3 aligns the dichroic dye contained in a composition (composition for forming a polarizing film) for forming the polarizing film 4, thereby adjusting the absorption axis direction of the polarizing film 4 to a desired direction. The absorption axis direction of the polarizing film 4 is, for example, the same direction as the regulating force direction of the alignment film 3. The angle between the longitudinal direction of the polarizing film 1 and the regulating force direction of the alignment film 3 is, for example, 45°±5°.
[0030] The alignment film 3 has resistance to dissolution when the composition for forming a polarizing film is applied, and also has heat resistance when the solvent is removed and when the dichroic dye is oriented. Examples of the alignment film 3 include a photoalignment film, an alignment film containing an oriented polymer, and a groove alignment film having a concave-convex pattern or a plurality of grooves on the surface. The thickness of the alignment film 3 is, for example, 10 nm to 1200 nm, preferably 10 to 400 nm, more preferably 10 to 200 nm, and particularly preferably 10 nm to 100 nm, in consideration of sufficient expression of the alignment control force. In this case, in a polarizing film 1 having an alignment film 3 having a thickness in this range, interference unevenness due to interfacial reflection of incident light can be suitably suppressed.
[0031] Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and their hydrolyzates such as polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. The oriented polymers can be used alone or in combination of two or more kinds.
[0032] The alignment film 3 containing an alignment polymer is usually obtained by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter also referred to as an "alignment polymer composition") to a substrate 2 and removing the solvent, or by applying an alignment polymer composition to a substrate 2, removing the solvent, and rubbing (rubbing method).
[0033] The solvent is preferably an organic solvent, and examples of the organic solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; and chlorinated hydrocarbon solvents such as chloroform and chlorobenzene. The solvents can be used alone or in combination of two or more. The content of the solvent is preferably 100 to 1900 parts by mass, more preferably 150 to 900 parts by mass, and further preferably 180 to 600 parts by mass, based on 100 parts by mass of the orientable polymer composition.
[0034] The concentration of the oriented polymer in the oriented polymer composition may be within a range in which the oriented polymer material can be completely dissolved in the solvent, but is preferably 0.1% to 20% in terms of solid content relative to the solution, and more preferably 0.1% to 10%. For the oriented polymer composition, a commercially available oriented film material may be used as is. Examples of commercially available oriented film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).
[0035] Examples of the method for applying the oriented polymer composition to the substrate 2 include known methods such as coating methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography. Examples of the method for removing the solvent contained in the oriented polymer composition include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0036] A rubbing treatment can be performed as necessary to impart an orientation regulating force to the orientation film 3 (rubbing method). As a method for imparting an orientation regulating force by the rubbing method, for example, a method in which an orientation polymer composition is applied to the substrate 2 and annealed to bring the orientation polymer film formed on the surface of the substrate 2 into contact with a rubbing roll rotating with a rubbing cloth wrapped around it can be mentioned.
[0037] The photo-alignment film is usually obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter also referred to as a "photo-alignment film-forming composition") to the substrate 2 and irradiating it with polarized light (preferably polarized UV). The photo-alignment film is more preferable in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the polarized light to be irradiated.
[0038] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that are the origin of liquid crystal alignment ability, such as molecular alignment induction or isomerization reaction, dimerization reaction, photocrosslinking reaction or photodecomposition reaction, which are generated by irradiation with light. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond) and a carbon-oxygen double bond (C=O bond) is particularly preferred.
[0039] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.
[0040] Among them, photoreactive groups involved in photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film having excellent thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred.
[0041] A photo-alignment-inducing layer can be formed on the substrate 2 by applying the composition for forming a photo-alignment film onto the substrate 2. Examples of the solvent contained in the composition include the same solvents as those described in the "alignment polymer composition" section, and the solvent can be appropriately selected depending on the solubility of the polymer or monomer having a photoreactive group.
[0042] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted depending on the type of polymer or monomer and the thickness of the desired photo-alignment film, but is preferably at least 0.2% by mass, more preferably in the range of 0.3 to 10% by mass, based on the mass of the composition for forming a photo-alignment film. The composition for forming a photo-alignment film may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, within a range that does not significantly impair the properties of the photo-alignment film.
[0043] The method for applying the composition for forming a photo-alignment film to the substrate 2 may be the same as the method for applying the alignment composition to the substrate 2. Methods for removing the solvent from the applied composition for forming a photo-alignment film may be, for example, natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0044] The method of irradiating polarized light may be a method of directly irradiating polarized UV onto the composition for forming a photo-alignment film coated on the substrate 2 after removing the solvent, or a method of irradiating polarized light from the substrate 2 side and then transmitting the polarized light. It is particularly preferable that the polarized light is substantially parallel light. The wavelength of the irradiated polarized light is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) with a wavelength in the range of 250 to 400 nm is particularly preferable.
[0045] Examples of light sources used for polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferred. Among these, high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are preferred because of the high emission intensity of ultraviolet light with a wavelength of 313 nm. Polarized UV can be irradiated by irradiating light from the light source through an appropriate polarizer. Examples of such polarizers include polarizing filters, polarizing prisms such as Glan-Thompson and Glan-Taylor, and wire grid type polarizers. If masking is performed during rubbing or polarized light irradiation, multiple regions (patterns) with different liquid crystal orientation directions can also be formed.
[0046] A groove alignment film is a film that has a concave-convex pattern or multiple grooves on the film surface. When a polymerizable liquid crystal compound is applied to a film that has multiple linear grooves arranged at equal intervals, the liquid crystal molecules are aligned in the direction along the grooves.
[0047] Methods for obtaining a groove alignment film include a method in which the surface of a photosensitive polyimide film is exposed to light through an exposure mask having slits in a pattern shape, followed by development and rinsing to form an uneven pattern; a method in which a layer of uncured UV-curable resin is formed on a plate-shaped master having grooves on its surface, the formed resin layer is transferred to the substrate 2, and then cured; and a method in which a roll-shaped master having multiple grooves is pressed against an uncured UV-curable resin film formed on the substrate 2 to form unevenness, followed by curing.
[0048] The polarizing film 4 is configured to include a dichroic dye compound. The dichroic dye compound is a dye compound having different absorbance in the long axis direction of the molecule and absorbance in the short axis direction of the molecule. The polarizing film 4 configured with the dichroic dye compound has an absorption axis direction in a predetermined direction and a transmission axis direction perpendicular to the absorption axis direction. In addition, the polarizing film 4 configured with the dichroic dye compound has a maximum absorption wavelength in a predetermined wavelength range.
[0049] In this embodiment, as described above, the angle between the longitudinal direction of the polarizing film 1 and the regulating force direction of the alignment film 3 is 45°±5°, and the absorption axis direction of the polarizing film 4 is parallel to the regulating force direction of the alignment film 3. Therefore, the angle between the longitudinal direction of the polarizing film 1 and the absorption axis direction of the polarizing film 4 is 45°±5°. Note that the angle here means the smaller angle between the two axes, that is, an angle of 90° or less. The polarizing film 4 has a maximum absorption wavelength in the range of, for example, 380 nm to 780 nm.
[0050] Examples of the dichroic dye include an acridine dye, an oxazine dye, a cyanine dye, a naphthalene dye, an azo dye, and an anthraquinone dye, and among these, an azo dye is preferred. Examples of the azo dye include a monoazo dye, a bisazo dye, a trisazo dye, a tetrakisazo dye, and a stilbene azo dye, and among these, a bisazo dye and a trisazo dye are preferred.
[0051] The azo dye includes a compound represented by the following formula (I) (hereinafter sometimes referred to as "compound (I)"). K 1 (-N=NK 2 ) p -N=NK 3 (I) [In formula (I), K 1 and K 3 each independently represents a phenyl group which may have a substituent, a naphthyl group which may have a substituent, or a monovalent heterocyclic group which may have a substituent. 2 represents a p-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, or a divalent heterocyclic group which may have a substituent. p represents an integer of 1 to 4. When p is an integer of 2 or more, a plurality of K 2 may be the same or different. The -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO-, or -N=CH- bond as long as the compound exhibits absorption in the visible region.
[0052] Examples of the monovalent heterocyclic group include groups in which one hydrogen atom has been removed from a heterocyclic compound such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, benzoxazole, etc. Examples of the divalent heterocyclic group include groups in which two hydrogen atoms have been removed from the above-mentioned heterocyclic compounds.
[0053] K 1 and K 3 Phenyl, naphthyl and monovalent heterocyclic groups in 2 Examples of the substituent that the p-phenylene group, the naphthalene-1,4-diyl group, and the divalent heterocyclic group in the formula (I) may optionally have include an alkyl group having 1 to 4 carbon atoms; an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, or a butoxy group; a fluorinated alkyl group having 1 to 4 carbon atoms, such as a trifluoromethyl group; a cyano group; a nitro group; a halogen atom; and a substituted or unsubstituted amino group, such as an amino group, a diethylamino group, or a pyrrolidino group (the substituted amino group refers to an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. An unsubstituted amino group is -NH2).
[0054] Among the compounds (I), compounds represented by any one of formulas (I-1) to (I-8) are preferred, compounds represented by any one of formulas (I-1) to (I-3) are more preferred, and compounds represented by any one of formulas (I-1) and (I-3) are even more preferred. [ka] [In formulas (I-1) to (I-8), B 1 ~B 30 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the definitions of a substituted amino group and an unsubstituted amino group are as described above), a chlorine atom, or a trifluoromethyl group. n1 to n4 each independently represent an integer of 0 to 3. When n1 is 2 or more, multiple B2 may be the same or different, and when n2 is 2 or more, a plurality of B 6 may be the same or different, and when n3 is 2 or more, a plurality of B 9 may be the same or different, and when n4 is 2 or more, a plurality of B 14 may be the same or different.]
[0055] The anthraquinone dye is preferably a compound represented by formula (I-9). [ka] [In formula (I-9), R 1 ~R 8 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0056] The oxazone dye is preferably a compound represented by formula (I-10). [ka] [In formula (I-10), R 9 ~R 15 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0057] The acridine dye is preferably a compound represented by formula (I-11). [ka] [In formula (I-11), R 16 ~R 23 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0058] In the above formulas (I-9), (I-10), and (I-11), R x Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a toluyl group, a xylyl group, and a naphthyl group.
[0059] As the cyanine dye, the compounds represented by formula (I-12) and formula (I-13) are preferred. [ka] [In formula (I-12), D 1 and D. 2 represent, independently of each other, a group represented by any one of formulas (I-12a) to (I-12d). [ka] n5 represents an integer from 1 to 3. [ka] [In formula (I-13), D 3 and D. 4 represent, independently of each other, a group represented by any one of formulas (I-13a) to (I-13h). [ka] n6 represents an integer from 1 to 3.
[0060] Among these dichroic dyes, azo dyes are preferred from the viewpoint of alignment.
[0061] The polarizing film 4 can be formed by applying a polarizing film-forming composition containing a dichroic dye compound onto the alignment film 3 and drying the composition. The application method can be the same as the application method for the composition for forming a photo-alignment film described above. From the viewpoint of improving the alignment of the dichroic dye, the content of the dichroic dye compound in the polarizing film-forming composition is preferably 0.1 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, even more preferably 0.1 to 10 parts by mass, and particularly preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the solid content of the polarizing film-forming composition. The solid content here refers to the total amount of components excluding the solvent from the polarizing film-forming composition.
[0062] The composition for forming a polarizing film may contain a polymerizable liquid crystal compound, a solvent, a polymerization initiator, a sensitizer, a polymerization inhibitor, a leveling agent, and a polymerizable non-liquid crystal compound. In the polarizing film 4 containing the polymerizable liquid crystal compound, the strength is improved and color unevenness is reduced. When the composition for forming a polarizing film contains a polymerizable liquid crystal compound, the composition for forming a polarizing film may be dried to obtain a dried film, which may be cured. Curing refers to polymerizing the polymerizable liquid crystal compound contained in the dried film. Examples of polymerization methods include heating and light irradiation. The orientation state of the dichroic dye contained in the dried film can be fixed by curing.
[0063] The polymerizable liquid crystal compound is a compound having a polymerizable group and exhibiting liquid crystallinity. The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. The photopolymerizable group is a group that can undergo a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Examples of the compound exhibiting liquid crystallinity include a thermotropic liquid crystal and a lyotropic liquid crystal, and the thermotropic liquid crystal is preferable in terms of the ability to precisely control the film thickness. The compound exhibiting liquid crystallinity may be a nematic liquid crystal or a smectic liquid crystal in a thermotropic liquid crystal. The polymerizable liquid crystal compound may be a monomer, but may also be an oligomer or a polymer in which a polymerizable group is polymerized.
[0064] The polymerizable liquid crystal compound is preferably a liquid crystal compound that forms a smectic phase from the viewpoint of obtaining higher polarization characteristics. Examples of the smectic phase include smectic B phase, smectic D phase, smectic E phase, smectic F phase, smectic G phase, smectic H phase, smectic I phase, smectic J phase, smectic K phase, and smectic L phase, and smectic B phase, smectic F phase, or smectic I phase is preferable, and smectic B phase is more preferable. These smectic phases may be higher-order smectic phases.
[0065] When the liquid crystal phase formed by the polymerizable liquid crystal compound is one of these higher order smectic phases, a polarizing film 4 with higher orientation order can be obtained. In a polarizing film 4 with a high degree of orientation order, a Bragg peak derived from a higher order structure such as a hexatic phase or a crystalline phase is obtained in an X-ray diffraction measurement. The Bragg peak is a peak derived from the periodic structure of the molecular orientation. When the liquid crystal phase formed by the polymerizable liquid crystal compound is one of these higher order smectic phases, a polarizing film 4 with a periodic interval of the molecular orientation of, for example, 3.0 Å to 6.0 Å can be obtained.
[0066] Examples of the polymerizable liquid crystal compound include a compound represented by the following formula (B1) and a polymer of the compound (hereinafter, the compound and the polymer are collectively referred to as "polymerizable liquid crystal compound (B1)"). U 1 -V 1 -W 1 -X 1 -Y 1 -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (B1) [In formula (B1), X 1 , X 2 and X 3 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. A hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. However, X 1 , X 2 and X 3 At least one of Y is an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group. 1 and Y 2 are each independently a single bond or a divalent linking group. 1 represents a hydrogen atom or a polymerizable group. 2 represents a polymerizable group. 1 and W 2 are each independently a single bond or a divalent linking group. 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH2- constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or NH-.]
[0067] In the polymerizable liquid crystal compound (B1), X 1, X 2 , and X 3 At least one of X is an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group. 1 and X 3 is preferably a cyclohexane-1,4-diyl group which may have a substituent, and the cyclohexane-1,4-diyl group is more preferably a trans-cyclohexane-1,4-diyl group. Examples of the optional substituent of the 1,4-phenylene group which may have a substituent or the cyclohexane-1,4-diyl group which may have a substituent include an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, and a butyl group, a cyano group, and a halogen atom such as a chlorine atom or a fluorine atom. It is preferably unsubstituted. Also, Y 1 and Y 2 If X is the same structure, 1 , X 2 , and X 3 It is preferable that at least one of X has a different structure. 1 , X 2 , and X 3 When at least one of the above has a different structure, smectic liquid crystallinity tends to be easily exhibited.
[0068] Y 1 and Y 2 are each independently -CH2CH2-, -CH2O-, -CH2CH2O-, -COO-, -OCOO-, a single bond, -N=N-, -CR a =CR b -, -C≡C-, -CR a =N- or CO-NR a - is preferred. a and R b each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 is more preferably -CH2CH2-, -COO-, or a single bond, and Y 2 More preferably, X is -CHCH- or CHO-. 1 , X 2 , and X3 If all have the same structure, Y 1 and Y 2 It is preferable that Y have different structures. 1 and Y 2 When the structures are different from each other, smectic liquid crystallinity tends to be easily exhibited.
[0069] U 2 is a polymerizable group. 1 is a hydrogen atom or a polymerizable group, and is preferably a polymerizable group. 1 and U 2 are preferably both polymerizable groups, and more preferably both photopolymerizable groups. The photopolymerizable group means a group that can be involved in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator described later.
[0070] U 1 and a photopolymerizable group represented by U 2 The polymerizable groups represented by may be different from each other, but are preferably the same type of group. Examples of the polymerizable group include vinyl group, vinyloxy group, 1-chlorovinyl group, isopropenyl group, 4-vinylphenyl group, acryloyloxy group, methacryloyloxy group, oxiranyl group, and oxetanyl group. Among them, radical polymerizable groups are preferred, acryloyloxy group, methacryloyloxy group, vinyl group, and vinyloxy group are more preferred, acryloyloxy group and methacryloyloxy group are even more preferred, and acryloyloxy group is even more preferred.
[0071] V 1 and V 2 Examples of the alkanediyl group represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group, and an icosane-1,20-diyl group. 1 and V 2is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms. Examples of the substituent that the alkanediyl group may have include a cyano group and a halogen atom, but the alkanediyl group is preferably unsubstituted, and more preferably an unsubstituted and linear alkanediyl group. 1 and W 2 are each independently preferably a single bond, -O-, -S-, -COO-, or -OCOO-, and more preferably a single bond or -O-.
[0072] Examples of the polymerizable liquid crystal compound (B1) include compounds represented by the following formulae (B-1) to (B-25). When the polymerizable liquid crystal compound (B1) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans form. [ka] [ka] [ka] [ka] [ka]
[0073] Among these, at least one selected from the group consisting of compounds represented by formula (B-2), formula (B-3), formula (B-4), formula (B-5), formula (B-6), formula (B-7), formula (B-8), formula (B-13), formula (B-14), formula (B-15), formula (B-16), and formula (B-17) is preferred.
[0074] The exemplified polymerizable liquid crystal compounds can be used alone or in combination. When two or more polymerizable liquid crystal compounds are combined, it is preferable that at least one of them is a polymerizable liquid crystal compound, and it is more preferable that two or more of them are polymerizable liquid crystal compounds. By combining them, liquid crystallinity may be temporarily maintained even at a temperature below the liquid crystal-crystal phase transition temperature. When two polymerizable liquid crystal compounds are combined, the mixing ratio is usually 1:99 to 50:50, preferably 5:95 to 50:50, and more preferably 10:90 to 50:50.
[0075] The polymerizable liquid crystal compound can be produced by a known method such as that described in Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996) and Japanese Patent No. 4719156.
[0076] The content of the polymerizable liquid crystal compound in the solid content of the composition for forming an optically absorptive anisotropic film is preferably 50% by mass or more, more preferably 70% by mass or more, and preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 90% by mass or less. In this specification, the solid content in the composition for forming an optically absorptive anisotropic film refers to the total amount of components excluding volatile components such as solvents from the composition for forming an optically absorptive anisotropic film.
[0077] Examples of the solvent include the same solvents as those described in the "Orientable polymer composition" section, and the content of the solvent is preferably 100 to 1900 parts by mass, more preferably 150 to 900 parts by mass, and even more preferably 180 to 600 parts by mass, relative to 100 parts by mass of the composition for forming an optically absorptive anisotropic film.
[0078] As the polymerization initiator, a photopolymerization initiator is preferable. As the photopolymerization initiator, a photopolymerization initiator having light absorption at a wavelength of 300 nm to 380 nm is usually used. The photopolymerization initiator is a compound capable of initiating a polymerization reaction of a polymerizable liquid crystal compound, and can initiate a polymerization reaction at a lower temperature. Specifically, a photopolymerization initiator capable of generating active radicals or acids by the action of absorbed light can be mentioned, and among them, a photopolymerization initiator that generates radicals by the action of light is preferable.
[0079] Examples of the photopolymerization initiator include a benzoin compound, a benzophenone compound, an alkylphenone compound, an acylphosphine oxide compound, a triazine compound, an iodonium salt, and a sulfonium salt. These polymerization initiators can be used alone or in combination.
[0080] Benzoin compounds include, for example, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.
[0081] Examples of the benzophenone compound include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.
[0082] Examples of the alkylphenone compound include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethan-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.
[0083] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0084] Examples of triazine compounds include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethene.
[0036] 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine.
[0085] Commercially available photopolymerization initiators can be used. Commercially available photopolymerization initiators include "Irgacure (registered trademark) 907", "Irgacure (registered trademark) 184", "Irgacure (registered trademark) 651", "Irgacure (registered trademark) 819", "Irgacure (registered trademark) 250", "Irgacure (registered trademark) 369" (Ciba Japan Co., Ltd.); "Seikuol (registered trademark) BZ", "Seikuol (registered trademark) Z", "Seikuol (registered trademark) 100", "Seikuol (registered trademark) 200", "Seikuol (registered trademark) 1 ... Examples of such compounds include "Kayacure (registered trademark) BEE" (Seiko Chemical Co., Ltd.); "Kayacure (registered trademark) BP100" (Nippon Kayaku Co., Ltd.); "Kayacure (registered trademark) UVI-6992" (Dow Chemicals); "ADEKA Optomer SP-152", "ADEKA Optomer SP-170" (ADEKA Corporation); "TAZ-A", "TAZ-PP" (Nippon SiberHegner Co., Ltd.); and "TAZ-104" (Sanwa Chemical Co., Ltd.).
[0086] The content of the polymerization initiator can be appropriately adjusted according to the type and amount of the polymerizable liquid crystal compound contained in the composition for forming an optically absorptive anisotropic film, but is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, and is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization initiator is equal to or more than the above lower limit, the polymerizable liquid crystal compound can be polymerized without disturbing the alignment. When the content of the polymerization initiator is equal to or less than the above upper limit, the long-term storage stability can be improved, and the occurrence of alignment defects in the obtained polarizing film can be more easily suppressed or prevented.
[0087] The sensitizer is preferably a photosensitizer. Examples of the photosensitizer include xanthone compounds such as xanthone and thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and alkoxy group-containing anthracene (e.g., dibutoxyanthracene); phenothiazine and rubrene. The sensitizer can be used alone or in combination of two or more kinds.
[0088] When the composition for forming an optically absorptive anisotropic film contains a sensitizer, the polymerization reaction of the polymerizable liquid crystal compound contained in the composition can be further promoted. The amount of the sensitizer used can be appropriately adjusted depending on the type and amount of the polymerization initiator and the polymerizable liquid crystal compound, but is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0089] In order to make the polymerization reaction of the composition for forming an optically absorptive anisotropic film proceed more stably, the composition may contain an appropriate amount of a polymerization inhibitor, which makes it easier to control the degree of the polymerization reaction of the polymerizable liquid crystal compound.
[0090] Examples of the polymerization inhibitor include radical scavengers such as hydroquinone, alkoxy group-containing hydroquinone, alkoxy group-containing catechol (e.g., butylcatechol, etc.), pyrogallol, and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenols; β-naphthylamines, and β-naphthols.
[0091] When the composition for forming an optically absorptive anisotropic film contains a polymerization inhibitor, its content can be appropriately adjusted depending on the type and amount of the polymerizable liquid crystal compound, the amount of the sensitizer used, etc., but is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. If the content of the polymerization inhibitor is within this range, the polymerizable liquid crystal compound can be polymerized without disturbing the alignment.
[0092] The optically absorptive anisotropic film-forming composition may contain one or more leveling agents. The leveling agent has the function of adjusting the fluidity of the optically absorptive anisotropic film-forming composition and making the coating film obtained by applying the composition flatter, and specifically includes a surfactant. As the leveling agent, at least one selected from the group consisting of a leveling agent mainly composed of a polyacrylate compound and a leveling agent mainly composed of a fluorine atom-containing compound is preferable.
[0093] Leveling agents based on polyacrylate compounds include "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-358N", "BYK-361N", "BYK-380", "BYK-381" and "BYK-392" [BYK Chemie].
[0094] Leveling agents containing fluorine-containing compounds as the main component include "Megafac (registered trademark) R-08", "R-30", "R-90", "F-410", "F-411", "F-443", "F-445", "F-470", "F-471", "F-477", "F-479", "F-482" and "F-483" [DIC Corporation]; "Surflon (registered trademark) S-381" and "S-3 Examples of such compounds include "82", "S-383", "S-393", "SC-101", "SC-105", "KH-40" and "SA-100" [AGC Seimi Chemical Co., Ltd.]; "E1830", "E5844" [Daikin Fine Chemical Research Institute Ltd.]; "F-TOP EF301", "F-TOP EF303", "F-TOP EF351" and "F-TOP EF352" [Mitsubishi Materials Electronic Chemicals Co., Ltd.].
[0095] When the composition for forming an optically absorptive anisotropic film contains a leveling agent, the content thereof is preferably 0.05 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, the obtained polarizing film tends to be smoother and less prone to unevenness.
[0096] <Polarizing film> The present disclosure includes a polarizing film that is a cured product of the composition for forming a polarizing film. The polarizing film of the present disclosure is a film having a polarizing function, and a dichroic dye is encapsulated in an aligned polymerizable liquid crystal. Since the polarizing film of the present disclosure is formed from the composition for forming a polarizing film, it has little or no alignment defects and has excellent polarizing performance.
[0097] The polarizing film of the present disclosure can be produced, for example, by a method including a step (ii) of forming a coating film of the composition for forming a polarizing film, and drying and removing the organic solvent from the coating film, and a step (iii) of aligning and curing the polymerizable liquid crystal compound in a smectic liquid crystal phase state.
[0098] In step (ii), the composition for forming a polarizing film is applied onto a substrate, an alignment film, or another layer (e.g., a functional layer) described below to form a coating film, and the organic solvent is removed by drying under conditions in which the polymerizable liquid crystal compound contained in the resulting coating film is not polymerized, to obtain a dry film. The polarizing film may be directly applied onto a substrate or another layer (e.g., a functional layer), but it is preferably applied onto an alignment film having alignment regularity.
[0099] In step (ii), the drying method may be, for example, natural drying, ventilation drying, heat drying, or reduced pressure drying. When the polymerizable liquid crystal compound is a polymerizable smectic liquid crystal compound, it is preferable to make the liquid crystal state of the polymerizable smectic liquid crystal compound contained in the dried film a nematic phase (nematic liquid crystal state), and then transfer it to a smectic phase. In order to form a smectic phase via a nematic phase, for example, a method is adopted in which the dried film is heated to a temperature at which the polymerizable smectic liquid crystal compound contained in the dried film transitions to a nematic liquid crystal state, and then cooled to a temperature at which the polymerizable smectic liquid crystal compound shows a smectic liquid crystal state.
[0100] Step (iii) is a step of orienting and curing the polymerizable liquid crystal compound in the dried film in the state of a smectic liquid crystal phase. Hereinafter, a method of photopolymerizing the polymerizable liquid crystal compound while maintaining the liquid crystal state of the smectic phase after the liquid crystal state of the polymerizable liquid crystal compound in the dried film is changed to a smectic phase in step (ii) will be described. In the photopolymerization, the light irradiated to the dried film is appropriately selected according to the type of photopolymerization initiator contained in the dried film, the type of polymerizable liquid crystal compound (particularly, the type of photopolymerizable group possessed by the polymerizable liquid crystal compound) and the amount thereof.
[0101] Specific examples of the light include at least one light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays, and γ-rays, and active electron beams. Among them, ultraviolet light is preferred because it is easy to control the progress of the polymerization reaction and photopolymerization devices widely used in the field can be used. It is preferable to select the type of polymerizable liquid crystal compound and photopolymerization initiator contained in the polymerizable liquid crystal composition so that the composition can be photopolymerized by ultraviolet light. In addition, the polymerization temperature can be controlled by irradiating the dried film with light while cooling it with an appropriate cooling means during polymerization. By adopting such a cooling means, if the polymerization of the polymerizable liquid crystal compound is carried out at a lower temperature, a polarizing film can be appropriately formed even if a substrate having a relatively low heat resistance is used. During photopolymerization, a patterned polarizing film can also be obtained by masking, developing, or the like.
[0102] Examples of the light source of the active energy rays include a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave excited mercury lamp, and a metal halide lamp.
[0103] The UV irradiation intensity is usually 10 to 3,000 mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photopolymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 to 3,000 mJ / cm. 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 It is.
[0104] By carrying out photopolymerization, the polymerizable liquid crystal compound is polymerized while maintaining the liquid crystal state of the smectic phase, preferably the high-order smectic phase, to form a polarizing film. The polarizing film obtained by polymerizing the polymerizable liquid crystal compound while maintaining the liquid crystal state of the smectic phase has an advantage of having higher polarization performance due to the action of the dichroic dye, compared to conventional host-guest type polarizing films, i.e., polarizing films made of a liquid crystal state of a nematic phase. Furthermore, it has an advantage of having superior strength compared to films coated with only a dichroic dye or a lyotropic liquid crystal.
[0105] The thickness of the polarizing film can be appropriately selected depending on the display device to which it is applied, and is preferably 0.1 to 5 μm, more preferably 0.3 to 4 μm, and further preferably 0.5 to 3 μm.
[0106] In the polarizing film 1 as described above, the refractive index difference for visible light between the polarizing film 4 and the alignment film 3 satisfies the following formula (6), and the refractive index difference for visible light between the alignment film 3 and the substrate 2 satisfies the following formula (7). In formula (6), n (polarizing film) represents the refractive index in the transmission axis direction of the polarizing film. |n(polarizing film)-n(alignment film)|≦0.06 …(6) |n(alignment film)-n(substrate)|≦0.06 …(7)
[0107] The refractive index difference between the polarizing film 4 and the alignment film 3 for visible light is preferably 0.04 or less, more preferably 0.02 or less. The refractive index difference between the alignment film 3 and the substrate 2 for visible light is preferably 0.04 or less, more preferably 0.02 or less.
[0108] In such a polarizing film 1, by controlling the refractive index difference between the alignment film 3 and the substrate 2 and between the alignment film 3 and the substrate 2 within the above range, it is possible to suppress the interfacial reflection of incident light between the polarizing film 4 and the alignment film 3 and between the alignment film 3 and the substrate 2. Therefore, it is possible to suppress interference unevenness due to interfacial reflection of incident light.
[0109] In this embodiment, the thickness of the alignment film 3 is 10 nm to 400 nm. In this case, in a polarizing film 1 in which the thickness of the alignment film 3 is in this range, interference unevenness due to interfacial reflection of incident light can be suitably suppressed.
[0110] In this embodiment, a hard coat layer 5 is adjacent to the surface of the substrate 2 opposite the alignment film 3. When producing the polarizing film 1, it is conceivable that the substrate 2 will warp due to shrinkage that occurs when the polarizing film 4 is cured, and wrinkles will occur in the obtained polarizing film 1. In contrast, by providing the substrate 2 with the hard coat layer 5, warping of the substrate 2 due to shrinkage that occurs when the polarizing film 1 is cured can be suppressed, and wrinkles can be suppressed in the obtained polarizing film 1.
[0111] In this embodiment, the substrate 2, the alignment film 3, and the polarizing film 4 are long. That is, in this embodiment, the polarizing film 1 is a long polarizing film 1 that can suppress interference unevenness caused by interfacial reflection of incident light. By continuously bonding polarizing films 1 cut out from the long polarizing film 1 to various display devices, it is possible to efficiently manufacture display devices using the polarizing film 1 in which interference unevenness caused by interfacial reflection of incident light is suppressed.
[0112] In this embodiment, the angle between the longitudinal direction and the slow axis direction of the substrate 2 is 0°±5° or 90°±5°, and the angle between the slow axis direction of the substrate 2 and the absorption axis direction of the polarizing film 4 is 45°±5°. This results in a polarizing film 1 that exhibits high ellipticity.
[0113] [Example] The present disclosure will be described in more detail below with reference to examples. In the following examples, "%" and "parts" are "mass%" and "parts by mass" unless otherwise specified. The configurations and evaluation results of the polarizing films in each example and comparative example are summarized in Figures 2 and 3.
[0114] [Preparation of composition for forming photoalignment film] The following components were mixed, and the resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a photoalignment film (1). Photo-aligned polymer: 2 parts [ka] (Polymer described in JP 2013-033249 A, number average molecular weight: about 28,200, Mw / Mn: 1.82) Solvent: o-xylene 98 parts
[0115] [Preparation of composition for forming polarizing film] The following components were mixed and stirred for 1 hour at 80° C. to obtain a composition for forming a polarizing film (1). The dichroic dye used was an azo dye described in the examples of JP-A-2013-101328. ·Polymerizable liquid crystal compound: A1 90 parts [ka] (A1) ·Polymerizable liquid crystal compound: A2 10 parts [ka] (A2) Dichroic dye: Azo dye A 2.5 parts [ka] Dichroic dye: Azo dye B 2.5 parts [ka] ·Dichroic dye: Azo dye C 2.5 parts [ka] Photopolymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Chiba Specialty Chemicals Co., Ltd.) 6 parts Leveling agent: Polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) 1.2 parts Solvent: 400 parts methyl ethyl ketone
[0116] [Preparation of substrate] A protective film of a cyclic olefin resin (ZEON Corporation, ZEONORFILM ZM series (registered trademark)) was used as the substrate for the polarized film in Examples 1, 3 to 5, and 7. A protective film of a cyclic olefin resin (ZEON Corporation, ZEONORFILM ZT series (registered trademark)) was used as the substrate for the polarized film in Example 2.
[0117] A protective film of a cyclic olefin resin (ZEONORFILM ZD series (registered trademark), manufactured by ZEON Corporation) was used as the substrate of the polarizing film according to Example 6. In the polarizing film according to Comparative Example 1, a uniaxially stretched film WRF-S (modified polycarbonate resin) was used as the substrate. The thickness of the obtained substrate was 50 μm, and the in-plane retardation value at a wavelength of 550 nm was 144.6 nm.
[0118] [Preparation of hard coat layer forming composition] The following components were mixed and stirred at 50° C. for 4 hours to obtain a resin composition (1) for forming a hard coat layer. Polyfunctional acrylate compound having the following structure: 50 parts (dipentaerythritol hexaacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester A-DPH"), the number of atoms in the chain connecting the branch point closest to the acryloyl group in the branched structure to the acryloyl group is 2.) [ka] Urethane acrylate polymer: 50 parts of urethane acrylate (Daicel-Allnex Corporation's "Ebecryl 4858", functional group number 2, weight average molecular weight Mw 450, functional group number per unit molecular weight 44.4 × 10-4) Radical polymerization initiator: 2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane (BASF, "Irgacure 907") 3 parts Solvent: 10 parts methyl ethyl ketone
[0119] [Formation of hard coat layer] The composition for forming a hard coat layer (1) was applied to the substrate by a bar coating method (#2 30 mm / s). The obtained coating film of the composition for forming a hard coat layer (1) was exposed to light at a dose of 500 mJ / cm using a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.). 2 A substrate with a hard coat layer was obtained by irradiating the substrate with ultraviolet light (365 nm standard). The thickness of the hard coat layer was measured with a laser microscope (OLS3000, manufactured by Olympus Corporation) and found to be 1.5 μm.
[0120] [Preparation of polarizing film] After the substrate surface of the substrate with the hard coat layer was subjected to a corona treatment, the composition for forming a photo-alignment film (1) was applied by a bar coating method, and this was dried at 120°C to obtain a dried coating film. Next, the dried coating film was irradiated with polarized UV to form a photo-alignment film, and a laminate having a hard coat layer / substrate / photo-alignment film in this order was obtained. When measured with a laser microscope (OLS3000 manufactured by Olympus Corporation), the thickness of the photo-alignment film was 100 nm in Examples 1 to 3, 6, and 7, and the thickness of the photo-alignment film was 200 nm in Example 4. In addition, the thickness of the photo-alignment film was 400 nm in Example 5. The polarized UV treatment was performed using a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.) under the condition of a measurement intensity of 100 mJ at a wavelength of 365 nm.
[0121] The polarizing film-forming composition (1) was applied to the surface of the photo-alignment film in the obtained laminate by a bar coating method, and the polymerizable liquid crystal compound was subjected to phase transition to a liquid phase by heating and drying for 1 minute in a drying oven at 120°C, and then cooled to room temperature to cause the polymerizable liquid crystal compound to undergo phase transition to a smectic liquid crystal state. Next, a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.) was used to apply an exposure dose of 1000 mJ / cm2. 2 The coating film formed by the polarizing film-forming composition (1) was irradiated with ultraviolet light of wavelength 365 nm (based on 365 nm). As a result, the polymerizable liquid crystal compound contained in the dried coating film was polymerized while maintaining the smectic liquid crystal state of the polymerizable liquid crystal compound, and a polarizing film having a hard coat layer / substrate / photo-alignment film / polarizing film in this order was obtained. When measured with a laser microscope (OLS3000 manufactured by Olympus Corporation), the thickness of the polarizing film was 2.3 μm.
[0122] [Preparation of long polarizing film] Long polarizing films according to each of the Examples and Comparative Examples were continuously produced by a roll to roll method. Long substrates according to each of the Examples and Comparative Examples were continuously unwound, and the surfaces of the substrates were subjected to plasma treatment. Then, a slot die coater was used to discharge the photoalignment film-forming composition (1) onto the center of the substrate to form a first coating film. Furthermore, the substrate on which the first coating film was formed was transported through a ventilated drying oven set at 100°C for 2 minutes to remove the solvent, thereby forming a first dry film. Polarized UV light was irradiated in a predetermined direction at 20 mJ / cm along the longitudinal direction of the substrate on which the first dry film was formed. 2 (based on 313 nm) to impart an alignment control force to the first dried film, thereby forming a long photo-aligned film.
[0123] Next, a composition for forming a polarizing film was discharged onto the center of the obtained long-length photo-alignment film using a slot die coater, forming a second coating film. Furthermore, the substrate on which the second coating film was formed was transported through a ventilated drying oven set at 110°C for 2 minutes to remove the solvent, forming a second dry film. UV light was irradiated to the substrate on which the second dry film was formed at 1000 mJ / cm. 2(365 nm standard) was irradiated to cure the polymerizable liquid crystal compound contained in the second dry film, thereby forming a long polarizing film.
[0124] The film was then continuously wound into a roll to obtain a 200 m long polarizing film according to each Example and Comparative Example. The angle between the longitudinal direction of the long polarizing film and the slow axis direction of the substrate was 0° in Examples 1, 3 to 5, and 7 and Comparative Example 1, 90° in Example 2, and 45° in Example 6. The angle between the longitudinal direction of the long polarizing film and the absorption axis direction of the polarizing film was 45° in Examples 1, 3 to 5, and Comparative Example 1, 45° in Example 2, 0° in Example 6, and 46° in Example 7.
[0125] [Refractive index measurement] The refractive indexes of the substrate, the photo-alignment film, and the hard coat layer (average refractive index at a wavelength of 589 nm) were measured using a refractometer (Multi-wavelength Abbe Refractometer DR-M4 manufactured by Atago Co., Ltd.). The refractive index of the substrate in Examples 1 to 7 was 1.53. The refractive index of the substrate in Comparative Example 1 was 1.62. The refractive index of the photo-alignment film in Examples 1 to 7 and Comparative Example 1 was 1.55. The refractive index of the hard coat layer in Example 3 was 1.53.
[0126] Regarding the refractive index in the transmission axis direction of the polarizing film, a polarizing film sample for evaluating the refractive index for each Example and Comparative Example was prepared as follows. First, a composition for forming a polarizing film for evaluating the refractive index was prepared with a composition excluding the dye. As the substrate, a protective film made of an unstretched cyclic olefin resin having a thickness of 23 μm and an in-plane retardation value of 0 (ZEONORFILM (registered trademark), manufactured by ZEON Corporation) was used. Except for these, a polarizing film sample for evaluating the refractive index for each Example and Comparative Example was formed in the same manner as in the above Example.
[0127] For the polarizing film sample for refractive index evaluation, the front phase difference value and the phase difference value when tilted 40° from the fast axis center were measured by changing the incident angle of light on the sample using an automatic birefringence meter KOBRA-WPR manufactured by Oji Scientific Instruments Co., Ltd. The average refractive index at each wavelength was measured using an ellipsometer M-220 manufactured by JASCO Corporation. The film thickness of the polarizing film was measured using an optical nanogauge film thickness meter C12562-01 manufactured by Hamamatsu Photonics K.K. Based on the obtained front phase difference value, phase difference value when tilted 40° from the fast axis center, average refractive index, and film thickness, the three-dimensional refractive index was calculated with reference to the Oji Scientific Instruments technical documentation (http: / / www.oji-keisoku.co.jp / products / kobra / reference.html).
[0128] The refractive index in the transmission axis direction of the polarizing film in Examples 1 to 7 and Comparative Example 1 was 1.53. As a result, |n(polarizing film)-n(alignment film)| was 0.02 in all of Examples 1 to 7 and Comparative Example 1. Furthermore, |n(alignment film)-n(substrate)| was 0.02 in all of Examples 1 to 7, but |n(alignment film)-n(substrate)| was 0.07 in Comparative Example 1.
[0129] [Visual inspection] Each of the long polarizing films produced in the Examples and Comparative Examples was cut into a 70 mm x 150 mm square, a λ / 4 wave plate was attached to the polarizing film side via a pressure-sensitive adhesive, and an aluminum plate was further attached to the λ / 4 wave plate side via a pressure-sensitive adhesive to obtain a sample for appearance inspection according to each of the Examples and Comparative Examples. The obtained samples for appearance inspection were visually inspected for the presence or absence of interference unevenness from a position inclined 20° from the vertical direction of the front.
[0130] In the visual inspection, samples were rated as follows: "A" was used when the area where interference unevenness was visible was less than 2% of the sample area; "B" was used when the area where interference unevenness was visible was between 2% and less than 5% of the sample area; "C" was used when the area where interference unevenness was visible was between 5% and less than 15% of the sample area; and "D" was used when the area where interference unevenness was visible was 15% or more of the sample area.
[0131] The results were "A" in Examples 1 to 3, 6, and 7, "B" in Example 4, "C" in Example 5, and "D" in Comparative Example 1. From these results, it was confirmed that by suppressing the refractive index difference between the alignment film and the substrate and the refractive index difference between the alignment film and the substrate to 0.06 or less, it is possible to suppress the interfacial reflection of incident light between the polarizing film and the alignment film and between the alignment film and the substrate, and thus it is possible to suppress interference unevenness due to interfacial reflection of incident light in the polarizing film.
[0132] [Curl evaluation] Each of the long polarizing films produced in the Examples and Comparative Examples was cut into a 70 mm x 150 mm square, and a λ / 4 wavelength plate was attached to the polarizing film side with a pressure-sensitive adhesive using a laminator to obtain a curl evaluation sample for each of the Examples and Comparative Examples. The shape of the obtained curl evaluation sample was visually observed.
[0133] In the curl evaluation, since the workability of laminating to a panel is good, a gently convex shape on the substrate side was evaluated as "A", and a flat shape was evaluated as "B". Example 3, in which a hard coat layer is adjacent to the surface opposite to the orientation surface of the substrate, was evaluated as "A", while Examples 1, 2, 4 to 7 and Comparative Example 1, which do not have a hard coat layer, were evaluated as "B".
[0134] [Curling test] Each of the long polarizing films produced in the Examples and Comparative Examples was cut to a width of 50 mm and a length of 300 mm (longitudinal direction), and the film was wrapped around an iron bar with a diameter of 6 mm in the longitudinal direction, and then placed in an oven at 140° C. and left to stand for 3 minutes. Each film was taken out to a room temperature environment, the iron bar was removed, and the curling tendency of each film was confirmed.
[0135] The curl test is a test assuming that a roll of a long polarizing film is stored in a high temperature environment for a long period of time. From the viewpoint of long-term storage stability, in the curl test, a film with a curl in which the central axis in the width direction of the film is parallel to the long side of the film was rated as "A", and a film with a curl in which the central axis in the width direction of the film is not parallel to the long side of the film was rated as "B". As a result, Examples 1 to 5, 7 and Comparative Example 1 were rated as "A", and Example 6 was rated as "B".
[0136] The gist of the present disclosure is as follows: [1] to [5]. [1] A polarizing film comprising a substrate, an alignment film, and a polarizing film laminated in this order, wherein an angle between a slow axis direction of the substrate and an absorption axis direction of the polarizing film is 45°±5°, a refractive index difference between the polarizing film and the alignment film for visible light satisfies the following formula (1), and a refractive index difference between the alignment film and the substrate for visible light satisfies the following formula (2): |n(polarizing film)-n(alignment film)|≦0.06 … (1) |n(alignment film)-n(substrate)|≦0.06 … (2) (In formula (1), n (polarizing film) represents the refractive index in the transmission axis direction of the polarizing film.) [2] The polarizing film according to [1], wherein the alignment film has a thickness of 10 nm to 400 nm. [3] The polarizing film according to [1] or [2], wherein a hard coat layer is adjacent to the surface of the substrate opposite to the alignment film. [4] The polarizing film according to any one of [1] to [3], wherein the substrate, the alignment film, and the polarizing film are long. [5] The polarizing film according to [4], wherein the angle between the longitudinal direction and the slow axis direction of the substrate is 0°±5° or 90°±5°. [Explanation of symbols]
[0137] Reference Signs List 1: polarizing film, 2: substrate, 3: alignment film, 4: polarizing film, 5: hard coat layer.
Claims
1. A polarizing film having a substrate, an alignment film, and a polarizing film laminated in this order, the angle between the slow axis direction of the substrate and the absorption axis direction of the polarizing film is 45°±5°; A polarizing film, wherein a refractive index difference between the polarizing film and the alignment film for visible light satisfies the following formula (1), and a refractive index difference between the alignment film and the substrate for visible light satisfies the following formula (2): |n (polarizing film) - n (alignment film) | ≦ 0.06 ... (1) |n (alignment film)-n (substrate)|≦0.06 ... (2) (In formula (1), n (polarizing film) represents the refractive index in the transmission axis direction of the polarizing film.)
2. The polarizing film according to claim 1 , wherein the thickness of the alignment film is from 10 nm to 400 nm.
3. The polarizing film according to claim 1 , wherein a hard coat layer is adjacent to the surface of the substrate opposite to the alignment film.
4. The polarizing film according to any one of claims 1 to 3, wherein the substrate, the alignment film, and the polarizing film are long.
5. The polarizing film according to claim 4 , wherein an angle between the longitudinal direction and the slow axis direction of the substrate is 0°±5° or 90°±5°.
Citation Information
Patent Citations
Dichroic Guest-Host Polarizers Containing Oriented Polymer Films
JP2007510946A